Heat dissipation insulation plate having both high heat dissipation property and high electric insulation property
The use of highly heat-resistant thermoplastic resin and oriented thermally conductive filler particles in a composite insulating board addresses the challenge of achieving both high thermal conductivity and dielectric breakdown strength, enabling effective heat dissipation and insulation in high-temperature environments.
Patent Information
- Application Number
- JP2023082699
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
AI Technical Summary
Existing composite insulating boards fail to achieve both high thermal conductivity and dielectric breakdown strength, with most materials either having insufficient thermal conductivity or dielectric breakdown strength, limiting their application in high-temperature environments like SiC power modules.
A method involving highly heat-resistant thermoplastic resin and plate-shaped thermally conductive filler particles, such as boron nitride, oriented to enhance thermal conductivity and dielectric breakdown strength, using a manufacturing process that includes particle size adjustment, electrostatic adsorption, and controlled orientation through centrifugal forces to create a dense, oriented structure.
The resulting composite insulating board achieves thermal conductivity of 35 W/m·K or more with dielectric breakdown strength of 95 kV/mm or higher, suitable for high-temperature applications like SiC power modules, offering improved heat dissipation and electrical insulation.
Smart Images

Figure 2024166537000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite insulating board containing a thermally conductive filler and a thermoplastic resin, and a method for producing the same. More specifically, a composite material having high thermal conductivity, high insulation and high heat resistance is provided. The present invention relates to an insulating plate and a method for manufacturing the same. [Background technology]
[0002] New powertrains such as hybrid vehicles, electric vehicles, and fuel cell vehicles use storage batteries. In order to operate the drive motor with a DC power source, the DC is converted to AC by an inverter. In addition, in order to recover regenerative energy, a converter converts AC to DC and stores the energy. Power modules such as IGBTs are used in AC / DC converters like these. The on-resistance of the semiconductor generates heat, but this must be kept below the junction temperature of the semiconductor element. Therefore, cooling by air or water is required. The junction temperature is In this case, the temperature is about 150°C, but considering the thermal degradation of the element, the temperature of the element during operation is usually 75 to 80°C. The heat dissipation design is such that the temperature can be kept at around 5℃. In the case of water cooling, Instead of heat sink fins, a water-cooled jacket with a conduit for passing a cooling medium through an insulating substrate is used. It is joined to the power module. Therefore, the insulating substrate has good thermal conductivity in the thickness direction. The higher the dielectric breakdown strength, the higher the required withstand voltage. The thickness of the insulating substrate can be made thinner, improving heat transfer. The insulating substrate used is a rigid substrate that does not bend or break easily, e.g. For example, the thickness is about 100 μm to 1 mm. Ceramic plates such as silicon nitride, which have high thermal conductivity, are used, but from the perspective of reducing costs, Therefore, there is a demand for thinner substrate thicknesses.
[0003] However, due to the difficulty of manufacturing and the problem of mechanical strength, the ceramic plate is not being made thinner. Therefore, instead of this, a new type of insulation consisting of polymer insulating material and filler is being developed. Research and development of insulating substrates (composite insulating plates) using composite insulating materials is being carried out in various places.
[0004] Many of the composite insulating materials currently being developed are based on thermosetting resins such as epoxy resins. It is made by mechanically mixing inorganic fillers such as alumina, which has a higher thermal conductivity than resin. can be.
[0005] The filler should have high thermal conductivity and thermal diffusivity, and should have electrical properties such as The higher the volume resistivity and dielectric breakdown strength, the better. Alumina is a common choice because of its
[0006] In such a composite insulating board, the gaps between the alumina filler particles due to contact between the particles form a conductive layer. The uneven distribution of alumina filler particles is a weak point in electrical insulation due to the difference in dielectric constant with the resin. Since field concentration occurs and the insulation performance is reduced, there is no substitute for ceramic plates. In order to solve these problems, research is being conducted to improve the dispersibility of filler particles and Research using nanoparticles has also been conducted, and composite insulation with a thermal conductivity of about 6 to 12 W / m K has been developed. A plate has been developed (Non-Patent Document 1).
[0007] In addition to alumina, inorganic fillers include aluminum nitride (AlN) and silicon nitride (S Among these, BN is a hexagonal crystal with a high volume resistivity. Its thermal conductivity is 15 to 30 W / m K, which is equivalent to that of alumina. Although there is anisotropy depending on the crystal direction, it shows a value 2 to 10 times higher (60 to 200 W / m K). Aluminum nitride has good thermal conductivity with a thermal conductivity of 150 to 200 W / m K. However, it is extremely expensive. For this reason, BN is used as a composite material, although it has anisotropic thermal conductivity. Research is being conducted in various places to utilize it as a filler for insulating plates (Non-Patent Document 2).
[0008] For example, the techniques disclosed in Patent Document 1 and Non-Patent Document 3 use a thermally-insulated resin such as an epoxy resin. BN is mixed with a curable resin in a liquid state before curing, kneaded, and then cured to create a composite insulating board. When producing the film, the BN is oriented along the electric field by applying an electric field while in a liquid state before hardening. This shows the law.
[0009] In addition, in the above-mentioned Non-Patent Document 4, a composite insulating plate is made using a thermoplastic resin as an insulating base material. This is also being attempted. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2013-159748 A [Patent Document 2] JP 2017-37833 A [Patent Document 3] Patent No. 7174973 [Patent Document 4] JP 2019-153575 A [Non-patent literature]
[0011] [Non-Patent Document 1] Wang, et al.: IEEE Trans. on DEI, 18(6), “Development of Epoxy / BN Composites with High Thermal Conductivity and Sufficient Dielectric Breakdown Strength” pp.1963-1972(2011) [Non-Patent Document 2] X.Huang, et al.: IEEJ Trans on FM,133(6), “Boron Nitride Based Poly(phenylene sulfide) Composites with Enhanced Thermal Conductivity and Breakdown Strength”, IEEJ Transactions on Fundamentals and Materials, Vol.133, No.3, pp.66-70(2013) [Non-Patent Document 3] Kosako et al.: Proceedings of the 44th Electrical and Electronic Insulating Materials System Symposium, "Reduction of Filler Loading Ratio in Filler-Oriented Epoxy Composites by AC Electric Field", pp. 47-51 (2011) [Non-Patent Document 4] Imai, et al.: Proceedings of the 44th Electrical and Electronic Insulating Materials System Symposium, "Materials Design of Composite Dielectric Materials for High-Frequency Applications," pp. 37-40 (2011) Summary of the Invention [Problem to be solved by the invention]
[0012] However, in the methods of Patent Document 1 and Non-Patent Document 3, the epoxy resin is The kinetic viscosity is at least 10 centistokes, and the BN is highly viscous and almost completely oriented by the electric field. Furthermore, in the above-mentioned Non-Patent Document 1, BN is added to the liquid state of epoxy resin before it is cured. However, due to the viscosity of the liquid, the particles are not oriented. It is not possible to do so.
[0013] In the composite insulating boards disclosed in Non-Patent Documents 1 and 2, the dielectric breakdown strength is 1, which meets the market demand. Those exceeding 0.1 kV / mm have a thermal conductivity of 1 W / m K or less and do not meet the market demand of 10 W. / m K. On the other hand, materials with a thermal conductivity of more than 10 W / m K are The dielectric breakdown strength is 60kV / mm, which is lower than the market requirement. However, no material has been obtained that satisfies both the requirements for dielectric breakdown strength and the requirements for dielectric breakdown strength.
[0014] Furthermore, in the above-mentioned Non-Patent Document 4, a composite insulating plate is made using a thermoplastic resin as an insulating base material. Attempts have also been made to use polypropylene as the thermoplastic resin and heat it above its thermoplastic temperature. A method has been proposed in which BN is melt-kneaded after heating and then injection-molded, but the thermoplastic nature of the molten state Resin has such high viscosity that it is difficult to achieve the orientation by the electric field or centrifugal force mentioned above, and it is difficult to disperse BN uniformly. Advanced manufacturing techniques are required.
[0015] In Patent Document 2, a composite insulating plate having both good thermal conductivity and sufficient insulation properties as described above is disclosed. Considering that the thermal conductive filler has not yet been provided, By controlling the filling rate appropriately and improving the packing density, good thermal conductivity and sufficient dielectric breakdown strength are achieved. However, the present invention relates to a composite insulating board having a certain degree of rigidity and a method for manufacturing the same. In order to increase the degree of freedom, it is necessary to develop an insulating material that has both high thermal conductivity and high dielectric breakdown strength. For example, in the case of SiC power modules, the maximum operating temperature is Since the temperature reaches about 200℃, it is required to have high heat resistance exceeding 200℃. It is being done.
[0016] In Patent Document 3, the present inventors have reported a method for producing a material having a higher thermal conductivity and a higher thermal conductivity than conventional materials by using an electrostatic adsorption method. We propose a manufacturing method for a high heat resistance composite material with high dielectric breakdown strength. A thermoplastic resin and plate-shaped thermally conductive filler particles having a higher thermal conductivity than the high heat resistant thermoplastic resin. A composite insulating board including a dielectric layer and a dielectric constant layer having a thermal conductivity of 15 W / m K in the thickness direction of the composite insulating board. A composite insulating plate in which the thermally conductive filler particles are oriented so that the thermal conductivity is 35 W / m K or less. The dielectric breakdown strength of the composite insulating board in the thickness direction is 95 kV / mm or more. The present invention proposes a method for manufacturing a composite insulating board having the above-mentioned features.
[0017] In addition, the present inventors disclosed in Patent Document 4 (JP 2019-153575 A) that a heat-resistant thermoplastic resin is The insulating material is a thermoplastic polyimide, and the thermally conductive filler particles are boron nitride. It is characterized by an average breaking strength of 200 kV / mm and a thermal conductivity of 11 W / m K. The composite insulating plate has an average dielectric breakdown strength of 80 kV / mm and a thermal conductivity of 42 W / We proposed a manufacturing method for a composite insulating board characterized by a thermal conductivity of 1.0 m K.
[0018] However, we are currently working on the creation of a heat-dissipating, electrically insulating substrate that meets the requirements for future electrical and thermal properties. In order to increase the freedom of module design, we have developed a new type of module that has higher thermal conductivity and is highly flexible. There is a need for composite materials that have the required level of dielectric breakdown strength.
[0019] The present invention has been made in view of the above problems, and its object is to provide a high-temperature The present invention provides a method for producing a composite insulating board having both electrical conductivity and high insulating properties. [Means for solving the problem]
[0020] The above object of the present invention is achieved by the following means.
[0021] 1. A high heat resistant thermoplastic resin and a plate-shaped heat conductive material having a higher thermal conductivity than the high heat resistant thermoplastic resin. In a composite insulating board containing conductive filler particles, the thermal conductivity in the thickness direction of the composite insulating board is The thermally conductive filler particles are oriented so that the thermal conductivity is between 35W / m K and 45W / m K. A composite insulating board having a dielectric breakdown strength of 95 kV / A composite insulating board having a thickness of 1.0 mm or more.
[0022] 2. A high heat resistant thermoplastic resin and a plate-shaped heat conductive material having a higher thermal conductivity than the high heat resistant thermoplastic resin. In a composite insulating board containing conductive filler particles, the thermal conductivity in the thickness direction of the composite insulating board is The thermally conductive filler particles are oriented so that the thermal conductivity is between 5 W / m K and 10 W / m K. A composite insulating plate having a dielectric breakdown strength of 200 kV / A composite insulating board having a thickness of 1.0 mm or more.
[0023] 3. The method according to claim 1, wherein the highly heat-resistant thermoplastic resin is a thermoplastic polyimide. 3. A composite insulating board according to claim 2.
[0024] 4. The method according to any one of claims 1 to 3, characterized in that the thermally conductive filler particles are boron nitride. Composite insulating board.
[0025] 5. The composite particles used in the composite insulating board include high heat resistant thermoplastic resin particles and the high heat resistant Composite particles containing plate-shaped thermally conductive filler particles having higher thermal conductivity than thermal thermoplastic resin particles. and the highly heat-resistant thermoplastic resin particles are adsorbed to the thermally conductive filler particles.
[0026] 6. The method according to claim 5, wherein the highly heat-resistant thermoplastic resin is a thermoplastic polyimide. The composite microparticles described herein.
[0027] 7. The method according to claim 5 or 6, wherein the thermally conductive filler particles are boron nitride. Composite microparticles.
[0028] 8. A crushing step of crushing the high heat resistant thermoplastic resin to reduce its diameter; Among the high heat resistant thermoplastic resin particles crushed by the method, only the thermoplastic particles having a desired particle size or less are crushed. a selection step of selecting the high-temperature filler having the thermally conductive filler material as a main particle and having an adjusted particle size; and adsorbing heat-resistant thermoplastic resin particles onto the surfaces of the primary particles. A method for producing particles.
[0029] 9. The thermally conductive filler particles are used as main particles, and the high heat resistant thermoplastic resin particles are used as the main particles. 8. The method according to claim 8, further comprising the step of subjecting the entire surface of the substrate to a cleaning treatment after the step of adsorbing the polymer on the substrate. A method for producing the composite particles described above.
[0030] 10. A particle size adjustment process for adjusting the particle size of high heat resistant thermoplastic resin and thermal conductive filler particles The main particles are the nuclei, and the particle size on the surface of the main particles is adjusted through a particle size adjustment process. The composite particles having the thermoplastic resin particles adsorbed thereon are contained in a liquid. A slurry preparation step of preparing a slurry having a viscosity lower than the melt viscosity of the thermoplastic resin; The slurry produced in the slurry producing step is introduced into a cavity having a volume of An introduction step, and applying centrifugal force in a predetermined direction to the slurry introduced into the cavity in the introduction step. By this action, the composite particles are separated from the liquid by solid-liquid separation while forming a cavity. a centrifugal separation step of depositing the particles on a plane intersecting the direction of the centrifugal force; The composite particles are deposited in the cavity by the centrifugal force in the same direction as the centrifugal force. a pressing step of pressing the molded body in the same direction to form a molded body; The high heat resistant thermoplastic resin particles are removed from the cavity, and the high heat resistant thermoplastic resin particles are heated to a temperature equal to or lower than the melting point of the resin constituting the high heat resistant thermoplastic resin particles. In the above environment, a hot pressing process is performed in a direction intersecting the pressing direction in the pressing process. and a step of manufacturing a composite insulating board.
[0031] 11. The particle size adjusting step comprises at least breaking the high heat resistant thermoplastic resin to reduce its particle size. 11. A method for producing a composite insulating board as described in 10 above, further comprising a crushing step.
[0032] 12. The particle size adjusting step comprises at least breaking the high heat resistant thermoplastic resin to reduce its particle size. A crushing step of crushing the high heat resistant thermoplastic resin particles, and selecting only thermoplastic particles having a desired particle size or smaller. A method for producing the composite insulating board described above.
[0033] 13. In the slurry preparation process, the composite particles are washed, and then the high heat resistance heat The method of claim 1, further comprising the step of preparing a slurry having a viscosity lower than the melt viscosity of the plastic resin. 13. A method for producing a composite insulating board as described in claim 12. Effect of the Invention
[0034] According to the composite insulating board of the present invention, the thermal conductivity in the thickness direction of the composite insulating board is 35 W / m K or more. The thermal conductive filler particles are oriented in the direction of heat transfer so that the thermal conductivity is 45 W / m K or less. Here, the improvement of the degree of orientation can improve the thermal conductivity in the thickness direction. The degree of orientation of the material is set to a thermal conductivity of 35 W / m K or less, which reduces the decrease in dielectric breakdown strength. Therefore, it is possible to suppress the thermal conductivity of 95 kV / mm or more while maintaining good thermal conductivity in the thickness direction. This has the effect of providing a composite insulating board having a dielectric breakdown strength of
[0035] According to the method for producing a composite insulating board of the present invention, a slurry containing composite particles in a liquid is heated to a predetermined temperature. The material is introduced into a cavity having a volume of 100 mm and centrifugal force is applied in a predetermined direction to solidify the material. The composite particles are separated from the liquid by liquid separation while the centrifugal force in the cavity acts in the direction of the composite particles. The particles are then pressed in the direction of centrifugal force to form composite particles. Secondly, the temperature is increased by 100°C to 300°C, which is the temperature at which the thermoplastic resin melts. The thickness of the composite insulating board is increased by pressing the molded body in the direction perpendicular to the centrifugal force at a high temperature. The distance between individual thermally conductive filler particles is shortened in the direction, and there are no voids on the outer surface of the particles. It is also coated with thermoplastic resin, providing a composite material with good thermal conductivity and sufficient dielectric breakdown strength. This has the effect of providing an insulating plate. [Brief description of the drawings]
[0036] [Figure 1] FIG. 2 is a schematic cross-sectional view of a composite insulating plate. [Diagram 2] 1A to 1C are diagrams showing a process for producing a composite insulating board. [Diagram 3] FIG. 13 is a schematic diagram of a molded body released from a mold in the demolding step S5. [Figure 4] FIG. 1 is a diagram showing the relationship between thermal conductivity and dielectric breakdown strength of various composite insulating boards. [Diagram 5] FIG. 1 is a diagram showing the relationship between thermal conductivity and dielectric breakdown strength of various composite insulating boards. [Figure 6] 1 is an electron microscope photograph of a composite particle. [Figure 7] FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0037] Hereinafter, an embodiment of the present invention will be described in detail.
[0038] One embodiment of the composite insulating plate is a plate-shaped thermally conductive filler in a matrix of high heat resistant thermoplastic resin. The particles are dispersed.
[0039] The high heat resistant thermoplastic resin contained in the composite insulating board has insulating properties and its volume resistivity is 1 0 15 In addition, the maximum operating temperature of SiC power modules is 200°C. In the present invention, the high heat-resistant thermoplastic resin is a thermoplastic resin having a heat-resistant temperature of more than 200°C. It is a thermoplastic resin with a glass transition temperature of 200°C or higher. Examples of thermoplastic resins that can withstand temperatures above 00°C include polyamide-imide (PAI), ... and polyamide-imide (PAI). Polyethersulfone (PES), polyimide (PI), etc. Polyimide is most preferably used in this case. Generally, polyimide does not have thermoplasticity. However, the polyimide that can be used in the present invention is a thermoplastic polyimide. The polyimide is not particularly limited as long as it has thermoplastic properties. A thermoplastic resin having a repeating structural unit of the chemical formula (1) described in US Pat. No. 5,399,242. Polyimide resin, thermoplastic polyimide resin having a repeating structural unit of chemical formula (3), Thermoplastic polyimide resin having repeating structural units of chemical formula (4) and chemical formula (5), A thermoplastic polyimide resin having a repeating structural unit of the formula (6) is preferably used. The most preferred is a thermoplastic polyimide resin having a repeating structural unit of the chemical formula (3). The thermoplastic polyimide having a repeating structural unit represented by the chemical formula (3) can be easily used. As the resin, a commercially available product manufactured by Mitsui Chemicals, Inc. under the trade name AURUM can be used.
[0040] By using such highly heat-resistant thermoplastic resins, This is not possible with a simple replacement of thermoplastic resins with low heat resistance as in Patent Document 2. It has been found that a composite insulating board having both good thermal conductivity and high dielectric breakdown strength can be provided. It has come.
[0041] The mechanism by which this excellent thermal conductivity and dielectric breakdown strength can be achieved has been described, for example, by The topless process is carried out at a temperature higher than the glass transition temperature of the thermoplastic resin. Thermoplastic resins exhibit relatively small changes in softening at temperatures above their glass transition temperature, and The thermally conductive filler particles are more stably distributed because they are less susceptible to temperature fluctuations. Furthermore, the particle size of the high heat resistant thermoplastic resin particles can be adjusted. I believe this is a synergistic effect.
[0042] Furthermore, since such a high heat resistant thermoplastic resin has sufficient heat resistance, The insulating plate is made of SiC, which has a maximum operating temperature of about 200°C, which was not possible with previous technology. It can also be used as a power module.
[0043] The thermally conductive filler particles contained in the composite insulating board preferably have a high thermal conductivity and a high thermal diffusivity. In terms of electricity, the higher the specific volume resistivity and dielectric breakdown strength, the better.
[0044] Generally, thermally conductive filler particles are made of alumina (Al2O3), silica (SiO2) and alumina. Hydrate (Al2O3·H2O), titanium oxide (TiO2), aluminum nitride (AlN), boron nitride (BN), Examples include silicon nitride (SiC), and any of these can be used in the present invention.
[0045] Here, the thermally conductive filler particles used in this embodiment have a plate-like particle shape. The term "plate-like" refers to a particle having a diameter to thickness ratio of 2 or more, and is more preferred. In general, this ratio is 5 or more. For example, particles having a layered crystal structure tend to become plate-like. In addition, the thermally conductive filler particles may be made of particles having different thermal conductivity. The "anisotropy of thermal conduction" refers to the in-plane direction of the plate-like thermally conductive filler particles. The thermal conductivity of the thermally conductive filler particles varies depending on the thickness direction. As the density of the insulating plate increases, gaps appear between the particles, and the density of the insulating plate does not increase. Thermal conductivity does not increase. In addition, as the average particle size becomes smaller, the packing density increases, but the matrix The number of interfaces with the material increases, which leads to a decrease in insulation performance. The diameter is 0.5 μm to 60 μm, and more preferably, the average particle diameter is 20 μm to 5 0 μm is used.
[0046] Any of the above-mentioned thermally conductive filler particles can be used in the present invention, but most Preferably, hexagonal boron nitride (hereinafter referred to as BN) can be used. The crystal structure of BN particles is a layered crystal. Since the BN particles are cleaved along the crystal plane, they become plate-shaped. The diameter is 0.5 to 60 μm, and the thickness is about 0.1 to 3 μm. The volume resistivity of BN is generally The thermal conductivity of BN is twice as high as that of alumina in the thickness direction. It is 10 times larger in the in-plane direction.
[0047] In this embodiment, the particle size of the thermally conductive filler particles is measured by a laser diffraction scattering method. For example, a laser scattering particle size measuring device (Shimadzu Corporation, SAL The particle size distribution was measured using a 50% cumulative distribution (D-3100), and the particle size at 50% cumulative distribution (D50) was calculated. This is called the "average particle size."
[0048] Although not particularly limited, a specific example of BN of the present invention is "PT-110 (trade name) ) (manufactured by Momentive Performance Materials Japan, LLC, average particle size 45 In addition to this, plate-shaped thermally conductive filler particles can be crushed and disintegrated to obtain the desired size. Particles of a constant average size can be obtained.
[0049] It is preferable to adjust the particle size of the highly heat-resistant thermoplastic resin. The method for crushing the particles is not particularly limited, but a crushing method is preferably used. For example, a method using a bead mill, a roll mill, or a freeze-grinding method can be used. In addition, it is also possible to use a method for selecting only thermoplastic particles with a desired particle size or smaller. As a method for selecting only thermoplastic particles having a desired particle size or less, Known methods can be used, for example, centrifugation and sieving. .
[0050] The blending amount of the thermally conductive filler particles in the composite insulating board is in the range of 40 to 90% by volume. If the amount of the thermally conductive filler particles is less than 40% by volume, sufficient thermal conductivity cannot be obtained. If the amount is more than 90% by volume, the thermoplastic resin on the outer surface of the thermally conductive filler particles will be insufficient, resulting in poor insulation. The composite insulating board will have insufficient breaking strength. The preferred blending amount is in the range of 55 to 80 volume percent. do.
[0051] High heat resistance By adjusting the particle size of the thermoplastic resin particles, the thermally conductive filler particles can be made highly heat resistant. The thermoplastic resin particles are tightly adhered and the thermally conductive filler particles are densely oriented. This makes it possible to set a higher content of thermally conductive filler particles, resulting in higher thermal conductivity. This is also a feature and advantage of the present invention.
[0052] FIG. 1 is a schematic diagram of a cross section of a composite insulating board according to the present embodiment. The upper side of the paper is shown as the surface of the composite insulating board.
[0053] Such a composite insulating board has thermally conductive filler particles 1 dispersed in a thermoplastic resin 2, The filler particles are coated with the thermoplastic resin, adhered to each other, and present in the thermoplastic resin. When in use, it is set so that both sides are in contact with the semiconductor element and the heat dissipation fins. When in use, the direction of the arrow in Figure 1 is the direction in which the electric field is applied. The in-plane direction of the thermally conductive filler particles 1 is set to a predetermined value with respect to the desired direction (thickness direction of the composite insulating board). The orientation is in the range of the orientation degree.
[0054] In this embodiment, the "degree of orientation" of the thermally conductive filler particles constituting the composite insulating board The thickness direction (vertical direction) of the composite insulation board is taken as the standard and the plate-shaped thermally conductive filler particles How much each in-plane direction of the molecule 1 is tilted (aligned) with respect to the thickness direction In other words, it is an index showing the alignment of the thermally conductive filler particles 1 in the direction in which heat is to be propagated. The degree of thermal conductivity is specified by the thermal conductivity of the composite insulating board. The angle formed with respect to the plate surface of the composite insulation board is determined by the individual thermally conductive fillers present in the composite insulation board. The thermal resistance per unit volume in the thickness direction of the composite insulating plate is not constant for each particle. The thermal resistance of the thermally conductive filler particles present in the volume and the thermal elasticity of the filler particles filling the gaps between the thermally conductive filler particles are The thermal resistance of the plastic resin can be calculated by the series and parallel combination. If the amount of filler is the same, the thermal conductivity of the composite insulation board is determined by the amount of the thermally conductive filler particles in the composite insulation board. There is a certain relationship with the overall orientation degree. Therefore, the orientation degree of the thermally conductive filler particles in the composite insulating board is , can be expressed as the thermal conductivity of the composite insulating plate.
[0055] This relationship also depends on the amount of thermally conductive filler particles mixed, and the dielectric breakdown strength also depends on the amount of thermally conductive filler particles mixed. Since the amount of material particles mixed depends on the orientation, the thermal conductivity and dielectric breakdown strength are can be expressed.
[0056] The thermal conductivity can be adjusted, for example, by adjusting the particle size of the highly heat-resistant thermoplastic resin. By reducing the number of coarse particles, the thermal conductivity becomes higher. It will be a little lower.
[0057] The orientation of the thermally conductive filler particles in the composite insulation board of this embodiment is such that the thermal conductivity of the composite insulation board is 3 The degree of orientation is between 5W / m K and 45W / m K. Thermal conductivity is 15W / m K. With the degree of orientation below this, the thermal conductivity of the composite insulating board may be insufficient depending on the application. In the orientation where the thermal conductivity is 35 W / m K or more, the dielectric breakdown strength of the composite insulating board gradually It gets worse.
[0058] The density of the composite insulating board of this embodiment is 1.7 g / cm 3 That's it. 1.7g / cm 3 below In this case, the thermal conductivity of the composite insulating plate is insufficient.
[0059] The thermally conductive filler particles and thermoplastic resin in the composite insulating board each have their own inherent dielectric breakdown strength. However, due to the difference in the dielectric constant between the two, there is a distortion of the electric field at the interface, and the electric field is high. This creates weak points in insulation. Since the in-plane direction of the thermally conductive filler particles is oriented in the electric field direction, the particle interfaces are continuous. On the other hand, by increasing the degree of orientation, the thermal conductivity is improved. As described above, the degree of orientation is a trade-off between these two properties, so the dielectric breakdown strength must be sufficient and the thermal conductivity must be good. The conditions of the manufacturing method of the present invention are appropriately controlled to obtain a degree of orientation that is appropriate for the intended use. It is possible to provide a composite insulating board that exhibits the required dielectric breakdown strength and thermal conductivity.
[0060] The method for producing the above-mentioned composite insulating board is also within the scope of the present invention.
[0061] A method for manufacturing a composite insulating board according to an embodiment of the present invention will be described with reference to FIGS. It should be noted that the following embodiment is merely an example of the present invention and does not change the gist of the present invention. It goes without saying that the embodiment can be modified as appropriate without departing from the scope of the present invention.
[0062] FIG. 2 is a process diagram showing a method for producing a composite insulating board according to the first embodiment. Particle size adjustment process (P) to adjust the particle size of the heat-resistant thermoplastic resin, A slurry process for producing a slurry containing composite particles on which a thermoplastic resin is adsorbed and composited. Step (S1), introduction step (S2) of introducing the slurry in which the composite particles are dispersed into the mold, A centrifugation process (S3) in which the composite particles are precipitated by centrifugal force to separate the solid and liquid, and the precipitated sediment A pressing process (S4) is performed to pressurize the molded body, a demolding process (S5) is performed to remove the molded body from the mold, and the molded body is It is manufactured through a hot pressing process (S6) in which pressure is applied while heating.
[0063] The composite particles used in the manufacturing method of this embodiment may be prepared in advance. In this embodiment, the manufacturing process includes a composite particle preparation process (S0). The method for producing a composite insulating board is also provided. In the embodiment, the manufacturing method (P) is provided. A method for manufacturing a composite insulating board is configured.
[0064] The composite particles used in the composite insulating board and the method for producing the composite particles are also within the scope of the present invention. do.
[0065] The composite particles used in this manufacturing process have a larger particle size on the surface of the main particle (a particle with a larger particle size) than the main particle. The small particles are adsorbed to the surface of the substrate, and the particles are integrated as a single particle. The main particles are thermally conductive filler particles, and the adsorption particles are made of a high heat resistant thermoplastic resin. It is a fat particle.
[0066] The composite particles are made of thermally conductive filler particles, which are the main particles, and thermoplastic resin particles, which are the adsorption particles. The relationship between the average particle size of each material greatly affects the dielectric breakdown strength and thermal conductivity of the composite insulating board. The particle size adjustment process (P) for adjusting the particle size of the high heat resistant thermoplastic resin is In the process for adjusting the particle size of the resin to the above-mentioned preferred range, for example, the thermoplastic resin is crushed. The crushed particles are then subjected to a predetermined It is preferable to carry out a step (P1) of selecting the size of the powder.
[0067] In the composite particle preparation process (S0), the surface of the main particle (thermally conductive filler particle) with a larger particle diameter is The smaller particle (thermoplastic resin particle) is adsorbed as the adsorbent particle to form a composite particle. In this embodiment, the surface charge of the adsorption particles and the thermally conductive filler particles are The surface charges of the particles are adjusted to be opposite to each other, and then the two particles are placed in a liquid. By mixing, the thermoplastic resin particles (adsorbent particles) are attached to the thermally conductive filler particles (main particles) by electrostatic attraction. The adsorbent particles are adsorbed onto the surface of the substrate.
[0068] Here, the surface charge of the adsorbed particles is adjusted to be negative, and the surface charge of the main particles is adjusted to be positive. The surface charge of the adsorbent particles is adjusted to be positive, and the surface charge of the main particles is adjusted to be negative. is also good.
[0069] Specifically, in order to increase the hydrophilicity and the negative surface potential, the surface is adsorbed to a surfactant. The particles were then soaked in two different polyelectrolyte solutions in turn. The concentration of each solution is sufficient for the entire surface of the adsorbent particles to be adsorbed. Before immersion, the adsorbent particles were washed in ion-exchanged water. The potential was adjusted to be negative. On the other hand, the surface potential of the thermally conductive filler particles was finally adjusted to be positive in a similar manner. The adsorbed particles with a negative surface potential and the main particles with a positive surface potential were Composite particles in which the adsorbent particles are adsorbed onto the main particle surface through electrostatic interaction after mixing in ion-exchanged water. was prepared.
[0070] The composite particles thus produced are treated in a slurry process (S1) described below by dissolving the composite particles in a low viscosity liquid. In a more preferred embodiment, the composite particles are washed before being mixed with the body to form a slurry. The specific cleaning method is to use adsorbed particles with a negative surface potential and The main particles with positive potential were mixed in ion-exchanged water and thoroughly stirred to adsorb the particles. Leave it for a while until the particles settle. When the particles have settled, do not discharge the composite particles. Carefully discard the supernatant. Add ion-exchanged water and stir thoroughly. The above procedure is repeated 2 to 6 times. By this procedure, the thermoplastic resin with large particle size is selectively removed. The particles are released, and composite particles are formed in which the thermoplastic resin particles having smaller particle sizes are firmly adsorbed.
[0071] The slurry process (S1) is a process in which composite particles are mixed with a low viscosity liquid to form a slurry. In this process, the composite particles are slurried using a low-viscosity liquid that does not dissolve them, allowing the particles to be slurried under low centrifugal force. The composite particles can be easily densified by using ionic substances as the solvent. It is desirable to use a low-viscosity liquid with a kinetic viscosity of less than 1 centimeter at room temperature. The viscosity is about Tokes or less. Ion-exchanged water is preferable.
[0072] The introduction step (S2) is a step of putting the slurry made in the step S1 into a mold. In this embodiment, the mold is a bottomed container with an open top, preferably In the above embodiment, a flat plate is used.
[0073] The centrifugal separation step (S3) applies centrifugal force to orient the composite particles and separate them into solid and liquid. The centrifugal force is calculated as follows: Centrifugal force = (rotation speed) x (distance from the center of rotation to the composite particle) x (The weight of the composite particles) is calculated. Centrifugal force is applied to the slurry introduced into the cavity. By this, the composite particles of the slurry are separated from the liquid while crossing the direction of the centrifugal force. The composite particles are dispersed in a low viscosity liquid such as water to form a slurry. The composite particles are easily precipitated by centrifugal force, and the composite particles are easily precipitated by centrifugal force. The orientation of the molecules can be improved.
[0074] Instead of dispersing it in a low-viscosity liquid, it is simply placed in a mold in a dry powder state and subjected to mechanical pressure only. There is a method to increase the density of the composite particles, but the composite particles are difficult to move with each other and the composite particles are not oriented. Furthermore, gaps are likely to form between the particles, preventing a dense structure.
[0075] On the other hand, according to the present manufacturing method, in the centrifugation step (S3), centrifugal force is applied to the mold. The composite particles are then oriented and settled so that the plate surface of the composite particles intersects the direction of centrifugal force. This causes the water to settle and form sediments.
[0076] The pressing step (S4) is a step of applying centrifugal force to the sediment produced in the centrifugal separation step (S3). In the previous centrifugation process (S3), the Only the centrifugal force determined by the weight of the composite particles can be applied to the composite particles. In order to further increase the density of the deposits, mechanical pressure is applied in the same direction as the centrifugal force. There is a process in place.
[0077] The demolding step (S5) is a step of removing the molded body produced in the pressing step (S4) from the mold. FIG. 3 is a schematic diagram of the compact taken out. The compact is in a state where the composite particles are in agglomerated form. The plate surface of the thermally conductive filler particles constituting the composite particle is aligned with the bottom surface of the molded body. It is an attitude.
[0078] The hot pressing process (S6) is performed in the direction crossing the centrifugal force (shown in FIG. 3), i.e., the direction of the composite particles. A process of pressing while heating in the in-plane direction at a temperature above the melting point of the thermoplastic resin and below its heat resistance temperature. In addition, when the thermoplastic resin is substantially amorphous, the melt flow rate with respect to the temperature is The temperature at which the melt starts to flow is treated as the melting point. The duration of hot pressing is the time required for thermoplasticity. The time is appropriately determined depending on the melting temperature of the thermoplastic resin. When the temperature reaches or exceeds 100°C, the resin melts and flows to the interface of the thermally conductive filler particles, eliminating gaps between the resin layers. The temperature during hot pressing is set to a temperature equal to or higher than the melting point of the thermoplastic resin, which is determined by its composition. The higher the heating temperature in the hot press, the greater the fluidity of the resin, and the more easily it flows between the filler particles. Therefore, in order to increase the thermal conductivity, the packing density of the filler particles is increased. Even if the gaps between particles become smaller, the resin flows in easily, preventing a decrease in dielectric breakdown strength. The upper limit of the heating temperature is lower than the temperature at which the polymer that constitutes the resin begins to deteriorate. The temperature is set by increasing the pressure of the hot press, which shortens the distance between the thermally conductive filler particles. At the same time, voids in the thermoplastic resin can be eliminated, increasing the density of the composite insulating board. A force is applied to bring the aligned thermally conductive filler particles closer together in the in-plane direction, improving thermal conductivity. The gaps between conductive filler particles are eliminated or the distance between them is reduced, lowering the thermal resistance In addition, the ends (sides) of some of the thermally conductive filler particles come into direct contact with each other. This is because in the composite particles, the thermoplastic resin particles are adsorbed to the plate surface of the thermally conductive filler particles, The particle size of the thermoplastic resin particles is large enough compared to the thickness of the thermally conductive filler particles on the plate, so the thermal conductivity Since it is difficult for the conductive filler particles to adhere to the sides, the pressure of the hot press causes the thermally conductive filler particles to adhere to the sides. If this process is carried out in a vacuum, it is possible to further eliminate voids in the resin. This makes it possible to improve the dielectric breakdown strength.
[0079] The insulating properties and thermal conductivity of the composite insulating board produced by the manufacturing method of the present invention are as follows: The values measured by the evaluation method are used. Since the properties of the material are significantly different, the measurement value in the direction of actual use, i.e., the thickness direction, is used.
[0080] The method for evaluating the insulation property will be described. The composite insulating board of the present invention was polished with abrasive paper to a thickness of about 1 mm. The sample was sandwiched between a pair of McKeon type electrodes and insulated from the air on the sample surface. To prevent edge damage, the sample and electrodes were molded with epoxy resin. A DC ramp voltage with a rise rate of 1 kV / sec was applied at room temperature, and the dielectric breakdown voltage was measured. The breakdown strength (kV / mm) is calculated by dividing the dielectric breakdown voltage by the actual sample thickness after the McKeon electrode system is fabricated. The test was carried out multiple times, preferably 10 times or more, with different samples, and the average The average value is taken as the "dielectric breakdown strength."
[0081] The method for evaluating thermal conductivity is described below. The disks were cut out as samples, and the thermal diffusivity ( m 2 The thermal conductivity (W / m K) is calculated by the following equation: The value calculated from the measured value and the density measured at room temperature using the Archimedes method is the "thermal conductivity". . EXAMPLES
[0082] Below, an experimental example for verifying the effect of the manufacturing method of the present invention will be described. This is a graph showing the relationship between dielectric breakdown strength and thermal conductivity. The vertical axis of the graph shows dielectric breakdown strength (kV / mm), and the horizontal axis shows thermal The conductivity (W / m K) is shown in the figure. The plots of x and + marks are based on the above-mentioned Non-Patent Document 1, These are the results disclosed in 2, 3 and 4.
[0083] In Non-Patent Document 1, BN and epoxy resin are used as thermally conductive filler particles, and the manufacturing conditions are The researchers then fabricated a composite insulating board and measured its dielectric breakdown strength and thermal conductivity. The dielectric breakdown strength of the composite insulating board produced here exceeds the market requirement of 100 kV / mm. However, their thermal conductivity is around 1 W / m K or less, which is extremely low compared to the 10 W / m K required by the market. On the other hand, those with thermal conductivity exceeding 10 W / m K have a dielectric breakdown strength of 6 The thermal conductivity and dielectric breakdown strength are both at 0 kV / mm, which is lower than the market requirement. Nothing has been found that satisfies both.
[0084] Similarly, in Patent Document 2, the dielectric breakdown strength of a composite insulating plate having the same structure is 60 kV / mm or less. The thermal conductivity is extremely low at 1 W / m K or less.
[0085] Similarly, in Patent Document 3, the present inventors have disclosed a highly heat-resistant thermoplastic resin and and plate-shaped thermally conductive filler particles having a higher thermal conductivity than resin. The thermal conductivity of the insulating board in the thickness direction is 15W / m K or more and 35W / m K or less. A composite insulating plate in which thermally conductive filler particles are oriented in a thickness direction of the composite insulating plate. A method for producing a composite insulating board, characterized in that the dielectric breakdown strength is 120 kV / mm or more. proposed the law.
[0086] Similarly, in Patent Document 4, the present inventors disclose that the heat-resistant thermoplastic resin is a thermoplastic polyimide, The thermally conductive filler particles are made of boron nitride, and the average dielectric breakdown strength is 200 kV. A composite insulating plate having a thermal conductivity of 11 W / m K and an insulating It is characterized by an average breakdown strength of 80 kV / mm and a thermal conductivity of 42 W / m K. We have proposed a manufacturing method for a composite insulating board.
[0087] (Experimental Example 1; the present invention) If the main particle BN particle is shortened, the insulation property becomes higher, but the thickness also becomes thinner, so the heat Therefore, if the length of the BN particles is made shorter and the thickness is made thicker, both properties will be improved. Assuming that the material would stretch, the average grain size of the BN particles in the longitudinal direction was set to 20 μm and the thickness to 6 μm.
[0088] In addition, when the median diameter of the PI particles was 11 um, the BN particle content could not be increased. By using the particles that have been further frozen and crushed (secondary crushing), the BN particle content can be increased. Figure 6 shows the electrostatic adsorption of BN particles with an average particle size of 20 μm and amorphous PI particles with D50 = 3.4 μm. This is an electron microscope image of a PI / BN composite particle produced by the method. PI particles are adsorbed on the surface of the BN particle. It is clear that this is the case.
[0089] The density of the sample I (the present invention) in the plot I in FIG. 5 was measured by the Archimedes method. The volume fraction of the BN particles is 87%. The thermal conductivity of sample I is 42 W / m K, and the dielectric breakdown voltage is The average strength was 109 kV / mm.
[0090] This result shows that the material has the best thermal conductivity and electrical insulation properties compared to previous samples. This is because the composite particles were made using the electrostatic adsorption method. In the ferrite material, the orientation and grain shape of BN allow the material to maintain an acceptable dielectric breakdown strength. This shows that it is possible to improve the thermal conductivity.
[0091] (Experimental Example 2) Except for changing the ratio of PI particles, the same procedure as in the above Example (Experimental Example 1) was used to obtain the profile J in FIG. The volume content of BN particles was 79%, and the thermal conductivity was 38 W / m At 100 K, the average dielectric breakdown strength was 145 kV / mm.
[0092] (Experimental Example 3) The K profile in FIG. 5 was measured in the same manner as in the above Example (Experimental Example 1) except that the ratio of PI particles was changed. The volume content of BN particles was 43%, and the thermal conductivity was 39.3W. / m·K, and the average dielectric breakdown strength was 220 kV / mm.
[0093] (Experimental Example 4) The L profile in FIG. 5 was obtained in the same manner as in the above Example (Experimental Example 1) except that the ratio of PI particles was changed. The volume content of BN particles was 42%, and the thermal conductivity was 6 W / m At 100 K, the average dielectric breakdown strength was 227 kV / mm.
[0094] The thermoplastic resin sample is a polymeric resin that exhibits good insulation and heat resistance. Polyimide (PI particles) was used. The median diameter (D50) was 11 μm. In order to increase the BN particle content in the powder, irregular particles with a median diameter (D50) of 3.4 μm were used. The thermally conductive filler particles are the hexagonal BN "PT-620 (product name)" (Momenti The average grain size in the in-plane direction was 2 BN has a plate-like crystal grain shape similar to graphite, and its thermal conductivity in the in-plane direction is 200W. / m·K, which is more than three times the thermal conductivity of 60 W / m·K in the thickness direction. Composite particles were prepared by the process of S0 using fat and thermally conductive filler particles.
[0095] Figure 6 shows the results of the experiment using pre-aggregated BN particles with an average particle size of 20 μm and amorphous PI particles with D50 = 3.4 μm. The SEM images show the BN particles. It can be seen that PI particles are adsorbed on the surface of the
[0096] Next, in order to increase the hydrophilicity of the PMMA particle surface and at the same time increase the negative surface potential, a concentration of 5 g / PMMA particles were immersed in sodium deoxycholate (SDC), a surfactant of L. Polydiallyldimethylammonium chloride (PDDA) with a concentration of 50 g / L, The PMMA particles were then immersed in sodium polystyrene sulfonate (PSS) with a concentration of 10 g / L. The concentrations of PDDA and PSS were set to be sufficient for them to adsorb to the entire PMMA surface. Before immersing in the solution, the PMMA particles were washed in ion-exchanged water. The surface potential of the BN particles was adjusted to be negative. The PMMA adsorption particles were made with a negative surface potential, and the BN main particles were made with a positive surface potential. The PMMA particles were adsorbed on the surface of the BN main particles by electrostatic interaction. Composite particles were prepared.
[0097] The composite particles produced in step S0 are converted to ions with a conductivity of 1 to 10 μS / cm in step S1. The mixture was dissolved in exchanged water to form a slurry.
[0098] In the S2 process, the slurry made in the S1 process is poured into a 12 mm x 40 mm, 3 mm thick mold. It was introduced into a formwork with a plate-shaped cavity (Figure 7).
[0099] In the S3 step, the mold containing the slurry from the S2 step is centrifugally separated in the direction of the arrow in the figure. The centrifugal force was applied for 10 minutes at about 5 μN per composite particle. The composite particles were allowed to settle as the particles were separated. The centrifugal force per particle is Centrifugal force = (number of rotations) x The calculation was made by multiplying the weight of the composite particles by the distance from the center of rotation. pm, average distance from center of rotation to composite particle: 1700 mm, weight of composite particle: 2.87 ×10 -9 g[=(PMMA density: 1.2g / cm 3 ) × (PMMA particle volume: 3.35 × 10 -11 c m 3 )+(BN density: 2.1g / cm 3 )×(BN volume: 1.35×10 -9 cm 3 )]. Formwork By applying centrifugal force in the direction intersecting with the bottom surface (A surface), the plate-like surface of the composite particles is pressed against the bottom surface of the mold. The slurry liquid escapes through the gaps in the formwork, forming a 12mm x 13 A deposit of composite particles was formed with a thickness of 3 mm.
[0100] In step S4, mechanical pressure is applied in the same direction as the centrifugal force with a plate of the same shape as the opening 3 of the formwork. Add 12mm x 13mm and 3mm thick deposit to 12mm x 10mm and 3mm thick. The mixture was compressed into a molded body.
[0101] In step S5, the molded body produced in step S4 was removed from the mold.
[0102] In step S6, the molded body produced in step S5 is heated to a temperature above the melting point of PMMA in the 3 mm thickness direction. The PMMA softens at 80 to 100°C and at 160 to 200°C. In order to melt and thermoform the material at 260℃, the material was hot pressed at 160℃. The pressure is 50 MPa on a φ10 mm surface.
[0103] The density of the composite insulating board in this comparative example is 1.84 g / cm 3 The amount of BN particles was 59% by volume. The density of the BN particles used here is 2.1 g / cm 3 , PMMA particle density is 1.2g / cm 3 It was.
[0104] As described above, a composite insulating board can be manufactured by the embodiment of the manufacturing method. The present invention includes a composite insulating board produced by this production method. [Explanation of symbols]
[0105] 1. Thermally conductive filler particles 2 Thermoplastic resin 3 Formwork opening (cavity opening)
Claims
1. A highly heat-resistant thermoplastic resin and a plate-shaped thermally conductive material having a higher thermal conductivity than the highly heat-resistant thermoplastic resin. In a composite insulating board containing a thermally insulating filler particle, the thermal conductivity in the thickness direction of the composite insulating board is 35 A composite material in which the thermally conductive filler particles are oriented so that the thermal conductivity is 45 W / m.K or more and 45 W / m.K or less. A composite insulating board having a dielectric breakdown strength of 95 kV / mm A composite insulating board characterized by the above.
2. 2. The method according to claim 1, wherein the highly heat-resistant thermoplastic resin is a thermoplastic polyimide. Composite insulating board.
3. 3. The method according to claim 1, wherein the thermally conductive filler particles are boron nitride. Composite insulating board.
Citation Information
Patent Citations
Resin composition, and method for producing the same
JP2013159748A
Composite insulation sheet and manufacturing method of composite insulation sheet
JP2017037833A
Heat releasing composite insulation sheet with high heat resistant performance added
JP2019153575A
Composite insulating board and method for manufacturing the same
JP7174973B2