Metal laminate and production method thereof

A metal laminate with a thin metal layer on a fluororesin and oxide sheet addresses adhesiveness issues by direct application, enhancing performance and simplifying manufacturing, suitable for high-frequency and flexible circuit boards.

JP2024166544AInactive Publication Date: 2024-11-29DAIKIN INDUSTRIES LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023082707
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for forming thin metal layers on fluororesin sheets for high-frequency printed wiring boards face challenges in achieving adequate adhesiveness and require multiple manufacturing steps, leading to increased costs and potential deterioration in performance due to conductor and dielectric losses.

Method used

A metal laminate is created by directly providing a thin metal layer on a sheet containing fluororesin and oxide, using dry plating or similar methods, with specific properties such as a thickness of 8 μm or less and a tape peel strength of 3 or more, to enhance adhesiveness and simplify the manufacturing process.

Benefits of technology

The metal laminate achieves excellent adhesiveness between the fluororesin sheet and metal layer, improves performance, and reduces manufacturing complexity while maintaining low conductor and dielectric losses, making it suitable for flexible circuit boards and millimeter wave antennas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166544000001
    Figure 2024166544000001
  • Figure 2024166544000002
    Figure 2024166544000002
Patent Text Reader

Abstract

To provide a metal laminate with a thin film metal layer having good adhesion between a sheet and a metal layer.SOLUTION: The metal laminate is produced by providing a metal layer on one side or both sides of a sheet containing fluorine resin and oxide, and the film thickness of the metal layer is 8 μm or less and the tape peel strength is 3 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to metal laminates and methods for producing the same. [Background technology]

[0002] There is a demand for high-frequency printed wiring boards with small transmission loss. It is known that fluororesin films are used in such high-frequency printed wiring boards (Patent Document 1, etc.). In addition, Patent Document 2 describes the use of fluororesin containing filler as a wiring board material.

[0003] Furthermore, Patent Document 3 discloses a wiring board used as a printed circuit board, in which a metal film is formed by plating on a fluororesin substrate having an uneven surface. Patent Document 4 discloses a two-layer flexible substrate in which a nickel-chromium alloy underlayer is formed on at least one side of an insulating film, and a copper conductor layer is formed thereon. Patent Document 5 discloses a method for producing a flexible printed circuit board in which a layer made of a metal oxide is provided on a polymer film, and a metal film is then formed on the layer. Patent Document 6 discloses a metal-clad laminate in which a coating film having a specific surface roughness (Rz) is disposed on a base film, and a metal film is formed thereon by at least one of plating, sputtering, and vapor deposition. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-8260 A [Patent Document 2] International Publication No. 2021-235460 [Patent Document 3] JP 2004-356547 A [Patent Document 4] International Publication No. 2008-090654 [Patent Document 5] JP 2010-192861 A [Patent Document 6] International Publication No. 2021-199811 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present disclosure is to provide a metal laminate plate having a thin metal layer that exhibits excellent adhesion between a fluororesin sheet and a metal layer. [Means for solving the problem]

[0006] The present disclosure relates to a metal laminate plate having a metal layer on one or both sides of a sheet containing a fluororesin and an oxide, the metal layer having a thickness of 8 μm or less and a tape peel strength of 3 or more. The present disclosure also provides a metal laminate plate having a metal layer on one or both sides of a sheet containing a fluororesin and an oxide, wherein the melting point of the fluororesin is 320°C or higher, the heat of fusion of the sheet is 20 mJ / mg or less, and the film thickness of the metal layer is 8 μm or less.

[0007] The sheet preferably has a coefficient of linear expansion (CTE) of 100 ppm / K or less. The fluororesin is preferably polytetrafluoroethylene.

[0008] The oxide is preferably silica. The silica is preferably in the form of spherical particles. As the silica, it is preferable to use silica particles treated with a silane coupling agent. The average particle size of the silica is preferably 10 μm or less. The content of the oxide is preferably 30% by mass or more based on the total amount of the sheet.

[0009] The metal layer is preferably formed of one or more metals selected from the group consisting of copper, gold, silver and platinum. The metal layer is preferably made of copper.

[0010] The sheet preferably has a dielectric loss tangent value of 0.0015 or less at 10 GHz. The sheet preferably has a thickness of 5 to 250 μm.

[0011] The present disclosure also relates to a method for producing a metal laminate, comprising a step (A) of providing a metal layer by a dry plating method on one or both sides of a sheet containing a fluororesin and an oxide. The present disclosure also relates to a method for producing a metal laminate, comprising a step (A) of providing a metal layer on one or both sides of a sheet containing a fluororesin and an oxide by any one of a vacuum deposition method, a sputtering method, and an ion plating method.

[0012] It is preferable to have a step (B) of heating the sheet to 300 to 400°C. The metal layer is preferably a copper layer. It is preferable to further include a step (C) of thickening the provided metal layer by a wet plating method.

[0013] The present disclosure also relates to a circuit board having the above-mentioned metal laminate. The present disclosure also relates to an antenna formed from the circuit board described above. The present disclosure is also a millimeter wave antenna for mobility formed from a circuit board. Effect of the Invention

[0014] The metal laminate plate of the present disclosure is a metal laminate plate having a thin metal layer, and has excellent adhesion between a fluororesin sheet and the metal layer. Moreover, the present disclosure enables the metal laminate plate to be efficiently produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present disclosure will be described in detail below. There is a demand for thinner circuit boards to be used in millimeter wave antennas for mobility, etc. For this reason, metal foil is not used as the conductor layer of the metal laminate that becomes the circuit board, and a thin metal layer is formed on a resin sheet by a dry plating method or a wet plating method. Conventionally, when forming a thin metal layer by a dry plating method or a wet plating method, as described in the above-mentioned prior art documents, in order to ensure adhesion to a resin sheet, it has been considered to provide an uneven surface on the resin sheet, or to provide a coating film as an adhesive layer on the resin sheet, or to provide a metal underlayer of an alloy or metal oxide. However, these methods require many manufacturing steps, which increases the cost of the metal laminate, and the conductor loss and dielectric loss of the resulting metal laminate may be large, resulting in poor performance as a circuit board.

[0016] The present disclosure makes it possible to provide a metal laminate having a thin metal layer that exhibits excellent adhesion between a resin sheet and a metal layer without using the above-mentioned methods. The metal laminate of the present disclosure is characterized in that a metal layer is provided directly on one or both sides of a sheet containing a fluororesin and an oxide by a dry plating method or the like.

[0017] The metal laminate plate of the present disclosure has excellent adhesiveness even when a thin metal layer is directly provided on the sheet because the sheet contains an oxide. This makes it possible to improve the performance of the metal laminate plate. In addition, the manufacturing process of the metal laminate plate can be simplified, which is also advantageous in terms of cost.

[0018] The reason for this is not yet clear, but it is presumed that the partial precipitation of oxides on the sheet surface improves adhesion to the metal layer.

[0019] The present disclosure relates to a metal laminate plate having a metal layer on one or both sides of a sheet containing a fluororesin and an oxide, the metal layer having a thickness of 8 μm or less and a tape peel strength of 3 or more.

[0020] As described above, the metal laminate of the present disclosure is obtained by forming a metal layer directly on a sheet containing a fluororesin and an oxide by a dry plating method or the like. Since the sheet contains an oxide, the metal laminate has a certain level of tape peel strength even when a metal layer is formed directly on the sheet. The metal laminate described above has a thin metal layer with a thickness of 8 μm or less, and therefore can be suitably used for flexible circuit boards, circuit boards used in high frequency bands of 110 GHz or more, and millimeter wave antennas for mobility purposes formed from circuit boards, which require thinner materials.

[0021] The tape peel strength in the present disclosure is evaluated by the following method. Using Nichiban Cellotape (registered trademark) (tape width: 18 mm) used in the JIS-K5600 adhesion test (cross-cut method), a 15 mm long cellotape was applied to the metal layer surface of the metal laminate so as to eliminate any air bubbles. The applied tape was peeled off at an angle of 90°, and the metal layer (area 270 mm2) of the metal laminate to which the cellotape had been applied was removed. 2 The area of ​​metal peeled off from the test piece was calculated using image analysis (Python) and evaluated as follows. 1: 95% or more of the metal has peeled off 2: More than 60% but less than 95% of the metal has peeled off 3: More than 40% but less than 60% of the metal has peeled off 4: More than 5% but less than 40% of the metal has peeled off 5: Less than 5% metal removed, peeled off

[0022] If the tape peel strength is 3 or more, the adhesion between the sheet and the metal layer is good, and therefore the performance of the metal laminate is also good. The tape peel strength is preferably 4 or greater, and 5 is most preferred.

[0023] The present disclosure also provides a metal laminate plate having a metal layer on one or both sides of a sheet containing a fluororesin and an oxide, wherein the melting point of the fluororesin is 320°C or higher, the heat of fusion of the sheet is 20 mJ / mg or less, and the film thickness of the metal layer is 8 μm or less.

[0024] The melting point of the fluororesin of the metal laminate sheet is within the above range, which is advantageous in that it can be used at higher temperatures. The melting point of the fluororesin is preferably 325° C. or higher, and more preferably 330° C. or higher. There is no particular upper limit to the melting point of the fluororesin, but it is preferably 390° C. or lower.

[0025] The melting point of the fluororesin can be suitably adjusted to 320° C. or higher by adjusting the composition of the fluororesin.

[0026] Having the heat of fusion of the metal laminate sheet within the above range is advantageous in that the tape peel strength is good. The heat of fusion of the sheet is preferably 18 mJ / mg or less, more preferably 17 mJ / mg or less. The lower limit of the heat of fusion of the sheet is not particularly limited, but is preferably 5 mJ / mg or more.

[0027] The heat of fusion of the metal laminate sheet can be suitably controlled to 20 mJ / mg or less by subjecting the sheet to a heat treatment or the like. Heat treatment of the sheet changes the crystallinity of the fluororesin and reduces the heat of fusion. When the heat of fusion is small, the sheet becomes hard, and when an attempt is made to peel off the metal layer, the sheet becomes damaged at the interface with the metal, rather than the base material of the sheet, resulting in strong tape peel strength.

[0028] The melting point is the temperature corresponding to the maximum value on the heat of fusion curve when a sheet is extracted from the metal laminate by etching and the temperature is raised from 230°C to 380°C at 10°C / min using a differential scanning calorimeter DSC (DSC7000X manufactured by Hitachi High-Technologies Corporation). The heat of fusion is a value determined from a heat of fusion curve when the removed sheet is heated from 230° C. to 380° C. at a rate of 10° C. / min using a differential scanning calorimeter DSC (DSC7000X manufactured by Hitachi High-Technologies Corporation).

[0029] (Oxide) The sheet used in this disclosure is characterized as including an oxide. Examples of the oxide include silica, alumina, titanium oxide, zinc oxide, tin oxide, calcium oxide, magnesium oxide, etc. Two or more of these may be used in combination. Among these, silica, alumina, and titanium oxide are preferable because they can reduce the dielectric loss tangent (Df). In particular, silica is preferable because it can reduce the linear expansion coefficient of the sheet and therefore can increase the tape peel strength between the sheet and the metal layer after heat treatment. In addition, the combined use of silica and alumina is preferable because it allows the relative dielectric constant (Dk) at 10 GHz to be adjusted to around 3.

[0030] The oxide is not particularly limited in shape, but is particularly preferably spherical, which is preferable in that it is easy to process uniformly during drilling and has a small specific surface area and therefore low transmission loss. The silica used is preferably spherical silica particles.

[0031] The above-mentioned spherical oxide means that the particle shape is close to a perfect sphere, and specifically, the sphericity is preferably 0.80 or more, more preferably 0.85 or more, even more preferably 0.90 or more, and most preferably 0.95 or more. The sphericity is calculated by taking a photograph with an SEM and calculating the value from the area and perimeter of the observed particle as (sphericity) = {4π × (area) ÷ (perimeter) 2}. The closer to 1, the closer to a perfect sphere. Specifically, the average value measured for 100 particles using an image processing device (Spectris Corporation: FPIA-3000) is used.

[0032] The oxide used in the present disclosure preferably has a D90 / D10 of 2 or more (preferably 2.3 or more, 2.5 or more) and a D50 of 10 μm or less when the volume is integrated from the smallest particle size. Furthermore, it is preferable that the D90 / D50 is 1.5 or more (more preferably 1.6 or more). It is preferable that the D50 / D10 is 1.5 or more (more preferably 1.6 or more). It is more preferable that the D50 is 5 μm or less. Since it is possible for the oxide with a small particle size to enter the gaps between the oxide with a large particle size, it is possible to achieve excellent filling properties and high fluidity. In particular, it is preferable that the particle size distribution has a high frequency on the side of small particle size compared to a Gaussian curve. The particle size can be measured by a laser diffraction / scattering type particle size distribution measuring device. Since coarse particles make it difficult to form a thin sheet, it is preferable that coarse particles having a particle size equal to or larger than a certain size are removed by a filter or the like.

[0033] The average particle size of the oxide is not particularly limited, but is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 2.5 μm or less. If the average particle size exceeds 10 μm, it may become difficult to form the sheet into a thin film. The lower limit of the average particle size of the oxide is preferably 0.5 μm or more. If the lower limit of the average particle size of the oxide is less than 0.5 μm, the oxide may aggregate, and a sufficient effect may not be obtained. The average particle size here is the D50 value measured by a laser analysis type particle size distribution analyzer.

[0034] The average particle size of the silica is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 2.5 μm or less. The lower limit of the average particle size of the silica is preferably 0.5 μm or more.

[0035] The oxide preferably has a water absorption of 1.0% or less, more preferably 0.5% or less. If the water absorption of the oxide is within the above range, the sheet can be prevented from absorbing moisture, and thus a sheet can be obtained in which an increase in dielectric tangent due to moisture absorption is prevented. The water absorption of an oxide is based on the mass of the oxide when dry. To measure water absorption, a dry sample is left at 40°C and 80% RH for 1 hour, and the water generated by heating to 200°C is measured using a Karl Fischer moisture meter, and then calculated.

[0036] The dielectric loss tangent of the silica at 10 GHz is preferably 0.0025 or less. This value is preferable because the sheet has low loss. The upper limit is more preferably 0.002, and even more preferably 0.0015. On the other hand, the lower limit of the dielectric loss tangent is preferably 0.00001.

[0037] In this disclosure, the dielectric loss tangent of silica measured at 10 GHz was measured using a cylindrical cavity resonator and a network analyzer, with a filler powder sample filled in a quartz tube and loaded into the resonator. The characteristics of the resonator (resonant frequency and Q value) were obtained before and after inserting the sample, and the dielectric loss tangent was calculated from the results. This measurement method complies with the Japanese Industrial Standard JIS2565 Microwave Ferrite Core Test Method, and measurements were performed in an environment with a room temperature of 25°C and a humidity of 40%.

[0038] Alternatively, the oxide can be obtained by etching a metal laminate, heating the resulting sheet at 600°C for 30 minutes in an air atmosphere to burn off the fluororesin, extracting the oxide, and then measuring the parameters thereof using the method described above.

[0039] The oxide is preferably surface-treated. By performing the surface treatment in advance, the agglomeration of the oxide can be suppressed, and the oxide can be well dispersed in the sheet. This is preferable in that it can suppress the presence or generation of oxide lumps in the sheet. The presence or generation of oxide lumps in the sheet makes the sheet more likely to tear, but this can be suppressed by using a surface-treated oxide.

[0040] The surface treatment is not particularly limited, and any known treatment can be used.Specific examples of the surface treatment include treatment with a silane coupling agent such as epoxysilane, aminosilane, isocyanatesilane, vinylsilane, acrylicsilane, hydrophobic alkylsilane, phenylsilane, and fluorinated alkylsilane having a reactive functional group, plasma treatment, and fluorination treatment.

[0041] Among these, it is preferable to use one which is surface-treated with a silane coupling agent and has an oxide coated with the silane coupling agent. Coating with a silane coupling agent is advantageous in that it improves dispersibility in the sheet and reduces the linear expansion coefficient. In the present disclosure, it is preferable to use silica particles treated with a silane coupling agent as the silica.

[0042] Examples of the silane coupling agent include epoxy silanes such as γ-glycidoxypropyltriethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, amino silanes such as aminopropyltriethoxysilane and N-phenylaminopropyltrimethoxysilane, isocyanate silanes such as 3-isocyanatepropyltrimethoxysilane, vinyl silanes such as vinyltrimethoxysilane, and acrylic silanes such as acryloxytrimethoxysilane.

[0043] The spherical silica particles may be commercially available silica particles that satisfy the above-mentioned properties. Examples of commercially available silica particles include Denka fused silica FB grade (manufactured by Denka Co., Ltd.), Denka fused silica SFP grade (manufactured by Denka Co., Ltd.), Excelica (manufactured by Tokuyama Corporation), high-purity synthetic spherical silica particles Admafine (manufactured by Admatechs Co., Ltd.), Admanano (manufactured by Admatechs Co., Ltd.), and Admafuse (manufactured by Admatechs Co., Ltd.).

[0044] The above-mentioned alumina particles and titanium oxide particles may be commercially available alumina particles and titanium oxide particles that satisfy the above-mentioned properties. Examples of commercially available alumina particles include LS-210B (manufactured by Nippon Light Metal Co., Ltd.) and LS-110F (manufactured by Nippon Light Metal Co., Ltd.). Examples of commercially available titanium oxide particles include TITONE SA-1 (manufactured by Sakai Chemical Industry Co., Ltd.).

[0045] The oxide is preferably contained in a proportion of 30% by mass or more of the entire sheet. This amount is preferable in that it maintains a low dielectric constant and low loss while providing low thermal expansion. In addition, when the amount of the oxide is within this range, the heat of fusion of the heat-treated sheet is 20 mJ / mg or less, and the oxide is partially precipitated on the sheet surface, which is preferable in that it provides excellent adhesion to the metal layer. The amount of the oxide is more preferably 40% by mass or more, and even more preferably 50% by mass or more. The upper limit of the amount of the oxide is not particularly limited, but is preferably 80% by mass or less, and more preferably 70% by mass or less.

[0046] In the present disclosure, in addition to the above oxides, one or more inorganic particles selected from ceramics, talc, mica, calcium carbonate, potassium titanate, glass fibers, glass pieces, glass beads, silicon carbide, calcium fluoride, boron nitride, barium sulfate, molybdenum disulfide, and potassium carbonate whiskers may be used in combination. The content of these in the sheet is preferably 20% by mass or less.

[0047] (Fluorine resin) The sheet used in the present disclosure contains a fluororesin. Since fluororesin has low dielectric properties, it can be suitably used for the purpose of the present disclosure.

[0048] The fluororesin that can be used in the present disclosure is not particularly limited, and examples thereof include polytetrafluoroethylene (PTFE), tetrafluoroethylene [TFE] / hexafluoropropylene [HFP] copolymer [FEP], TFE / alkyl vinyl ether copolymer [PFA], TFE / HFP / alkyl vinyl ether copolymer [EPA], TFE / chlorotrifluoroethylene [CTFE] copolymer, TFE / ethylene copolymer [ETFE], polyvinylidene fluoride [PVdF], tetrafluoroethylene having a molecular weight of 300,000 or less [LMW-PTFE], etc. These may be used alone or in combination of two or more.

[0049] Among them, polytetrafluoroethylene resin (PTFE) is particularly preferable from the viewpoint of low dielectric properties. PTFE having fibrillation properties is preferable. PTFE having fibrillation properties means PTFE that can be paste-extruded from unsintered polymer powder.

[0050] PTFE may be modified polytetrafluoroethylene (hereinafter referred to as modified PTFE), homopolytetrafluoroethylene (hereinafter referred to as homoPTFE), or a mixture of modified PTFE and homoPTFE. From the viewpoint of maintaining good moldability of polytetrafluoroethylene, the content of modified PTFE in the polymeric PTFE is preferably 10% by weight or more and 98% by weight or less, and more preferably 50% by weight or more and 95% by weight or less. The homo-PTFE is not particularly limited, and homo-PTFE disclosed in JP-A-53-60979, JP-A-57-135, JP-A-61-16907, JP-A-62-104816, JP-A-62-190206, JP-A-63-137906, JP-A-2000-143727, JP-A-2002-201217, WO 2007 / 046345 pamphlet, WO 2007 / 119829 pamphlet, WO 2009 / 001894 pamphlet, WO 2010 / 113950 pamphlet, WO 2013 / 027850 pamphlet, etc. can be suitably used. Among these, homo-PTFE having high stretchability and disclosed in JP-A-57-135, JP-A-63-137906, JP-A-2000-143727, JP-A-2002-201217, WO 2007 / 046345, WO 2007 / 119829, WO 2010 / 113950 and the like is preferred.

[0051] The modified PTFE is composed of TFE and a monomer other than TFE (hereinafter referred to as a modified monomer). The modified PTFE may be, but is not limited to, one that is uniformly modified by the modified monomer, one that is modified at the beginning of the polymerization reaction, one that is modified at the end of the polymerization reaction, etc. The modified PTFE is preferably a TFE copolymer obtained by subjecting a small amount of a monomer other than TFE to polymerization together with TFE within a range that does not significantly impair the properties of the TFE homopolymer. The modified PTFE may be, for example, those disclosed in JP-A-60-42446, JP-A-61-16907, JP-A-62-104816, JP-A-62-190206, JP-A-64-1711, JP-A-2-261810, JP-A-11-240917, JP-A-11-240918, WO 2003 / 033555 pamphlet, WO 2005 / 061567 pamphlet, WO 2007 / 005361 pamphlet, WO 2011 / 055824 pamphlet, WO 2013 / 027850 pamphlet, etc., which can be suitably used. Among these, modified PTFEs having high stretchability and disclosed in JP-A-61-16907, JP-A-62-104816, JP-A-64-1711, JP-A-11-240917, WO 2003 / 033555, WO 2005 / 061567, WO 2007 / 005361, WO 2011 / 055824 and the like are preferred.

[0052] The modified PTFE contains TFE units based on TFE and modified monomer units based on modified monomers. The modified monomer units are a part of the molecular structure of the modified PTFE and are derived from the modified monomer. The modified PTFE contains the modified monomer units in an amount of preferably 0.001 to 0.500% by weight, more preferably 0.01 to 0.30% by weight, of the total monomer units. The total monomer units are the parts derived from all monomers in the molecular structure of the modified PTFE.

[0053] The modifying monomer is not particularly limited as long as it can be copolymerized with TFE, and examples thereof include perfluoroolefins such as hexafluoropropylene (HFP), chlorofluoroolefins such as chlorotrifluoroethylene (CTFE), hydrogen-containing fluoroolefins such as trifluoroethylene and vinylidene fluoride (VDF), perfluorovinyl ethers, perfluoroalkylethylenes (PFAE), ethylene, etc. The modifying monomer used may be one type or multiple types.

[0054] The perfluorovinyl ether is not particularly limited, and examples thereof include perfluorounsaturated compounds represented by the following general formula (1). CF2 = CF-ORf (1) (In the formula, Rf represents a perfluoro organic group.)

[0055] In this specification, a perfluoro organic group is an organic group in which all hydrogen atoms bonded to carbon atoms are replaced with fluorine atoms. The perfluoro organic group may have an ether oxygen.

[0056] An example of the perfluorovinyl ether is perfluoro(alkyl vinyl ether) (PAVE) in which Rf in the above general formula (1) is a perfluoroalkyl group having 1 to 10 carbon atoms. The number of carbon atoms in the perfluoroalkyl group is preferably 1 to 5. Examples of the perfluoroalkyl group in PAVE include a perfluoromethyl group, a perfluoroethyl group, a perfluoropropyl group, a perfluorobutyl group, a perfluoropentyl group, and a perfluorohexyl group. Preferred examples of PAVE include perfluoropropyl vinyl ether (PPVE) and perfluoromethyl vinyl ether (PMVE).

[0057] The perfluoroalkylethylene (PFAE) is not particularly limited, and examples thereof include perfluorobutylethylene (PFBE), perfluorohexylethylene (PFHE), and the like.

[0058] The modifying monomer in the modified PTFE is preferably at least one selected from the group consisting of HFP, CTFE, VDF, PAVE, PFAE and ethylene.

[0059] The fluororesin is preferably non-melt processable. Non-melt processable means that the resin does not have sufficient fluidity even when heated to the melting point or higher, and cannot be molded by a melt molding method generally used for resins. PTFE corresponds to this.

[0060] In the present disclosure, it is preferable to use such a non-melt-processable fluororesin and form it into a fluororesin sheet by a molding method that fibrillates the fluororesin. The molding method will be described later.

[0061] The PTFE preferably has a standard specific gravity (SSG) of 2.0 to 2.3. When such PTFE is used, a PTFE membrane having high strength (cohesion and puncture strength per unit thickness) is easily obtained. PTFE having a large molecular weight has a long molecular chain, and therefore it is difficult to form a structure in which the molecular chains are regularly arranged. In this case, the length of the amorphous part increases, and the degree of entanglement between the molecules increases. When the degree of entanglement between the molecules is high, the PTFE membrane is unlikely to deform under an applied load and is considered to exhibit excellent mechanical strength. In addition, when a PTFE having a large molecular weight is used, a PTFE membrane having a small average pore size is easily obtained.

[0062] The lower limit of the SSG is more preferably 2.05, and even more preferably 2.1.The upper limit of the SSG is more preferably 2.25, and even more preferably 2.2.

[0063] Standard specific gravity (SSG) was measured by preparing a sample in accordance with ASTM D-4895-89 and measuring the specific gravity of the obtained sample by the water displacement method.

[0064] In the present disclosure, the molecular weight (number average molecular weight) of the PTFE constituting the PTFE powder is preferably in the range of, for example, 2 million to 12 million. The lower limit of the molecular weight of the PTFE may be 3 million or 4 million. The upper limit of the molecular weight of the PTFE may be 10 million.

[0065] The number average molecular weight of PTFE can be measured by a method based on standard specific gravity and a method based on dynamic viscoelasticity when melted. The method based on standard specific gravity can be performed by a water displacement method based on ASTM D-792 using a sample molded based on ASTM D-4895 98. The method based on dynamic viscoelasticity is described, for example, by S. Wu in Polymer Engineering & Science, 1988, Vol. 28, 538 and the same document, 1989, Vol. 29, 273.

[0066] The PTFE preferably has a refractive index in the range of 1.2 to 1.6. By having such a refractive index, it is preferable in terms of low dielectric constant. The refractive index can be adjusted to be within the above range by a method of adjusting the polarizability or flexibility of the main chain. The lower limit of the refractive index is more preferably 1.25, more preferably 1.30, and most preferably 1.32. The upper limit of the refractive index is more preferably 1.55, more preferably 1.50, and most preferably 1.45.

[0067] The refractive indexes are values ​​measured using a refractometer (Abbemat 300).

[0068] The PTFE preferably has a maximum endothermic peak temperature (crystalline melting point) of 340±7°C.

[0069] The PTFE may be a low-melting-point PTFE having a maximum peak temperature of 338°C or lower on an endothermic curve on a crystalline melting curve measured by a differential scanning calorimeter, or a high-melting-point PTFE having a maximum peak temperature of 342°C or higher on an endothermic curve on a crystalline melting curve measured by a differential scanning calorimeter.

[0070] The low melting point PTFE powder is a powder produced by emulsion polymerization, and has the above-mentioned maximum endothermic peak temperature (crystalline melting point), a dielectric constant (ε) of 2.08 to 2.2, and a dielectric tangent (tan δ) of 1.9×10 -4 ~4.0×10 -4 Examples of commercially available products include Polyflon fine powders F201, F203, F205, F301, and F302 manufactured by Daikin Industries, Ltd., CD090 and CD076 manufactured by Asahi Glass Co., Ltd., and TF6C, TF62, and TF40 manufactured by DuPont.

[0071] The high melting point PTFE powder is also a powder produced by emulsion polymerization, and has the above-mentioned maximum endothermic peak temperature (crystalline melting point), a dielectric constant (ε) of 2.0 to 2.1, and a dielectric tangent (tan δ) of 1.6×10 -4 ~2.2×10 -4 As commercially available products, for example, Polyflon fine powder F104 and F106 manufactured by Daikin Industries, Ltd., CD1, CD141, and CD123 manufactured by Asahi Glass Co., Ltd., and TF6 and TF65 manufactured by DuPont can be mentioned.

[0072] The powder in which both PTFE polymer particles are secondary aggregated usually has an average particle size of 250 to 2000 μm. In particular, granulated powder obtained by granulation using a solvent is preferred from the viewpoint of improving the flowability when filling a mold in preforming.

[0073] Powdered PTFE that satisfies the above-mentioned parameters can be obtained by a conventional manufacturing method, for example, by following the manufacturing methods described in International Publication No. 2015-080291 and International Publication No. 2012-086710.

[0074] (Sheet) In the present disclosure, as described above, it is important to use a sheet containing a fluororesin and an oxide. The sheet may contain other components other than these as necessary, or may be composed only of a fluororesin and an oxide. The content of other components is preferably 10% by mass or less.

[0075] The sheet used in the present disclosure preferably has a coefficient of linear expansion (CTE) of 100 ppm / K or less. The above range is preferable in that the sheet has low shrinkage and excellent dimensional stability. The upper limit is more preferably 80 ppm / K, further preferably 70 ppm / K, and most preferably 50 ppm / K. The lower limit is not particularly limited, but is more preferably 10 ppm / K, and further preferably 20 ppm / K.

[0076] The linear expansion coefficient in this disclosure is a value obtained by performing TMA measurement using a TMA-7100 (manufactured by Hitachi High-Tech Science Corporation) in a tensile mode, using a sheet cut to a length of 20 mm, width of 5 mm, and thickness of 150 μm as a sample piece, setting the chuck distance to 10 mm, applying a load of 49 mN, and determining the linear expansion coefficient from the displacement of the sample from 0 to 150°C at a heating rate of 2°C / min.

[0077] The sheet preferably has a relative dielectric constant (Dk) of 3.5 or less at 10 GHz. Having the sheet within this range is preferable in terms of low dielectric loss. The upper limit of the relative dielectric constant is more preferably 3.2, and even more preferably 3.1, while the lower limit of the relative dielectric constant is preferably 2.0, and more preferably 2.5.

[0078] The sheet preferably has a dielectric loss tangent (Df) of 0.0015 or less at 10 GHz. By setting the dielectric loss tangent within this range, it is preferable that the loss of electrical signals in the circuit can be kept low. The dielectric loss tangent is more preferably 0.0012 or less, and even more preferably 0.0011 or less. On the other hand, the lower limit of the dielectric loss tangent is preferably 0.00001.

[0079] The relative permittivity (Dk) and dielectric loss tangent (Df) at 10 GHz of the sheet in this disclosure were determined by measuring Dk and Df at 25°C and 10 GHz using a split cylinder type dielectric constant / dielectric loss tangent measuring device (manufactured by EM Lab).

[0080] The sheet can also be removed from the metal laminate by etching, and the above parameters can then be measured using the above methods.

[0081] The sheet preferably has a thickness of 5 to 250 μm. Even if the sheet is thin, it can sufficiently achieve its purpose. From this viewpoint, it is more preferably 200 μm or less, and even more preferably 150 μm or less. Furthermore, if the sheet can be processed to a thickness of 100 μm or less as necessary, it is preferable because it can be widely applied to substrates of various thicknesses.

[0082] (Sheet manufacturing method) The sheet can be obtained by mixing the above-mentioned fluororesin and oxide and forming a film. The manufacturing method is not limited, but paste extrusion molding, powder rolling molding, etc. are suitable.

[0083] As described above, it is preferable to use a non-melt processable fluororesin as the fluororesin used for the sheet. When using such a fluororesin, it is preferable to form it into a sheet by fibrillating powdered PTFE as a raw material.

[0084] The powdered PTFE preferably has a primary particle size of 0.05 to 10 μm. The use of such a powder has the advantage of excellent moldability and dispersibility. The primary particle size here is a value measured in accordance with ASTM D 4895.

[0085] The powdered PTFE preferably contains 50% by mass or more, more preferably 80% by mass or more, of polytetrafluoroethylene resin having a secondary particle diameter of 500 μm or more. By containing PTFE having a secondary particle diameter of 500 μm or more within this range, it is advantageous in that a sheet with high strength can be produced. By using PTFE with a secondary particle size of 500 μm or more, a sheet with lower resistance and excellent toughness can be obtained.

[0086] The lower limit of the secondary particle diameter is more preferably 300 μm, and even more preferably 350 μm. The upper limit of the secondary particle diameter is more preferably 700 μm or less, and even more preferably 600 μm or less. The secondary particle diameter can be determined, for example, by a sieving method.

[0087] The powdered PTFE has an average primary particle size of preferably 50 nm or more, more preferably 100 nm or more, even more preferably 150 nm or more, and particularly preferably 200 nm or more, since this allows the production of a sheet with higher strength and excellent homogeneity. The larger the average primary particle diameter of PTFE, the more suppressed the increase in paste extrusion pressure when the powder is used for paste extrusion molding, and the better the moldability. The upper limit is not particularly limited, but may be 500 nm. From the viewpoint of productivity in the polymerization process, it is preferably 350 nm.

[0088] The above average primary particle diameter can be determined by preparing a calibration curve of the transmittance of 550 nm projected light per unit length of an aqueous dispersion of PTFE obtained by polymerization, the polymer concentration of which is adjusted to 0.22% by mass, and the average primary particle diameter determined by measuring the unidirectional diameter in a transmission electron microscope photograph, measuring the above transmittance for the aqueous dispersion to be measured, and then based on the calibration curve.

[0089] The PTFE used in the present disclosure may have a core-shell structure.The PTFE having a core-shell structure may include, for example, modified polytetrafluoroethylene, which contains a core of high molecular weight polytetrafluoroethylene and a shell of lower molecular weight polytetrafluoroethylene or modified polytetrafluoroethylene in a particle.As such modified polytetrafluoroethylene, for example, the polytetrafluoroethylene described in JP-A-2005-527652 may be included.

[0090] The specific methods for paste extrusion molding and powder rolling molding are not particularly limited, but the general methods are described below.

[0091] (Paste extrusion molding) The method for producing the sheet may include a step (1a) of mixing a raw material composition containing a fluororesin and an oxide obtained using a hydrocarbon surfactant with an extrusion aid, a step (1b) of paste extrusion molding the obtained mixture, a step (1c) of rolling the extrudate obtained by extrusion molding, a step (1d) of drying the rolled sheet, and a step (1e) of firing the dried sheet to obtain a molded product. The paste extrusion molding can also be carried out by adding a conventionally known additive such as a pigment to the raw material composition.

[0092] The extrusion aid is not particularly limited, and generally known ones can be used, such as hydrocarbon oils.

[0093] (Powder rolling molding) The sheet can also be formed by powder rolling molding. Powder rolling molding is a method in which a resin powder is fibrillated by applying a shear force to the resin powder, and then molded into a sheet. The method may include a step of subsequently firing the powder to obtain a molded body. More specifically, A step (1) of applying a shear force to a raw material composition containing a fluororesin and an oxide while mixing the raw material composition. A step (2) of forming the mixture obtained by the step (1) into a bulk form; and A step (3) of rolling the bulk mixture obtained in the step (2) into a sheet. The composition can be obtained by a manufacturing method having the following steps. The method may further include a step (4) of firing the sheet-like material obtained above at 200 to 400° C. for 1 to 60 minutes. Additionally, step (2) may be omitted.

[0094] When forming a sheet by such powder rolling molding, it is preferable to form a mixture of only the fluororesin and the oxide.

[0095] The sheet of the present disclosure may also be formed by a casting method in which a solution or dispersion containing a fluororesin and an oxide is prepared, and then the solution or dispersion is applied onto a substrate and dried.

[0096] (Metal Laminate) The above sheet can be used as a sheet for a circuit board by laminating it with other substrates. The metal laminate of the present disclosure is a metal laminate having a metal layer provided on one or both sides of the above-mentioned sheet. The metal laminate of the present disclosure can be particularly suitably used for circuit board applications.

[0097] The metal layer is preferably made of one or more metals selected from the group consisting of copper, gold, silver, and platinum. In particular, the metal layer is more preferably made of copper. Copper is preferable because it has a small conductor loss.

[0098] (Metal Laminate Manufacturing Method) The method for producing a metal laminate according to the present disclosure is carried out, for example, by providing a metal layer by dry plating or the like on one or both sides of the sheet containing a fluororesin and an oxide produced as described above. The present disclosure also relates to a method for producing a metal laminate, comprising a step (A) of providing a metal layer by a dry plating method on one or both sides of a sheet containing a fluororesin and an oxide.

[0099] The dry plating method may be any of vacuum deposition, sputtering, and ion plating, among which ion plating is preferred because it can produce a film with strong adhesion. The above methods may be carried out by a general method.

[0100] The metal layer is preferably a layer made of one or more metals selected from the group consisting of copper, gold, silver and platinum. In particular, the metal layer is more preferably a copper layer.

[0101] Moreover, the method for producing a metal laminate of the present disclosure preferably includes a step (B) of heating the sheet to 300 to 400°C. The step (B) may be carried out before or after the step (A).

[0102] By carrying out the heat treatment in step (B), such as baking, the crystallinity of the fluororesin changes and the heat of fusion decreases. The smaller heat of fusion makes the sheet harder, and when an attempt is made to peel off the metal layer, the sheet undergoes interfacial destruction rather than destruction of the base material, resulting in increased tape peel strength. On the other hand, an unfired sheet is soft, and even if the metal is in close contact with the sheet, the base material of the sheet will be destroyed during a tape peel strength test, resulting in low tape peel strength.

[0103] In particular, in step (B), it is preferable to bake the sheet after drying during the production of the sheet. By firing the sheet before forming the metal layer on it, the strength of the sheet can be increased in advance and then the metal layer can be applied, thereby improving the tape peel strength of the resulting metal laminate.

[0104] In the case where the sheet is formed, dried and then fired, the firing step is preferably performed by heating the sheet to a temperature equal to or higher than the melting point of the fluororesin.

[0105] In addition, in step (B), the metal layer may be fired after it is formed. In this case, it is preferable to fire the metal laminate by heating to a temperature equal to or higher than the melting point of the fluororesin. In order to prevent the metal layer from being oxidized during heating, it is preferable to perform the firing in a vacuum or in an inert gas atmosphere.

[0106] In the present disclosure, a metal laminate is obtained by forming a metal layer on the sheet surface by dry plating or the like as described above, and the thickness of the metal layer is 8 μm or less.

[0107] The method for producing a metal laminate of the present disclosure may further include a step (C) of thickening the metal layer formed as described above by a wet plating method. By using a wet plating method, it is possible to increase the thickness of the film in a short time and at low cost. When the above step (C) is included, the above step (B) may be carried out after the step (C).

[0108] Wet plating methods include electrolytic plating and electroless plating. In particular, electroless plating is preferred from the viewpoint of uniform plating coverage. Each of the above methods may be carried out by a general method.

[0109] The metal layer formed by thickening may be the same as or different from the previous metal layer, but is preferably the same as the previous metal layer.

[0110] In the above step (C), the thickness of the entire metal layer after thickening is preferably 8 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. Note that the thickness of the entire metal layer after thickening may exceed 8 μm.

[0111] The metal-clad laminate of the present disclosure may further include layers other than the metal layer and the fluororesin sheet. The layers other than the metal layer and the fluororesin sheet are preferably at least one selected from the group consisting of polyimide, modified polyimide, liquid crystal polymer, polyphenylene sulfide, cycloolefin polymer, polystyrene, epoxy resin, bismaleimide, polyphenylene oxide, modified polyphenylene ether, polyphenylene ether, and polybutadiene.

[0112] The layers other than the metal layer and the sheet are not particularly limited as long as they are made of the above-mentioned resins. The thickness of the layers other than the metal layer and the sheet is preferably within the range of 12.5 to 260 μm.

[0113] The use of the metal laminate of the present disclosure is not particularly limited, and it is suitably used as a circuit board. The present disclosure also relates to a circuit board having the above-mentioned metal laminate. A circuit board is a plate-shaped component for electrically connecting electronic components such as semiconductors and capacitor chips and simultaneously arranging and fixing them in a limited space. There is no particular limitation on the configuration of the circuit board formed from the metal laminate of the present disclosure. The circuit board may be any of a rigid board, a flexible board, and a rigid-flexible board. The circuit board may be any of a single-sided board, a board, a double-sided board, and a multilayer board (such as a built-up board). In particular, it can be suitably used for flexible boards and rigid boards. In particular, it can be suitably used as a high-frequency printed circuit board of 10 GHz or more.

[0114] In the present disclosure, the high-frequency circuit does not only mean a circuit that transmits only high-frequency signals, but also includes a circuit in which a transmission line that transmits a signal other than a high-frequency signal is arranged on the same plane, such as a transmission line that converts a high-frequency signal into a low-frequency signal and outputs the generated low-frequency signal to the outside, or a transmission line for supplying power to drive a high-frequency compatible component. It can also be used as a circuit board for an antenna, a filter, etc. The metal laminate of the present disclosure has a thin metal layer, so it is flexible and can be suitably used as a flexible circuit board that can be bent freely.

[0115] The present disclosure also relates to an antenna formed from the circuit board, and is particularly suitable as a millimeter wave antenna for mobility. The present disclosure also relates to a millimeter wave antenna for mobility formed from the above circuit board.

[0116] In this disclosure, mobility refers to all means and methods related to movement and transportation, including automobiles in general, such as private cars, buses, taxis, and trucks, as well as two-wheeled vehicles such as motorcycles, bicycles, and mopeds, railways, senior cars, and compact personal mobility vehicles for one person.Mobility is not necessarily limited to vehicles that move on the ground, but may also be vehicles that move in the air or underwater, such as aircraft.

[0117] A circuit board can be manufactured by a general method using the above-mentioned metal laminate.

[0118] The metal laminate of the present disclosure is used as an electric / electronic component, for example, an antenna used in electronic devices and communication devices such as ETC, GPS, wireless LAN, and mobile phones, a high-speed transmission connector, a CPU socket, a millimeter wave and quasi-millimeter wave radar such as a collision prevention radar, an RFID tag, a capacitor, an inverter part, a cable covering material, an insulating material for secondary batteries such as lithium ion batteries, a speaker diaphragm, etc.

[0119] Examples of high-speed communication-compatible substrates include base station antenna substrates, antenna distribution substrates, substrates for RRH (Remote Radio Head) which is the radio part of a wireless base station, substrates for the control part or baseband part (BBU: Base Band Unit) of a wireless base station, transceiver substrates for high-speed communication, substrates for RNC (Radio Network Controller), substrates for high-speed transmitters, substrates for high-speed receivers, substrates for high-speed signal multiplexing circuits, substrates for WiFig using the 60 GHz band, substrates for data transfer used in servers for data centers, etc. Examples of high-speed communication-compatible substrates include antenna substrates, for example, substrates for massive multi-element antennas (Massive MIMO) for large-capacity communication required by standards after 5G. Furthermore, examples include receiving antennas for space-transmission wireless power supply using microwaves.

[0120] In dielectric waveguides, materials with low dielectric loss are required to transmit high-frequency millimeter waves or submillimeter waves with low loss. The metal laminate of the present disclosure can be suitably used as an insulating material for dielectric waveguides that transmit millimeter waves, submillimeter waves, and the like. Examples of dielectric waveguide lines include cylindrical dielectric lines, rectangular dielectric lines, elliptical dielectric lines, tubular dielectric lines, image lines, insular image lines, trapped image lines, rib guides, strip dielectric lines, inverted strip lines, H guides, and nonradiative dielectric lines (NRD guides).

[0121] The metal laminate for circuit boards may be a laminate having the above-mentioned sheet, a metal layer, and a base layer. The base layer is not particularly limited, and preferably has a fabric layer made of glass fiber and a resin film layer.

[0122] The glass fiber fabric layer is a layer made of glass cloth, glass nonwoven fabric, or the like. The glass cloth may be commercially available, and is preferably treated with a silane coupling agent to enhance affinity with the fluororesin. The glass cloth may be made of E glass, C glass, A glass, S glass, D glass, NE glass, low dielectric constant glass, etc., and is preferably made of E glass, S glass, or NE glass because of its easy availability. The fiber may be woven in either plain or twill weave. The thickness of the glass cloth is usually 5 to 90 μm, and preferably 10 to 75 μm, but it is preferable to use a glass cloth thinner than the fluororesin film to be used.

[0123] The laminate may use a glass nonwoven fabric as a fabric layer made of glass fibers. The glass nonwoven fabric is a fabric in which short glass fibers are fixed with a small amount of a binder compound (resin or inorganic substance), or a fabric in which the shape is maintained by entangling short glass fibers without using a binder compound, and a commercially available product can be used. The diameter of the short glass fibers is preferably 0.5 to 30 μm, and the fiber length is preferably 5 to 30 mm. Specific examples of the binder compound include resins such as epoxy resin, acrylic resin, cellulose, polyvinyl alcohol, and fluororesin, and inorganic substances such as silica compounds. The amount of the binder compound used is usually 3 to 15 mass % based on the short glass fibers. Examples of the material of the short glass fibers include E glass, C glass, A glass, S glass, D glass, NE glass, and low dielectric constant glass. The thickness of the glass nonwoven fabric is usually 50 μm to 1000 μm, and preferably 100 to 900 μm. In the present application, the thickness of the glass nonwoven fabric refers to a value measured in accordance with JIS P8118:1998 using a digital gauge DG-925 (load 110 grams, face diameter 10 mm) manufactured by Ono Sokki Co., Ltd. In order to increase the affinity with the fluororesin, the glass nonwoven fabric may be treated with a silane coupling agent.

[0124] Most nonwoven glass fabrics have a very high porosity of 80% or more, so it is preferable to use a sheet that is thicker than a sheet made of fluororesin and compress it by pressure.

[0125] The glass fiber fabric layer may be a layer in which a glass cloth and a glass nonwoven fabric are laminated together, whereby the properties of the two fabrics are combined to obtain suitable properties. The glass fiber fabric layer may be in the form of a prepreg impregnated with a resin.

[0126] In the above laminate, the glass fiber fabric layer and the fluororesin sheet may be bonded at the interface, or the glass fiber fabric layer may be partially or entirely impregnated with the fluororesin sheet. Furthermore, a prepreg may be prepared by impregnating a fabric made of glass fiber with the fluororesin composition. The prepreg thus obtained may be further laminated with the above-mentioned fluororesin sheet. In this case, the fluororesin composition used in preparing the prepreg is not particularly limited, and the above-mentioned sheet may be used.

[0127] The resin film used as the substrate layer is preferably a heat-resistant resin film or a thermosetting resin film. Examples of the heat-resistant resin film include polyimide, modified polyimide, liquid crystal polymer, polyphenylene sulfide, etc. Examples of the thermosetting resin include those containing epoxy resin, bismaleimide, polyphenylene oxide, modified polyphenylene ether, polyphenylene ether, polybutadiene, etc.

[0128] The heat-resistant resin film and the thermosetting resin film may contain reinforcing fibers. The reinforcing fibers are not particularly limited, but for example, glass cloth, particularly low dielectric type, is preferable. The heat-resistant resin film and the thermosetting resin film are not particularly limited in terms of dielectric properties, linear expansion coefficient, water absorption coefficient, and other properties, but for example, the dielectric constant at 20 GHz is preferably 3.8 or less, more preferably 3.4 or less, and even more preferably 3.0 or less. The dielectric loss tangent at 20 GHz is preferably 0.0030 or less, more preferably 0.0025 or less, and even more preferably 0.0020 or less. The linear expansion coefficient is preferably 100 ppm / K or less, more preferably 70 ppm / K or less, and even more preferably 40 ppm / K or less. The water absorption coefficient is preferably 1.0% or less, more preferably 0.5% or less, and even more preferably 0.1% or less.

[0129] When a laminate having a sheet and a metal layer is laminated with a base layer such as a resin film layer, the laminate can be laminated by adhering the sheet layer side of the laminate to the base layer. In this case, the sheet layer side of the laminate may be surface-treated before lamination to improve the adhesive performance. The surface treatment here is not particularly limited, and examples thereof include plasma treatment.

[0130] In the laminate, the order in which the metal layer, the substrate, and the above-mentioned sheets are laminated and the manufacturing method are not particularly limited, and a layer configuration according to the purpose can be adopted. Specific examples of the above-mentioned stacking order include a base layer / sheet / metal layer, and a metal layer / sheet / base layer / sheet / metal layer. If necessary, other layers may also be included. EXAMPLES

[0131] The present disclosure will now be described in detail with reference to examples. In the following examples, unless otherwise specified, "parts" and "%" represent "parts by mass" and "% by mass", respectively.

[0132] The silica used in each of the Examples and Comparative Examples was SC6500-SQ (average particle size: 2.1 μm) manufactured by Admatechs Co., Ltd., and spherical silica obtained by surface-treating SC6500-SQ (average particle size: 2.1 μm) manufactured by Admatechs Co., Ltd. with 3-aminopropyltriethoxysilane (treatment amount of 1% by mass based on the mass of silica particles) as shown in Table 1.

[0133] The fluororesin particles (PTFE) used in each example had the following properties. Average particle size: 500μm Apparent density: 460g / L Standard specific gravity: 2.17

[0134] (Examples 1 to 4) (Paste extrusion molding) The fluororesin particles (PTFE) and silica were weighed out in the prescribed amounts in the ratio shown in Table 1 and mixed in a mixer in the presence of dry ice. The temperature during mixing was -10°C or lower. 21% oil (Isopar H) was added to the obtained mixed powder, mixed, and aged for about 5 hours. The aged composition was preformed under a pressure of 3 MPa, and the preformed body was extruded at 40° C. and 50 mm / min to obtain an extrusion sample. The extruded sample was rolled with two rolls (roll gap: set to 500 to 80 μm) to obtain a sample with a film thickness of 125 μm. The sample was dried at 200° C. for 2 hours and calcined at 360° C. for 15 minutes to obtain a sheet.

[0135] (Ion plating) The sheet was introduced into a physical vapor deposition (PVD) apparatus, and a copper film was formed by ion plating under the following conditions to obtain a metal laminate. The thickness of the copper layer was 0.113 μm. RF output: 100W, deposition pressure: 4.0×10 -2 Pa, deposition rate: 16.1 Å / S

[0136] (Examples 5 to 8) (Vacuum deposition) Each of the sheets used in Examples 1 to 4 was introduced into a physical vapor deposition (PVD) apparatus, and a copper film was formed by vacuum deposition under the following conditions to obtain a metal laminate. The thickness of the copper layer was 0.102 μm. RF output: None, deposition pressure: 1.15×10 -2 Pa, deposition rate: 21.9 Å / S

[0137] (Examples 9 to 12) Metal laminates were obtained in the same manner as in Example 1, except that no firing was performed during sheet molding, and instead, a film was formed by ion plating, and then firing was performed by heating at 360°C for 15 minutes under vacuum.

[0138] (Examples 13 to 16) A metal laminate was obtained in the same manner as in Example 5, except that no firing was performed during sheet molding, and instead, a film was formed by vacuum deposition, and then firing was performed by heating at 360°C for 15 minutes under vacuum.

[0139] Comparative Example 1 A metal laminate was obtained in the same manner as in Example 1, except that silica was not used.

[0140] Comparative Example 2 A metal laminate was obtained in the same manner as in Example 9, except that silica was not used.

[0141] Comparative Example 3 (PFA sheet molding) PFA (TFE / PAVE (mass%): 94.6 / 5.4, melting point: 310°C, MFR: 14 g / 10 min) was extruded at 350°C to obtain a sheet with a thickness of 100 µm. (Ion plating) A copper layer was formed on the obtained PFA sheet by ion plating in the same manner as in Example 1 to obtain a metal laminate.

[0142] Comparative Example 4 (FEP sheet molding) FEP (TFE / HFP (mass%): 90 / 10, melting point: 270°C, MFR: 6 g / 10 min) was extruded at 300°C to obtain a sheet with a thickness of 100 µm. (Ion plating) A copper layer was formed on the obtained FEP sheet by ion plating in the same manner as in Example 1 to obtain a metal laminate.

[0143] Comparative Example 5 A metal laminate was obtained in the same manner as in Example 5, except that silica was not used.

[0144] Comparative Example 6 A metal laminate was obtained in the same manner as in Example 13, except that silica was not used.

[0145] Comparative Example 7 A copper layer was formed by vacuum deposition in the same manner as in Example 5, except that the PFA sheet obtained in Comparative Example 3 was used, to obtain a metal laminate.

[0146] Comparative Example 8 A copper layer was formed by vacuum deposition in the same manner as in Example 5, except that the FEP sheet obtained in Comparative Example 4 was used, to obtain a metal laminate.

[0147] Comparative Example 9 A metal laminate was obtained in the same manner as in Example 4, except that no firing was performed during sheet forming and ion plating.

[0148] Comparative Example 10 A metal laminate was obtained in the same manner as in Example 8, except that no firing was performed during sheet forming and vacuum deposition.

[0149] Each of the obtained samples was measured and evaluated based on the following criteria. The evaluation of the sheets was carried out on the collected sheets by the following method.

[0150] [Metal layer thickness] The thickness of the metal layer was measured using a stylus type surface roughness tester.

[0151] [Tape peel strength] Using Nichiban Cellotape (registered trademark) (tape width: 18 mm) used in the JIS-K5600 adhesion test (cross-cut method), a 15 mm long cellotape was attached to the copper layer of the metal laminate without any air bubbles. The attached tape was peeled off at a 90° angle, and the copper layer (area 270 mm2) of the metal laminate to which the cellotape had been attached was removed. 2 The area of ​​copper peeled off from the test piece was calculated using image analysis (Python) and evaluated as follows. 1: 95% or more of the copper has peeled off 2: 60% or more but less than 95% of the copper has peeled off 3: 40% or more but less than 60% of the copper has peeled off 4: 5% or more but less than 40% of the copper has peeled off 5: Less than 5% copper, peeled off

[0152] [Etching of Metal Laminates] The metal laminate was etched with an aqueous solution of ferric chloride, washed with running fresh water for 2 to 5 minutes, washed with distilled water, and dried in a thermostatic chamber at 80±3°C for approximately 60 minutes to recover a single sheet (dielectric layer).

[0153] [Sheet thickness] The thickness of the sheet was measured using a micrometer.

[0154] [XPS measurement of sheet surface] The measurements were performed using a scanning X-ray photoelectron spectroscopy (XPS / ESCA) PHI5000VersaProbeII (ULVAC-PHI, Inc.).

[0155] [Melting point of fluororesin and heat of fusion of sheet (DSC measurement)] The heat of fusion and the melting point were measured using a DSC (Hitachi High-Tech DSC7000X) when the temperature was increased from 230°C to 380°C at a rate of 10°C / min.

[0156] [Dissipation factor of sheet (Df)] The dielectric constant and dielectric loss tangent were measured at 25°C and 10 GHz using a split cylinder type dielectric constant / dielectric loss tangent measuring device (manufactured by EM Lab).

[0157] [Coefficient of linear expansion (CTE) of sheet] TMA measurements were performed in tensile mode using a TMA-7100 (Hitachi High-Tech Science Corporation). A fluororesin sheet cut to a length of 20 mm, width of 5 mm, and thickness of 150 μm was used as a sample piece. The chuck distance was set to 10 mm, and the linear expansion coefficient was calculated from the displacement of the sample from 0 to 150°C at a heating rate of 2°C / min while applying a load of 49 mN. The results are shown in Tables 1 and 2.

[0158] [Table 1]

[0159] [Table 2]

[0160] (Example 17) The metal laminate obtained in Example 2 was subjected to copper sulfate plating (step (C)) to form a conductor layer with a thickness of 18 μm. The obtained metal laminate was subjected to a tape peel strength test, and the strength was confirmed to be 5.

[0161] From the above results, the metal laminates of the Examples have high tape peel strength and excellent performance in terms of adhesion between the sheet and the metal layer. Furthermore, the results of the XPS measurement show that the silica-added sheet has silica present on its surface. [Industrial Applicability]

[0162] The metal laminate of the present disclosure can be suitably used as a circuit board, and can be particularly suitably used for a millimeter wave antenna.

Claims

1. A metal laminate comprising a sheet containing a fluororesin and an oxide, the sheet having a metal layer provided on one or both sides thereof, the metal layer having a thickness of 8 μm or less and a tape peel strength of 3 or more.

2. A metal laminate plate having a metal layer provided on one or both sides of a sheet containing a fluororesin and an oxide, wherein the melting point of the fluororesin is 320°C or higher, the heat of fusion of the sheet is 20 mJ / mg or less, and the film thickness of the metal layer is 8 μm or less.

3. 3. The metal laminate according to claim 1, wherein the sheet has a coefficient of linear expansion (CTE) of 100 ppm / K or less.

4. 3. The metal laminate according to claim 1, wherein the fluororesin is polytetrafluoroethylene.

5. 3. The metal laminate according to claim 1, wherein the oxide is silica.

6. 6. The metal laminate of claim 5, wherein said silica is in the form of spherical particles.

7. 6. The metal laminate according to claim 5, wherein the silica is silica particles treated with a silane coupling agent.

8. 6. The metal laminate according to claim 5, wherein the average particle size of the silica is 10 μm or less.

9. 3. The metal laminate according to claim 1, wherein the content of the oxide is 30 mass% or more based on the total amount of the sheet.

10. 3. The metal laminate according to claim 1, wherein the metal layer is formed of one or more metals selected from the group consisting of copper, gold, silver and platinum.

11. 3. The metal laminate according to claim 1, wherein the metal layer is made of copper.

12. 3. The metal laminate according to claim 1, wherein the sheet has a dielectric tangent value of 0.0015 or less at 10 GHz.

13. 3. The metal laminate according to claim 1, wherein the sheet has a thickness of 5 to 250 μm.

14. A method for producing a metal laminate, comprising: (A) providing a metal layer on one or both sides of a sheet containing a fluororesin and an oxide by a dry plating method.

15. A method for producing a metal laminate, comprising the step (A) of providing a metal layer on one or both sides of a sheet containing a fluororesin and an oxide by any one of a vacuum deposition method, a sputtering method, and an ion plating method.

16. The method for producing a metal laminate according to claim 14 or 15, further comprising a step (B) of heating the sheet to 300 to 400°C.

17. The method for producing a metal laminate according to claim 14 or 15, wherein the metal layer is a copper layer.

18. The method for producing a metal laminate according to claim 14 or 15, further comprising a step (C) of thickening the provided metal layer by a wet plating method.

19. A circuit board comprising the metal laminate according to claim 1 or 2.

20. 20. An antenna formed from the circuit board of claim 19.

21. A millimeter wave antenna for mobility formed from the circuit board according to claim 19.

Citation Information

Patent Citations

  • Fluororesin board, wiring board, and manufacturing methods of respective same boards

    JP2004356547A

  • Method of manufacturing flexible printed circuit board

    JP2010192861A

  • Printed wiring board for high frequency use

    JP2015008260A

  • Two-layer flexible substrate, method for manufacturing the two-layer flexible substrate, and flexible printed wiring board manufactured from the two-layer flexible substrate

    WO2008090654A1

  • Metal-clad laminated plate

    WO2021199811A1