Composition for vulcanization adhesives
A water-based vulcanized adhesive using a vinyl silane coupling agent and water dispersion polyolefin resin addresses environmental and health concerns in conventional adhesives, ensuring effective bonding of metal and nonpolar rubber.
Patent Information
- Application Number
- JP2023083079
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-19
Smart Images

Figure 2024166758000006 
Figure 2024166758000001 
Figure 2024166758000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a vulcanizable adhesive composition. [Background technology]
[0002] As a method for bonding metal and non-polar rubber, for example, Patent Document 1 discloses a method in which an adhesive layer is interposed between an unvulcanized rubber material and a metal. The adhesive layer has a two-layer structure having an undercoat adhesive layer and a topcoat adhesive layer. A phenol resin-based adhesive is used as the undercoat adhesive, and an adhesive containing chlorinated polyethylene is used as the topcoat adhesive. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2004-27068 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the conventional techniques described above, organic solvents are used as the adhesive contained in the adhesive layer. Therefore, there are concerns about environmental pollution due to the volatilization of these solvents and health hazards to workers. Therefore, the conventional techniques described above have room for improvement from the viewpoints of the environment and hygiene and safety in the workplace.
[0005] An object of one aspect of the present invention is to provide a vulcanizable adhesive composition that maintains conventional adhesive performance, while suppressing environmental pollution and providing excellent hygiene and safety in the workplace. [Means for solving the problem]
[0006] In order to solve the above problems, a composition for a vulcanizable adhesive according to one embodiment of the present invention contains a vinyl silane coupling agent, a water-dispersed polyolefin resin, and water. Effect of the Invention
[0007] According to one aspect of the present invention, it is possible to realize a vulcanization adhesive composition that maintains conventional adhesive performance while being aqueous, thereby suppressing environmental pollution and being excellent in terms of hygiene and safety in the workplace. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a schematic diagram showing the surface of a sample subjected to a peel test in the examples of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and various modifications are possible within the described scope. The technical scope of the present invention also includes embodiments in which the technical means disclosed in the different embodiments are appropriately combined. In this specification, "A to B" representing a numerical range means "A or more, B or less."
[0010] <1. Composition for vulcanizing adhesive> (Vinyl silane coupling agent) The vulcanization adhesive composition according to one embodiment of the present invention contains a vinyl silane coupling agent. The vinyl silane coupling agent is not particularly limited, but examples thereof include vinyl trimethoxy silane ((CH3O)3SiCH=CH2), vinyl triethoxy silane ((C2H5O)3SiCH=CH2), and the like.
[0011] The lower limit of the amount of the vinyl silane coupling agent in the vulcanizable adhesive composition is preferably 1% by weight or more, more preferably 2% by weight or more, and even more preferably 3% by weight or more, based on 100% by weight of the total weight of the vulcanizable adhesive composition. The upper limit may be 5% by weight, and is preferably 4% by weight or less, based on 100% by weight of the total weight of the vulcanizable adhesive composition.
[0012] (Water-dispersed polyolefin resin) The vulcanization adhesive composition according to one embodiment of the present invention contains a water-dispersed polyolefin resin. In this specification, the water-dispersed polyolefin resin refers to an aqueous dispersion in which a modified polyolefin resin is dispersed in water. As the water-dispersed polyolefin resin, a commercially available product can be used as is. Examples of commercially available water-dispersed polyolefin resins include SB-1230N (Arrowbase (registered trademark), manufactured by Unitika Co., Ltd.), SE-1200 (Arrowbase (registered trademark), manufactured by Unitika Co., Ltd.), and SD-1200 (Arrowbase (registered trademark), manufactured by Unitika Co., Ltd.).
[0013] (water) The vulcanization adhesive composition according to one embodiment of the present invention contains water. As the water, ion-exchanged water, distilled water, RO water, etc. can be used. Here, "RO water" refers to water from which impurities have been removed through an RO (=Reverse Osmosis) membrane.
[0014] The lower limit of the amount of water in the vulcanizable adhesive composition is preferably 40% by weight or more, and more preferably 60% by weight or more, based on the total weight of the vulcanizable adhesive composition being 100% by weight. The upper limit of the amount of water in the vulcanizable adhesive composition may be 95% or less, based on the total weight of the vulcanizable adhesive composition being 100% by weight.
[0015] (Surfactant) The vulcanization adhesive composition according to one embodiment of the present invention may contain a surfactant. Although known surfactants can be used as the surfactant, it is preferable to use a nonionic surfactant from the viewpoint of adhesion. The nonionic surfactant is not particularly limited, but examples thereof include polyoxyethylene sorbitan monolaurate and polyoxyethylene lauryl ether.
[0016] (Water-soluble solvent) The vulcanization adhesive composition according to one embodiment of the present invention may further contain a water-soluble solvent. Examples of the water-soluble solvent include propylene glycol, ethylene glycol, ethylene glycol monobutyl ether, etc. Among these, propylene glycol is preferred from the viewpoint of hygiene and safety.
[0017] [Weight ratio of components contained in the vulcanizable adhesive composition] From the viewpoint of adhesion between metal and non-polar rubber, the weight ratio of the vinyl silane coupling agent and the water-dispersed polyolefin resin contained in the composition for vulcanization adhesive is preferably 1:2 to 3:1, and more preferably 3:4 to 2:1. When the water-dispersed polyolefin resin contained in the composition for vulcanization adhesive is in the form of an aqueous solution, the weight of water contained as a solvent in the water-dispersed polyolefin resin is included in the weight of the water-dispersed polyolefin resin in the above weight ratio.
[0018] When the vulcanization adhesive composition contains a water-soluble solvent, the blending amount of the water-soluble solvent may be more than 0% by weight to 55% by weight, and is preferably about 30% by weight, based on the total weight of the vulcanization adhesive composition being 100% by weight. When the composition is blended with only a water-soluble solvent without blending water, the adhesiveness of the resulting vulcanization adhesive composition is not sufficient. When both water and a water-soluble solvent are blended, if the blending amount of the water-soluble solvent is within the above range, the resulting vulcanization adhesive composition has sufficient adhesiveness, but it is preferable from the viewpoint of adhesiveness that the ratio of the water-soluble solvent to water is small within the above range. Note that, when the water-dispersed polyolefin resin contained in the vulcanization adhesive composition is in the form of an aqueous solution, the weight of water contained as a solvent in the aqueous solution of the water-dispersed polyolefin resin is not included in the weight of water contained in the vulcanization adhesive composition in the above weight ratio.
[0019] The weight ratio of the vinyl silane coupling agent to the surfactant contained in the vulcanization adhesive composition is preferably 4:1 to 4:5, and more preferably 4:1 to 4:3, from the viewpoint of adhesion between metal and non-polar rubber.
[0020] As described above, the vulcanization adhesive composition according to one embodiment of the present invention is aqueous and therefore has little adverse effect on the human body and the environment, and therefore can contribute to the achievement of the Sustainable Development Goals (SDGs), such as Goal 12 "Ensure sustainable consumption and production patterns" and Goal 13 "Take urgent action to combat climate change and its impacts."
[0021] Moreover, according to the vulcanization adhesive composition according to one embodiment of the present invention, metal and non-polar rubber can be bonded. The non-polar rubber is preferably a peroxide vulcanization system shaped by peroxide vulcanization, and examples thereof include ethylene-propylene-diene copolymer rubber (EPDM) and styrene-butadiene copolymer rubber (SBR). The bonding method is not particularly limited, and for example, the vulcanization adhesive composition is applied to a metal that has been subjected to a chemical conversion treatment or a metal that has been subjected to a zinc plating treatment, and dried at room temperature for 3 to 7 minutes. Then, a baking treatment is performed at 160 to 200°C for 5 to 30 minutes. Next, an unvulcanized compound of non-polar rubber is bonded to the metal that has been subjected to the baking treatment, and press vulcanization is performed at 160 to 200°C for 2 to 15 minutes, thereby vulcanization bonding the metal and the non-polar rubber.
[0022] Furthermore, in order to bond metal and non-polar rubber, the conventional technology requires the adhesive to be applied in a top coat and a bottom coat. On the other hand, the vulcanization adhesive composition according to one embodiment of the present invention can bond metal and non-polar rubber in a single layer. This improves work efficiency and reduces costs such as electricity costs.
[0023] <2. Vulcanizing adhesive> An embodiment of the present invention also includes a vulcanizing adhesive comprising the composition for vulcanizing adhesive according to the embodiment of the present invention. The vulcanizing adhesive may be the composition for vulcanizing adhesive according to the embodiment of the present invention itself.
[0024] <3. Summary> The present invention includes the following configurations. <1> A composition for vulcanization adhesive comprising a vinyl silane coupling agent, a water-dispersed polyolefin resin, and water. <2> The vinyl silane coupling agent and the water-dispersed polyolefin resin are contained in a weight ratio of 1:2 to 3:1. <1> The vulcanizable adhesive composition according to claim 1 . <3> Further comprising a surfactant, <1> or <2> The vulcanizable adhesive composition according to claim 1 . <4> The surfactant is a nonionic surfactant. <3> The vulcanizable adhesive composition according to claim 1 . <5> Further comprising a water-soluble solvent, <1> ~ <4> 13. The vulcanizable adhesive composition according to claim 12, <6> The water-soluble solvent is propylene glycol. <5> The vulcanizable adhesive composition according to claim 1 . <7> Used for vulcanization adhesion between metal and non-polar rubber. <1> ~ <6> 13. The vulcanizable adhesive composition according to claim 12, <8> <1> ~ <7> A vulcanizable adhesive comprising the vulcanizable adhesive composition according to any one of the above items. EXAMPLES
[0025] Hereinafter, one embodiment of the present invention will be described in detail with reference to examples, although the present invention is not limited to these examples.
[0026] Materials used in the Examples and Comparative Examples Vinyl silane coupling agent Vinyltrimethoxysilane: KBM-1003 (Shin-Etsu Chemical Co., Ltd.) Mercaptosilane coupling agent 3-Mercaptopropyltrimethoxysilane: KBM-803 (Shin-Etsu Chemical Co., Ltd.) Water-dispersed polyolefin resin SB-1230N (Arrow Base (registered trademark), manufactured by Unitika Ltd.) ●Water-soluble phenolic resin Resole type phenolic resin (highly water-soluble phenolic resin aqueous solution): BRL-141B (manufactured by Aica Kogyo Co., Ltd.) Surfactants Polyoxyethylene sorbitan monolaurate (non-ionic surfactant): Sorbon T-20 (manufactured by Toho Chemical Industry Co., Ltd.) ●Water Ion-exchanged water Water-soluble solvent Propylene glycol: Fujifilm Wako Pure Chemical Industries, Ltd. [Examples 1 to 15, Comparative Examples 1 to 5] The components shown in the following Tables 1 to 5 were mixed to obtain compositions for vulcanization adhesives, and the compositions were applied onto metal plates. The metal plates used were hollow, disk-shaped metal plates made of chemically treated metal plates (SPCC) or galvanized metal plates (SECC).
[0027] After coating, the coating was dried at room temperature for 5 minutes and baked for 10 minutes at 180°C. Next, an unvulcanized EPDM compound was bonded onto the metal plate that had been baked, and press-vulcanized at 180°C for 4 minutes to obtain a sample.
[0028] [Reference example 1] The unvulcanized compound to be bonded to the metal plate was changed to an unvulcanized NBR compound, and press vulcanization was carried out at 190°C for 2 minutes to obtain a sample.
[0029] (Evaluation of Adhesion) A needle-based peel test was performed on the obtained sample, and the rubber remaining rate was visually confirmed. Specifically, as shown in FIG. 1, the tip of a needle was pressed against the surface of the sample (1) (the side on which the unvulcanized EPDM or NBR compound was vulcanized and molded) to make six scratches (2). Thereafter, the areas where rubber remained other than the areas scratched by the needle tip were visually confirmed, and the rubber remaining rate was calculated based on the following formula. It can be said that the higher the rubber remaining rate, the better the adhesion. The evaluation results of adhesion are shown in Tables 1 to 5. (Area where rubber remains after peel test) / (Area where rubber is molded before peel test) x 100
[0030] [Table 1]
[0031] As shown in Table 1, when a sample was prepared using a mercaptosilane coupling agent as the silane coupling agent and a water-soluble phenolic resin as the resin, if the target rubber to be bonded was nitrile butadiene rubber (NBR), the rubber residual rate was 100% whether the metal plate was SPCC or SECC, and it was confirmed that the metal and rubber could be bonded (Reference Example 1).On the other hand, when the target rubber was a non-polar rubber (ethylene-propylene-diene copolymer rubber (EPDM)), the rubber residual rate was 0% whether the metal plate was SPCC or SECC, and it was confirmed that the metal and non-polar rubber did not adhere to each other (Comparative Example 1).
[0032] Furthermore, from the results of the adhesion evaluation of Comparative Example 2, it was confirmed that when a sample was prepared using a vinyl silane coupling agent as the silane coupling agent and a water-soluble phenolic resin as the resin, metal and non-polar rubber did not adhere to each other.
[0033] [Table 2]
[0034] From Examples 1 and 2, it was confirmed that metal and non-polar rubber can be bonded even when only water is used as the solvent without using a water-soluble solvent.
[0035] [Table 3]
[0036] In Comparative Example 3, which does not contain a vinyl silane coupling agent, and Comparative Example 4, which does not contain a water-dispersed polyolefin resin, the rubber residual rate was 0% in both SPCC and SECC metal plates in the adhesive evaluation. These results make it clear that both a vinyl silane coupling agent and a water-dispersed polyolefin resin are necessary to bond metal and non-polar rubber.
[0037] It was also confirmed that Examples 1, 4 to 8 had a higher rubber residual rate when the metal plate was either SPCC or SECC, compared with Examples 3 and 9. That is, it was revealed that when the vinyl silane coupling agent and the water-dispersed polyolefin resin were contained in a weight ratio of 1:2 to 3:1, the rubber residual rate was high and excellent adhesion was achieved.
[0038] [Table 4]
[0039] In Comparative Example 5, the rubber residual rate was 0% for both SPCC and SECC, confirming that metal and non-polar rubber do not adhere to each other when water is not used as a solvent and only a water-soluble solvent is used.
[0040] [Table 5]
[0041] From Example 11, it was confirmed that metal and non-polar rubber can be bonded even when a surfactant is not blended. Also, from a comparison of Example 11 with Examples 2 and 12 to 15, it was confirmed that the rubber residual rate tends to be higher when a surfactant is blended compared to when a surfactant is not blended. Furthermore, from a comparison of Examples 12 to 14 with Examples 2 and 15, it was confirmed that if the amount of surfactant blended is too large, the rubber residual rate tends to be slightly lower. [Industrial Applicability]
[0042] The present invention can be utilized as a vulcanizing adhesive. [Explanation of symbols]
[0043] 1: Sample 2: Needle tip scratches
Claims
1. A composition for vulcanization adhesive comprising a vinyl silane coupling agent, a water-dispersed polyolefin resin, and water.
2. 2. The vulcanizable adhesive composition according to claim 1, comprising the vinyl silane coupling agent and the water-dispersed polyolefin resin in a weight ratio of 1:2 to 3:
1.
3. 10. The vulcanizable adhesive composition of claim 1 further comprising a surfactant.
4. 4. The vulcanizable adhesive composition of claim 3, wherein the surfactant is a non-ionic surfactant.
5. The vulcanizable adhesive composition of claim 1 further comprising a water-soluble solvent.
6. 6. The vulcanizable adhesive composition according to claim 5, wherein the water-soluble solvent is propylene glycol.
7. The vulcanization adhesive composition according to any one of claims 1 to 6, which is used for vulcanization adhesion between metal and non-polar rubber.
8. A vulcanizable adhesive comprising the vulcanizable adhesive composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Rubber composition and composite material
JP1997302190A
Rubber and metal bonding method and structure using the same
JP2001260235A
Improved adhesive composition containing sulfur-impregnated particulate solid
JP2015534592A
Vulcanization adhesive and composite formed article
WO2003035786A1
Improved bonding composition comprising a sulfur impregnated particulate solid
WO2014040645A1