Melting bag, lump-like body packaging hot-melt adhesive agent using the same, wraparound label, and pet bottle container
The melt bag with a resin composition of styrene copolymer, ethylene-vinyl copolymer, and silicone oil addresses blocking issues in hot melt adhesives, enhancing workability and environmental sustainability by preventing lump adhesion and maintaining adhesive strength.
Patent Information
- Application Number
- JP2023083148
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-29
AI Technical Summary
Existing hot melt adhesives face issues with lump blocking and require release materials for handling, leading to environmental burdens and reduced workability, with existing physical and chemical countermeasures failing to effectively prevent blocking.
A melt bag composed of a resin composition containing styrene copolymer, ethylene-vinyl copolymer, and silicone oil, with specific molecular weight and viscosity ranges, provides superior blocking resistance and adhesive strength, eliminating the need for release materials.
The melt bag effectively prevents blocking and maintains adhesive strength, reducing environmental impact and improving work efficiency by eliminating the need for release materials.
Smart Images

Figure 2024166801000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a melting bag, a mass in which a hot melt adhesive is packaged using the melting bag, a body-wrapped label, and a PET bottle container. [Background technology]
[0002] Hot melt adhesives are melted and bonded to objects, and then cooled down, and the adhesive function is immediately apparent, so the advantage of not needing a curing period has been rediscovered, and their use in packaging and industrial applications is expanding. In response to recent social changes that emphasize reducing the burden on the environment, the advantage of not needing a solvent or drying process during use has also been rediscovered, and their use is continuing to expand.
[0003] As the range of application of hot melt expands, there is a demand for improved workability. In the summer, hot melt blocks stick together (blocking), and when removing them from the packed cardboard boxes, etc., they become huge blocks, which significantly reduces workability. Therefore, hot melts that are sticky at room temperature in particular are packed, transported, and stored in a state wrapped in release paper or release film, which is peeled off and discarded when the hot melt is used, but the disposal of these release materials has also come to be seen as an environmental burden.
[0004] Therefore, a specification called a melting bag was developed in which hot melt is packaged in a hard material and the hot melt is melted while still packaged when it is used (Patent Document 1). This avoids the environmental burden of disposing of the release material, and also eliminates the work of peeling off the release material every time a lump of hot melt is melted, dramatically improving work efficiency.
[0005] In recent years, measures have been taken to prevent blocking, such as increasing the strength of the melting bag (Patent Document 2) or embossing the shape (Patent Document 3). However, these methods have the problem of being unable to completely prevent blocking between the lumps of hot melt adhesive wrapped in the melting bag, and so not only physical measures but also chemical measures have been required. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2004-002581 A [Patent Document 2] WO2014 / 194087 publication [Patent Document 3] JP 2019-065164 A Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, the present invention aims to provide a melting bag which has better blocking resistance between lumps than conventional ones through a chemical approach, and in which the anti-blocking agent does not adversely affect the adhesive properties of the hot melt adhesive, and a mass, a body-wrapped label, and a PET bottle container in which hot melt adhesive is packaged using the same. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. That is, an embodiment of the present invention is a melt bag formed from a resin composition containing at least one of a styrene-based copolymer (A1) and an ethylene-vinyl-based copolymer (A2), and a silicone oil (B).
[0009] Another embodiment of the present invention is the melt bag described above, which contains 0.1 to 10 mass % of silicone oil (B) based on 100 mass % of the resin composition.
[0010] Another embodiment of the present invention is the melting bag, wherein the molecular weight of the silicone oil (B) calculated from the kinetic viscosity is 650 or more and 100,000 or less.
[0011] Another embodiment of the present invention is the melt bag, wherein the thickness is 25 to 500 μm.
[0012] Another embodiment of the present invention is the melt bag, which is for packaging hot melt adhesive.
[0013] Another embodiment of the present invention is a mass in which a hot melt adhesive is packaged in a melt bag, the melt bag being the mass described above.
[0014] Another embodiment of the present invention is the above lump, wherein the difference between the softening point of the hot melt adhesive and the softening point of the melting bag is within 50°C.
[0015] Another embodiment of the present invention is a body wrap label having a base material and a sheet-like molding of the lump laminated on a part or the whole surface of the base material.
[0016] Another embodiment of the present invention is a container having the above-mentioned body-wrapped label attached thereto.
[0017] Another embodiment of the present invention is the container, the material of which is polyethylene terephthalate. Effect of the Invention
[0018] According to the present invention described above, it is possible to provide a melting bag having better blocking resistance and adhesive strength than conventional bags, and a mass, a body-wrap label, and a PET bottle container in which a hot melt adhesive is packaged using the melting bag. [Brief description of the drawings]
[0019] [Figure 1] FIG. 2 is a schematic cross-sectional view partially showing the lump of the present invention. [Diagram 2] Graph showing the relationship between dynamic viscosity and molecular weight (see page 5 of "Shin-Etsu Silicones: KF-96 Performance Test Results") DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The melting bag of the present invention, and the mass, body-wrapped label and PET bottle container using the same will be described in more detail below, but the present invention is not limited thereto. The hot melt adhesive packed in the melting bag is called a lump. Note that the hot melt adhesive includes hot melt pressure sensitive adhesives. In this specification, the term "molecular weight" means the average molecular weight.
[0021] In this specification, a numerical range specified by using "~" includes the numerical values before and after "~" as the lower and upper limit values. In this specification, hot melt adhesives may be abbreviated as "hot melt". Unless otherwise noted, the various components appearing in this specification may be used independently as a single type or as a combination of two or more types. Moreover, unless otherwise specified, "parts" and "%" represent "parts by mass" and "% by mass", respectively.
[0022] <Melting bag> The melt bag of the present invention is preferably used for packaging hot melt adhesives, but is not limited thereto as long as it can contribute technically to articles other than hot melt adhesives. The melting bag contains at least one of a styrene copolymer (A1) and an ethylene-vinyl copolymer (A2), and a silicone oil (B). A material (resin composition) containing at least one of a styrene copolymer (A1) and an ethylene-vinyl copolymer, and a silicone oil (B) is heated and melted, and a film can be formed (manufactured) by a known method.
[0023] The softening point of the melting bag is preferably 50° C. or higher as a lower limit, more preferably 60° C. or higher, even more preferably 70° C. or higher, and particularly preferably 80° C. or higher as a lower limit. The softening point is preferably 150° C. or lower, more preferably 130° C. or lower, even more preferably 110° C. or lower, and particularly preferably 100° C. or lower as an upper limit. When the softening point is within the above range, blocking resistance and adhesive strength are easily exhibited. The softening point is measured in accordance with JIS K-2207 (petroleum asphalt) 6.4 Softening point test method (ring and ball method).
[0024] The thickness of the melting bag is preferably 25 to 500 μm, more preferably 50 to 500 μm, further preferably 50 to 300 μm, and particularly preferably 50 to 200 μm. When the thickness is within the above range, it is easy to achieve both blocking resistance and adhesive strength.
[0025] The amount of volatile organic compounds (VOCs) contained in the melting bag is preferably 3% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, and preferably substantially free. By keeping the amount of VOCs within the above range, the melting bag is easily adapted to applications where hygiene is important, such as the food and medical industries.
[0026] ≪Resin composition≫ In the present invention, the resin composition refers to a material for forming a melt bag, and contains at least one of a styrene-based copolymer (A1) and an ethylene-vinyl-based copolymer (A2), and a silicone oil (B).
[0027] <Styrene-based copolymer (A1)> Styrene-based copolymer (A1) is a type of thermoplastic elastomer. Thermoplastic elastomers are elastic materials that have the same properties as vulcanized rubber at room temperature, and at high temperatures, they are polymeric materials that can be molded using existing molding machines, just like ordinary thermoplastic resins. Thermoplastic elastomers have both elastic rubber components (soft segments: soft phase) in the molecule and molecular restraint components (hard segments: hard phase) to prevent plastic deformation, so they have properties intermediate between rubber and plastic. Styrene copolymers generally have a polystyrene block and a rubber middle block, with the polystyrene portion forming a physical crosslink (domain) and becoming the crosslinking point, and the middle rubber block giving the product rubber elasticity. The middle soft segment includes polybutadiene (B), polyisoprene (I) and polyolefin elastomers (ethylene-propylene (EP), ethylene-butylene (EB), butylene-butadiene (BB)), and depending on the arrangement with the hard segment polystyrene (S), they are divided into linear type and branched type (radial type).
[0028] Examples of styrene-based copolymers include styrene-butadiene-styrene block copolymer (hereinafter sometimes abbreviated as SBS), styrene-ethylene / butylene-styrene block copolymer (hereinafter sometimes abbreviated as SEBS), styrene-ethylene / propylene-styrene block copolymer (hereinafter sometimes abbreviated as SEPS), styrene-isoprene-styrene block copolymer (hereinafter sometimes abbreviated as SIS), and styrene-butylene / butadiene-styrene block copolymer (hereinafter sometimes abbreviated as SBBS).
[0029] The styrene copolymer (A1) preferably has a styrene content of 10 to 50 mass%, more preferably a styrene content of 15 to 45 mass%, and even more preferably a styrene content of 20 to 40 mass%. When the styrene content is within this range, blocking resistance is excellent, and it is easy to balance with the adhesive strength of the hot melt adhesive. The styrene content is the content (mass %) of styrene in 100 mass % of the styrene-based copolymer.
[0030] When the styrene copolymer (A1) is used, it is preferable to further contain a process oil, a tackifier, and a wax. By containing these, the melting bag itself can have performance close to that of a hot melt adhesive, which is preferable.
[0031] The weight average molecular weight (Mw) of the styrene-based copolymer (A1) is preferably 10,000 to 300,000, more preferably 50,000 to 200,000, further preferably 80,000 to 150,000, and particularly preferably 100,000 to 150,000. By setting the molecular weight within the above range, it is easy to achieve both blocking resistance and adhesive strength. The weight average molecular weight is a value calculated as polystyrene by measuring by gel permeation chromatography (GPC).
[0032] The content of the styrene copolymer (A1) is preferably 5 to 70 mass%, more preferably 10 to 60 mass%, and even more preferably 10 to 50 mass%, based on 100 mass% of the resin composition. By containing the styrene copolymer (A1) in the above range, it is easy to achieve both blocking resistance and adhesive strength.
[0033] <Ethylene-vinyl copolymer (A2)> The ethylene-vinyl copolymer (A2) in the present invention is a type of thermoplastic elastomer, similar to the styrene copolymer (A1). The ethylene moiety is a hard segment, and the vinyl moiety is a soft segment, and is used as a hot melt material by utilizing its high adhesiveness. The vinyl moiety is generally derived from vinyl acetate, and the ratio of the ethylene moiety in the entire resin and the ratio of the vinyl moiety are appropriately adjusted to obtain the desired performance. These ethylene-vinyl copolymers may be used alone or in combination of two or more kinds.
[0034] The vinyl content of the ethylene-vinyl copolymer (A2) is preferably 1 to 30 mass%, more preferably 2 to 20 mass%, and further preferably 3 to 15 mass%. When the ethylene-vinyl copolymer (A2) contains two or more kinds of ethylene-vinyl copolymers, the vinyl content can be calculated from the vinyl content and the blending ratio of each ethylene-vinyl copolymer. The melt mass flow rate (hereinafter, MFR) of the ethylene-vinyl copolymer (A2) is preferably 30 to 2000 g / 10 min, more preferably 60 to 1000 g / 10 min. In this specification, the MFR is the outflow amount (g / 10 min) at 190° C. and a load of 2,160 g measured in accordance with JIS K 7210 for 10 min. When the ethylene-vinyl copolymer (A2) contains two or more kinds of ethylene-vinyl copolymers, the MFR can be determined by measuring the mixture after kneading in an extruder.
[0035] The content of the ethylene-vinyl copolymer (A2) is preferably 1 to 50 mass%, more preferably 5 to 40 mass%, and even more preferably 15 to 30 mass%, in 100 mass% of the resin composition. By containing the ethylene-vinyl copolymer in the above range, it is easy to achieve both blocking resistance and adhesive strength.
[0036] <Low density polyethylene> When an ethylene-vinyl copolymer (A2) is used as the resin composition, it is preferable to further contain low-density polyethylene (LDPE). Low-density polyethylene is a thermoplastic resin with a branched structure in which the repeating unit ethylene is randomly bonded, and since it has more branched structures than linear low-density polyethylene, it tends to have low crystallinity and a low melting point. By using low-density polyethylene in combination, the crystallinity of the melting bag is increased, making it easier to design to prevent blocking. The content of low-density polyethylene (LDPE) is preferably 50 to 99 mass%, more preferably 55 to 95 mass%, and even more preferably 60 to 90 mass%, based on 100 mass% of the resin composition. By containing low-density polyethylene (LDPE) in the above range, it is easy to achieve both blocking resistance and adhesive strength.
[0037] The density of the low density polyethylene is preferably 0.910 to 0.930 g / cm 3 More preferably, it is in the range of 0.915 to 0.925 g / cm 3 The range is particularly preferably 0.917 to 0.922 g / cm 3 The range is.
[0038] The melting peak temperature of the low-density polyethylene is preferably in the range of 95 to 120°C, more preferably in the range of 100 to 115°C, and particularly preferably in the range of 105 to 110°C. The melting peak temperature was measured using a differential scanning calorimetry (DSC) device.
[0039] The MFR of the low-density polyethylene is preferably in the range of 1 to 200 g / 10 minutes, more preferably in the range of 1 to 50 g / 10 minutes, even more preferably in the range of 1 to 20 g / 10 minutes, and particularly preferably in the range of 5 to 20 g / 10 minutes.
[0040] <Silicone oil (B)> Silicone oil (B) is known as a material that mainly provides releasability and peelability, and known silicone oils can be used in the present invention. Examples of silicone oil (B) include polydimethylsiloxane, polymethylphenylsilicone, polymethylhydrogensilicone, and modified silicone oils such as epoxy-modified, alkyl-modified, amino-modified, carboxyl-modified, alcohol-modified, fluorine-modified, alkylaralkylpolyether-modified, epoxy-polyether-modified, and polyether-modified silicone oils modified at the end or side chain. Polydimethylsiloxane is preferred. Among these, it is preferable to use a material having pseudo-adhesive properties. Examples of pseudo-adhesive materials are those that exert a force to maintain a contact state at the contact surface when in contact with other substances, such as the KF96 series manufactured by Shin-Etsu Chemical Co., Ltd., the TSK series manufactured by Momentive Performance Materials Japan LLC, the DOESIL SH200 series manufactured by Dow Toray Co., Ltd., the WACKER AK series manufactured by Asahi Kasei Wacker Silicone Co., Ltd., and the TSF451 series manufactured by Momentive Performance Materials Japan LLC. These can be used alone or in combination of two or more types. In the present invention, the silicone oil (B) is required to impart blocking resistance to the mass, and when it is subsequently used as an adhesive, to suppress peeling performance and exhibit adhesive function.
[0041] The content of the silicone oil (B) is preferably 0.1 to 10 mass%, more preferably 0.3 to 10 mass%, and even more preferably 0.5 to 5 mass%, based on 100 mass% of the resin composition. By including the silicone oil (B) in the above range, it is easy to achieve both blocking resistance and adhesive strength.
[0042] The molecular weight of the silicone oil (B) calculated from the kinetic viscosity is preferably 350 to 1,000,000, more preferably 650 to 500,000, further preferably 1,300 to 100,000, and particularly preferably 3,500 to 10,000. By including the silicone oil (B) in the above range, it is easy to achieve both blocking resistance and adhesive strength.
[0043] The resin composition preferably further contains a process oil and / or a tackifier.
[0044] <Process oil> Process oils are generally used as plasticizers for rubber and thermoplastic elastomers. They are process oils produced in oil refineries and are broadly classified into paraffinic process oils, aromatic process oils, and naphthenic process oils. Process oils are mixtures of paraffin chains, aromatic rings, and naphthenic rings. Process oils are classified as paraffinic process oils when the paraffin chain carbon content of the total carbon is 50% or more by weight, aromatic process oils when the aromatic carbon content of the total carbon is 30% or more by weight, and naphthenic process oils when the naphthenic ring carbon content of the total carbon is 30% or more by weight.
[0045] The content of the process oil is preferably 5 to 90 mass%, more preferably 10 to 80 mass%, further preferably 15 to 70 mass%, particularly preferably 20 to 60 mass%, based on 100 mass% of the resin composition. By containing the process oil in the above range, excellent adhesive strength is achieved.
[0046] <Tackifier> A tackifier is a polymer with a relatively low molecular weight, ranging from several hundred to several thousand. It exhibits liquid or solid properties at room temperature, and adding a tackifier imparts fluidity and tackiness, improving adhesive strength. In the present invention, a tackifier that is a solid at room temperature is preferable. If it is a solid at room temperature, it has excellent resistance to crushing, while also fulfilling its original function of increasing adhesive strength when used as a hot melt.
[0047] Tackifiers are broadly classified into natural resin-based and synthetic resin-based. Natural resin-based agents include rosin-based resins and terpene-based resins, while synthetic resin-based agents include petroleum-based resins, phenol-based resins, xylene-based resins, etc. Any of the tackifiers can be used alone or in combination depending on the application.
[0048] The content of the tackifier is preferably 1 to 50 mass%, more preferably 5 to 45 mass%, and even more preferably 10 to 40 mass%, based on 100 mass% of the resin composition. By containing the tackifier in the above range, excellent adhesive strength is achieved.
[0049] To the extent that the problem of the present invention can be solved, waxes such as polyethylene wax, polypropylene wax, Fischer-Tropsch wax, paraffin wax, and microcrystalline wax, α-methylstyrene resin, and other thermoplastic elastomers can be used as components contained in the resin composition that forms the melt bag. Other examples of thermoplastic elastomers include urethane-based, polyester-based, polyamide-based, and 1,2-butadiene-based elastomers. If necessary, antioxidants, age resistors, etc. may be added to prevent thermal deterioration and thermal decomposition.
[0050] [Production of resin composition] The resin composition can be prepared by mixing the above-mentioned materials while heating them in a known manner. Diluting them with organic solvents increases workability but limits application, so it is preferable to avoid using organic solvents as much as possible.
[0051] <Lump> The lump is a hot melt adhesive packaged in a melting bag. The weight is preferably 10 g to 5000 g. If the weight is within the above range, it is easy to handle and has excellent workability in terms of the number of times it can be filled, which is preferable. The thickness of the melting bag can be appropriately adjusted depending on the weight. After forming (manufacturing) the melt bag, a mass can be obtained by filling it with hot melt adhesive so that as little air as possible gets in. From the viewpoint of energy efficiency, this process is preferably cooled immediately after forming the film or carried out underwater.
[0052] (Hot melt adhesive) For example, when the hot melt adhesive is intended for adhesive use, it is preferable that the resin system contains a styrene copolymer, which is easy to exhibit various adhesive properties. As the styrene copolymer, the material used in the resin composition for manufacturing the melt bag described above can be used as it is. In terms of compatibility in a melting furnace, it is more preferable to use the same type of material as the resin composition. Specifically, it is preferable to include at least one of a styrene-based copolymer (A1) and an ethylene-vinyl-based copolymer (A2). The types of the styrene copolymer (A1) and / or the ethylene-vinyl copolymer (A2), the silicone oil (B), the process oil and the tackifier can be appropriately selected depending on the application of the hot melt. For example, for recycling purposes, a tackifier with a high acid value of 100 mgKOH / g or more is preferred since it is required to be releasable by an alkaline aqueous solution. Also, for environmentally friendly products, a tackifier with a high biomass degree of 80% or more is preferred.
[0053] The softening point of the hot melt adhesive is preferably 40° C. to 110° C., more preferably 50° C. to 100° C., and even more preferably 60° C. to 90° C. A hot melt adhesive having a softening point within the above range exhibits tackiness at room temperature, and therefore has excellent compatibility with melting bags while enjoying the advantages of being made into a mass, and also easily exhibits cohesive force when used as a hot melt.
[0054] The softening point of the hot melt adhesive is preferably within 50° C. of the softening point of the melting bag, more preferably within 40° C., even more preferably within 30° C., and particularly preferably within 20° C. By being within the above range, the compatibility of the two is excellent.
[0055] <Wrapping label> In the present invention, the body-wrapped label is a label to be applied to the body of a container, and is formed by laminating a sheet-like product obtained by molding the above-mentioned lump onto a part or the entire surface of a substrate. Labels are affixed to products to indicate the contents and to improve the design to stimulate consumer purchasing desire, and are used for a variety of purposes, including on food and beverages, seasonings, cosmetics and toiletries, medicines and reagents. Examples of the substrate for the body-wrapped label include plastic films and sheets, paper, nonwoven fabric, foams, etc. The label may or may not have a printed back surface. The product obtained by forming the lump into a sheet may be laminated on the entire surface of the label, or may be laminated on only a part of the label. Methods for forming the lump into a sheet and laminating it on the label (coating methods) include the general roll coating method, as well as the slit coating method, spiral spray method, and foaming melt method.
[0056] The thickness of the sheet-like molded product (hot melt adhesive layer) of the lump in the body-wrapped label is preferably 1 to 500 μm, more preferably 5 to 300 μm, further preferably 10 to 100 μm, and particularly preferably 15 to 50 μm. When the thickness is within the above range, the desired adhesive strength is easily achieved.
[0057] <Container> The container in the present invention refers to a container to which the above-mentioned body-wrapped label is attached. The material of the container may be glass, metal, plastic, paper, etc., but is not particularly limited. The shape of the container may be round or non-round, such as rectangular. A representative container is a plastic bottle. The method of attaching the body-wrapped label may be a conventionally known method, and is not particularly limited. EXAMPLES
[0058] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited thereto. In the examples, unless otherwise specified, "parts" means "parts by mass", "%" means "% by mass", and "RH" means relative humidity. The blending amounts in the tables are in parts by mass. Note that blanks in the tables indicate that no blending was performed.
[0059] <Molecular weight of silicone oil> The molecular weight of the silicone oil was determined by reading the molecular weight corresponding to the kinetic viscosity of the silicone oil using the graph showing the relationship between kinetic viscosity and molecular weight on page 5 of "Shin-Etsu Silicones: KF-96 Performance Test Results." The kinematic viscosity can be measured according to JIS K2283. In the present invention, the values published on the website of Shin-Etsu Chemical Co., Ltd. were used.
[0060] The abbreviations used in Tables 1 to 4 are as follows: [Styrene-based copolymer (A1)] G1642: Kraton G1642 (Kraton Polymers, styrene content: 21% by mass, weight average molecular weight: 124,000) G1650: Kraton G1650 (Kraton Polymers, styrene content: 30% by mass, weight average molecular weight: 96,000) G1726: Kraton G1726 (Kraton Polymers, styrene content: 30% by mass, weight average molecular weight: 46,000) [Ethylene-vinyl copolymer (A2)] EVA: Ethylene-vinyl acetate copolymer (vinyl acetate content 20% by weight) [Low density polyethylene] LDPE: Low density polyethylene (melting peak temperature 107℃, density 0.919g / cm 3 )
[0061] [Process oil] PW-90: Diana Process PW-90 (Idemitsu Kosan, paraffin-based process oil)
[0062] [Tackifier] P-100: Alcon P-100 (Arakawa Chemical Co., Ltd., hydrogenated petroleum resin, softening point: 100°C) Haritac F (Harima Chemicals, hydrogenated rosin type, acid value: 170 mg KOH / g, softening point: 80°C)
[0063] [wax] H1: Sasol H1 (manufactured by Sasol Chemical Industries, Fischer-Tropsch wax, softening point: 112°C) C80: Sasol C80 (manufactured by Sasol Chemical Industries, Fischer-Tropsch wax, softening point: 88°C)
[0064] [Silicone oil (B)] 1000CS: Shin-Etsu Silicone KF96-1000CS (Shin-Etsu Chemical Co., Ltd., molecular weight calculated from kinetic viscosity: 27,000) 5CS: Shin-Etsu Silicone KF96-5CS (manufactured by Shin-Etsu Chemical Co., Ltd., molecular weight calculated from kinetic viscosity: 650) 10CS: Shin-Etsu Silicone KF96-10CS (manufactured by Shin-Etsu Chemical Co., Ltd., molecular weight calculated from kinetic viscosity: 1,300) 50CS: Shin-Etsu Silicone KF96-50CS (manufactured by Shin-Etsu Chemical Co., Ltd., molecular weight calculated from kinetic viscosity: 3,500) 10,000CS: Shin-Etsu Silicone KF96H-10,000CS (manufactured by Shin-Etsu Chemical Co., Ltd., molecular weight calculated from kinetic viscosity: 55,000) 100,000CS: Shin-Etsu Silicone KF96H-100,000CS (manufactured by Shin-Etsu Chemical Co., Ltd., molecular weight calculated from kinetic viscosity is 110,000)
[0065] <Manufacture of hot melt adhesive Q-1> In a stainless steel beaker equipped with a stirrer, 5 parts of Sasol C80 as a wax, 40 parts of PW-90 as a process oil, and 30 parts of Haritac F as a tackifier were added and heated to melt. The heating was performed carefully so that the contents were 130 to 150 ° C. After melting, the mixture was stirred to make a homogeneous molten liquid, and then 25 parts of G1726 as a styrene copolymer (A1) was added to the molten liquid while maintaining the temperature at 130 to 150 ° C and continuing to stir. After the addition was completed, the mixture was heated and stirred at a temperature of 130 to 150 ° C to completely melt G1726. The mixture was then cooled to prepare hot melt adhesive Q-1.
[0066] [Table 1]
[0067] Example 1 <Production of Resin Composition P-1> In a stainless steel beaker equipped with a stirrer, 5 parts of Sasol H1 as a wax, 59.9 parts of PW-90 as a process oil, 5 parts of P-100 as a tackifier, and 0.1 parts of 1000CS as a silicone oil were added and melted by heating. The heating was performed carefully so that the contents were 130 to 150 ° C. After melting, stirring was performed to obtain a homogeneous molten liquid, and then 30 parts of G1642 as a styrene copolymer (A1) was added to the molten liquid while maintaining the temperature at 130 to 150 ° C and continuing to stir, and after the addition was completed, the mixture was heated and stirred at a temperature of 130 to 150 ° C. Then, it was cooled to prepare a resin composition P-1. <Production of melt bag and lump 1> Next, the resin composition P-1 was put into a melt bag molding machine, and the temperature was set to 100° C. to form a melt bag with a thickness of 200 μm. 500 g of the hot melt adhesive Q-1 was extruded toward the melt film while heating, and the film was molded by wrapping it in water, and then cooled in water as it was to obtain a lump 1. The amount of the melt bag was 2% by mass relative to the lump 1.
[0068] (Examples 2 to 22, Comparative Example 1) Resin compositions (P-2 to 22, P'-1) were produced in the same manner as in Example 1, except that the compositions and blending amounts (parts by mass) were changed to those shown in Tables 2 to 4. Next, in the same manner as in Example 1, melt bags and lumps in Examples 2 to 22 and Comparative Example 1 were obtained by filling the melt bags with hot melt. In Tables 1 to 4, hot melt is abbreviated as HM.
[0069] [Table 2]
[0070] [Table 3]
[0071] [Table 4]
[0072] <Blocking resistance> A release film was laid on a small piece of cardboard, molten hot melt adhesive was poured onto it, and the adhesive was allowed to cool naturally and harden to produce a flat-surfaced block-shaped hot melt adhesive. A melting bag (10 cm square, 200 μm thick) was layered on the resulting block-shaped hot melt adhesive, and a melting bag (10 cm square, 200 μm thick) and a block-shaped hot melt adhesive were layered on top of that in that order to produce a block-shaped hot melt adhesive / melting bag / / melting bag / block-shaped hot melt adhesive laminate. A 10 kg weight was placed on this laminate, and it was stored at 40°C for 24 hours. After cooling in the air, the melting bags were peeled apart by hand to evaluate the crush resistance. The evaluation criteria are as follows: [Evaluation Criteria] ◎: No peeling sound or peeling strength, excellent. Good: Slight peeling sound, some peeling strength, good. △: Blocking occurred, but the molten bag did not break even when peeled off, and there was no problem in practical use. ×: Blocking occurred and the melted bag would break when peeled off, which would be problematic in practical use.
[0073] <Adhesive strength> A 15g / m2 coating of the lump was applied to the printed surface of a label printed on a 30μm thick OPP film. 2 Thus, a label with a hot melt adhesive was obtained. The label with the hot melt adhesive was attached to the non-printed surface of a 30 μm thick OPP film at 23° C., pressed back and forth with a hand roller, and cut to a width of 15 mm. After storing for 24 hours under conditions of 23° C. and 65% RH, it was peeled off at 180° (peel speed: 300 mm / min) in a thermostatic chamber at 23° C. (Evaluation Criteria) ◎: 1.5N / 15mm or more: Very good ○: 1.0N / 15mm or more, less than 1.5N / 15mm: Good △: 0.5N / 15mm or more, less than 1.0N / 15mm: usable ×: Less than 0.5N / 15mm: Not practical
[0074] The results in Tables 2 to 4 show that the aggregates of Examples 1 to 22 were excellent in blocking resistance and adhesive strength, whereas the aggregate of Comparative Example 1 did not satisfy all of the above characteristics. [Explanation of symbols]
[0075] 1 Melting Bag 2. Hot melt adhesives
Claims
1. A melt bag formed from a resin composition containing at least one of a styrene-based copolymer (A1) and an ethylene-vinyl-based copolymer (A2), and a silicone oil (B).
2. The melt bag according to claim 1, comprising 0.1 to 10 mass% of the silicone oil (B) based on 100 mass% of the resin composition.
3. 3. The melting bag according to claim 1, wherein the molecular weight of the silicone oil (B) calculated from the kinetic viscosity is from 650 to 100,000.
4. The melt bag according to claim 1 or 2, wherein the membrane thickness is 25 to 500 μm.
5. 3. The melt bag according to claim 1 or 2, for packaging hot melt adhesives.
6. A mass in which a hot melt adhesive is packaged in a melt bag, the melt bag being the melt bag according to claim 1 or 2.
7. 7. The mass according to claim 6, wherein the difference between the softening point of the hot melt adhesive and the softening point of the melting bag is within 50°C.
8. 8. A label wrapped around a body, comprising a substrate and the sheet-like molding of the lump according to claim 7 laminated on a part or the whole surface of the substrate.
9. A container having the body label according to claim 8 attached thereto.
10. 10. The container according to claim 9, wherein the material of the substrate is polyethylene terephthalate.
Citation Information
Patent Citations
Material and method for packaging hot melt adhesive
JP2002362661A
Packaged hot melt pressure-sensitive adhesive
JP2016526086A
Ethylene-vinyl acetate copolymer resin, film, molding, foam, and sheet
JP2023113129A
Film suitable for melted bag and melted bag
JP2004002581A
Thermoplastic resin film, melting bag and packaged hot melt adhesive
JP2019065164A