Resin composition, electric wire, and cable

A resin composition with a substituted gallic acid ester improves flame retardancy and maintains tensile strength stability during heat aging, addressing the limitations of existing compositions.

JP2024167268AActive Publication Date: 2024-12-03PROTERIAL LTD

Patent Information

Application Number
JP2024140777
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03
Estimated Expiration
2041-02-04

AI Technical Summary

Technical Problem

Existing resin compositions, such as those described in Patent Document 1, do not provide sufficient flame retardancy and experience significant changes in tensile strength during heat aging, which is undesirable for electric wires and cables.

Method used

A resin composition comprising an ethylene polymer, a metal hydroxide, and a gallic acid ester with at least one hydroxyl group substituted with an alkoxy, phenoxy, or silyl ether group to enhance flame retardancy while minimizing changes in tensile strength during heat aging.

Benefits of technology

The resin composition maintains high flame retardancy and suppresses changes in tensile strength and elongation during heat aging, ensuring stability under heating conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167268000001_ABST
    Figure 2024167268000001_ABST
Patent Text Reader

Abstract

To provide a resin composition that is excellent in fire retardancy and suppresses changes in tensile strength at the time of heat aging, and electric wires and cables that are formed with the use of the resin composition.SOLUTION: A fire-retardant resin composition includes: (A) an ethylene-based polymer; and (B) a metal hydroxide and (C) a chemical compound in which at least one of three hydroxyl groups contained in gallic acid is substituted with an alkoxy group, a phenoxy group, or a silyl ether group, as fire retardants.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a resin composition, an electric wire, and a cable. [Background technology]

[0002] An electric wire includes a conductor and a coating layer provided around the conductor. A cable includes, for example, a stranded wire formed by twisting such electric wires together and a sheath provided around the stranded wire. The coating layer of the electric wire and the sheath of the cable are generally made of an electrically insulating material whose main raw material is rubber, resin, or the like.

[0003] The coating layer of electric wires and the sheath of cables are required to have various properties according to their applications. For example, electric wires and cables for electronic devices and railway vehicles are required to be made of halogen-free materials that suppress the generation of toxic and corrosive gases during combustion, and to have high flame retardancy.

[0004] As a material that meets such requirements, Patent Document 1 describes a resin composition in which a metal hydroxide such as magnesium hydroxide is added as a flame retardant to a resin component whose base polymer is an ethylene-based polymer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2015-2062 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, according to the investigations of the present inventors, when higher flame retardancy is required, the resin composition described in Patent Document 1 may not be sufficient. On the other hand, the present inventors have found that by adding a compound having multiple phenolic hydroxyl groups in the molecule, such as a gallic acid ester, the flame retardancy is significantly improved due to the high radical trapping effect of the phenolic hydroxyl groups. The radical trapping effect refers to the effect of the phenolic hydroxyl groups capturing the generated radicals. As a result, the flame retardant can capture the radicals generated from the combustion product during combustion, suppressing the reaction between the resin composition and oxygen.

[0007] However, as a result of further investigations by the present inventors, it was newly discovered that when a resin composition containing a compound having multiple phenolic hydroxyl groups in the molecule is aged by heat, the tensile strength increases, and as a result, the rate of change in tensile strength from the initial state becomes large.

[0008] One aspect of the present disclosure provides a resin composition that is excellent in flame retardancy and suppresses change in tensile strength during heat aging, and an electric wire and cable formed using the resin composition. [Means for solving the problem]

[0009] One aspect of the present disclosure is a flame-retardant resin composition comprising: (A) an ethylene-based polymer; and, as a flame retardant, (B) a metal hydroxide; and (C) a compound in which at least one of three hydroxyl groups in gallic acid is substituted with an alkoxy group, a phenoxy group, or a silyl ether group. Effect of the Invention

[0010] According to one aspect of the present disclosure, there is provided a resin composition that has excellent flame retardancy and suppresses change in tensile strength during heat aging, and an electric wire and a cable formed using the resin composition. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view showing a structure of an electric wire according to a first embodiment. [Diagram 2] FIG. 6 is a cross-sectional view showing the structure of an electric wire according to a second embodiment. [Diagram 3] FIG. 2 is a cross-sectional view showing the structure of an example of a cable. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] A resin composition according to one embodiment of the present disclosure includes (A) an ethylene-based polymer, (B) a metal hydroxide, and (C) at least one compound selected from the group consisting of a compound in which at least one of three hydroxyl groups in gallic acid is substituted with an alkoxy group, a phenoxy group, or a silyl ether group, and a compound in which at least one of three hydroxyl groups in a gallic acid ester is substituted with an alkoxy group, a phenoxy group, or a silyl ether group.

[0013] As described below, such a resin composition has excellent flame retardancy, and is inhibited from changing in tensile strength during heat aging. Also, the resin composition is inhibited from changing in elongation during heat aging. As mentioned above, according to the study by the present inventors, a compound having multiple phenolic hydroxyl groups in a molecule, such as a gallic acid ester, can improve the flame retardancy of a resin composition. However, when a resin composition containing such a compound is heat-aged, the tensile strength increases from the initial state while the elongation decreases, resulting in a large rate of change in these properties. This situation is not preferable because it goes against the design concept that it is better to have small changes in physical properties under heating conditions for a relatively short time.

[0014] The reason for this phenomenon is believed to be that the phenolic hydroxyl group captures radicals that may be generated during the manufacture of the coating layer of the electric wire and the sheath of the cable, and releases the captured radicals during heat aging, thereby promoting the crosslinking reaction of the base polymer. For example, in some cases, a resin composition is crosslinked to improve the heat resistance of the coating layer of the electric wire and the sheath of the cable, and radicals may be generated during this crosslinking.

[0015] The present inventors considered that in order to simultaneously achieve both radical scavenging during combustion and suppression of radical donation during heat aging, it is effective to protect the phenolic hydroxyl group, temporarily reducing the reactivity of the phenolic hydroxyl group while returning it to the original hydroxyl group during combustion. That is, by replacing only hydrogen with another structure while leaving the oxygen of the phenolic hydroxyl group, the reactivity of the phenolic hydroxyl group is suppressed, and it is considered that the change in tensile strength during heat aging is suppressed. In addition, if the replaced part is eliminated in the high temperature environment during combustion and returns to the original hydroxyl group, the radical trapping effect is restored, and it is considered that high flame retardancy can be maintained. Therefore, the present inventors have variously examined the protection of the hydroxyl group of compounds such as gallic acid esters.

[0016] As a result, they found that by substituting at least one of the three hydroxyl groups in gallic acid or a gallic acid ester with an alkoxy group, a phenoxy group, or a silyl ether group, it is possible to suppress changes in tensile strength and other properties during heat aging while maintaining high flame retardancy.

[0017] Hereinafter, the resin composition, electric wire, and cable according to one embodiment of the present disclosure will be described in detail. <Resin composition> The resin composition is a halogen-free flame-retardant resin composition. Each component contained in the resin composition will be described in detail below. Note that, below, the component (B) and the component (C) may be collectively described as a flame retardant. [Component (A)] Examples of the ethylene-based polymer of the component (A) include ethylene-vinyl acetate copolymer, ethylene-acrylic acid ester copolymer, and ethylene-α-olefin copolymer. The component (A) preferably contains an ethylene-vinyl acetate copolymer. The component (A) is preferably a base polymer in the resin composition.

[0018] [(B) Component] Examples of the metal hydroxide of component (B) include magnesium hydroxide, aluminum hydroxide, hydrotalcite, boehmite, calcium hydroxide, iron (II) hydroxide, iron (III) hydroxide, etc. It is preferable that component (B) contains magnesium hydroxide.

[0019] Magnesium hydroxide may be, for example, surface-untreated or surface-treated. Examples of surface-untreated magnesium hydroxide include natural magnesium hydroxide obtained by crushing brucite ore, and synthetic magnesium hydroxide. Examples of surface-treated magnesium hydroxide include magnesium hydroxide that is surface-treated with a silane coupling agent, a phosphoric acid ester, a fatty acid (e.g., stearic acid, oleic acid, etc.), or a fatty acid salt.

[0020] The magnesium hydroxide is preferably surface-treated with a silane coupling agent, because the magnesium hydroxide surface-treated with a silane coupling agent has high affinity with component (A), and therefore the tensile properties of the resin composition are improved.

[0021] The content of the (B) component in the resin composition is preferably 50 parts by mass or more and 300 parts by mass or less, more preferably 100 parts by mass or more and 250 parts by mass or less, relative to 100 parts by mass of the (A) component. When the content of the (B) component is 50 parts by mass or more relative to 100 parts by mass of the (A) component, higher flame retardancy can be obtained in the obtained electric wire, cable, etc. Also, when the content of the (B) component is 300 parts by mass or less relative to 100 parts by mass of the (A) component, adhesion and aggregation between metal hydroxide particles is suppressed, so that the flowability of the resin composition is not easily reduced, and the processability of the resin composition, for example, processability by extrusion molding, is good.

[0022] [(C) component] The compound of component (C) is at least one of the following compounds: a compound in which at least one of three hydroxyl groups in gallic acid is substituted with an alkoxy group, a phenoxy group, or a silyl ether group; and a compound in which at least one of three hydroxyl groups in a gallic acid ester is substituted with an alkoxy group, a phenoxy group, or a silyl ether group. Gallic acid is a compound represented by the following formula (1).

[0023] [ka]

[0024] The carboxylic acid group in gallic acid may remain in the carboxylic acid structure or may be esterified as long as the hydroxyl group is protected. As the ester, an alkyl ester having a small number of carbon atoms, for example, a lower alkyl ester having 1 to 4 carbon atoms, is preferred. As the gallic acid ester, at least one selected from methyl gallate represented by the following formula (2) and propyl gallate represented by the following formula (3) is particularly preferred.

[0025] [ka]

[0026] [ka]

[0027] In the compound of component (C), at least one of the three hydroxyl groups may be substituted. The position of the substituent may be any of the 3rd, 4th, and 5th positions. From the viewpoint of further suppressing radical donation during heat aging, it is preferable that a plurality of hydroxyl groups (i.e., two or three) are substituted, and it is more preferable that all hydroxyl groups are substituted. It is unclear why the effect of suppressing radical donation during heat aging is exerted even if all hydroxyl groups are not necessarily protected, but the present inventors believe that this is due to a decrease in radical scavenging power due to steric hindrance.

[0028] The alkoxy group for the substituent is preferably an alkoxy group having 1 to 4 carbon atoms, such as a methoxy group, an ethoxy group, or a butoxy group, and from the viewpoint of availability, a methoxy group is more preferable. Examples of compounds substituted with an alkoxy group include 3,4,5-trimethoxybenzoic acid (also known as eudesmic acid) and its alkyl esters, 3,5-dimethoxy-4-hydroxybenzoic acid (also known as syringic acid) and its alkyl esters, etc. Examples of alkyl esters of eudesmic acid include alkyl esters having 1 to 4 carbon atoms, such as methyl eudesmate and propyl eudesmate. Examples of alkyl esters of syringic acid include alkyl esters having 1 to 4 carbon atoms, such as methyl syringate.

[0029] As the compound substituted with an alkoxy group, from the viewpoint of further suppressing radical donation during heat aging, eudesmic acid and its alkyl esters are preferred, and eudesmic acid is more preferred. Examples of compounds substituted with a phenoxy group include 3,4,5-triphenoxybenzoic acid and its alkyl esters, 4-phenoxy-3,5-dihydroxybenzoic acid and its alkyl esters, 3-phenoxy-4,5-dihydroxybenzoic acid and its alkyl esters, 3,4-diphenoxy-5-dihydroxybenzoic acid and its alkyl esters, etc. In these cases, the alkyl ester is preferably an alkyl ester having 1 to 4 carbon atoms.

[0030] Examples of the silyl ether group as a substituent include trialkylsilyloxy groups having 1 to 4 carbon atoms, such as a trimethylsilyloxy group, a triethylsilyloxy group, and a tri-t-butylsilyloxy group. As the silyl ether group, a trimethylsilyloxy group is more preferable because it is easily deprotected during combustion.

[0031] The silyl ether group can be introduced into a compound by silyl-etherifying a hydroxyl group using a silane compound. Examples of the silane compound used for silyl-etherification include chlorosilane compounds such as trimethylchlorosilane, triethylchlorosilane, and tri-t-butylchlorosilane. Protection with a silyl ether group can be easily achieved, for example, by dropping a chlorosilane compound into a solution in which gallic acid or a gallic acid ester is dissolved together with a base, and allowing the reaction to occur.

[0032] When an ethylene-vinyl acetate copolymer is used as the ethylene-based polymer of component (A), the substituent is preferably a silyl ether group, because in an acidic environment caused by elimination of acetic acid during combustion, the silyl ether group is quickly deprotected and the compound quickly returns to the original gallic acid or gallate, making it easier to maintain flame retardancy.

[0033] Examples of compounds substituted with silyl ether groups include 3,4,5-tris(trimethylsilyloxy)benzoic acid and its alkyl esters, 3,5-di(trimethylsilyloxy)-4-hydroxybenzoic acid and its alkyl esters, 3-trimethylsilyloxy-4,5-dihydroxybenzoic acid and its alkyl esters, and 3,4,5-tris(tri-t-butylsilyloxy)benzoic acid and its alkyl esters. Examples of alkyl esters of 3,4,5-tris(trimethylsilyloxy)benzoic acid include alkyl esters having 1 to 4 carbon atoms, such as propyl 3,4,5-tris(trimethylsilyloxy)benzoate. Examples of alkyl esters of 3,5-di(trimethylsilyloxy)-4-hydroxybenzoic acid include alkyl esters having 1 to 4 carbon atoms, such as propyl 3,5-di(trimethylsilyloxy)-4-hydroxybenzoate. Examples of alkyl esters of 3-trimethylsilyloxy-4,5-dihydroxybenzoic acid include alkyl esters having 1 to 4 carbon atoms, such as propyl 3-(trimethylsilyloxy)-4,5-dihydroxybenzoate. Examples of alkyl esters of 3,4,5-tris(tri-t-butylsilyloxy)benzoic acid include alkyl esters having 1 to 4 carbon atoms, such as propyl 3,4,5-tris(tri-t-butylsilyloxy)benzoate.

[0034] As the substituent, from the viewpoint of further suppressing radical donation during heat aging, of the alkoxy group, phenoxy group, and silyl ether group, the alkoxy group and the silyl ether group are preferred, and the alkoxy group is more preferred.

[0035] The content of the (C) component is preferably 1 part by mass or more and 50 parts by mass or less, and more preferably 2 parts by mass or more and 30 parts by mass or less, per 100 parts by mass of the (A) component. When the content of the (C) component is 1 part by mass or more per 100 parts by mass of the (A) component, high flame retardancy is obtained in the obtained electric wire, cable, etc. Also, when the content of the (C) component is 50 parts by mass or less per 100 parts by mass of the (A) component, the tensile strength of the resin composition is improved.

[0036] [Other ingredients] In addition to the above components, the resin composition may contain other components as necessary to the extent that the above properties are not affected. Examples of other components include flame retardants, flame retardant assistants, crosslinking agents, crosslinking assistants, processing assistants, coupling agents, surface treatment agents, colorants, lubricants, compatibilizers, antioxidants, ozone deterioration inhibitors, ultraviolet absorbers, light stabilizers, metal chelators, softeners, plasticizers, etc.

[0037] <Electric wire> [First embodiment] 1 is a halogen-free, flame-retardant insulated wire according to the first embodiment. The wire 10 includes a conductor 1, an insulating layer 2 as a coating layer that coats the conductor 1, and a separator 3 provided between the conductor 1 and the insulating layer 2.

[0038] The conductor 1 may be a commonly used metal wire, such as a copper wire, a copper alloy wire, an aluminum wire, a gold wire, or a silver wire. The conductor 1 may be a metal wire plated with a metal such as tin or nickel. The conductor 1 may be a twisted wire in which metal wires are twisted together. The twisted wire may be a concentric twisted wire, a bunched twisted wire, or a composite twisted wire in which these are further twisted concentrically. The conductor 1 may be a compressed conductor in which a twisted wire is compressed. A compressed conductor is preferable because it allows the diameter of the electric wire to be reduced.

[0039] The insulating layer 2 is formed of the above resin composition. The thickness of the insulating layer 2 is not particularly limited, but is preferably 0.15 mm or more and 2 mm or less. The separator 3 is formed of, for example, a polyester tape. By providing the separator 3, when a stranded conductor is used as the conductor 1, it is possible to suppress the resin composition from penetrating into the inside of the conductor 1 when the resin composition is extruded, i.e., when the insulating layer 2 is formed. The electric wire 10 does not necessarily need to include the separator 3.

[0040] The electric wire 10 can be manufactured, for example, as follows. First, the above-mentioned components (A) to (C) and materials containing other components are melt-kneaded to obtain a resin composition. As the kneading device, for example, a Banbury mixer, a batch type kneader such as a pressure kneader, a continuous type kneader such as a twin-screw extruder, or other known kneading device can be used.

[0041] Then, the conductor 1 is prepared, and the separator 3 is wound around the conductor 1. After that, the separator 3 is covered with a resin composition using an extrusion molding machine, thereby forming the insulating layer 2 with a predetermined thickness.

[0042] Then, the insulating layer 2 is crosslinked by, for example, an electron beam crosslinking method, a chemical crosslinking method, or the like. Although the crosslinking is not essential, it is preferable to crosslink the insulating layer 2 because the heat resistance of the insulating layer 2 is improved by subjecting the insulating layer 2 to the crosslinking treatment. When the electron beam crosslinking method is used, the insulating layer 2 is irradiated with an electron beam of, for example, 1 Mrad to 30 Mrad (0.01 MGy to 0.3 MGy). When the chemical crosslinking method is used, for example, a crosslinking agent is added to a resin composition in advance, and the resin composition is molded into the insulating layer 2 of the electric wire 10, and then the insulating layer 2 is heat-treated. Note that the electron beam crosslinking method is used in the examples described later.

[0043] [Second embodiment] The electric wire 20 shown in FIG. 2 is a halogen-free flame-retardant insulated wire according to the second embodiment. The electric wire 20 differs from the electric wire 10 according to the first embodiment in that the insulating layer 2 is composed of two layers and in that the electric wire 20 does not include a separator 3. Specifically, the electric wire 20 includes a conductor 1, an insulating inner layer 2a provided around the conductor 1, and an insulating outer layer 2b provided around the insulating inner layer 2a. The insulating inner layer 2a is formed of an insulating resin such as polyethylene. The insulating outer layer 2b is formed of the above-mentioned resin composition. The insulating outer layer 2b corresponds to a coating layer. The electric wire 20 may include a separator 3, similar to the electric wire 10. The insulating layer 2 may include three or more layers.

[0044] <Cable> 3 is a halogen-free flame-retardant cable. The cable 30 includes a core 4, a sheath 5 as a covering layer that covers the core 4, and a separator 6 and a shield braid 7 provided between the core 4 and the sheath 5.

[0045] The core 4 has a three-core stranded wire 4a formed by twisting together three of the electric wires 10, and a spacer 4b provided around the three-core stranded wire 4a. The spacer 4b is made of staple yarn, paper tape, jute, etc. The core 4 does not necessarily have to have the spacer 4b.

[0046] The sheath 5 is formed of the resin composition. The separator 6 is the same as the separator 3 in the electric wire 10. The shield braid 7 is provided around the separator 6 and has an electrical shielding function. The shield braid 7 is formed of, for example, a metal tape or copper wire woven in a mesh shape. The shield braid 7 may be provided inside the separator 6, and the cable 30 may not include the shield braid 7.

[0047] The cable 30 can be manufactured, for example, as follows. First, three electric wires 10 are manufactured by the same method as above. Then, the three electric wires 10 are twisted together with the fillers 4b to form the core 4, and the separator 6 and the shield braid 7 are provided around the core 4. Then, the surroundings of these are covered with a resin composition by an extrusion molding machine. This allows the sheath 5 to be formed with a predetermined thickness.

[0048] Then, if necessary, the sheath 5 is cross-linked in the same manner as above, whereby the cable 30 can be manufactured. It should be noted that other electric wires may be used instead of the electric wire 10. Moreover, instead of the three-core stranded wire 4a, a single core consisting of one electric wire may be used, or a multi-core stranded wire other than the three-core stranded wire may be used. Moreover, another layer, for example, another insulating layer, may be provided between the core 4 and the sheath 5.

[0049] <Other uses of the resin composition> The resin composition can be used for wires and cables of various applications and sizes. For example, the applications of the wires and cables include electronic devices, railroad cars, automobiles, wiring inside panels, wiring inside devices, and wiring inside buildings. Since wires and cables for electronic devices or railroad cars require particularly high flame retardancy, the resin composition can be suitably used for wires and cables for electronic devices or railroad cars. The type of cable is not particularly limited, and may be, for example, a power cable, a signal cable, or the like.

[0050] The resin composition can be used not only for the electric wires and cables but also for other applications, such as films, panels, mats, pipes, protective materials, fillers, fibers, resin molded products, resin substrates, stationery, building materials, connectors, bushes, grommets, terminal blocks, and terminal internal insulators. EXAMPLES

[0051] Hereinafter, one embodiment of the present disclosure will be described with reference to an example, but the present disclosure is not limited to the following example. <Production of resin composition for cable sheath> Each of the materials according to Examples 1 to 8 and Comparative Examples 1 to 4 shown in Table 1 below was dry-blended at room temperature, and the mixed materials were melt-kneaded in a pressure kneader at a discharge temperature of 190° C. to produce a resin composition for cable sheath. The content of each material in Table 1 is expressed in parts by mass.

[0052] In the resin compositions according to Examples 1, 2, and 6 to 8, (C1) eudesmic acid represented by the following formula (4) was used as the component (C). Note that, in the resin compositions according to Examples 1, 2, and 6 to 8, the content of (C1) eudesmic acid was varied.

[0053] [ka]

[0054] In the resin composition according to Example 3, (C2) methyl syringate represented by the following formula (5) was used as the component (C).

[0055] [ka]

[0056] In the resin composition according to Example 4, (C3) silyl-protected propyl gallate 1 (propyl 3,4,5-tris(trimethylsilyloxy)benzoate represented by the following formula (6)) was used as the component (C). The silyl-protected propyl gallate 1 was synthesized as follows. Propyl gallate was dissolved in acetone, and 5 equivalents of triethylamine per equivalent of hydroxyl group of propyl gallate and 5 equivalents of trimethylchlorosilane per equivalent of hydroxyl group of propyl gallate were added and reacted. Thereafter, acetone and triethylamine were removed to obtain silyl-protected propyl gallate 1. It was confirmed by FT-IR that the original hydroxyl group in the obtained silyl-protected propyl gallate 1 was protected.

[0057] [ka]

[0058] In the resin composition according to Example 5, (C4) silyl-protected propyl gallate 2 (propyl 3,4,5-tris(tri-t-butylsilyloxy)benzoate represented by the following formula (7)) was used as the component (C). Silyl-protected propyl gallate 2 was synthesized in the same manner as silyl-protected propyl gallate 1, except that tri-t-butylchlorosilane was used instead of trimethylchlorosilane.

[0059] [ka]

[0060] The resin composition according to Comparative Example 1 did not use the component (C), unlike the resin compositions according to Examples 1 to 8. The resin compositions according to Comparative Examples 2 to 4 used propyl gallate in which no hydroxyl groups were protected, instead of the component (C).

[0061] <Cable creation> By extrusion molding using a 20 mm single-screw extruder of "Labo Plastomill (registered trademark)" manufactured by Toyo Seiki Seisakusho, which is an extrusion coating device for electric wire manufacturing, a cross-sectional area of ​​0.5 mm 2 An insulating layer having a coating thickness of 0.2 mm was formed around the compressed tin-plated copper stranded wire. A resin composition produced by melt-kneading each material according to Comparative Example 1 shown in Table 1 in the same manner as the resin composition for the sheath was used to form the insulating layer. The cylinder temperature was 160°C, and the wire drawing speed was 4.0 m / min. Thereafter, the insulating layer of the produced electric wire was subjected to a crosslinking treatment by an electron beam crosslinking method under a condition of 7.5 Mrad, thereby crosslinking the resin composition constituting the insulating layer.

[0062] Three of the obtained electric wires were twisted together, and a polyester tape was wound around the twisted electric wire as a separator, and then a shield braid was applied therearound. Then, a 60 mm single screw extruder was used to extrude a sheath having a coating thickness of 0.45 mm around the shield braid, which was made of the resin composition for the sheath according to the above-mentioned Examples 1 to 8 and Comparative Examples 1 to 4. Thereafter, the sheath was subjected to a crosslinking treatment by an electron beam crosslinking method under a condition of 7.5 Mrad, thereby producing a cable having an outer diameter of 4.5 mm.

[0063] [Table 1]

[0064] <Evaluation method> (1) Initial tensile test The sheath was stripped from the prepared cable, and a dumbbell-shaped test piece was punched out from the stripped sheath. The dumbbell-shaped test piece was subjected to a tensile test in accordance with JIS C3005:2000 to measure the tensile strength and elongation. The tensile test was performed at a pulling speed of 250 mm / min.

[0065] (2) Heat aging test A dumbbell-shaped test piece prepared in the same manner as in the initial tensile test in (1) above was heated in a Geer oven at 135°C for 168 hours. Thereafter, a tensile test was performed in the same manner as in the initial tensile test using the dumbbell-shaped test piece after heat aging to measure the tensile strength and elongation. The rate of change in tensile strength and elongation after heat aging compared to those before heat aging (i.e., at the time of the initial tensile test) was calculated.

[0066] (3) Cable combustion test A 600mm length was taken from the prepared cable and used as a test sample. Using the test sample, a combustion test was conducted in accordance with IEC60332-1, and the distance from the upper support material to the burnt area was measured. The longer the distance from the upper support material to the burnt area, the shorter the fire spread distance and the higher the flame retardancy. When the test sample is completely burned, the distance from the upper support material to the burnt area will be 0mm.

[0067] (4) Overall Judgment For the tensile strength in the initial tensile test, samples with a tensile strength of 8 MPa or more were judged as passing, and samples with a tensile strength of less than 8 MPa were judged as failing. For the elongation in the initial tensile test, samples with an elongation of 125% or more were judged as passing, and samples with an elongation of less than 125% were judged as failing.

[0068] Regarding the rate of change in tensile strength and elongation in the heat aging test, those that were within ±30% were judged as passing, and those that were greater than ±30% were judged as failing. For the combustion test, similar to IEC 60332-1, those with a distance of 50 mm or more from the upper support to the burnt area were judged to have passed, and those with a distance of less than 50 mm were judged to have failed.

[0069] Finally, specimens that passed all of the tensile strength and elongation in the initial tensile test, the rate of change in tensile strength and elongation in the heat aging test, and the combustion test were judged to have passed, while those that failed any of them were judged to have failed. The evaluation results are shown in Table 1. In Table 1, specimens that passed were indicated with a circle, and those that failed were indicated with an x.

[0070] <Evaluation Results> As shown in Table 1, Examples 1 to 8 passed all the items of the initial tensile test, heat aging test, and combustion test.

[0071] On the other hand, Comparative Example 1, which does not contain component (C), failed the combustion test. Comparative Examples 2 and 3, which contain propyl gallate with no protected hydroxyl groups instead of component (C), passed the initial tensile test and the combustion test but failed the heat aging test. Comparative Example 4, which contains only a relatively small amount of propyl gallate, failed both the heat aging test and the combustion test.

[0072] <Consideration> As shown in Comparative Examples 1 to 4, it can be said that the resin composition passes the combustion test only when a gallic acid ester is blended with the resin composition. However, as shown in Comparative Examples 2 to 4, the gallic acid ester fails the heat aging test because the hydroxyl groups are not protected.

[0073] Comparing Example 1 and Comparative Example 2, it can be said that the gallic acid ester and the (C) component have the same flame retardant effect. In other words, it can be said that whether or not the hydroxyl group of the gallic acid ester is protected has almost no effect on the flame retardant property. This suggests the possibility that the substituent is eliminated during combustion.

[0074] Furthermore, when comparing Examples 1, 2, 6, and 7 with Example 8, the tensile strength in the initial tensile test is higher, so it can be said that it is preferable for the resin composition to contain 2 parts by mass or more and 30 parts by mass or less of the (C) component per 100 parts by mass of the total amount of the (A) component. [Explanation of symbols]

[0075] 1...conductor, 2...insulating layer (coating layer), 2a...inner insulating layer, 2b...outer insulating layer (coating layer), 3, 6...separator, 4...core, 4a...three-core stranded wire, 4b...interposer, 5...sheath, 7...shield braid, 10, 20...electric wire, 30...cable.

Claims

1. (A) an ethylene-based polymer; As a flame retardant (B) a metal hydroxide; (C) a compound in which at least one of three hydroxyl groups of gallic acid is substituted with an alkoxy group, a phenoxy group, or a silyl ether group; A flame-retardant resin composition comprising:

2. (A) an ethylene-based polymer; As a flame retardant (B) a metal hydroxide; (C) a compound in which one or three of three hydroxyl groups of a gallic acid ester are substituted with an alkoxy group, a phenoxy group, or a silyl ether group; A flame-retardant resin composition comprising:

3. The flame-retardant resin composition according to claim 1 or 2, wherein the flame-retardant resin composition comprises 2 parts by mass or more and 30 parts by mass or less of the (C) component relative to 100 parts by mass of the (A) component.

4. An electric wire comprising a conductor and a coating layer that coats the conductor, The coating layer is formed from the flame-retardant resin composition according to any one of claims 1 to 3.

5. A cable comprising a sheath formed from the flame-retardant resin composition according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Crosslinked polyethylene, polyvinyl chloride insulated control cable sheath material

    CN108250599A

  • Composition and use thereof

    JP1992233977A

  • Polyolefin resin composition

    JP1996283473A

  • Biodegradable flame-retardant, flame-retardant resin composition containing the same and molded article

    JP2002348575A

  • Flame-retardant insulated wire and flame-retardant cable

    JP2020077634A

Cited By

  • Flame retardant resin composition and cable and electric wire therewith

    JP2024012947A

  • Resin composition, electric wire, and cable

    JP2024161044A

  • Resin composition, electric wire, and cable

    JP7768313B2