Exhaust gas purification device

The exhaust gas purification device achieves enhanced warm-up performance and reduced performance deterioration by employing a strategic arrangement of catalyst layers containing rhodium, oxygen storage materials, and palladium, optimizing the catalyst distribution for improved emission control.

JP2024167807AActive Publication Date: 2024-12-04TOYOTA JIDOSHA KK +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023084149
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04
Estimated Expiration
2043-05-22

AI Technical Summary

Technical Problem

Existing exhaust gas purification devices for internal combustion engines in vehicles face challenges in achieving high warm-up performance and minimizing performance deterioration over time.

Method used

The device incorporates a specific configuration of catalyst layers on a base material, including a first layer with rhodium and oxygen storage material, a second layer with rhodium and pyrochlore and fluorite type Ce-Zr composite oxides, and a third layer with palladium, optimized in terms of distance and mass distribution to enhance warm-up performance and reduce deterioration.

Benefits of technology

The configuration results in an exhaust gas purification device with improved warm-up performance and minimal performance degradation, effectively reducing harmful emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167807000001_ABST
    Figure 2024167807000001_ABST
Patent Text Reader

Abstract

To provide an exhaust gas purification device having high warming performance and high NOx purification performance.SOLUTION: An exhaust gas purification device includes: a base material having an upstream end and a downstream end; a first catalyst layer provided on the base material in a first area between the downstream end and a first position, and containing rhodium; a second catalyst layer provided on the base material in a second area between the upstream end and a second position, and containing the rhodium and an oxygen storage material; and a third catalyst layer provided on the second catalyst in a third area between the upstream end and a third position, and containing palladium. The oxygen storage material in the second catalyst layer includes a pyrochlore-type Ce-Zr composite oxide and a fluorite type Ce-Zr composite oxide at the weight ratio of 0.2:1 to 0.4:1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an exhaust gas purification device. [Background technology]

[0002] Exhaust gas discharged from internal combustion engines used in automobiles and other vehicles contains harmful components such as carbon monoxide (CO), hydrocarbons (HC), and nitrogen oxides (NOx). Regulations on the emission of these harmful components are becoming stricter every year, and exhaust gas purification devices containing precious metals such as platinum (Pt), palladium (Pd), and rhodium (Rh) as catalysts are used to remove these harmful components.

[0003] Patent Document 1 describes an exhaust gas purification device that satisfies requirements for warm air performance, HC purification performance, and durability. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-205051 A Summary of the Invention [Problem to be solved by the invention]

[0005] It is desirable to further improve the warm-up characteristics of exhaust gas purification devices, and it is also desirable to further reduce the performance degradation of exhaust gas purification devices during use.

[0006] Therefore, the present disclosure provides an exhaust gas purification device that has high warm-up properties and is less susceptible to performance degradation due to use. [Means for solving the problem]

[0007] Aspects of the present disclosure include the following. [Aspect 1] An exhaust gas purification device, A substrate having a total length (Ls), the substrate having an upstream end where exhaust gas flows into the substrate and a downstream end where the exhaust gas flows out of the substrate; a first catalyst layer containing rhodium provided on the substrate in a first region between the downstream end and a first position separated by a first distance (La) from the downstream end toward the upstream end, the first distance (La) being 50% to 70% of a total length (Ls) of the substrate; a second catalyst layer including rhodium and an oxygen storage material provided on the substrate in a second region between the upstream end and a second position separated by a second distance (Lb) from the upstream end toward the downstream end, the second distance (Lb) being 50% or more of a total length (Ls) of the substrate, and the oxygen storage material including a pyrochlore-type Ce—Zr composite oxide and a fluorite-type Ce—Zr composite oxide in a weight ratio of 0.2:1 to 0.4:1; an exhaust gas purification device comprising: a third catalyst layer containing palladium and provided on the second catalyst layer in a third region between the upstream end and a third position separated by a third distance (Lc) from the upstream end toward the downstream end, the third distance (Lc) being 40% or less of a total length (Ls) of the substrate. [Aspect 2] 2. The exhaust gas purification device according to aspect 1, wherein a total mass of the first catalyst layer based on a volume of the substrate in the first region is 170 g / L or more. [Aspect 3] 3. The exhaust gas purification device according to claim 1 or 2, wherein a total mass of the third catalyst layer based on the volume of the substrate in the third region is greater than 0 g / L and less than or equal to 105 g / L. [Aspect 4] The exhaust gas purification device according to any one of aspects 1 to 3, wherein the first catalyst layer further contains an oxygen storage material. Effect of the Invention

[0008] The exhaust gas purification device of the present disclosure has high warm-up properties and is less susceptible to performance degradation due to use. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is an enlarged end view of a main part of an exhaust gas purification device according to one embodiment, cut along a plane parallel to the flow direction of exhaust gas, and shows a schematic configuration of partition walls of a substrate and their vicinity. [Diagram 2] FIG. 2 is a perspective view that illustrates an example of the base material. [Diagram 3] FIG. 3 is a graph showing the results of the time it took for the THC purification rate to reach 50% in the warm-up performance evaluation test. [Figure 4] FIG. 4 is a graph showing NOx-T50 in a catalyst activity evaluation test. [Diagram 5] FIG. 5 is a graph showing the NOx purification rate in a performance evaluation test when the temperature is decreasing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. In the drawings referred to in the following description, the same components or components having similar functions are given the same reference numerals, and repeated description may be omitted. In addition, the dimensional ratio of the drawings may differ from the actual ratio for convenience of explanation, and some components may be omitted from the drawings. In addition, in this application, a numerical range expressed using the symbol "~" includes the numerical values ​​described before and after the symbol "~" as the lower limit and upper limit, respectively. The upper limit and lower limit of the numerical range described in this application can be arbitrarily combined. In this application, the description "on ~" includes both "directly on ~" and "indirectly on ~" unless otherwise specified in the context. In this application, "including ~" means that additional components may be included, and includes "essentially consisting of ~" and "consisting of ~". "Essentially consisting of ~" means that additional components that do not have a substantial adverse effect may be included. "Consisting of ~" means that only the materials described are included, but does not exclude the inclusion of unavoidable impurities.

[0011] An exhaust gas purification device 100 according to an embodiment will be described with reference to Figures 1 and 2. The exhaust gas purification device 100 according to the embodiment includes a substrate 10, a first catalyst layer 20, a second catalyst layer 30, and a third catalyst layer 40.

[0012] (1) Base material 10 The shape of the substrate 10 is not particularly limited, but for example, as shown in Fig. 2, the substrate 10 may be composed of a frame portion 12 and partition walls 16 that divide the space inside the frame portion 12 to define a plurality of cells 14. The partition walls 16 extend between a first end (first end face) I and a second end (second end face) J of the substrate 10, and define a plurality of cells 14 extending between the first end I and the second end J.

[0013] The substrate 10 may be formed, for example, from a ceramic material having high heat resistance, such as cordierite (2MgO·2Al2O3·5SiO2), alumina, zirconia, or silicon carbide, or from a metal foil, such as a stainless steel foil.

[0014] 1 and 2, dashed arrows indicate the flow direction of exhaust gas in the exhaust gas purification device 100 and the substrate 10. Exhaust gas flows into the cells 14 of the substrate 10 through the first end I and flows out of the cells 14 of the substrate 10 through the second end J. Therefore, hereinafter, the first end I will also be referred to as the upstream end I and the second end J as the downstream end J, as appropriate. In this specification, the length between the upstream end I and the downstream end J, i.e., the total length of the substrate 10, will be represented as Ls.

[0015] (2) First catalyst layer 20 The first catalyst layer 20 is formed on the substrate 10 in a first region X between the downstream end J and a first position P separated by a first distance La from the downstream end J toward the upstream end I (i.e., in the opposite direction to the flow direction of the exhaust gas). The first distance La is 50% to 70% of the total length Ls of the substrate 10. The first catalyst layer 20 may have a length equal to the first distance La in the extension direction of the cells 14.

[0016] The first catalyst layer 20 includes rhodium. The rhodium mainly functions as a catalyst for reducing NOx. The rhodium may be in particulate form. The rhodium may be supported on a support particle. The support particle may include a metal oxide.

[0017] The first catalytic layer 20 may include an oxygen storage material that stores oxygen in an atmosphere under an oxygen-rich atmosphere and releases oxygen under an oxygen-deficient atmosphere. Examples of oxygen storage materials include ceria (CeO2), composite oxides of ceria and other oxides (e.g., composite oxides of ceria and zirconia (ZrO2) (Ce-Zr composite oxide), alumina (Al2O3), composite oxides of ceria and zirconia (Al-Ce-Zr composite oxide)), materials to which additives have been added, and mixtures of these. Examples of additives include lanthana (La2O3), yttria (Y2O3), neodymia (Nd2O3), or praseodymia (Pr6O 11 ), and these materials can improve the heat resistance of the oxygen storage material. The additive may form a composite oxide together with the main component of the oxygen storage material. In particular, a Ce-Zr composite oxide may be used as the oxygen storage material because it has a high oxygen storage capacity (Oxygen storage capacity, OSC) and is relatively inexpensive. The Ce-Zr composite oxide may have a pyrochlore or fluorite structure. The oxygen storage material in the first catalyst layer 20 may include a pyrochlore-type Ce-Zr composite oxide and a fluorite-type Ce-Zr composite oxide.

[0018] The first catalyst layer 20 may further include other optional components, such as a binder and an additive.

[0019] The total mass of the first catalyst layer 20 may be 170 g / L or more based on the volume of the substrate 10 in the first region X. As a result, the first catalyst layer 20 has a large heat capacity, and therefore when low-temperature exhaust gas flows into the exhaust gas purification device 100, a decrease in temperature of the first catalyst layer 20 is mitigated, allowing the exhaust gas purification device 100 to exhibit good exhaust gas purification performance.

[0020] The first catalyst layer 20 can be formed, for example, as follows. First, an aqueous solution of a rhodium salt, an oxygen storage material, and optional components are mixed to prepare a slurry. The slurry is applied onto the substrate 10 in the first region X to form a slurry layer. The slurry layer is dried and fired by heating. Thus, the first catalyst layer 20 is formed on the substrate 10 in the first region X.

[0021] (3) Second catalyst layer 30 The second catalyst layer 30 is formed on the substrate 10 in a second region Y between the upstream end I and a second position Q separated by a second distance Lb from the upstream end I toward the downstream end J (i.e., in the exhaust gas flow direction). The second distance Lb is 50% or more of the total length Ls of the substrate 10. The sum of the first distance La and the second distance Lb is equal to or more than the total length Ls of the substrate 10. As a result, the entire region of the substrate 10 is covered with at least one of the first catalyst layer 20 or the second catalyst layer 30, so that the exhaust gas purification device 100 can have good exhaust gas purification performance. The second catalyst layer 30 may have a length equal to the second distance Lb in the extension direction of the cells 14.

[0022] The second catalyst layer 30 includes rhodium. The rhodium mainly functions as a catalyst for reducing NOx. The rhodium may be in particulate form. The rhodium may be supported on support particles. The support particles may include a metal oxide.

[0023] The second catalyst layer 30 contains an oxygen storage material. Examples of the oxygen storage material are as described above. The oxygen storage material in the second catalyst layer 30 contains a pyrochlore-type Ce—Zr composite oxide and a fluorite-type Ce—Zr composite oxide in a weight ratio of 0.2:1 to 0.4:1. This allows the exhaust gas purification device 100 to have high warm-up performance and reduces deterioration of the performance of the exhaust gas purification device during use.

[0024] The second catalyst layer 30 may further contain other optional components, such as a binder and an additive.

[0025] The second catalyst layer 30 can be formed, for example, as follows. First, an aqueous solution of a rhodium salt, an oxygen storage material, and optional components are mixed to prepare a slurry. The slurry is applied onto the substrate 10 in the second region Y to form a slurry layer. The slurry layer is dried and fired by heating. Thus, the second catalyst layer 30 is formed on the substrate 10 in the second region Y.

[0026] (4) Third catalyst layer 40 The third catalyst layer 40 is formed on the second catalyst layer 30 in a third region Z between the upstream end I and a third position R separated by a third distance Lc from the upstream end I toward the downstream end J (i.e., in the flow direction of exhaust gas). By forming the third catalyst layer 40 on the second catalyst layer 30, the exhaust gas purification device 100 can have high warm-up properties. The third distance Lc is 40% or less, particularly 30% or less, of the total length Ls of the substrate 10. This allows the exhaust gas purification device 100 to have high warm-up properties. The third catalyst layer 40 may have a length equal to the third distance Lc in the extension direction of the cells 14.

[0027] The third catalyst layer 40 includes palladium. The palladium functions primarily as a catalyst for oxidizing HC. The palladium may be in particulate form. The palladium may be supported on support particles. The support particles may include a metal oxide.

[0028] The third catalyst layer 40 may include an oxygen storage material. Examples of the oxygen storage material are as described above. The oxygen storage material in the third catalyst layer 40 may include a fluorite-type Ce—Zr composite oxide.

[0029] The third catalyst layer 40 may further contain other optional components, such as a binder and an additive.

[0030] The total mass of the third catalyst layer 40 may be more than 0 g / L and not more than 105 g / L based on the volume of the substrate 10 in the third region Z. As a result, the third catalyst layer 40 has a small heat capacity, so that the temperature of the third catalyst layer 40 rises in a short time during warm-up, and good exhaust gas purification performance can be achieved. In other words, the exhaust gas purification device 100 can have high warm-up properties.

[0031] The third catalytic layer 40 can be formed, for example, as follows. First, an aqueous solution of a palladium salt, an oxygen storage material, and optional components are mixed to prepare a slurry. The slurry is applied onto the second catalytic layer 30 in the third region Z to form a slurry layer. The slurry layer is dried and fired by heating. Thus, the third catalytic layer 40 is formed on the second catalytic layer 30 in the third region Z.

[0032] The exhaust gas purification device 100 according to the embodiment can be applied to various vehicles equipped with an internal combustion engine.

[0033] The present invention is not limited to the above-described embodiment. Various modifications, additions, and deletions can be made without departing from the technical idea or scope of the present invention described in the claims. EXAMPLES

[0034] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0035] (1) Materials used in the Examples and Comparative Examples a) Substrate (honeycomb substrate) Material: Cordierite Capacity: 875cc Wall thickness: 2mil (50.8μm) Cell Density: 600 cells per square inch Cell cross-sectional shape: hexagonal

[0036] b) Material 1 A material obtained by adding La2O3 to Al2O3 (La2O3: 1wt%~10wt%).

[0037] c) Material 2 (fluorite type Ce-Zr composite oxide) A material with a fluorite structure (CeO2: 15wt%~30wt%) obtained by adding small amounts of Nd2O3, La2O3, and Y2O3 to an Al2O3-CeO2-ZrO2 composite oxide.

[0038] d) Material 3 (Pyrochlore-type Ce-Zr composite oxide) A composite oxide containing CeO2 and ZrO2 with approximately equal molecular weights, and a trace amount of rare earth metal oxide, such as Pr6O 11 A material with a pyrochlore structure (CeO2: 45mol%~65mol%, ZrO2: 45mol%~65mol%) obtained by adding La2O3, Y2O3, and Nd2O3 and reducing it at high temperature.

[0039] e) Material 4 Palladium nitrate solution

[0040] f) Material 5 Rhodium nitrate solution

[0041] g) Material 6 Barium sulfate

[0042] (2) Construction of exhaust gas purification device Example 1 Materials 1, 2, 3, and 5 were added to the stirred distilled water and mixed to prepare a suspended slurry 1. Slurry 1 was poured into the cell from the downstream end of the substrate, and excess slurry was blown off with a blower. As a result, the partition walls of the substrate were coated with slurry 1 in a first region between the downstream end of the substrate and a first position separated by a distance of 50% of the total length of the substrate from the downstream end of the substrate toward the upstream end of the substrate. The substrate was placed in a dryer with an internal temperature maintained at 120° C. for 2 hours to evaporate the water in slurry 1. Then, the substrate was baked in an electric furnace at 500° C. for 2 hours. As a result, a first catalyst layer was formed.

[0043] The amount of material 1 contained in the first catalyst layer based on the volume of the substrate in the first region was 80 g / L, the amount of material 2 was 60 g / L, the amount of material 3 was 30 g / L, and the amount of Rh particles derived from material 5 was 0.3 g / L.

[0044] Next, materials 1, 2, 3, and 5 were added to the stirred distilled water and mixed to prepare a suspended slurry 2. The slurry 2 was poured into the cell from the upstream end of the substrate, and excess slurry was blown off with a blower. As a result, the partition walls of the substrate were coated with the slurry 2 in the second region between the upstream end of the substrate and a second position separated by a distance of 50% of the total length of the substrate from the upstream end of the substrate toward the downstream end of the substrate. The substrate was placed in a dryer with an internal temperature maintained at 120° C. for 2 hours to evaporate the water in the slurry 2, and then calcined in an electric furnace at 500° C. for 2 hours. As a result, a second catalyst layer was formed.

[0045] The amount of material 1 contained in the second catalyst layer based on the volume of the substrate in the second region was 66 g / L, the amount of material 2 was 45 g / L, the amount of material 3 was 9 g / L, and the amount of Rh particles derived from material 5 was 0.3 g / L.

[0046] Next, materials 1, 2, 4, and 6 were added to the stirred distilled water and mixed to prepare a suspended slurry 3. The slurry 3 was poured into the cell from the upstream end of the substrate, and excess slurry was blown off with a blower. As a result, a layer of the slurry 3 was formed in a third region between the upstream end of the substrate and a third position separated by a distance of 30% of the total length of the substrate from the upstream end of the substrate toward the downstream end of the substrate. The substrate was placed in a dryer with an internal temperature maintained at 120° C. for 2 hours to evaporate the water in the slurry 3, and then calcined in an electric furnace at 500° C. for 2 hours. As a result, a third catalyst layer was formed on the second catalyst layer.

[0047] The amount of material 1 contained in the third catalyst layer based on the volume of the substrate in the third region was 30 g / L, the amount of material 2 was 50 g / L, the amount of Pd particles derived from material 4 was 5.0 g / L, and the amount of material 6 was 20 g / L.

[0048] In this manner, the exhaust gas purification device of Example 1 was obtained.

[0049] Example 2 An exhaust gas purification device was prepared in the same manner as in Example 1, except that the amount of material 1 contained in the second catalyst layer, based on the volume of the substrate in the second region, was 58 g / L, the amount of material 2 was 45 g / L, the amount of material 3 was 17 g / L, and the amount of Rh particles derived from material 5 was 0.3 g / L.

[0050] Comparative Example 1 An exhaust gas purification device was prepared in the same manner as in Example 1, except that the amount of material 1 contained in the second catalyst layer, based on the volume of the substrate in the second region, was 70 g / L, the amount of material 2 was 45 g / L, the amount of material 3 was 4.5 g / L, and the amount of Rh particles derived from material 5 was 0.3 g / L.

[0051] Comparative Example 2 An exhaust gas purification device was prepared in the same manner as in Example 1, except that the amount of material 1 contained in the second catalyst layer, based on the volume of the substrate in the second region, was 41 g / L, the amount of material 2 was 45 g / L, the amount of material 3 was 34 g / L, and the amount of Rh particles derived from material 5 was 0.3 g / L.

[0052] Comparative Example 3 An exhaust gas purification device was produced in the same manner as in Comparative Example 1, except that the amount of material 1, the amount of material 2, the amount of material 3, and the amount of Rh particles derived from material 5 contained in the first catalyst layer, based on the volume of the substrate in the first region, were 60 g / L, 60 g / L, 30 g / L, and 0.3 g / L, respectively, and that the second catalyst layer was formed after the third catalyst layer was formed (i.e., the third catalyst layer was formed between the substrate and the second catalyst layer).

[0053] Comparative Example 4 An exhaust gas purification device was produced in the same manner as in Comparative Example 1, except that the amount of material 1 contained in the third catalyst layer, based on the volume of the substrate in the third region, was 50 g / L, the amount of material 2 was 50 g / L, the amount of Pd particles derived from material 4 was 5.0 g / L, and the amount of material 6 was 20 g / L, and that the second catalyst layer was formed after the third catalyst layer was formed (i.e., the third catalyst layer was formed between the substrate and the second catalyst layer).

[0054] Table 1 summarizes the weight ratio (P:F) of material 2 (fluorite-type Ce-Zr composite oxide) and material 3 (pyrochlore-type Ce-Zr composite oxide) in the second catalytic layer, the hierarchical relationship between the second catalytic layer and the third catalytic layer, the total amount of the first catalytic layer based on the volume of the substrate in the first region, the total amount of the second catalytic layer based on the volume of the substrate in the second region, and the total amount of the third catalytic layer based on the volume of the substrate in the third region in each of the examples and comparative examples.

[0055] [Table 1]

[0056] (3) Aging treatment The exhaust gas purification devices of the Example and Comparative Example were each connected to the exhaust system of a 4.6L V8 engine. While maintaining the bed temperature of the exhaust gas purification device at 950°C for 50 hours, a stoichiometric mixture (air-fuel ratio A / F=14.6) and a lean mixture containing excess oxygen (A / F>14.6) were alternately introduced into the engine at a time ratio of 3:1 at a fixed interval. This aging treatment was performed on the exhaust gas purification device.

[0057] (4) Warm-up performance evaluation After the temperature in the center of the aged exhaust gas purification device was cooled to 50°C, it was connected to the exhaust system of a 2.5L L-type 4-cylinder engine. An air-fuel mixture with an A / F ratio of 14.4 was introduced into the engine, and exhaust gas from the engine at approximately 500°C was introduced into the exhaust gas purification device. The THC content of the exhaust gas at the upstream and downstream ends of the exhaust gas purification device was measured to determine the THC purification rate. Table 2 and Figure 3 show the time it took for the THC purification rate to reach 50% after the 500°C exhaust gas was first introduced into the exhaust gas purification device. The shorter the time it took for the THC purification rate to reach 50%, the better the warm-up performance.

[0058] As shown in FIG. 3, the exhaust gas purification devices of Examples 1 and 2 and Comparative Example 1, in which P:F was 0.1:1 to 0.4:1, exhibited higher warm-up performance than the exhaust gas purification device of Comparative Example 2, in which P:F was 0.75:1.

[0059] The exhaust gas purification device of Comparative Example 4, in which the total amount of the third catalyst layer was 125 g / L, showed lower warm-up performance than the exhaust gas purification device of Comparative Example 3, in which the total amount of the third catalyst layer was 105 g / L. This is considered to be because the total amount of the third catalyst layer was larger in Comparative Example 4, i.e., the heat capacity was larger, and therefore it took more time for the temperature of the exhaust gas purification device to rise. Note that the total amount of the first catalyst layer was also different between Comparative Example 3 and Comparative Example 4, but since the first catalyst layer was kept at a relatively low temperature during the warm-up performance evaluation test, it is considered that the amount of THC purified by the first catalyst layer was small. Therefore, it is considered that the effect of the difference in the total amount of the first catalyst layer on the warm-up performance was small.

[0060] The exhaust gas purification device of Comparative Example 1, in which the second catalyst layer was the lower layer and the third catalyst layer was the upper layer, exhibited higher warm-up performance than the exhaust gas purification device of Comparative Example 3, in which the second catalyst layer was the upper layer and the third catalyst layer was the lower layer. Note that the total amount of the first catalyst layer was also different between Comparative Example 1 and Comparative Example 3, but as described above, it is considered that the effect of the difference in the total amount of the first catalyst layer on the warm-up performance was small.

[0061] (5) Catalytic activity evaluation The aged exhaust gas purification device was connected to the exhaust system of a 2.5L L-type 4-cylinder engine. An air-fuel mixture with an A / F of 14.4 was introduced into the engine, and the exhaust gas from the engine at 600°C was cooled to 200°C by a heat exchanger and introduced into the exhaust gas purification device. The heat exchanger was controlled to raise the temperature of the exhaust gas introduced into the exhaust gas purification device from 200°C at a constant rate, and during this time, the NOx content of the exhaust gas at the upstream and downstream ends of the exhaust gas purification device was measured to determine the NOx purification rate. Note that the exhaust flow rate was made sufficiently large and the exhaust temperature rise rate was made sufficiently small so that the exhaust gas purification device always had a uniform temperature in the gas flow direction. The exhaust temperature when the NOx purification rate reached 50% (NOx-T50) is shown in Table 2 and Figure 4. The lower the NOx-T50, the higher the catalytic activity of the exhaust gas purification device.

[0062] 4, the exhaust gas purification devices of Examples 1 and 2 and Comparative Example 2, in which P:F was 0.2:1 to 0.75:1, exhibited higher catalytic activity than the exhaust gas purification device of Comparative Example 1, in which P:F was 0.1:1. This is believed to be because, in Examples 1 and 2 and Comparative Example 2, the high oxygen storage and release capacity of the pyrochlore-type Ce-Zr composite oxide reduced the deterioration of the exhaust gas purification device due to the aging treatment.

[0063] The exhaust gas purification device of Comparative Example 1 exhibited lower catalytic activity than the exhaust gas purification devices of Comparative Examples 3 and 4, in which the second catalyst layer was the upper layer and the third catalyst layer was the lower layer. However, the exhaust gas purification devices of Examples 1 and 2 and Comparative Example 2 exhibited catalytic activity equal to or higher than the exhaust gas purification devices of Comparative Examples 3 and 4.

[0064] (6) Performance evaluation at low temperatures The aged exhaust gas purification device was connected to the exhaust system of a 2.5L L-type 4-cylinder engine. An air-fuel mixture with an A / F ratio of 14.4 was introduced into the engine, and the exhaust from the engine was introduced into the exhaust gas purification device. The temperature of the exhaust at the upstream end of the exhaust gas purification device was first set to 600°C and then lowered to below 500°C. During this time, the NOx content of the exhaust at the upstream and downstream ends of the exhaust gas purification device was measured to determine the NOx purification rate. Table 2 and Figure 5 show the NOx purification rate when the exhaust temperature at the upstream end of the exhaust gas purification device reached 500°C. A higher NOx purification rate means higher performance at lower temperatures.

[0065] 5, the exhaust gas purification devices of Examples 1 and 2 and Comparative Examples 1, 2, and 4, in which the total amount of the first catalyst layer was 170.3 g / L, showed higher performance during temperature drop than the exhaust gas purification device of Comparative Example 3, in which the total amount of the first catalyst layer was 150.3 g / L. This is believed to be because, in Examples 1 and 2 and Comparative Examples 1, 2, and 4, the total amount of the first catalyst layer was larger, i.e., the heat capacity was larger, which alleviated the decrease in temperature of the exhaust gas purification device during the temperature drop of the exhaust gas.

[0066] [Table 2] [Explanation of symbols]

[0067] 10: substrate, 12: frame, 14: cell, 16: partition wall, 20: first catalyst layer, 30: second catalyst layer, 40: third catalyst layer, 100: exhaust gas purification device, I: upstream end (first end), J: downstream end (second end), P: first position, Q: second position, R: third position, X: first region, Y: second region, Z: third region

Claims

1. An exhaust gas purification device, A substrate having a total length (Ls), the substrate having an upstream end where exhaust gas flows into the substrate and a downstream end where the exhaust gas flows out of the substrate; a first catalyst layer including rhodium provided on the substrate in a first region between the downstream end and a first position separated by a first distance (La) from the downstream end toward the upstream end, the first distance (La) being 50% to 70% of a total length (Ls) of the substrate; a second catalyst layer including rhodium and an oxygen storage material provided on the substrate in a second region between the upstream end and a second position separated by a second distance (Lb) from the upstream end toward the downstream end, the second distance (Lb) being 50% or more of a total length (Ls) of the substrate, and the oxygen storage material including a pyrochlore-type Ce—Zr composite oxide and a fluorite-type Ce—Zr composite oxide in a weight ratio of 0.2:1 to 0.4:1; an exhaust gas purification device comprising: a third catalyst layer containing palladium and provided on the second catalyst layer in a third region between the upstream end and a third position separated by a third distance (Lc) from the upstream end toward the downstream end, wherein the third distance (Lc) is 40% or less of a total length (Ls) of the substrate.

2. 2. The exhaust gas purification device according to claim 1, wherein a total mass of the first catalyst layer based on a volume of the substrate in the first region is 170 g / L or more.

3. 3. The exhaust gas purification device according to claim 1, wherein a total mass of the third catalyst layer based on a volume of the substrate in the third region is more than 0 g / L and not more than 105 g / L.

4. The exhaust gas purification device according to claim 1 or 2, wherein the first catalyst layer further comprises an oxygen storage material.

Citation Information

Patent Citations

  • Exhaust gas purification catalyst

    JP2015093267A

  • Exhaust gas purification catalyst

    JP2019084467A

  • Exhaust gas purifier

    JP2022061298A

  • Exhaust gas purifying catalyst

    JP2023008520A

  • Exhaust gas purifying catalyst

    WO2017163985A1