Nitriding treatment component and method of manufacturing the same
A nitrided part with a hardened and conforming layer on a steel substrate addresses crack resistance and emission reduction by forming layers with controlled thickness and composition, enhancing durability and reducing gas emissions.
Patent Information
- Application Number
- JP2023084583
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional nitriding treatments for steel materials reduce CO2 emissions but result in nitrided layers with inferior crack resistance and reduced durability under mechanical stress, particularly in sliding/rolling parts.
A nitrided part with a hardened layer and conforming layer is formed on a steel substrate, where the hardened layer has a specific thickness and nitrogen concentration, and the conforming layer contains iron oxide, enhancing crack resistance while reducing gas emissions.
The nitrided part exhibits superior crack resistance and reduced gas emissions by forming a hardened layer with controlled thickness and nitrogen concentration, and a conforming layer with iron oxide, improving durability under mechanical stress.
Smart Images

Figure 2024168147000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal part subjected to nitriding treatment, and more particularly to a part made of a steel material subjected to nitriding treatment and a method for manufacturing the same. [Background technology]
[0002] Sliding / rolling parts such as cogs and gears in power transmission devices are used in harsh environments where they are repeatedly subjected to mechanical loads, and wear resistance is one of the most important mechanical properties. Sliding / rolling parts are usually made of steel materials, and are often carburized as a surface treatment to ensure wear resistance.
[0003] Gas carburizing, which uses gases whose main components are CO2, H2, CH4, etc., is currently the mainstream method for carburizing steel materials. However, the current gas carburizing process emits large amounts of CO2 gas, which is inconvenient for the current CO2 gas emission reduction efforts. Therefore, there is a demand for alternative surface treatment technologies that can reduce CO2 gas emissions.
[0004] In response to such demands, for example, Patent Document 1 (JP 2017-137547 A) discloses a nitriding method for penetrating and diffusing nitrogen into a workpiece made of a steel material, the nitriding method comprising the steps of: inductively heating the workpiece at a frequency that results in a current penetration depth of 2 mm or more; and spraying nitriding gas onto the surface of the workpiece.
[0005] According to Patent Document 1, it is possible to suppress the decomposition of the nitriding gas on the surface of the workpiece while maintaining the diffusion rate of nitrogen decomposed from the nitriding gas into the workpiece, and as a result, it is possible to shorten the nitriding treatment time. In addition, although it is not directly mentioned in Patent Document 1, it is expected that the amount of CO2 gas emitted will be reduced because it is not a carburizing treatment. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-137547 A Summary of the Invention [Problem to be solved by the invention]
[0007] As mentioned above, there is a strong demand for reducing CO2 gas emissions in the manufacturing of industrial products these days. By changing the conventional carburizing treatment of steel materials to the nitriding treatment disclosed in Patent Document 1, it is expected that the amount of CO2 gas emitted during surface treatment can be reduced.
[0008] On the other hand, the nitrided layer formed by the conventional nitriding treatment is likely to be harder than the carburized layer and is advantageous in terms of wear resistance, but since the diffusion coefficient of nitrogen in steel materials is smaller than that of carbon, the thickness of the layer formed is likely to be thinner than that of the carburized layer. Therefore, when sliding / rolling parts are subjected to repeated mechanical loads, the conventional nitrided layer is prone to cracking due to stress concentration when unexpected foreign objects are caught in the layer, which causes another problem that the durability of the sliding / rolling parts is reduced due to factors other than wear.
[0009] The present invention has been made to solve the above-mentioned requirements and problems, and its object is to provide a nitriding-treated part and a manufacturing method thereof, which are excellent in crack resistance compared to parts with conventional nitriding layers formed, while reducing CO2 gas emissions compared to the formation of a carburized layer by conventional gas carburizing treatment, in surface treatment of steel materials. [Means for solving the problem]
[0010] (I) One aspect of the present invention is a nitriding-treated part having a steel material as a base material, The nitriding treated component has a hardened layer and a conforming layer in a surface layer region of the base material, The hardened layer has an average thickness of 10 μm or more and 100 μm or less and a nitrogen concentration of 0.05% by mass or more and 5% by mass or less, The conforming layer is formed on the outer layer side of the hardened layer, has an average thickness of 5 μm or more and 50 μm or less, and contains iron oxide.
[0011] In the present invention, the following improvements and modifications can be freely combined in the above-mentioned nitriding treated part (I). (i) The hardened layer has a Vickers hardness of 680 Hv or more, and the running-in layer has a Vickers hardness of 500 Hv or less. (ii) The substrate has a martensitic structure.
[0012] (II) Another aspect of the present invention is a method for producing the above-mentioned nitriding treated part, a substrate preparation step of preparing the substrate having a desired shape; a hardened layer / conformity layer forming step of forming the hardened layer and the conformity layer on the surface layer region of the base material; and a quenching process for forming a martensite structure in the base material having the hardened layer and the running-in layer formed thereon, The hardened layer / conformity layer forming step includes: a surface treatment aqueous solution preparation step of preparing an aqueous surface treatment solution comprising an aqueous solution of a compound having a triazine ring and / or a compound having a nitrogen-carbon double bond; a nitriding / oxidizing step of immersing the substrate in the surface treatment aqueous solution and heating the substrate by a high-frequency induction heating method to cause nitrogen to penetrate into a surface layer region of the substrate and oxidize iron components of the substrate. The present invention provides a method for producing a nitriding treated part, comprising the steps of:
[0013] In the present invention, the following improvements and modifications can be freely combined in the above-mentioned method for producing a nitriding treated part (II). (iii) The heating by the high-frequency induction heating method in the nitriding / oxidizing step is controlled so that the temperature of the surface of the base material is 700° C. or more and 950° C. or less. (iv) The quenching process includes heating by a high-frequency induction heating method, and the input is controlled so that the surface temperature of the base material is raised to 800°C or higher and 1100°C or lower by the high-frequency induction heating method and is a temperature higher than that of the nitriding-oxidizing process. Effect of the Invention
[0014] According to the present invention, in the surface treatment of steel materials, it is possible to provide a nitriding-treated part that is more excellent in crack resistance than a part having a conventional nitriding layer while reducing CO2 gas emissions compared to the formation of a carburized layer by a conventional gas carburizing process, and a manufacturing method thereof. Note that the problems, configurations and effects other than those described above will be made clear from the explanation of the embodiments described below. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a process diagram showing an example of a method for producing a nitriding treated part according to the present invention. [Diagram 2] 1 is a chart showing an example of the results of X-ray diffraction measurement of the surface of Example 1. [Diagram 3] 4 is an example of a secondary electron microscope image of a cross section of a surface region of Example 1. [Figure 4] 4 is a graph showing an example of the relationship between the depth direction distance from the surface and the nitrogen concentration in Example 1. [Diagram 5] 4 is a graph showing an example of the relationship between the depth direction distance from the surface and Vickers hardness in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] As described above, nitriding-treated parts hardened with a nitriding layer formed by conventional nitriding have a weakness in that the nitriding layer is prone to cracking when stress concentration occurs. The present inventors have conducted extensive research with the aim of overcoming the weakness of the crack resistance of nitriding-treated parts while reducing the amount of CO2 gas emitted in the formation of the hardened layer.
[0017] As a result, it was found that by immersing a substrate to be treated in a predetermined aqueous surface treatment solution and heating the substrate by high-frequency induction heating, a hardened layer can be formed on the surface region of the substrate, and a conforming layer can be formed on the outer side of the hardened layer. The present invention was completed based on this finding.
[0018] Hereinafter, the embodiments of the present invention will be described in detail along with the manufacturing procedure with reference to the drawings. However, the present invention is not limited to the embodiments described here, and can be appropriately combined with known techniques or improved based on known techniques without departing from the technical idea of the invention.
[0019] [Manufacturing method for nitriding treated parts] Fig. 1 is a process diagram showing an example of a method for producing a nitriding treated part according to the present invention. As shown in Fig. 1, the method for producing a nitriding treated part according to the present invention generally comprises a substrate preparation step S1, a hardened layer / run-in layer formation step S2, and a quenching step S3. The greatest feature of this production method is the hardened layer / run-in layer formation step S2.
[0020] Each step will now be described in more detail.
[0021] The substrate preparation step S1 is a step of preparing a substrate made of a steel material and having a desired shape. There is no particular limitation on the steel material used as the substrate, and any steel material that has been conventionally used as a material for sliding / rolling parts can be used as appropriate. For example, low-alloy steel that is mainly composed of iron, contains 0.02 to 2.14 mass% carbon, and contains 5 mass% or less of other alloying elements in total can be used as appropriate. There is also no particular limitation on the method of forming the substrate into the desired shape, and any conventional method can be used as appropriate. For example, a forging method or a powder metallurgy method can be used as appropriate.
[0022] The hardened layer / familiarization layer forming step S2 is a step of forming a hardened layer and a familiarization layer on the surface region of the substrate prepared in step S1, and includes a surface treatment aqueous solution preparation step S2a of preparing a predetermined surface treatment aqueous solution, and a nitriding / oxidizing step S2b of heating the substrate while immersed in the surface treatment aqueous solution to cause nitrogen to penetrate into the substrate and oxidize the iron components of the substrate.
[0023] The surface treatment aqueous solution is preferably an aqueous solution of a compound having a triazine ring and / or a compound having a nitrogen-carbon double bond. The solute concentration of the surface treatment aqueous solution is preferably 0.1 mass% or more and less than the saturation concentration at room temperature. As the compound having a triazine ring, for example, triazine or melamine can be preferably used. As the compound having a nitrogen-carbon double bond, for example, guanidine or biguanide can be preferably used.
[0024] The method of heating the substrate in the nitriding and oxidizing step S2b is not particularly limited, but for example, high-frequency induction heating can be suitably used. It is preferable that the input of the high-frequency induction heating is controlled so that the temperature of the substrate surface is 700°C or higher and 950°C or lower. This allows nitrogen to penetrate into the surface layer region of the substrate and oxidizes the iron components of the substrate, forming a hardened layer and a conforming layer.
[0025] In the present invention, the surface temperature of the substrate when heated in the aqueous solution is regarded as the heating temperature by the high-frequency induction heating method. It is also preferable to control the substrate so that it is not exposed from the aqueous solution during the heat treatment (for example, additional aqueous solution may be added as necessary).
[0026] The thickness of the hardened layer, the nitrogen concentration in the hardened layer, and the thickness of the conforming layer can be controlled by adjusting the heating temperature and the heating holding time. In the present invention, the hardened layer is preferably a layer having an average thickness of 10 μm to 100 μm and a nitrogen concentration of 0.05 mass % to 5 mass %, and the conforming layer is preferably a layer having an average thickness of 5 μm to 50 μm and containing iron oxide.
[0027] From the viewpoint of wear resistance, the hardened layer preferably has a Vickers hardness of 680 Hv or more, more preferably 700 Hv or more, whereas from the viewpoint of crack resistance, the running-in layer preferably has a Vickers hardness of 500 Hv or less, more preferably 450 Hv or less.
[0028] The quenching process S3 is a process for forming a martensite structure in the base material having the hardened layer and the running-in layer formed thereon. There is no particular limitation on the quenching method, and conventional methods can be used as appropriate. From the viewpoint of work efficiency, it is preferable to use a high-frequency induction heating method as in the elementary process S2b. It is preferable to control the input of the heating by the high-frequency induction heating method so that the surface temperature of the base material is 800°C or more and 1100°C or less, and is a temperature higher than that of the elementary process S2b.
[0029] Between the elementary step S2b and step S3, the temperature of the substrate may be lowered once, or the temperature of the substrate may be increased following the elementary step S2b without being lowered. In step S3, the substrate may not be immersed in the surface treatment aqueous solution. EXAMPLES
[0030] The present invention will be explained in more detail below with reference to various experiments, however, the present invention is not limited to the configurations and structures described in these experiments.
[0031] [Experiment 1] (Preparation of Example 1) First, a commercially available aluminum chromium molybdenum steel rod (JIS standard: SACM645, diameter 22 mm × length 40 mm) was prepared as a substrate (substrate preparation step).
[0032] Next, a surface treatment aqueous solution consisting of an aqueous melamine solution (concentration: 0.3% by mass) was prepared (a surface treatment aqueous solution preparation step).
[0033] Prior to the actual nitriding and oxidizing process, a control curve for the substrate heating temperature by high-frequency induction heating in an aqueous solution was created using a dummy specimen with a thermocouple attached to the substrate surface.
[0034] The above-mentioned substrate was immersed in the prepared surface treatment aqueous solution, and the substrate was heated by high-frequency induction heating based on the created control curve. The input of high-frequency waves was controlled so that the heating temperature was 780°C, and was maintained for 5 minutes (nitriding and oxidizing process). After maintaining this temperature for 5 minutes, the heating temperature was controlled so that it was 900°C, and was maintained for 1 minute, and the input of high-frequency waves was stopped to cool the substrate (quenching process). In this way, the sample of Example 1 was produced.
[0035] [Experiment 2] (Property Investigation of Example 1) The properties of Example 1 prepared in Experiment 1 were investigated.
[0036] An X-ray diffraction (XRD) device (Ultima III, manufactured by Rigaku Corporation) was used to perform XRD measurement of the surface of Example 1. FIG. 2 is a chart showing an example of the XRD measurement results of the surface of Example 1. As shown in FIG. 2, diffraction peaks of iron oxides (FeO, Fe2O3, Fe3O4) were detected, confirming that a layer containing iron oxide was formed. In addition, diffraction peaks of a body-centered cubic structure (BCC) were detected, confirming that the matrix phase was a martensite phase.
[0037] An electron probe microanalyzer (EPMA) device (manufactured by JEOL Ltd., model JXA-8530F) was used to perform microstructural observation and nitrogen concentration analysis on the cross section of the surface layer region of Example 1. In addition, a microbeakers hardness tester (manufactured by Matsuzawa Co., Ltd., model AMT-X) was used to measure the Vickers hardness on the cross section.
[0038] Fig. 3 is an example of a secondary electron microscope (SEM) image of a cross section of the surface region of Example 1. Fig. 4 is a graph showing an example of the relationship between the depth direction distance from the surface and the nitrogen concentration in Example 1. Fig. 5 is a graph showing an example of the relationship between the depth direction distance from the surface and the Vickers hardness in Example 1.
[0039] 3, it can be seen that two types of layers (a relatively white / bright layer with a thickness of about 50 μm and a relatively black / dark layer with a thickness of about 25 μm in the figure) are formed in the surface layer region (thickness of about 75 μm) of the substrate having a martensite structure. The black region between the embedding resin and Example 1 is a gap.
[0040] From Figure 4, it can be seen that the nitrogen concentration in the surface region (approximately 75 μm thick) is higher than that in the inner substrate, and gradually decreases as one moves in the depth direction from the surface. This indicates that nitrogen atoms penetrate and diffuse from the surface of the substrate.
[0041] It can be seen from FIG. 5 that there is a region in which the Vickers hardness is higher than that of the inner base material, and there is a region in which the Vickers hardness is lower on the outer layer side of the hard region.
[0042] Considering the results of Figures 2 to 5 in a unified manner, it can be said that in Example 1, a hardened layer with a higher nitrogen concentration and higher Vickers hardness than the substrate is formed in the surface layer region of the substrate having a martensite structure, and a conformable layer containing iron oxide and lower Vickers hardness is formed on the outer layer side. In addition, in Example 1, the treatment time in the nitriding and oxidizing process is short, so the amount of CO2 gas emitted can be reduced.
[0043] [Experiment 3] (Preparation and Property Investigation of Examples 2-3 and Comparative Examples 1-2) The same SACM645 rod as in Experiment 1 was prepared as the substrate, and the following surface treatment aqueous solutions were prepared: triazine aqueous solution (concentration 0.3% by mass), guanidine aqueous solution (concentration 0.3% by mass), ammonia aqueous solution (concentration 5% by mass), and melamine aqueous solution (concentration 0.3% by mass). Next, a nitriding and oxidizing process was carried out using each of the surface treatment aqueous solutions by adjusting the heating temperature and holding time of the high-frequency induction heating. The quenching process was carried out in the same manner as in Experiment 1, and samples of Examples 2 and 3 and Comparative Examples 1 and 2 were produced.
[0044] The properties of each of the obtained samples were investigated in the same manner as in Experiment 2. Samples in which both the desired hardened layer (nitrogen concentration of 0.05 mass% or more at a position 40 μm from the sample surface) and the desired running-in layer (a layer containing iron oxide formed on the sample surface and Vickers hardness of 500 Hv or less) were formed were judged to be "passed," while samples in which either the hardened layer or the running-in layer did not meet the requirements were judged to be "failed." The results are shown in Table 1.
[0045] [Table 1]
[0046] As shown in Table 1, it was confirmed that in Examples 2 and 3, the desired hardened layer and the desired conformable layer were formed even when a triazine aqueous solution or a guanidine aqueous solution was used as the surface treatment aqueous solution. On the other hand, in Comparative Example 1, when an ammonia aqueous solution was used as the surface treatment aqueous solution, the desired hardened layer was not formed and the sample was judged as "failed." In Comparative Example 2, when the heating temperature was set to 500°C, the desired hardened layer was not formed and the sample was judged as "failed."
[0047] As described above, in Examples 1 to 3, it was confirmed that a hardened layer having a higher nitrogen concentration and higher Vickers hardness than the substrate was formed in the surface layer region of the substrate having a martensite structure, and a familiarization layer containing iron oxide and having a low Vickers hardness was formed on the outer layer side. From this, it was confirmed that the nitriding-treated part according to the present invention can suppress and alleviate stress concentration due to foreign matter, etc., since the familiarization layer is formed on the outer layer side of the hardened layer, even if unexpected foreign matter, etc., is sandwiched when used as a sliding / rolling part, and crack resistance can be ensured. In addition, the nitriding-treated part according to the present invention can reduce the amount of CO2 gas emitted during surface treatment because the nitriding treatment time is short.
[0048] The above-mentioned embodiments and experiments are described to aid in understanding of the present invention, and the present invention is not limited to the specific configurations described. For example, it is possible to replace a part of the configuration of the embodiments with a configuration according to the technical common sense of a person skilled in the art, and it is also possible to add a configuration according to the technical common sense of a person skilled in the art to the configuration of the embodiments. In other words, it is possible to delete, replace, or add a part of the configuration of the embodiments or experiments in this specification without departing from the technical idea of the invention.
Claims
1. A nitriding-treated part based on a steel material, The nitriding treated part has a hardened layer and a conforming layer in a surface layer region of the base material, The hardened layer has an average thickness of 10 μm or more and 100 μm or less and a nitrogen concentration of 0.05% by mass or more and 5% by mass or less, The nitriding treated part, wherein the running-in layer is formed on the outer layer side of the hardened layer, has an average thickness of 5 μm or more and 50 μm or less, and contains iron oxide.
2. The nitriding treated part according to claim 1, The hardened layer has a Vickers hardness of 680 Hv or more, The nitriding treated part, wherein the running-in layer has a Vickers hardness of 500 Hv or less.
3. The nitriding treated part according to claim 1, A nitriding treated part, characterized in that the base material has a martensite structure.
4. The nitriding treated part according to claim 2, A nitriding treated part, characterized in that the base material has a martensite structure.
5. A method for producing the nitriding treated part according to any one of claims 1 to 4, comprising the steps of: a substrate preparation step of preparing the substrate having a desired shape; a hardened layer / conformity layer forming step of forming the hardened layer and the conformity layer on the surface layer region of the base material; and a quenching process for forming a martensite structure in the base material having the hardened layer and the running-in layer formed thereon, The hardened layer / familiarization layer forming step includes: preparing a surface treatment aqueous solution comprising an aqueous solution of a compound having a triazine ring and / or a compound having a nitrogen-carbon double bond; a nitriding / oxidizing step of immersing the substrate in the surface treatment aqueous solution and heating the substrate by a high-frequency induction heating method to cause nitrogen to penetrate into a surface layer region of the substrate and oxidize iron components of the substrate. A method for producing a nitriding treated part, comprising the steps of:
6. The method for producing a nitriding treated part according to claim 5, A method for manufacturing a nitriding treated part, characterized in that the heating by the high-frequency induction heating method in the nitriding / oxidizing step is controlled by input control so that the temperature of the surface of the base material is 700°C or higher and 950°C or lower.
7. The method for producing a nitriding treated part according to claim 6, The method for producing a nitriding treated part is characterized in that the quenching process includes heating by a high-frequency induction heating method, and input is controlled so that the surface temperature of the base material is 800°C or higher and 1100°C or lower by the high-frequency induction heating method and is a temperature higher than that of the nitriding / oxidizing process.