Method for preparing metal particle dispersion liquid
The described method improves dispersibility and achieves fine particle sizes in metal particle dispersions by heat-treating protective agents within specified molecular weight ranges and using specific agents, resulting in stable metal particle dispersions with reduced particle sizes.
Patent Information
- Application Number
- JP2023084873
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for preparing metal particle dispersions do not effectively improve dispersibility and achieve fine particle sizes, with the suitability of protective agents for these properties being unclear.
A method involving the preparation of a metal particle dispersion by heat-treating a protective agent with an average molecular weight between 5,000 and 32,500, mixing it with a metal ion-containing solution and a reducing agent, and performing a liquid phase reduction to disperse metal fine particles, with specific conditions for polyvinylpyrrolidone as the protective agent and triethanolamine as the reducing agent.
This method enhances dispersibility and reduces the average particle size of metal particles to 10 nm or less, preventing precipitation over extended periods.
Smart Images

Figure 2024168315000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for preparing a metal particle dispersion liquid. [Background technology]
[0002] Conventionally, as a method for preparing a metal particle dispersion, a liquid-phase reduction method is known in which a reduction reaction is carried out in a solution containing metal ions, and the resulting metal fine particles are coated with a protective agent. Patent Document 1 discloses that an organic polymer compound such as a carbon chain compound or a carbocyclic compound is used as the protective agent. Patent Document 2 discloses that polyvinylpyrrolidone, a copolymer containing vinylpyrrolidone, polyoxyethylene, etc. are used as a water-soluble polymer suspension stabilizer (protective agent). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-220435 A [Patent Document 2] Patent Publication No. 2021-073379 Summary of the Invention [Problem to be solved by the invention]
[0004] In the metal particle dispersion, there is a demand for improved dispersibility and finer metal particles. On the other hand, there are a wide variety of organic polymer compounds that can be used as the protective agent, and it is not clear which protective agent is suitable for improving the dispersibility and finer metal particles.
[0005] The present invention has been made in consideration of the above problems, and has an object to realize improved dispersibility and finer metal particles in a metal particle dispersion liquid. [Means for solving the problem]
[0006] A first aspect of the present invention is a method for preparing a metal particle dispersion liquid, comprising the steps of: a) preparing an ion-containing solution containing metal ions; b) subjecting a protective agent having an average molecular weight of 5,000 or more and 32,500 or less to a heat treatment; and c) mixing the ion-containing solution, a reducing agent, and the protective agent heated in step b) to prepare a metal particle dispersion liquid in which metal microparticles are dispersed in a liquid by a liquid-phase reduction method.
[0007] A second aspect of the present invention is the method for preparing a metal particle dispersion liquid according to the first aspect, wherein the metal particles are silver particles.
[0008] A third aspect of the present invention is the method for preparing a metal particle dispersion liquid according to the second aspect, wherein the protective agent is polyvinylpyrrolidone.
[0009] A fourth aspect of the present invention is the method for preparing a metal particle dispersion liquid according to the third aspect, wherein the K value of the protective agent is 12.0 or more and 27.0 or less.
[0010] A fifth aspect of the present invention is the method for preparing a metal particle dispersion liquid according to the second aspect, wherein the reducing agent is triethanolamine.
[0011] A sixth aspect of the present invention is the method for preparing a metal particle dispersion liquid according to any one of the first to fifth aspects, wherein the heating temperature in the heat treatment is 100°C or higher and 150°C or lower.
[0012] A seventh aspect of the present invention is a method for preparing a metal particle dispersion liquid of any one of Aspects 1 to 5 (or any one of Aspects 1 to 6), in which the average particle size of the metal microparticles in the metal particle dispersion liquid prepared in step c) is 10 nm or less. Effect of the Invention
[0013] The present invention can improve the dispersibility and reduce the size of metal particles in a metal particle dispersion liquid. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a diagram showing a flow of preparation of a metal particle dispersion liquid according to one embodiment. [Diagram 2] FIG. 2 is a diagram showing silver fine particles contained in a metal particle dispersion liquid of an example. [Diagram 3] FIG. 13 is a diagram showing silver fine particles contained in a metal particle dispersion liquid of a comparative example. [Figure 4] FIG. 2 is a diagram showing a molecular weight distribution curve. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Fig. 1 is a diagram showing a flow of preparation of a metal particle dispersion liquid according to one embodiment of the present invention. The metal particle dispersion liquid is a liquid in which metal fine particles are dispersed. The fine particles are nanoparticles with a particle size of less than 1 µm. The metal is, for example, any one of silver (Ag), gold (Au), copper (Cu), platinum (Pt), ruthenium (Ru), rhodium (Rh) and Ir (iridium), or a combination of two or more of them.
[0016] The metal particle dispersion liquid is supplied to, for example, a laser fragmentation in liquid (LFL) device, in which the metal particle dispersion liquid is irradiated with a laser, thereby further reducing the size of the metal microparticles in the metal particle dispersion liquid.
[0017] When preparing a metal particle dispersion liquid, first, a solution containing metal ions (hereinafter also referred to as a "metal ion-containing solution") is prepared (step S11). In step S11, for example, a powdered metal salt is added to a solvent and stirred to prepare a metal ion-containing solution. As the metal salt, for example, nitrate, sulfate, acetate, or chloride can be used. As the solvent, for example, glycerin, ethanol, or isopropanol can be used. The temperature during stirring is, for example, 20°C to 60°C, and the stirring time is, for example, 1 hour to 3 hours. The concentration of the metal ions in the metal ion-containing solution is not particularly limited as long as it is in a range that can be dissolved in the solvent, but is, for example, 0.5% by mass to 6% by mass.
[0018] Next, the protective agent is subjected to a heat treatment (step S12). As the protective agent, an organic polymer compound can be used, and for example, polyvinylpyrrolidone (PVP), polyethylene glycol (PEG), polyvinyl alcohol (PVA), etc. are preferably used. The average molecular weight of the protective agent before the heat treatment in step S12 is 5000 or more, preferably 7000 or more, and more preferably 10000 or more. The average molecular weight is 32500 or less, preferably 30000 or less, and more preferably 24500 or less. The average molecular weight of the protective agent is determined by Gel Permeation Chromatography (GPC). The GPC method is also called Size Exclusion Chromatography (SEC).
[0019] When PVP is used as the protective agent, the K value of the PVP before the heat treatment in step S12 is, for example, 12.0 or more, and preferably 13.9 or more. The K value of the PVP before the heat treatment is, for example, 27.0 or less, and preferably 25.9 or less. The above-mentioned K value is a viscosity characteristic value that correlates with the molecular weight, and is determined by applying the relative viscosity value at 25°C measured by a capillary viscometer to the following Fikentscher formula (Formula 1). Note that η in Formula 1 rel indicates the relative viscosity of an aqueous solution of PVP to water, and c indicates the concentration (%) of the protecting agent in the aqueous solution of PVP.
[0020] K = (1.5logη rel -1) / (0.15+0.003c)+(300c·logη rel +(c+1.5c logη rel ) 2 ) 1 / 2 / (0.15c+0.003c 2 )...(Formula 1) The heating temperature of the protective agent in step S12 is, for example, 100° C. or higher, and preferably 120° C. or higher. The heating temperature is, for example, 150° C. or lower, and preferably 130° C. or lower. The heating time of the protective agent in step S12 is, for example, 10 hours or higher, and preferably 18 hours or higher. The heating time is, for example, 24 hours or lower, and preferably 20 hours or lower.
[0021] In step S12, the heated powdered protective agent is added to a solvent and stirred to prepare a solution containing the protective agent (hereinafter, also referred to as a "protective agent-containing solution"). As the solvent, for example, glycerin, ethanol, isopropanol, or the like can be used. The temperature during stirring is, for example, 20°C to 60°C, and the stirring time is, for example, 1 hour to 3 hours. The concentration of the protective agent in the protective agent-containing solution is not particularly limited as long as it is in a range in which the protective agent can be dissolved in the solvent, and is, for example, 10% by mass to 20% by mass. Step S12 may be performed in parallel with step S11, or may be performed before step S11.
[0022] When steps S11 to S12 are completed, the metal ion-containing solution, the protective agent-containing solution (i.e., a solution containing a heat-treated protective agent), and the reducing agent are mixed to prepare a mixed solution. As the reducing agent, for example, triethanolamine (TEA), monoethanolamine, diethanolamine, N,N-dimethylethanolamine, monopropanolamine, 2-amino-2-methyl-1-propanolamine, dipropanolamine, or tripropanolamine can be used. The reducing agent is, for example, mixed with the metal ion-containing solution and the protective agent-containing solution as a reducing agent-containing solution in which the reducing agent is dissolved in a solvent. As the solvent, for example, glycerin, ethanol, or isopropanol can be used.
[0023] Next, the mixed solution is stirred to reduce the metal ions in the mixed solution to generate metal fine particles, and the surfaces of the metal fine particles are coated with a protective agent. This suppresses aggregation and precipitation of the metal fine particles, and a metal particle dispersion solution in which the metal fine particles are dispersed in the liquid is prepared (step S13). That is, in step S13, the metal particle dispersion solution is prepared by a liquid phase reduction method. The temperature during stirring of the mixed solution is, for example, 40°C to 90°C, and the stirring time is, for example, 1 hour to 4 hours. The metal particle dispersion solution prepared in step S13 is cooled and / or diluted as necessary.
[0024] The average particle size of the metal particles contained in the metal particle dispersion is, for example, 10 nm or less, and preferably 5 nm or less. The lower limit of the average particle size is not particularly limited, but is, for example, 1 nm or more. The average particle size is determined by observing 300 or more metal particles in a field of view using an electron microscope, and calculating the arithmetic average of the particle sizes of 150 or more metal particles among them. In other words, the average particle size is the particle size of the metal particles whose surfaces are covered with a protective agent.
[0025] Next, examples and comparative examples of the metal particle dispersion liquid according to the present invention will be described with reference to Table 1 below. In Examples 1 to 6, the metal particle dispersion liquid was prepared by the method shown in steps S11 to S13 described above. In Comparative Examples 1 to 4, the metal particle dispersion liquid was prepared in steps S11 and S13 without performing step S12 described above. That is, in Comparative Examples 1 to 4, the protective agent was not subjected to a heat treatment, and in step S13, the non-heat-treated protective agent was mixed with the ion-containing solution and the reducing agent-containing solution.
[0026] [Table 1]
[0027] In Example 1, in step S11, powdered silver nitrate was added to glycerin and stirred to prepare a metal ion-containing solution. The temperature during stirring was 40° C., and the stirring time was 1 hour. The concentration of silver ions in the metal ion-containing solution was about 3 mass %.
[0028] In step S12, the powdered PVP was heated in a thermostatic bath to perform a heat treatment on the PVP. The heating temperature of the PVP in the heat treatment was 100°C, and the heating time was 24 hours. As the PVP, "PVP K15" manufactured by Tokyo Chemical Industry Co., Ltd. was used. The K value of the PVP before the heat treatment was 12.0 to 18.0 in the catalog value of Tokyo Chemical Industry Co., Ltd. The average molecular weight of the PVP before the heat treatment was 10,000.
[0029] The average molecular weight was measured by the GPC method as described above. In the measurement of the average molecular weight by the GPC method, "Shodex RI-71 (manufactured by Showa Denko K.K.)" was used as a detector, "Shodex OHpack SB-806M HQ×2 (manufactured by Showa Denko K.K.)" was used as a column, and "LC-10ADvp (manufactured by Shimadzu Corporation)" was used as a pump. In addition, polyethylene oxide and polyethylene glycol were used as standard polymers.
[0030] The above-mentioned protective agent-containing solution was prepared by adding the heat-treated PVP to glycerin and stirring the mixture. The temperature during stirring was 90° C., and the stirring time was 1 hour. The concentration of PVP in the protective agent-containing solution was about 20% by mass.
[0031] In step S13, triethanolamine (TEA) was used as a reducing agent. The temperature during stirring of the mixed solution in step S13 was 90° C., and the stirring time was 1 hour. In the metal particle dispersion liquid prepared in step S13, the particle size of the silver fine particles (so-called silver nanoparticles) was 5 nm to 20 nm, and the average particle size was 12.2 nm. The average particle size of the metal fine particles was determined by the same method as above. The electron microscope used to measure the average particle size was a spherical aberration corrected transmission electron microscope (JEM-2200FS manufactured by JEOL Ltd.). In addition, as a result of keeping the metal particle dispersion liquid stationary, precipitation occurred on the 7th day after preparation.
[0032] Example 2 is similar to Example 1, except that the heating temperature of PVP in step S12 was 110° C. In Example 2, the particle diameter of the silver particles in the metal particle dispersion was 5 nm to 20 nm, and the average particle diameter was 10.5 nm. In addition, as a result of keeping the metal particle dispersion in a stationary state, precipitation occurred on the 10th day after preparation.
[0033] Example 3 is similar to Example 1, except that the heating temperature of PVP in step S12 was 120° C. In Example 3, the particle diameter of the silver particles in the metal particle dispersion was 5 nm to 20 nm, and the average particle diameter was 9.2 nm. Furthermore, as a result of keeping the metal particle dispersion in a stationary state, no precipitation occurred even after 10 days or more had passed.
[0034] Example 4 is similar to Example 1, except that the heating temperature of PVP in step S12 was 125°C. In Example 4, the particle diameter of the silver microparticles in the metal particle dispersion was 5 nm to 15 nm, and the average particle diameter was 6.6 nm. FIG. 2 shows the silver microparticles contained in the metal particle dispersion of Example 4, observed with the spherical aberration corrected transmission electron microscope described above. The black, roughly circular dots in FIG. 2 are silver microparticles (the same applies to FIG. 3 described later). Furthermore, as a result of keeping the metal particle dispersion in a stationary state, no precipitation occurred even after 10 days or more had passed. Note that the metal particle dispersion of Example 4 was further observed, and no precipitation occurred even after 1 year or more had passed.
[0035] Example 5 is similar to Example 1, except that the heating temperature of PVP in step S12 was 130° C. In Example 5, the particle diameter of the silver particles in the metal particle dispersion was 5 nm to 15 nm, and the average particle diameter was 5.4 nm. Furthermore, as a result of keeping the metal particle dispersion in a stationary state, no precipitation occurred even after 10 days or more had passed.
[0036] Example 6 is the same as Example 4, except that "PVP K25" manufactured by Nacalai Tesque, Inc. was used as the PVP. In Example 6, the average molecular weight of the PVP in a non-heat-treated state was 24,500. The average molecular weight was measured by the GPC method in the same manner as in Example 1. The K value of the PVP before the heat treatment was 23.0 to 27.0 in the catalog value of Nacalai Tesque, Inc. In Example 6, the particle diameter of the silver fine particles in the metal particle dispersion was 5 nm to 20 nm, and the average particle diameter was 6.3 nm. Furthermore, as a result of keeping the metal particle dispersion in a stationary state, no precipitation occurred even after 10 days or more had passed.
[0037] Comparative Example 1 is similar to Example 1, except that the heat treatment of PVP in step S12 was not performed. In Comparative Example 1, the particle size of the silver microparticles in the metal particle dispersion was 10 nm to 80 nm, and the average particle size was 18.6 nm. In Comparative Example 1, the average particle size of the silver microparticles was clearly larger than those in Examples 1 to 5. Furthermore, as a result of keeping the metal particle dispersion in a stationary state, precipitation occurred on the third day after preparation. This shows that the metal particle dispersion of Comparative Example 1 has lower dispersibility of silver microparticles than the metal particle dispersions of Examples 1 to 5.
[0038] Comparative Example 2 is similar to Example 6, except that the heat treatment of PVP in step S12 was not performed. In Comparative Example 2, the particle diameter of the silver particles in the metal particle dispersion was 5 nm to 25 nm, and the average particle diameter was 13.0 nm. In Comparative Example 2, the average particle diameter of the silver particles was clearly larger than that of Example 6. Furthermore, as a result of keeping the metal particle dispersion in a stationary state, no precipitation occurred even after 10 days or more had passed.
[0039] Comparative Example 3 is similar to Comparative Example 1, except that "PVP K30" manufactured by Tokyo Chemical Industry Co., Ltd. was used as the PVP. In Comparative Example 3, the average molecular weight of the PVP in a non-heat-treated state was 40,000. The average molecular weight was measured by the GPC method in the same manner as in Example 1. The K value of the PVP before heat treatment is 26.0 to 34.0 according to the catalog value of Tokyo Chemical Industry Co., Ltd.
[0040] In Comparative Example 3, the particle diameter of the silver particles in the metal particle dispersion was 10 nm to 50 nm, and the average particle diameter was 19.2 nm. FIG. 3 shows the silver particles contained in the metal particle dispersion of Comparative Example 3, observed with the spherical aberration corrected transmission electron microscope described above. Comparing FIG. 2 with FIG. 3, it can be seen that the particle diameter of the silver particles in Example 4 shown in FIG. 2 is obviously smaller than that in Comparative Example 3 shown in FIG. 3. Furthermore, in Comparative Example 3, the metal particle dispersion was kept stationary, and as a result, no precipitation occurred even after 10 days or more had passed. Note that when the metal particle dispersion was prepared using "PVP K30" of Comparative Example 3 in the above steps S11 to S13, the average particle diameter of the silver particles was larger than that in Comparative Example 3.
[0041] Comparative Example 4 is similar to Comparative Example 1, except that "PVP K12" manufactured by ACROS was used as the PVP. In Comparative Example 4, the average molecular weight of the PVP in a non-heat-treated state was 3500. The average molecular weight was measured by the GPC method in the same manner as in Example 1. The K value of the PVP before the heat treatment was 10.2 to 13.8 according to the catalog value of ACROS. In Comparative Example 4, no silver particles were generated in step S13. Similarly, when the above-mentioned steps S11 to S13 were performed using "PVP K12" of Comparative Example 4, no silver particles were generated in step S13.
[0042] FIG. 4 shows differential molecular weight distribution curves obtained by the above-mentioned GPC method for the PVPs of Examples 2, 3, and 5 and Comparative Examples 1 and 3. For Examples 2, 3, and 5, the molecular weight distribution curves of the PVPs after the heat treatment in step S12 are shown. For Comparative Examples 1 and 3, the molecular weight distribution curves of the PVPs that were not subjected to the heat treatment are shown. In FIG. 4, the molecular weight distribution curves of Examples 2, 3, and 5 are denoted by reference characters 81, 82, and 83, respectively, and the molecular weight distribution curves of Comparative Examples 1 and 3 are denoted by reference characters 91 and 92, respectively.
[0043] As shown in FIG. 4, in Examples 2, 3, and 5 in which the heat treatment (step S12) was performed on the PVP, the peak top molecular weight at the top of the molecular weight distribution curve is larger than that of Comparative Example 1 in which the heat treatment was not performed on the PVP. For this reason, it is considered that the dispersibility of the silver fine particles in the metal particle dispersion liquids of Examples 2, 3, and 5 is higher than that of Comparative Example 1. In addition, the peak top molecular weights of Examples 3 and 5 are larger than that of Example 2. For this reason, it is considered that the dispersibility (no precipitation) of the silver fine particles in the metal particle dispersion liquids of Examples 3 and 5 is higher than that of Example 2 (precipitation on the 10th day after preparation). Furthermore, the peak top molecular weights of Examples 2, 3, and 5 are smaller than that of Comparative Example 3 in which the average molecular weight in a non-heat-treated state is 40,000. For this reason, it is considered that the average particle size of the silver fine particles in the metal particle dispersion liquids of Examples 2, 3, and 5 is smaller than that of Comparative Example 3.
[0044] As described above, the method for preparing a metal particle dispersion liquid includes a step of preparing an ion-containing solution containing metal ions (step S11), a step of performing a heat treatment on a protective agent having an average molecular weight of 5000 or more and 32500 or less (step S12), and a step of mixing the ion-containing solution, a reducing agent, and the protective agent heated in step S12 to prepare a metal particle dispersion liquid in which metal particles are dispersed in the liquid by a liquid phase reduction method (step S13). This makes it possible to improve the dispersibility and micronize the metal particles in the metal particle dispersion liquid. From the viewpoint of further improving the dispersibility and micronizing the metal particles in the metal particle dispersion liquid, the average molecular weight is preferably 7000 or more (more preferably 10000 or more) and preferably 30000 or less (more preferably 24500 or less).
[0045] The metal particles are preferably silver particles. According to the above-mentioned method for preparing a metal particle dispersion liquid, it is possible to prepare a metal particle dispersion liquid in which silver particles having a small average particle size are dispersed with high dispersibility.
[0046] The protective agent is preferably polyvinylpyrrolidone (PVP), which makes it possible to suitably prepare a metal particle dispersion liquid in which fine silver particles having a small average particle size are dispersed with high dispersibility.
[0047] The K value of the protective agent (PVP) is preferably 12.0 or more and 27.0 or less. This makes it possible to suitably prepare a metal particle dispersion liquid in which silver particles having a small average particle size are dispersed with high dispersibility. From the viewpoint of further improving the dispersibility and further miniaturizing the metal particles in the metal particle dispersion liquid, the K value is more preferably 13.9 or more and more preferably 25.9 or less.
[0048] The reducing agent is preferably triethanolamine, which makes it possible to suitably prepare a metal particle dispersion liquid in which fine silver particles having a small average particle size are dispersed with high dispersibility.
[0049] The heating temperature in the above-mentioned heat treatment (step S12) is preferably 100° C. or higher and 150° C. or lower. This can favorably improve the dispersibility and fineness of the metal microparticles in the metal particle dispersion. Furthermore, the heating temperature is more preferably 120° C. or higher and 130° C. or lower. This can favorably improve the dispersibility and fineness of the metal microparticles in the metal particle dispersion.
[0050] As described above, the average particle size of the metal particles in the metal particle dispersion liquid prepared in step S13 is preferably 10 nm or less, which makes it possible to provide a metal particle dispersion liquid in which metal particles with a very small average particle size are dispersed.
[0051] The above-mentioned method for preparing a metal particle dispersion liquid can be modified in various ways.
[0052] For example, the average particle size of the fine metal particles in the metal particle dispersion may be greater than 10 nm.
[0053] Moreover, the heating temperature of the protective agent in step S12 may be lower than 100°C or higher than 150°C.
[0054] The protecting agent and reducing agent are not limited to the above examples, and various agents may be used.
[0055] The method for preparing the metal ion-containing solution in step S11 is not limited to the above example and may be modified in various ways. The type of metal is also not limited to the above example and may be modified in various ways.
[0056] The configurations in the above-described embodiment and each of the modified examples may be combined as appropriate as long as they are not mutually inconsistent. [Explanation of symbols]
[0057] S11~S13 steps
Claims
1. A method for preparing a metal particle dispersion, comprising the steps of: a) providing an ion-containing solution comprising metal ions; b) subjecting a protective agent having an average molecular weight of 5,000 or more and 32,500 or less to a heat treatment; c) mixing the ion-containing solution, a reducing agent, and the protective agent heated in the b) step to prepare a metal particle dispersion liquid in which metal fine particles are dispersed in a liquid by a liquid phase reduction method; A method for preparing a metal particle dispersion liquid, comprising:
2. A method for preparing the metal particle dispersion liquid according to claim 1, comprising the steps of: The method for preparing a metal particle dispersion liquid, wherein the metal particles are silver particles.
3. A method for preparing the metal particle dispersion liquid according to claim 2, comprising the steps of: The method for preparing a metal particle dispersion liquid, wherein the protective agent is polyvinylpyrrolidone.
4. A method for preparing the metal particle dispersion liquid according to claim 3, comprising the steps of: The method for preparing a metal particle dispersion liquid, wherein the protective agent has a K value of 12.0 or more and 27.0 or less.
5. A method for preparing the metal particle dispersion liquid according to claim 2, comprising the steps of: The method for preparing a metal particle dispersion liquid, wherein the reducing agent is triethanolamine.
6. A method for preparing the metal particle dispersion liquid according to any one of claims 1 to 5, comprising the steps of: The method for preparing a metal particle dispersion liquid, wherein the heating temperature in the heat treatment is 100° C. or more and 150° C. or less.
7. A method for preparing the metal particle dispersion liquid according to any one of claims 1 to 5, comprising the steps of: The method for preparing a metal particle dispersion liquid, wherein the metal fine particles in the metal particle dispersion liquid prepared in the step c) have an average particle size of 10 nm or less.
Citation Information
Patent Citations
Metal colloidal solution
JP2005248204A
Conductive substrate, and precursor thereof and manufacturing method therefor
JP2010080438A
Method for producing core shell type metal nanoparticle
JP2010185135A
Aqueous silver colloidal liquid and production method of the same, and coating material using aqueous silver colloidal liquid
JP2015105372A
Preparation method for silver powder production using micro-nano bubbles as seed crystal inducer