Mesoporous silica-containing molding and method for manufacturing the same

The use of a hydroxide sol binder with six-coordinated Al ions and alkali/earth metal ions in molding mesoporous silica particles addresses the issue of maintaining pore size and structure, resulting in a strong, organic-free molded article with preserved enzyme activity for enzyme reactions.

JP2024168327AInactive Publication Date: 2024-12-05NATIONAL INSTITUTE OF ADVANCED INDUSTRIAL SCIENCE & TECHNOLOGY

Patent Information

Application Number
JP2023084892
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing mesoporous silica molded articles face challenges in maintaining uniform pore size and structure, especially when used as enzyme carriers, due to the use of organic compounds that can alter the pore characteristics and reduce the crushing strength, making them unsuitable for viscous solutions and enzyme reactions.

Method used

A method involving the use of a hydroxide sol binder containing six-coordinated Al ions, Si, and alkali or alkaline earth metal ions to mold mesoporous silica particles, ensuring the preservation of pore size and structure, with a composition that minimizes organic content, thereby enhancing the mechanical strength and enzyme activity.

Benefits of technology

The resulting mesoporous silica-containing molded article maintains the original pore diameter and structure, providing enhanced enzyme activity and ease of handling, while being suitable for enzyme reactions without organic compound elution, particularly in the food field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168327000001_ABST
    Figure 2024168327000001_ABST
Patent Text Reader

Abstract

To provide a mesoporous silica-containing molding substantially free of organic compounds, maintaining the pore size of raw material mesoporous silica particles, having silica sites as the most adsorption sites in the surface composition of the molding, and larger than the conventional molding having a size of 100 μm.SOLUTION: A mesoporous silica-containing molding contains mesoporous silica particles of 50 mass% or more and 83 mass% or less and an inorganic viscous component containing at least one of an alkali metal and an alkaline earth metal, Si, and Al and binding the mesoporous silica particles, contains substantially no organic compound, has a ratio of the amount of Al to the amount of Si that is greater than 0 and less than 0.2, has a sum of half the molar ratio of the alkaline earth metal to Al and the molar ratio of the alkali metal to Al that is greater than 0 and less than 1, and has a size of 0.17 mm or greater and 11 mm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to an inorganic molded article containing mesoporous silica and a method for producing the same. [Background technology]

[0002] Natural porous microparticles with regular micropores or regular mesopores, such as clay, zeolite, diatomaceous earth, and activated carbon, have been attracting attention for their properties such as adsorption, ion exchange, and catalytic activity for molecules or ions. When using porous microparticles as an adsorbent or carrier for a specific molecule, it is important that the size of the specific molecule matches the pore size of the porous microparticle. However, it is difficult to control the pore size and structure of natural porous microparticles. For this reason, porous microparticles with uniform pore sizes of any desired size cannot be obtained from untreated natural products.

[0003] In recent years, therefore, there has been vigorous research and development into mesoporous silica, metal organic frames (MOFs), mesoporous metal oxides, and other synthetic materials in which the pore size is controlled by using organic additives in the formation of a template or frame. Of these, mesoporous silica has regular pores with a pore size of 2 nm to 50 nm, which is larger than the pore size of zeolites. When an enzyme is supported on a support with a pore size close to the size of the enzyme, the effect of suppressing the denaturation and desorption of the enzyme is high (Non-Patent Document 1). Since the size of the enzyme is several nm to several tens of nm, mesoporous silica is suitable as an enzyme support.

[0004] Mesoporous silica is usually synthesized as particles with a diameter of 0.1 μm to 150 μm and a large specific surface area. In order to industrially utilize mesoporous silica as an enzyme carrier, etc., it is necessary to make it into a size that is easy to handle. Several attempts to granulate mesoporous silica have been reported. The present inventors have proposed a porous pellet and a hollow fiber membrane molded body that maintains the pore size of mesoporous silica by compounding mesoporous silica, which serves as an enzyme carrier, with an organic polymer, which serves as a binder (Patent Document 1). However, when mesoporous silica is used for enzyme reactions in the food industry, etc., mesoporous silica containing an organic compound is not preferable.

[0005] A method for producing an inorganic molded body that can be used in an aqueous solution is known in which an organic binder is mixed with unfired mesoporous silica powder containing an organic structure directing agent used in the synthesis of mesoporous silica, the mixture is molded, and then fired at 400°C or higher to remove the organic matter (Patent Document 2). However, the crushing strength of this inorganic molded body obtained after firing is only 0.3 kgf / cm. 2 ~2.1kgf / cm 2 (0.03N / mm 2 ~0.21N / mm 2 ), which is insufficient for use in viscous solutions that require stirring. In addition, the pore structure of mesoporous silica is easily destroyed by sintering mesoporous silica powder. For this reason, the pore volume of the molded body obtained after sintering is smaller than the pore volume of the molded body before sintering.

[0006] When a mesoporous silica-containing compact is produced using only colloidal silica as a binder, instead of an organic polymer, the plasticity of the binder is low. Therefore, powder compression molding is essential to reduce the content of the binder in the mesoporous silica-containing compact. However, in powder compression molding, the spaces between the mesoporous silica particles become clogged, reducing the reactivity of the mesoporous silica-containing compact, or the mesoporous silica structure collapses, changing the pore size of the mesoporous silica (Non-Patent Document 2). In addition, when a mesoporous silica-containing compact is produced using alumina sol as a binder, the interface of the alumina particles also becomes an adsorption site (Non-Patent Document 1). If there is an enzyme immobilization site with properties different from the pores of the mesoporous silica to which the enzyme is to be immobilized, the activity of the immobilized enzyme decreases, which is not preferable. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 6990906 [Patent Document 2] International Publication No. 2014 / 112661 [Non-patent literature]

[0008] [Non-Patent Document 1] N. Nagai, et. al., J. Mater. Chem., 2012, 22, 3234. [Non-Patent Document 2] P. Topka et al., Chem. Eng. J., 2010, 168, 433. Summary of the Invention [Problem to be solved by the invention]

[0009] The present application has been made in consideration of these circumstances, and has as its objective the provision of a mesoporous silica-containing molded body that is substantially free of organic compounds, maintains the pore size of the raw material mesoporous silica particles, has a majority of the adsorption sites in its surface composition being silica moieties, and is larger than the 100 μm size of conventional molded bodies. [Means for solving the problem]

[0010] The present inventors have found that when mesoporous silica particles are molded using a hydroxide sol containing hexacoordinated Al ions, Si, and Na as a binder, a molded body having a size of 100-100 mm can be obtained. The present inventors also considered that in order to produce a molded body that maintains the pore structure of the raw material mesoporous silica particles, in addition to the progression of Si-O-Si or Si-O-Al crosslinking in the hydroxide sol and between the hydroxide sol and the surface of the mesoporous silica particles, non-bridging oxygen that relieves distortion of the molded body is also necessary around the crosslinked sites.

[0011] The inventors of the present application discovered that by molding mesoporous silica particles in the presence of alkali metal ions or alkaline earth metal ions using a hydroxide sol containing Si and 6-coordinated Al ions as a binder, oxygen partially crosslinks between the hydroxides in the molded body and at the binding sites between the mesoporous silica and the hydroxide. The obtained molded body has improved strength compared to a molded body using colloidal silica as a binder.

[0012] The pore size of the obtained molded body was within ±0.6 nm of the pore size of the raw material mesoporous silica particles. The pore size of the molded body and mesoporous silica particles is the mode on the mesopore (2 nm to 50 nm) size distribution curve (hereinafter, sometimes simply referred to as the "mode of mesopore size distribution") obtained by calculating the nitrogen adsorption measurement data by the Barrett-Joyner-Halenda (BJH) method. Furthermore, the obtained molded body showed good pore characteristics, with the kurtosis of this mesopore size distribution curve (hereinafter, sometimes simply referred to as the "kurtosis of mesopore size distribution" or "kurtosis of pore size") being 0.5 or more, with the normal distribution being 0. Based on these findings, the inventors of the present application further conducted research and completed the present invention.

[0013] The mesoporous silica-containing molded body of the present application contains 50% by mass or more and 83% by mass or less of mesoporous silica particles, and an inorganic binding component that contains at least one of an alkali metal and an alkaline earth metal, Si, and Al and binds the mesoporous silica particles, is substantially free of organic compounds, has a ratio of the amount of Al to the amount of Si that is greater than 0 and less than 0.2, has a sum of 1 / 2 the ratio of the amount of alkaline earth metal to the amount of Al and the ratio of the amount of alkali metal to the amount of Al that is greater than 0 and less than 1, and is 0.17 mm or more and 11 mm or less in size.

[0014] The method for producing a mesoporous silica-containing molded body of the present application includes a molding step of mixing and molding a hydroxide sol binder that is substantially free of organic compounds, contains hexacoordinated Al ions, amorphous silica, and at least one of an alkali metal and an alkaline earth metal, in which the ratio of the substance amount of Al ions to the substance amount of Si in the amorphous silica is 0.07 or more and 0.2 or less, and has a pH of 3 or more and 8 or less, with mesoporous silica particles, and then heating the mixture at 120°C or more and 200°C or less to obtain a molded article, and a washing step of washing the molded article in a liquid to obtain a molded body.

[0015] The hydroxide sol binder of the present application is a hydroxide sol binder for forming mesoporous silica particles, which is substantially free of organic compounds, contains hexacoordinated Al ions, amorphous silica, and at least one of an alkali metal and an alkaline earth metal, and has a viscosity of 50 mPa s or less.

[0016] The method for producing a hydroxide sol binder of the present application is a method for producing a hydroxide sol binder for forming mesoporous silica particles, and includes a first mixing step of obtaining a Si-Al composite hydroxide sol by adding amorphous silica to an aqueous solution that is substantially free of organic compounds and contains 6-coordinated Al ions at 25° C. at 70 mol % or more of all Al ions, so that the ratio of the substance amount of all Al ions to the substance amount of Si in the amorphous silica is 0.07 to 0.2, and a second mixing step of obtaining a hydroxide sol binder by adding an alkali metal hydroxide solution to the Si-Al composite hydroxide sol so that the pH is 3 to 8. Effect of the Invention

[0017] The mode of the mesopore size distribution of the mesoporous silica-containing molded body of the present application does not change much from the mode of the mesopore size distribution of the raw mesoporous silica particles. Therefore, for example, if the mesoporous silica-containing molded body of the present application is used as an enzyme carrier, the same enzyme activity as when the raw mesoporous silica particles are used as an enzyme carrier can be obtained. In addition, since the size of the mesoporous silica-containing molded body of the present application is 0.17 mm or more and 11 mm or less, solid-liquid separation is easier than mesoporous silica particles with a size of about 100 μm. Therefore, for example, if the mesoporous silica-containing molded body of the present application is used as an enzyme carrier, the handling of the enzyme reaction is excellent. Furthermore, the mesoporous silica-containing molded body of the present application does not substantially contain organic compounds. Therefore, for example, even if the mesoporous silica-containing molded body of the present application is used as an enzyme carrier in the food industry, the elution of organic compounds, which are harmful components, is suppressed. [Brief description of the drawings]

[0018] [Figure 1](a) An image of the molded body 1 taken from above, and (b) an image of the molded body 1 taken from the side. [Diagram 2] SEM images of the surface of compact 1 at different magnifications. [Diagram 3] 11 shows external images of molded bodies 2 of various sizes. [Figure 4] 1 shows powder X-ray diffraction charts of compact 1, compact 6, compact 7, compact 8, and compact 11. [Diagram 5] Powder X-ray diffraction charts of compact 2, compact 3, compact 4, compact 5, compact 9, compact 10, and compact 12. [Figure 6] 27Al NMR spectrum of compact 2. [Figure 7] 27Al NMR spectrum of compact 13. [Figure 8] 27Al NMR spectrum of compact 14. [Figure 9] Pore ​​size distribution curves of compact 1, compact 6, and compact 11. [Figure 10] Pore ​​size distribution curves of compact 2, compact 4, compact 5, compact 10, and compact 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The mesoporous silica-containing compact of the embodiment of the present application contains mesoporous silica particles and an inorganic binder component. The content of mesoporous silica particles in the mesoporous silica-containing compact is preferably 50% by mass or more and 83% by mass or less. This is because the mesoporous silica particles can exist as a compact having a size of 0.17 mm to 11 mm while suppressing the deterioration of their functions. The walls of the mesopores of the mesoporous silica particles are amorphous silica. The arrangement of the mesopores of the mesoporous silica particles has an ordered structure. There are several known types of this ordered structure and pore size. As the mesoporous silica particles, MCM41, MCM48, FSM, SBA, etc. can be mentioned according to the ordered structure and pore size.

[0020] The mesoporous silica particles of this embodiment may be composed of a plurality of kinds of mesoporous silica particles. The mesoporous silica particles may contain impurities such as Al, Mg, or Fe in an amount of 10 mass% or less. The pore size of the mesoporous silica particles is not particularly limited, but is preferably 2 nm to 10 nm, more preferably 2 nm to 8 nm, from the viewpoint of immobilizing an enzyme on the mesoporous silica-containing molded body. In this embodiment, mesoporous silica particles are used in which the surfactant used during synthesis is hardly left after baking or washing.

[0021] The particle size of the mesoporous silica particles is preferably 0.1 μm to 100 μm, more preferably 0.1 μm to 50 μm. The particle size of the mesoporous silica particles is the mode value on the particle size distribution curve of the mesoporous silica particles measured by dispersing the mesoporous silica particles in an aqueous solution by applying ultrasonic waves or the like and observing the mesoporous silica particles by dynamic light scattering or electron microscope observation. The mass of the mesoporous silica particles is 50% or more and 83% or less of the mass of the mesoporous silica-containing molded body. This is because the mesoporous silica particles can be used as a molded body with excellent handleability while maintaining the properties of the raw material mesoporous silica particles.

[0022] The inorganic binder component binds the mesoporous silica particles. The inorganic binder component contains at least one of an alkali metal and an alkaline earth metal, Si, and Al. Si is contained in the inorganic binder component as a component having a Si-OH structure, such as fumed silica or colloidal silica sol. Al is contained in the inorganic binder component as a component having a 6-coordinate Al-OH structure. When the inorganic binder component containing at least one of an alkali metal and an alkaline earth metal is heated, Si-O-Al crosslinking proceeds while non-bridging oxygen is generated in the inorganic binder component.

[0023] Due to the cross-linking of Si-O-Al and the presence of non-cross-linked oxygen in the inorganic binder component, the inorganic binder component can bind mesoporous silica particles while maintaining the pore structure of the mesoporous silica particles. Note that alkali metals and alkaline earth metals are not contained in the inorganic binder component as simple substances, but are contained in the inorganic binder component as stable ions. Similarly, in the hydroxide sol binder described later, alkali metals and alkaline earth metals are not contained as simple substances but are contained as ions.

[0024] The mesoporous silica-containing molded body substantially does not contain organic compounds. In the present application, when a solid or solid substance substantially does not contain organic compounds, it means that the content of organic compounds is less than 0.1% by mass in thermal analysis (TG-DTA), or that it does not contain organic compounds other than inevitable impurities. Also, in the present application, when a liquid substantially does not contain organic compounds, it means that it does not contain organic compounds other than inevitable impurities. The ratio of the amount of substance of Al (hereinafter sometimes simply referred to as "Al / Si") in the mesoporous silica-containing molded body to the amount of substance of Si (so-called molar amount) in the mesoporous silica-containing molded body (amount of substance of Al in mesoporous silica-containing molded body / amount of substance of Si in mesoporous silica-containing molded body. The same applies to other elements and compounds)) is greater than 0 and less than 0.2.

[0025] The mesoporous silica-containing molded body with 0 < Al / Si < 0.2 corresponds to a high-silica zeolite with SiO2 / Al2O3 > 10 (Si / Al > 5). The mesoporous silica-containing molded body corresponding to this high-silica zeolite is difficult to crystallize and is stable in an amorphous state, having properties similar to those of mesoporous silica particles. On the other hand, if Al / Si is too large, the ratio of the inorganic binder component containing Al in the mesoporous silica-containing molded body increases, and the properties derived from the mesoporous silica particles of the mesoporous silica-containing molded body deteriorate. That is, the properties of the mesoporous silica-containing molded body, such as hydrophilicity / hydrophobicity, interaction with the reaction solution, and chemical resistance, are affected by the properties of the inorganic binder component containing Al.

[0026] As a result, there is a risk that the mesoporous silica-containing molded body cannot be used in the same applications as the mesoporous silica particles. Therefore, in order to maintain the properties derived from the mesoporous silica particles in the mesoporous silica-containing molded body, it is preferable to reduce Al / Si and make the inorganic binder component have an amorphous structure. It is preferable that Al / Si is greater than 0 and less than 0.1. In addition, the ratio of alkaline earth metal (hereinafter referred to as "M") to the amount of Al in the mesoporous silica-containing molded body is preferably 0.01 to 0.05. AE ") to the amount of Al in the mesoporous silica-containing compact. A ") (M AE / (Al×2)+M A / Al) is greater than 0 and less than 1.

[0027] The alkali metal and alkaline earth metal cations remaining in the mesoporous silica-containing molded body are firmly adsorbed to the mesoporous silica-containing molded body so as to compensate for the charge generated in the inorganic binder component. AE / (Al×2)+M A When / Al is 1 or more, most of the Al contained in the inorganic binder component is present in a 4-coordinated manner in the -Si-O-Si- or -Si-O-Al- network that constitutes the inorganic binder component in order to compensate for the excess charge.

[0028] In this way, when the cations of alkali metals and alkaline earth metals compensate for the negative charge generated by Al, the 4-fold coordination state of Al is stabilized, and the -Si-O-Si- or -Si-O-Al- network at the binding sites between hydroxides in the mesoporous silica-containing compact and between mesoporous silica and hydroxides becomes more ordered and loses elasticity. As a result, it becomes difficult to eliminate the distortion between the inorganic binding component and mesoporous silica particles, making the mesoporous silica-containing compact more susceptible to cracking.

[0029] On the other hand, M AE / (Al×2)+M AWhen / Al is 0, that is, when the mesoporous silica-containing shaped body does not contain an alkali metal or an alkaline earth metal, hydroxides or oxides of Al are present outside the -Si-O-Si- network as defects in the mesoporous silica-containing shaped body. This is thought to result in insufficient strength of the bonding sites between hydroxides in the mesoporous silica-containing shaped body, or between mesoporous silica and hydroxides, and insufficient water resistance of the mesoporous silica-containing shaped body. As a result, it is not possible to obtain a mesoporous silica-containing shaped body having a practical strength. (M AE / (Al×2)+M A / Al) is preferably greater than 0 and smaller than 0.3.

[0030] The pore size of the mesoporous silica-containing compact of this embodiment is preferably within ±0.6 nm of the pore size of the raw material mesoporous silica particles, i.e., the initial pore size of the mesoporous silica particles. As described above, the pore size of the mesoporous silica-containing compact and the mesoporous silica particles is the mode of the mesopore size distribution. In this application, the physical property values ​​such as the initial pore size of the mesoporous silica particles are the physical property values ​​such as the pore size of the mesoporous silica particles as the raw material of the mesoporous silica-containing compact, i.e., the physical property values ​​such as the pore size of the mesoporous silica particles before being mixed with the binder. Furthermore, the kurtosis of the mesopore size distribution of the mesoporous silica-containing compact of this embodiment is preferably 0.5 or more.

[0031] In this way, the mesoporous silica-containing molded body of this embodiment contains mesoporous silica particles that function as an enzyme carrier or adsorbent, etc., without significantly changing their pore characteristics, so that the mesoporous silica particles can maintain their function as an enzyme carrier, etc., and their selective adsorption, etc. It is more preferable that the difference between the pore size of the mesoporous silica-containing molded body of this embodiment and the initial pore size of the mesoporous silica particles is 0.5 nm or less.

[0032] A mesoporous silica-containing compact having a pore size smaller than the initial pore size of the mesoporous silica particles is considered to have at least some of the pores of the mesoporous silica particles constituting the mesoporous silica-containing compact collapsed. The collapse of the pores of the mesoporous silica particles in the mesoporous silica-containing compact can be determined from the change in the initial specific surface area of ​​the mesoporous silica particles and the specific surface area of ​​the mesoporous silica-containing compact. For example, if the content of mesoporous silica particles in the mesoporous silica-containing compact is 50% by mass and 70% or more of the initial specific surface area of ​​the mesoporous silica particles can be maintained even after compaction, the specific surface area of ​​the mesoporous silica-containing compact is 35% or more of the initial specific surface area of ​​the mesoporous silica particles.

[0033] Thus, the ratio of the specific surface area of ​​the mesoporous silica-containing compact to the initial specific surface area of ​​the mesoporous silica particles (specific surface area of ​​the mesoporous silica-containing compact / initial specific surface area of ​​the mesoporous silica particles) is preferably 0.35 or more, more preferably 0.38 or more, and even more preferably 0.41 or more. The specific surface areas of the mesoporous silica-containing compact and the mesoporous silica particles can be calculated from the nitrogen adsorption isotherm by the BJH method.

[0034] The size of the mesoporous silica-containing molded body of this embodiment is 0.17 mm to 11 mm, preferably 1 mm to 11 mm, and more preferably 2 mm to 11 mm. In this application, the size of the molded body means the diameter of a sphere with the smallest volume that contains the entire molded body, and may be expressed as the "outer diameter" of the molded body. In addition, the shape of the mesoporous silica-containing molded body of this embodiment is not particularly limited, but is preferably granular. Granular molded bodies with a size of 0.17 mm to 11 mm can be easily separated into solid and liquid by filtration using a commercially available relatively coarse filter. In addition, if the mesoporous silica-containing molded body has a size of 2 mm or more, it can be separated by pinching with tweezers or the like without filtration using a filter material.

[0035] The mesoporous silica-containing molded body of this embodiment contains mesoporous silica particles that function as an enzyme carrier or adsorbent, and the pore size is not significantly reduced from the initial pore size, and has a practical size of 0.17 mm to 11 mm, so that it can be used for enzyme reactions in aqueous solutions, for example. The crushing strength of the mesoporous silica-containing molded body of this embodiment is 0.29 N / mm so that it will not collapse even when used with tweezers or shaken in a liquid using a vortex mixer. 2 The crushing strength of the molded article is measured based on a crushing strength test according to JIS Z 8841. In addition, for application to enzyme reactions, the mesoporous silica-containing molded article of the present embodiment is preferably water resistant at pH 4 to pH 9 and 40° C.

[0036] An example of a raw material for the inorganic binder is a hydroxide sol binder. The hydroxide sol binder of the embodiment of the present application is a binder for forming mesoporous silica particles, and does not substantially contain an organic compound. The hydroxide sol binder of the embodiment contains six-coordinate Al ions, amorphous silica, and at least one of an alkali metal and an alkaline earth metal. The six-coordinate Al ions are, for example, aluminum chloride, aluminum nitrate, aluminum sulfate, or aluminum hydroxide dissolved in water [Al(OH2)6]. 3+ is Al ion.

[0037] When amorphous silica and at least one of an alkali metal compound and an alkaline earth metal compound are added to hexacoordinated Al ions in a solution, some of the Al-OH in the HO-Si-O-Si-OH network of the amorphous silica crosslink to form tetracoordinated Al. In this way, a crosslinking reaction progresses in the hydroxide sol binder, and hexacoordinated Al and more tetracoordinated Al than hexacoordinated Al are present, allowing mesoporous silica particles to be molded into large, high-strength particles. Note that the molding in this application also includes shaping using a mold, i.e., molding.

[0038] On the other hand, even if a binder is prepared by adding amorphous silica and at least one of an alkali metal and an alkaline earth metal to a solution in which all Al ions are present in a 4-coordinated manner, such as an aqueous solution of sodium aluminate, it is not possible to form large mesoporous silica particles with high strength. Aluminum chloride hexahydrate is an example of a raw material for obtaining an aqueous solution containing 6-coordinated Al ions. Since chloride ions are stable under low pH conditions, after a molded product, which is a precursor of a mesoporous silica-containing molded body, is produced using a binder containing at least one of an alkali metal and an alkaline earth metal, the excess chloride ions can be easily washed and removed as an alkali metal salt or an alkaline earth metal salt.

[0039] Furthermore, in consideration of the ease of handling when molding the mesoporous silica particles, it is preferable for the hydroxide sol binder to have a low viscosity. Specifically, the viscosity of the hydroxide sol binder is preferably 50 mPa·s or less, more preferably 25 mPa·s, and even more preferably 10 mPa·s. If the viscosity of the hydroxide sol binder is 50 mPa·s or less, molding is possible with a larger amount of mesoporous silica particles contained therein, and furthermore, gelation of the hydroxide sol binder can be prevented for several days at room temperature in a sealed state.

[0040] Depending on the composition ratio of each component of the hydroxide sol binder, the degree of oxygen crosslinking and the charge state of Al and Si are controlled, and the viscosity of the hydroxide sol binder changes. The reaction between the mesoporous silica particles and the hydroxide sol binder proceeds by dehydrating and condensing by heating to form Si-O-Si or Si-O-Al when the Si-OH structure and Al-OH structure in the amorphous silica in the hydroxide sol binder are entangled with the surface of the mesoporous silica particles. If the water content in the hydroxide sol binder is increased in an attempt to reduce the viscosity of the hydroxide sol binder, the progress of this dehydrating and condensing, i.e., the reaction between the mesoporous silica particles and the hydroxide sol binder, does not proceed sufficiently, and the mesoporous silica particles aggregate. In order to suppress the aggregation of the mesoporous silica particles in the hydroxide sol binder, the H2O / Si in the hydroxide sol binder is preferably greater than 9.5 and less than 30, and more preferably greater than 13 and less than 28.

[0041] The viscosity of the hydroxide sol binder also varies significantly depending on the ratio of the amount of Al to the amount of Si in the amorphous silica in the hydroxide sol binder, i.e., the Al / Si ratio in the hydroxide sol binder. In order to reduce the viscosity of the hydroxide sol binder, the Al / Si ratio is preferably 0.045 or more and 0.25 or less, and more preferably 0.07 or more and 0.2 or less.

[0042] The viscosity of the hydroxide sol binder also changes depending on the pH. In order that the hydroxide sol binder does not exhibit thixotropy and does not gel, the pH of the hydroxide sol binder is preferably 3 or more and 8 or less, and more preferably 6 or more and 7 or less. In addition, at least one of the alkali metal and the alkaline earth metal in the hydroxide sol binder is preferably Na. In this case, the ratio of the substance amount of Na to the substance amount of Al ions (Na / Al in the hydroxide sol binder) is preferably greater than 0.6 and less than 2.

[0043] The method for producing a hydroxide sol binder according to the embodiment of the present application is a method for producing a hydroxide sol binder for forming mesoporous silica particles. The method for producing a hydroxide sol binder according to the embodiment includes a first mixing step and a second mixing step. In the first mixing step, amorphous silica is added to a specific aqueous solution that is substantially free of organic compounds and contains hexacoordinated Al ions such that the ratio of the substance amount of all Al ions to the substance amount of Si in the amorphous silica is 0.07 to 0.2, thereby obtaining a Si-Al composite hydroxide sol. This specific aqueous solution is an aqueous solution that contains hexacoordinated Al ions at 70 mol % or more of all Al ions at 25°C.

[0044] In the second mixing step, an alkali metal hydroxide solution is added to the Si-Al composite hydroxide sol so that the pH is 3 to 8, thereby obtaining a hydroxide sol binder. This alkali metal hydroxide solution does not substantially contain organic compounds. In this way, a hydroxide sol binder that is substantially free of organic compounds and has an appropriate viscosity is obtained. In at least one of the first and second mixing steps, the liquid may be stirred as necessary.

[0045] The method for producing a mesoporous silica-containing molded body according to the embodiment of the present application includes a molding step and a washing step. In the molding step, a hydroxide sol binder and mesoporous silica particles are mixed and molded, and then heated to obtain a molded product. In order to efficiently promote the generation of non-bridging oxygen and the crosslinking of Si-O-Al in the hydroxide sol binder, the heating temperature is preferably 120°C or more and 200°C or less. The ratio of the mass of the hydroxide sol binder to the mass of the mesoporous silica particles (mass of hydroxide sol binder / mass of mesoporous silica particles) is preferably 2 to 8, more preferably 4 to 6, in order to suppress a decrease in the pore size of the mesoporous silica particles and in consideration of the moldability of the mesoporous silica particles.

[0046] This hydroxide sol binder is substantially free of organic compounds, contains 6-coordinate Al ions, amorphous silica, and at least one of an alkali metal and an alkaline earth metal, has a ratio of the amount of substance of Al to the amount of substance of Si in the amorphous silica (Al / Si in the hydroxide sol binder) of 0.07 to 0.2, and has a pH of 3 to 8. It is preferable that at least one of the alkali metal and the alkaline earth metal in the hydroxide sol binder is Na. In this case, it is preferable that the ratio of the amount of substance of Na to the amount of substance of Al ions (Na / Al in the hydroxide sol binder) is greater than 0.6 and less than 2.

[0047] In the washing step, the molded product is washed in a liquid, for example, in water, to obtain a molded body. In order to remove the liquid from the molded product after washing, it is preferable to dry the molded product. This drying is preferably performed at a temperature and for a time that allows the liquid to be removed from the molded product. By washing the molded product, impurities can be removed. The molded product may be fired after the washing step. The firing temperature and firing time at this time are, for example, a firing temperature of about 200°C and a firing time of several hours to 24 hours, or a firing temperature of about 300°C to about 500°C and a firing time of 4 hours to 5 hours. Even if the molded product is fired, the caking sites in the molded product remain amorphous, and the pore size of the molded product before and after firing is almost unchanged. EXAMPLES

[0048] The mesoporous silica content (mass%) in the molded body was calculated by the formula: mass of raw mesoporous silica particles / (mass of raw mesoporous silica particles+mass of raw hydroxide sol binder excluding liquid components)×100. The pore volume and BET specific surface area (hereinafter "BET specific surface area" may be simply referred to as "specific surface area") of the molded body and its raw mesoporous silica (hereinafter collectively referred to as "porous body") were calculated by nitrogen adsorption measurement. The pore size of the porous body was taken as the "mode of mesopore size distribution" described above unless otherwise specified. The nitrogen adsorption measurement of the molded body was performed after vacuum heating at 150° C. overnight.

[0049] The kurtosis of the pore size of the compact is the kurtosis of the mesopore size distribution curve calculated by the BJH method, and is set to 0 when the distribution is normal. The crushing strength of the compact was determined as the average value of three or more spherical samples with diameters of 4 mm to 5 mm, based on JIS Z 8841. Whether the compact was crystalline or amorphous was analyzed by powder X-ray diffractometer (PXRD). The Al / Si and Na / Al ratios (both are substance amount ratios (so-called molar ratios) (hereinafter the same)) in the compact and the total content (mass%) of Na and Cl in the compact were calculated from composition analysis by SEM-EDX.

[0050] Production Example 1: Preparation of Binder A In a PFA (perfluoroalkoxyalkane polymer) bottle, 4.83 g (0.02 mol) of aluminum chloride (III) hexahydrate (FUJIFILM Wako Pure Chemical Industries, Ltd., 016-01865, special grade reagent (same below)) was dissolved in 5.03 g of distilled water to obtain an aluminum chloride aqueous solution. 20.04 g (0.1 mol) of colloidal silica (JGC Catalysts and Chemicals, Ltd., Cataloid SI30 (same below)) with a concentration of 30% by mass was diluted with 20.3 g of distilled water to obtain diluted colloidal silica. 1.16 g (0.03 mol) of sodium hydroxide (FUJIFILM Corporation, 194-18865, special grade reagent (same below)) was dissolved in 10.06 g of distilled water to obtain a sodium hydroxide aqueous solution.

[0051] While stirring the aluminum chloride aqueous solution in the PFA bottle, the diluted colloidal silica was dropped into the PFA bottle to obtain a silica-alumina slurry. While stirring this silica-alumina slurry, the sodium hydroxide aqueous solution was dropped into the PFA bottle, and the mixture was stirred for another 1 to 2 hours to obtain binder A (molar ratio Na:Al:Si:Cl:H2O=1.5:1:5:3:140). The viscosity, pH, and density (at 21.5°C (same below unless otherwise specified)) of binder A were 6.4 mPa s, 5 to 6, and 1.101 g / cm, respectively. 3 It was.

[0052] Example 1: Production of Molded Body 1 Based on the literature (Y. Urabe et. al., ChemBioChem, 2007, 8, 668-674), we synthesized FSM22 type mesoporous silica powder (hereinafter, simply referred to as "FSM powder"). The pore volume, specific surface area, and pore diameter of this FSM powder were 3.14 cm, respectively. 3 / g, 1414.6m 2 / g, and 7.2 nm. 0.11 g of this FSM powder was placed in a PFA cup, 0.64 g of binder A was added, and kneaded to obtain a sol precursor. This sol precursor was molded into a sphere with a diameter of 2 to 3 mm, and then dried at 120°C for 16 hours on a PFA plate in air to obtain a molded product. This molded product corresponds to the precursor of the finished green body. The shape of this molded product was like a spheroid cut perpendicular to the axis of rotation with the bottom flattened (hereinafter sometimes referred to as a "kagami mochi shape").

[0053] The molded product was washed by stirring in distilled water at 40°C for about 4 hours to remove NaCl. It was then dried in air at 60°C to obtain molded body 1. Figure 1(a) shows an image of molded body 1 from above, and Figure 1(b) shows an image of molded body 1 from the side. Figures 2(a) and 2(b) show two SEM images of the surface of molded body 1 at different magnifications. The SEM image in Figure 2(b) is an enlarged view of the center of the SEM image in Figure 2(a). As shown in Figures 2(a) and 2(b), mesoporous silica particles with a diameter of about 3 μm are connected at the caking sites to form macropores.

[0054] Example 2: Production of Molded Body 2 Instead of 0.11 g of FSM powder, MCM41 type mesoporous silica powder (Sigma-Aldrich, No. 643645, pore volume 0.9634 cm 3 / g, specific surface area 1091.3m 2Molded body 2 was obtained in the same manner as in Example 1, except that 1.0 g of binder A (pore size (catalog value) 2.1 nm to 2.7 nm) was used, 4.0 g of binder A was used, and the molded product was obtained by molding the sol precursor and then drying for 24 hours. The Al / Si and Na / Al ratios of molded body 2 were greater than 0. An external image of molded body 2 having a kagami mochi shape is shown in FIG. 3. Molded body 2 could be molded into a variety of sizes from 0.17 mm to 11 mm.

[0055] Example 3: Production of Molded Body 3 Molded body 3 was obtained in the same manner as in Example 2, except that the sol precursor was molded and then dried at 200° C. for 4 hours to obtain a molded product. Molded body 3 had an Al / Si ratio of greater than 0.

[0056] Example 4: Production of Molded Body 4 Molded body 4 was obtained in the same manner as in Example 2, except that 0.3 g of the MCM41 type mesoporous silica powder and 0.6 g of the binder A were used. The Na / Al ratio of molded body 4 was greater than 0.

[0057] Example 5: Production of Molded Body 5 Molded body 4 was fired at 500° C. for 5 hours to obtain molded body 5.

[0058] Example 6: Production of Molded Body 6 Molded body 1 was fired at 500° C. for 5 hours to obtain molded body 6. The Na / Al ratio of molded body 6 was greater than 0.

[0059] Production Example 2: Preparation of Binder B An aqueous solution of sodium hydroxide was obtained by dissolving 0.49 g of sodium hydroxide in 0.79 g of distilled water. This aqueous solution of sodium hydroxide was added to 11.97 g of the silica-alumina slurry of Production Example 1 and stirred to obtain binder B (molar ratio of Na:Al:Si:Cl:H2O = 3.1:1:5:3:154). The viscosity, pH, and density of binder B were 49 mPa s, >12, and 1.11 g / cm, respectively. 3 It was.

[0060] Example 7: Production of Molded Body 7 A molded body 7 was obtained in the same manner as in Example 1, except that 0.05 g of FSM powder was used and 0.35 g of binder B was used instead of 0.64 g of binder A. The Al / Si and Na / Al ratios of molded body 7 were greater than 0.

[0061] Production Example 3: Preparation of Binder C In a PFA bottle, 2.41 g (0.01 mol) of aluminum chloride (III) hexahydrate was dissolved in 4.8 g of distilled water to obtain an aluminum chloride aqueous solution. 10.02 g (0.05 mol) of colloidal silica with a concentration of 30% by mass was diluted with 7.0 g of distilled water to obtain diluted colloidal silica. 0.24 g (0.006 mol) of sodium hydroxide was dissolved in 5.28 g of distilled water to obtain a sodium hydroxide aqueous solution. Thereafter, the same procedure as in Production Example 1 was followed to obtain binder C (molar ratio Na:Al:Si:Cl:H2O = 0.6:1:5:3:140). The viscosity, pH, and density at 21.2 °C of binder C were 22 mPa s, 3-5, and 1.101 g / cm, respectively. 3 It was.

[0062] Example 8: Production of Molded Body 8 Molded body 8 was obtained in the same manner as in Example 1, except that 0.65 g of binder C was used instead of 0.64 g of binder A, and the molded product was obtained by drying the sol precursor for 20 hours after molding. The Na / Al ratio of molded body 8 was greater than 0. The total content of Na and Cl in molded body 8 was less than 0.4 mass%.

[0063] Production Example 4: Preparation of Binder D Binder D (molar ratio: Na:Al:Si:Cl:H2O = 0.6:1:19:3:252) was obtained by mixing 10.02 g of binder C and 10.72 g of colloidal silica with a concentration of 30 mass%. The viscosity and density of binder D at 20°C were 4 mPa s and 1.17 g / cm, respectively. 3 It was.

[0064] Example 9: Production of Molded Body 9 A molded body 9 was obtained in the same manner as in Example 2, except that binder D was used instead of binder A. The Na / Al ratio of molded body 9 was greater than 0. The total content of Na and Cl in molded body 9 was less than 0.4 mass%.

[0065] Production Example 5: Preparation of Binder E In a PFA bottle, 1.5g (0.004mol) of aluminum nitrate nonahydrate (FUJIFILM Wako Pure Chemical Corporation, 010-11812) was dissolved in 5.0g of distilled water to obtain an aluminum nitrate aqueous solution. 0.24g (0.006mol) of sodium hydroxide was dissolved in 4.15g of distilled water to obtain a sodium hydroxide aqueous solution. While stirring the aluminum nitrate aqueous solution in the PFA bottle, 4.0g (0.02mol) of colloidal silica with a concentration of 30% by mass was dropped into the PFA bottle to obtain a silica-alumina slurry. While stirring this silica-alumina slurry, the above-mentioned sodium hydroxide aqueous solution was dropped into the PFA bottle, and the mixture was further stirred for 1 to 2 hours to obtain binder E (molar ratio Na:Al:Si:H2O=1.5:1:5:140).

[0066] Example 10: Production of molded body 10 A molded body 10 was obtained in the same manner as in Example 2, except that binder E was used instead of binder A. The Na / Al ratio of the molded body 10 was greater than 0. The total content of Na and Cl in the molded body 10 was less than 0.4 mass%.

[0067] Comparative Example 1: Production of Molded Body 11 Instead of binder A, binder F, colloidal silica with a concentration of 30 mass% (viscosity 6 mPa s, pH 10, density at 20.5 °C 1.2 g / cm 3 A molded body 11 was obtained in the same manner as in Example 1, except that the binder F was used. The binder F did not contain Al.

[0068] Comparative Example 2: Production of Molded Body 12 A molded body 12 was obtained in the same manner as in Example 2, except that binder F was used instead of binder A.

[0069] Production Example 6: Preparation of Binder G In a PFA bottle, 4.83 g of aluminum chloride (III) hexahydrate was dissolved in 8.0 g of distilled water to obtain an aluminum chloride aqueous solution. 20.04 g of colloidal silica with a concentration of 30 mass% was diluted with 22.01 g of distilled water to obtain diluted colloidal silica. While stirring the aluminum chloride aqueous solution in the PFA bottle, the diluted colloidal silica was dropped into the PFA bottle to obtain binder G (molar ratio Na:Al:Si:H2O = < 0.016:1:5:128). The viscosity, pH, and density at 20.5 °C of binder G were 18 mPa s, 3-5, and 1.11 g / cm, respectively. 3 It was.

[0070] Comparative Example 3: Production of Molded Body 13 An attempt was made to manufacture the molded body 13 in the same manner as in Example 1, except that 0.65 g of binder G was used instead of binder A. However, when the molded product was stirred in water at 40°C, it crumbled into powder, and no molded body was obtained. Although molded body 13 was not obtained, the attempt to manufacture molded body 13 was made, and so the obtained molded product will be referred to as "molded body 13" for convenience (the same applies to other comparative examples in which no molded body was obtained, but only a molded product was obtained).

[0071] Production Example 7: Preparation of Binder H 0.04g (0.001mol) of sodium hydroxide was dissolved in 4.7g of distilled water to obtain a sodium hydroxide aqueous solution. 2.2g (0.02mol) of sodium aluminate (Nacalai Tesque, Inc., 31136-35, purity approximately 74% (same below)) was added to this sodium hydroxide aqueous solution and stirred to dissolve. Furthermore, 20.02g (0.1mol) of colloidal silica with a concentration of 30% by mass and 30.1g of distilled water were added and stirred to obtain binder H (molar ratio Na:Al:Si:H2O=1.1:1:5:137). Binder H contains ionic Al with 4 coordinates, but does not contain 6 coordinates Al ions.

[0072] Comparative Example 4: Production of Molded Body 14 An attempt was made to manufacture a molded body 14 in the same manner as in Example 1, except that binder H was used instead of binder A, and that a molded product was obtained by molding the sol precursor and then drying it for 24 hours. However, when the molded product was stirred in water at 40°C, it crumbled into powder, and no molded product was obtained.

[0073] Production Example 8: Preparation of Binder I A sodium hydroxide solution was obtained by dissolving 1.16g (0.03mol) of sodium hydroxide in 3.5g of distilled water. A diluted colloidal silica was obtained by diluting 20g (Si 0.1mol) of colloidal silica with a concentration of 30% by mass with 22g of distilled water. 1.74g of sodium aluminate (Al 0.016mol) was added to the above sodium hydroxide solution and dissolved by stirring, and the above diluted colloidal silica was further added and stirred to obtain binder I (molar composition ratio Na:Al:Si:H2O=2.9:1:6.4:136). Binder I contains 4-coordinate Al ions but does not contain 6-coordinate Al ions.

[0074] Comparative Example 5: Production of Molded Body 15 An attempt was made to manufacture a molded body 15 in the same manner as in Example 2, except that binder I was used instead of binder A. However, when the molded product was stirred in water at 40°C, it crumbled into powder, and a molded body could not be obtained.

[0075] Comparative Example 6: Production of Molded Body 16 An attempt was made to manufacture a green body 16 in the same manner as in Example 2, except that binder J, an alumina sol having an Al2O3 equivalent concentration of 10 mass% (Kawaken Fine Chemical Co., Ltd., 10A, nitric acid-containing pseudoboehmite sol (hereinafter the same)), was used instead of binder A. However, when the green body was stirred in water at 40°C, it dispersed, and a green body could not be obtained. The catalog values ​​of the particle minor axis, pH, and viscosity of binder J were 10 nm, 3 to 4, and 50 mPa s, respectively. Binder J does not contain amorphous silica.

[0076] Comparative Example 7: Production of Molded Body 17 The sol precursor was molded and then dried to obtain a molded product in the same manner as in Comparative Example 6. This molded product was fired at 500° C. for 5 hours to obtain a molded body 17.

[0077] Production Example 9: Preparation of Binder K Binder J was diluted with distilled water to obtain an alumina sol with an Al2O3-equivalent concentration of 3 mass % to obtain binder K. Binder K does not contain amorphous silica.

[0078] Comparative Example 8: Production of Molded Body 18 A molded body 18 was obtained in the same manner as in Comparative Example 7, except that 0.37 g of binder K was used instead of binder J, and 20 mg of FSM22 type mesoporous silica powder was used instead of MCM41 type mesoporous silica powder. However, molded body 18 was too fragile to be picked up with tweezers.

[0079] Production Example 10: Preparation of Binder L A sodium hydroxide solution was obtained by dissolving 0.06g (0.0015mol) of sodium hydroxide in 0.98g of distilled water. 1g (0.001mol) of binder J and 1g (0.005mol) of colloidal silica with a concentration of 30% by mass were mixed uniformly. The above sodium hydroxide solution was added to this uniform mixture and mixed to obtain binder L (molar ratio Na:Al:Si:H2O=1.5:1:5:140). Binder L contains 4- and 6-coordinate Al. However, more than 87% of this Al is not ionic.

[0080] Comparative Example 11: Production of Molded Body 19 Molded body 19 was obtained in the same manner as in Example 2, except that binder L was used instead of binder A, and the molded product was obtained by molding the sol precursor and then drying it for 20 hours.

[0081] [Table 1]

[0082] Table 1 shows the mesoporous silica content, pore volume, specific surface area, specific surface area of ​​the molded body / specific surface area of ​​mesoporous silica particles (initial specific surface area), pore size, kurtosis of pore size, crushing strength, Al / Si, and Na / Al of the molded bodies 1 to 10 of the examples and the molded bodies 11 to 19 of the comparative examples. The "binder / mesoporous silica (mass ratio)" of the raw material is the ratio of the mass of the binder containing moisture to the mass of the mesoporous silica particles. "-" indicates that it was not measured or could not be measured. There was little difference between the pore size of the molded bodies 1 to 10 and the pore size of the mesoporous silica particles of each raw material. That is, it was found that the method for producing a mesoporous silica-containing molded body of the present application can obtain a mesoporous silica-containing molded body that maintains the pore size of the mesoporous silica particles.

[0083] Among the compacts of the comparative examples, compacts 16 to 19 using binder J, binder K, or binder L containing boehmite were difficult to mold when the amount of binder used was small. Moreover, unsintered compacts 16, 18, and 19 did not have water resistance. Furthermore, sintered compact 17 had a significantly high Al / Si ratio, suggesting that the properties of boehmite were strongly reflected in the compacts.

[0084] Powder X-ray diffraction charts of the molded body 1, molded body 6, molded body 7, and molded body 8 of the Examples using FSM22 type mesoporous silica, and the molded body 11 of the Comparative Example are shown in Figure 4. Powder X-ray diffraction charts of the molded body 2, molded body 3, molded body 4, molded body 5, molded body 9, and molded body 10 of the Examples using MCM41 type mesoporous silica, and the molded body 12 of the Comparative Example are shown in Figure 5. As shown in Figures 4 and 5, all of the molded bodies using binders A to F were amorphous.

[0085] Furthermore, in the molded body 2, molded body 3, molded body 4, molded body 5, and molded body 10 of the examples using MCM41 type mesoporous silica, a peak indicating a periodic structure derived from MCM41 ("MCM structure" in the figure) was observed near 2θ=4°. On the other hand, this peak was not observed in the molded body 12 of the comparative example using the same MCM41 type mesoporous silica. This suggests that in the molded body 12 using the binder F, the mesoporous silica comes off during the molding process, or that the mesopore structure of the mesoporous silica particles is easily crushed.

[0086] Molded body 2, molded body 13, and molded body 14 27 The Al NMR spectra are shown in Figures 6 to 8. As shown in Figure 6, in the molded body 2 produced using the binder A containing NaOH, crosslinking by dehydration condensation of silanol and AlOH partially proceeded, and as a result, the amount of 4-coordinated Al incorporated into the silica chain was greater than the amount of 6-coordinated Al. On the other hand, as shown in Figure 7, in the molded body 13 produced using the binder G, which has the same Al / Si as the binder A but does not contain NaOH, the amount of 6-coordinated Al was greater than the amount of 4-coordinated Al.

[0087] In addition, when the Al ions are 4-coordinated before use in molding, as in binder H and binder I, all of the Al ions in the obtained compact 14 are 4-coordinated, as shown in Figure 8. However, the compact 14 did not have sufficient strength and water resistance. From this, it is considered that the crosslinking caused by the dehydration condensation of silanol and AlOH during the molding process contributes to the increase in strength of the compact due to the crosslinking bond between the mesoporous silica surface and the binder. Further promoting this crosslinking to order leads to crystallization of the compact and deterioration of the mesoporous silica particles. For this reason, it is preferable to leave non-crosslinked parts at the binding site between the mesoporous silica and the binder to relieve the distortion of this binding site, as this improves the strength of the compact.

[0088] The pore size distribution curves of compacts 1, 6, and 11 are shown in Fig. 9, and the pore size distribution curves of compacts 2, 4, 5, 10, and 12 are shown in Fig. 10. As shown in Figs. 9 and 10, compacts 1, 2, 4, 5, and 6 produced using binder A, and compact 10 produced using binder E, had mesopore distribution curves with large kurtosis. On the other hand, in compacts 11 and 12 produced using binder F, which is colloidal silica, most of the mesopores of the raw material mesoporous silica particles were crushed.

[0089] Example 9: Enzyme activity evaluation Glucose dehydrogenase was immobilized on four types of carriers, FSM powder, compact 1, compact 6, and compact 11, and the enzyme activity of each was examined by the following procedure. 11 NO3·HCl, pH 8.0, 1M, Fujifilmwako, 314-90065) was diluted with distilled water to obtain a 0.1M diluted buffer solution. 1.4mg of glucose dehydrogenase (Fujifilmwako, 071-02411, 100U) was dissolved in 27mL of this diluted buffer solution to prepare a 0.05mg / mL enzyme solution.

[0090] Next, 3 mg of FSM powder or 7 mg to 9 mg of compact 1, compact 6, or compact 11 was added to 2 mL of this enzyme solution containing 0.1 mg of enzyme, and the mixture was shaken at 100 rpm at room temperature for 24 hours to adsorb and immobilize the enzyme on the FSM powder and each compact. Then, the mixture was centrifuged at 5000 rpm. The amount of enzyme immobilized on the four types of carriers was calculated from the difference between the amount of enzyme in the supernatant after this centrifugation and the amount of enzyme in the initial enzyme solution. The amount of enzyme in the supernatant was calculated based on the absorption peak at a wavelength of 280 nm in ultraviolet-visible absorption analysis. Next, these carriers on which the enzyme was immobilized were washed with water and dried to obtain enzyme-immobilized carriers.

[0091] On the other hand, 1 g of β-diphosphopyridine nucleotide (Fujifilm Wako, 049-16461) was dissolved in 25 mL of distilled water to obtain β-NAD at 0.06 mmol / mL (40 mg / mL). + An aqueous solution was prepared. + Mix 1 mL of the aqueous solution with 30 mL of the above diluted buffer solution, and add 139.7 mg of D(+)-glucose (Fujifilm Wako, 045-31162) to obtain a glucose concentration of 25 μmol / mL and β-NAD + A reaction solution with a concentration of 1.9 μmol / mL was obtained.

[0092] The activity of the immobilized enzyme based on the NADH production reaction shown below was evaluated by the following procedure. β-D-glucose + β-NAD + →D-glucono-δ-lactone + NADH + H + 1 mL of this reaction solution and 3 mL of the above dilution buffer solution were added to the above four types of enzyme immobilization carriers (immobilized enzyme amount 24 μg to 40 μg), and after shaking gently several times at room temperature, the reaction solution was allowed to stand, and the change in absorbance of NADH in the reaction solution at a wavelength of 340 nm was measured by ultraviolet-visible absorption spectrometry. The change in absorbance from the start of the reaction until 120 minutes later was taken as the enzyme activity, and the enzyme activity per unit mass of the enzyme immobilization carrier was compared. The enzyme activity per unit mass of the enzyme immobilization carrier in which the carrier is FSM powder was taken as 1.0. The results are shown in Table 2.

[0093] [Table 2]

[0094] As shown in Table 2, the molded bodies of the examples had higher enzyme immobilization amounts and enzyme activities than the molded bodies of the comparative examples. Furthermore, molded body 1, despite containing a binder, showed enzyme activity at the same level as that of FSM powder, which is mesoporous silica. [Industrial Applicability]

[0095] The mesoporous silica-containing shaped body of the present application is substantially free of organic compounds and can be used as an enzyme carrier for enzyme reactions in the food and pharmaceutical fields. In addition, the surface of the mesoporous silica-containing shaped body of the present application is more hydrophobic than the surface of boehmite. Therefore, when the mesoporous silica-containing shaped body of the present application is used as an enzyme carrier, inhibition of enzyme activity by hydrophilic polymers and amines is suppressed compared to when boehmite is used as an enzyme carrier.

Claims

1. The composition comprises 50% by mass or more and 83% by mass or less of mesoporous silica particles, and an inorganic binder component that contains at least one of an alkali metal and an alkaline earth metal, Si, and Al and that binds the mesoporous silica particles together, Contains substantially no organic compounds The ratio of the amount of substance of Al to the amount of substance of Si is greater than 0 and less than 0.2, the sum of 1 / 2 of the ratio of the amount of substance of the alkaline earth metal to the amount of substance of Al and the ratio of the amount of substance of the alkali metal to the amount of substance of Al is greater than 0 and less than 1; A mesoporous silica-containing molded body having a size of 0.17 mm or more and 11 mm or less.

2. In claim 1, A mesoporous silica-containing molded article, wherein the pore size is within ±0.6 nm of the initial pore size of the mesoporous silica particles, and the pore size kurtosis is 0.5 or more.

3. In claim 1 or 2, Crushing strength is 0.29N / mm 2 The mesoporous silica-containing molded article is as described above.

4. In claim 3, A mesoporous silica-containing molded article, in which the ratio of the specific surface area of ​​the mesoporous silica particles to the initial specific surface area is 0.35 or more.

5. a molding step of mixing and molding a hydroxide sol binder that is substantially free of organic compounds, contains hexacoordinated Al ions, amorphous silica, and at least one of an alkali metal and an alkaline earth metal, in which the ratio of the substance amount of the hexacoordinated Al ions to the substance amount of Si in the amorphous silica is 0.07 to 0.2, and has a pH of 3 to 8, with mesoporous silica particles, and then heating at 120° C. to 200° C. to obtain a molded product; a washing step of washing the molded product in a liquid to obtain a molded body; The present invention relates to a method for producing a mesoporous silica-containing molded body having the above structure.

6. In claim 5, At least one of the alkali metal and the alkaline earth metal is Na; A method for producing a mesoporous silica-containing molded body, wherein a ratio of the substance amount of the Na ions to the substance amount of the Al ions is greater than 0.6 and less than 2.

7. A hydroxide sol binder for forming mesoporous silica particles, comprising: Contains substantially no organic compounds The silica gel composition contains 6-coordinated Al ions, amorphous silica, and at least one of an alkali metal and an alkaline earth metal, A hydroxide sol binder having a viscosity of 50 mPa·s or less.

8. In claim 7, a ratio of the amount of substance of the Al ions to the amount of substance of Si in the amorphous silica is 0.07 or more and 0.2 or less; A hydroxide sol binder having a pH of 3 or more and 8 or less.

9. A method for producing a hydroxide sol binder for forming mesoporous silica particles, comprising the steps of: a first mixing step of adding amorphous silica to an aqueous solution substantially free of organic compounds and containing 6-coordinated Al ions at 25° C. in an amount of 70 mol % or more of all Al ions, so that the ratio of the substance amount of all Al ions to the substance amount of Si in the amorphous silica is 0.07 to 0.2, thereby obtaining a Si-Al composite hydroxide sol; a second mixing step of adding an alkali metal hydroxide solution to the Si-Al composite hydroxide sol so that the pH is 3 or more and 8 or less to obtain the hydroxide sol binder; A method for producing a hydroxide sol binder comprising the steps of:

Citation Information

Patent Citations

  • Porous molded body of mesoporous microparticles, enzyme-carrying carrier, enzyme complex thereof, and method for producing the same

    JP6990906B2

  • Pure granular mesoporous silica, and method for producing same using organic bonding agent

    WO2014112661A1

Cited By

  • Inorganic particle-dispersed organosol having high dispersion stability and method for producing same

    WO2026177193A1