Biaxially oriented polypropylene film

A biaxially oriented polypropylene film with controlled resin compositions and layer structures addresses the need for cost-effective, environmentally friendly, and high-performance packaging by enhancing heat sealability, rigidity, and antifogging properties, suitable for thinner films.

JP2024168337APending Publication Date: 2024-12-05TOYOBO CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023084907
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional polypropylene resin films used for packaging require a lamination process with organic solvents, which is costly and environmentally detrimental, and thinner films lack rigidity and processability, necessitating improvements in heat sealability, rigidity, and heat resistance.

Method used

A biaxially oriented polypropylene film composed of specific polypropylene resin compositions with controlled layer structures and forming conditions, ensuring high stress at elongation, low thermal shrinkage, and excellent heat seal strength, incorporating an antifogging agent for enhanced performance.

Benefits of technology

The film maintains bag shape and reduces thickness while providing excellent heat-sealing properties, high rigidity, and minimal wrinkles, suitable for high-rigidity applications without additional laminates, with improved antifogging properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168337000001
    Figure 2024168337000001
  • Figure 2024168337000002
    Figure 2024168337000002
Patent Text Reader

Abstract

To provide a biaxially oriented polypropylene film which is excellent in rigidity and heat resistance.SOLUTION: A biaxially oriented polypropylene film, which is composed of a polypropylene-based resin composition, satisfies the following (1) to (3). (1) A stress on the extension of 5% at 23°C in a longitudinal direction is 35 MPa or more, and the stress in a width direction is 130 MPa or more. (2) A thermal shrinkage rate at 120°C in a longitudinal direction is 2.0% or less, and the thermal shrinkage in a width direction is 1.5% or less. (3) Heat seal strength at 130°C is 4.0 N / 15 mm or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a biaxially oriented polypropylene film. [Background technology]

[0002] Conventionally, polypropylene-based resin films have been widely used as heat-sealable films for packaging. An example of a polypropylene-based resin film having heat-sealability is a laminated polypropylene-based resin film obtained by laminating a non-oriented polyethylene-based resin film or a non-oriented polypropylene-based resin film and an oriented polypropylene-based resin film. However, although the laminated polypropylene-based resin film has sufficient seal strength, it requires a lamination process using an organic solvent, etc., which is undesirable from the viewpoints of cost and impact on the global environment.

[0003] Another example of a polypropylene-based resin film having heat sealability is a laminated polypropylene-based resin film obtained by stretching a laminated sheet of a layer made of a polypropylene-based resin having a high melting point and a layer made of a polyolefin-based resin having a low melting point. For example, Patent Documents 1 and 2 disclose laminated polypropylene-based resin films having improved heat seal strength by laminating a base layer made of a polypropylene-based resin and a seal layer made of a polyolefin-based resin having a low melting point via an intermediate layer, as examples of such laminated polypropylene-based resin films. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2022 / 118680 [Patent Document 2] International Publication No. 2018 / 181011 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, there has been a demand for reducing the volume of packaging materials due to environmental considerations, and this has led to a demand for thinner films. However, making the film thinner reduces the rigidity that determines processability, so higher rigidity is required. There is also a demand for improved bag-making processability, and further improvements were necessary.

[0006] An object of the present invention is to provide a biaxially oriented polypropylene film having excellent heat sealability, rigidity and heat resistance. [Means for solving the problem]

[0007] As a result of extensive research to achieve the above object, the present invention has been able to solve the above problems by adjusting the composition of the polypropylene resin composition constituting the film and controlling the film-forming conditions. That is, the present invention includes the following inventions. [1] A biaxially oriented polypropylene film made of a polypropylene-based resin composition, which satisfies the following (1) to (3): (1) The stress at 5% elongation at 23°C is 35 MPa or more in the longitudinal direction and 130 MPa or more in the transverse direction. (2) The thermal shrinkage rate at 120°C is 2.0% or less in the longitudinal direction and 1.5% or less in the transverse direction. (3) Heat seal strength at 130°C is 4.0 N / 15 mm or more. [2] The biaxially oriented polypropylene film according to [1] above, wherein the haze of the biaxially oriented polypropylene film is 7.0% or less. [3] The biaxially oriented polypropylene film according to [1] or [2] above, wherein the biaxially oriented polypropylene film contains an anti-fogging agent in an amount of 0.2% by mass or more and 1.0% by mass or less. [4] The biaxially oriented polypropylene film according to any one of the above [1] to [3], wherein the thickness of the biaxially oriented polypropylene film is 10 μm or more and 50 μm or less. Effect of the Invention

[0008] The polypropylene film of the present invention has excellent rigidity and heat resistance, and therefore is easy to maintain the shape of a bag when made into a packaging bag. In addition, the polypropylene film of the present invention has excellent heat sealability, and therefore can be suitably used for applications requiring high rigidity without laminating a sealant film, and can maintain strength even when the film is thin. In addition, there are few wrinkles in the sealed portion when heat sealed, and the appearance is excellent when made into a bag shape. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The biaxially oriented polypropylene film of the present invention will be described below.

[0010] [Layer structure of biaxially oriented polypropylene film] The biaxially oriented polypropylene film of the present invention is made of a polypropylene-based resin composition. The layer structure of the biaxially oriented polypropylene film of the present invention is not particularly limited, but it is preferable that the biaxially oriented polypropylene film has a base layer A made of a polypropylene-based resin composition and a seal layer C made of a polypropylene-based resin composition, and has an intermediate layer B made of a polypropylene-based resin composition between the base layer A and the seal layer C. Furthermore, the biaxially oriented polypropylene film of the present invention may have a functional layer D. The base layer A, the intermediate layer B, the sealing layer C, and the functional layer D will be described in detail below.

[0011] [Base material layer A] The base layer A made of a polypropylene-based resin composition is preferably made of a polypropylene-based resin composition mainly composed of a polypropylene homopolymer. Here, the term "main component" means that 80% by mass or more of the entire base layer A is a polypropylene homopolymer, more preferably 90% by mass or more of the entire base layer A is a polypropylene homopolymer, even more preferably 95% by mass or more of the entire base layer A is a polypropylene homopolymer, particularly preferably 97% by mass or more of the entire base layer A is a polypropylene homopolymer, and most preferably 99% by mass or more of the entire base layer A is a polypropylene homopolymer.

[0012] (Polypropylene homopolymer) The polypropylene homopolymer used in the base layer A is a polypropylene polymer that does not substantially contain α-olefin components other than propylene, specifically, a polypropylene (co)polymer having 1 mol% or less of α-olefin components other than propylene and 99 mol% or more of propylene as structural units. Even when it contains α-olefin components other than propylene, the content of α-olefin components other than propylene (total amount of ethylene and α-olefins having 4 or more carbon atoms) is 1 mol% or less as described above, preferably 0.3 mol% or less, more preferably 0.2 mol% or less, and even more preferably 0.1 mol% or less. Within the above range, crystallinity is likely to be improved.

[0013] Examples of α-olefin components having 4 or more carbon atoms include 1-butene, 1-pentene, 3-methyl-1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 5-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, and 1-eicosene.

[0014] The polypropylene homopolymer may be two or more different polypropylene homopolymers, and in that case, the total content is preferably within the above range. The polypropylene homopolymer used in the base layer A includes not only polypropylene homopolymers that do not contain any α-olefin components other than propylene, but also polypropylene copolymers whose constituent units are 1 mol % or less of α-olefin components other than propylene and 99 mol % or more of propylene.

[0015] Various suitable physical properties of the polypropylene homopolymer are described below. When two or more different polypropylene homopolymers are used, the physical property values ​​are the mass average values ​​of the physical properties of each polypropylene homopolymer.

[0016] The polypropylene homopolymer used in the base layer A has a melting point of preferably 160°C or more and 170°C or less, more preferably 161°C or more and 169°C or less, even more preferably 162°C or more and 168°C or less, particularly preferably 162°C or more and 167°C or less, and most preferably 162°C or more and 166°C or less. If the melting point is 160°C or more, rigidity and heat resistance at high temperatures are easily obtained. If the melting point is 170°C or less, it is easy to suppress the increase in cost in polypropylene production, and it is difficult to break during film formation. The melting point can also be further increased by blending a crystal nucleating agent with the above-mentioned polypropylene resin. The melting point is the main endothermic peak temperature associated with melting, which is observed when 5 mg of polypropylene homopolymer is packed into an aluminum pan, set in a differential scanning calorimeter (DSC), heated from 30°C to 230°C at a heating rate of 20°C / min in a nitrogen atmosphere and held at 230°C for 5 minutes to melt the polypropylene homopolymer, then cooled to 30°C at a heating rate of -10°C / min and held at 30°C for 5 minutes, and then heated at a heating rate of 10°C / min.

[0017] The polypropylene homopolymer used in the base layer A preferably has a mesopentad fraction ([mmmm]%), which is an index of stereoregularity, of 97.0 to 99.9%, more preferably 97.5 to 99.7%, and even more preferably 98.0 to 99.5%. If it is 97.0% or more, the crystallinity of the polypropylene resin is increased, the melting point, crystallinity, and crystal orientation of the crystals in the base layer A are improved, and rigidity and heat resistance at high temperatures are easily obtained. If it is 99.9% or less, the cost of polypropylene production is easily reduced, and the film is less likely to break during film formation. The mesopentad fraction is measured by a nuclear magnetic resonance method (the so-called NMR method). In order to make the mesopentad fraction of the polypropylene homopolymer fall within the above-mentioned range, a method of washing the obtained polypropylene polymer powder with a solvent such as n-heptane, a method of appropriately selecting a catalyst and / or a cocatalyst, and a method of appropriately selecting components of the polypropylene resin composition are preferably adopted.

[0018] The melt flow rate (MFR) of the polypropylene homopolymer used in the base layer A, when measured in accordance with JIS K 7210 (1995), condition M (230°C, 2.16 kgf), is preferably 5.0 to 30 g / 10 min, more preferably 5.5 to 25 g / 10 min, even more preferably 6.0 to 22 g / 10 min, particularly preferably 6.3 to 20 g / 10 min, and most preferably 6.5 to 10 g / 10 min. When the MFR of the polypropylene resin is 5.0 g / 10 min or more, the polypropylene resin constituting the base layer A contains a large amount of low molecular weight components, and thus, by adopting a width direction stretching process in the film forming process described later, the oriented crystallization of the polypropylene resin is promoted, the crystallinity of the base layer A is easily increased, and the entanglement of the polypropylene molecular chains in the amorphous portion is reduced, so that the heat resistance is easily improved. Furthermore, when the MFR of the polypropylene resin is 30 g / 10 min or less, the film formability of the film is easily maintained. In order to set the MFR of the polypropylene homopolymer within the above range, it is preferable to adopt a method of controlling the molecular weight or molecular weight distribution of the polypropylene homopolymer.

[0019] The polypropylene homopolymer used in the base layer A has a lower limit of Mw / Mn, which is an index of molecular weight distribution, of preferably 3.5, more preferably 4.0, even more preferably 4.5, and particularly preferably 5.0. The upper limit of Mw / Mn is preferably 30, more preferably 25, even more preferably 23, particularly preferably 21, and most preferably 20. Mw / Mn can be obtained by gel permeation chromatography (GPC). When Mw / Mn is within the above range, it is easy to increase the amount of components having a molecular weight of 100,000 or less.

[0020] The molecular weight distribution of polypropylene polymers can be adjusted by polymerizing components of different molecular weights in a series of plants in multiple stages, blending components of different molecular weights offline in a kneader, polymerizing by blending catalysts with different performances, or using a catalyst that can achieve a desired molecular weight distribution. The shape of the molecular weight distribution obtained by GPC may be a gentle molecular weight distribution with a single peak in a GPC chart with the logarithm (logM) of molecular weight (M) on the horizontal axis and the differential distribution value (mass fraction per logM) on the vertical axis, or a molecular weight distribution with multiple peaks or shoulders.

[0021] In the GPC cumulative curve of the propylene-based resin composition constituting the base layer A, the amount of components having a molecular weight of 100,000 or less is preferably 38% by mass or more, more preferably 38 to 65% by mass, even more preferably 40 to 60% by mass, particularly preferably 41 to 55% by mass, and most preferably 42 to 50% by mass. By making the amount of components having a molecular weight of 100,000 or less 38% by mass or more, it is easy to improve heat resistance. When the amount of components having a molecular weight of 100,000 or less is 65% by mass or less, the film strength is not likely to decrease. In this case, if a high molecular weight component or a long chain branched component having a long relaxation time is contained, it is easy to adjust the amount of components having a molecular weight of 100,000 or less contained in the polypropylene resin without significantly changing the overall viscosity, so that it is easy to improve the film formability without affecting the rigidity and heat resistance.

[0022] (Anti-fogging agent) It is preferable that an anti-fog agent is contained in the polypropylene resin composition constituting the base layer A. The biaxially oriented polypropylene film of the present invention can be processed into a packaging bag for use, and in particular, when fruits and vegetables are placed in the packaging bag, the addition of an anti-fog agent can prevent fogging of the packaging bag, since the physiological functions of the fruits and vegetables are maintained even after harvest.

[0023] As the antifogging agent, for example, known antifogging agents such as ethylene oxide adducts of aliphatic amines, ethylene oxide adducts of aliphatic amides, esters of ethylene oxide adducts of aliphatic amines and fatty acids, fatty acid esters of polyhydric alcohols, fatty acid amines, fatty acid amides, etc. Among them, it is preferable to include at least one selected from the group consisting of ethylene oxide adducts of aliphatic amines and esters of ethylene oxide adducts of aliphatic amines and fatty acids, and it is more preferable to include ethylene oxide adducts of aliphatic amines and esters of ethylene oxide adducts of aliphatic amines and fatty acids. The ester of the ethylene oxide adduct of an aliphatic amine and a fatty acid preferably includes at least one selected from the group consisting of stearyl diethanolamine monoester and stearyl diethanolamine diester. In addition, since packaging bags are often stored at room temperature rather than frozen, in order to maintain excellent anti-fogging properties over the long term during distribution, it is preferable to use an anti-fogging agent that continues to exhibit anti-fogging properties during repeated temperature changes between 5°C and 30°C, taking into consideration changes in temperature during storage and distribution, but is not limited to the above preferred embodiment and may be appropriately selected depending on the application. The anti-fogging agent may be used alone or in combination of two or more types.

[0024] Examples of stearyl diethanolamine monoesters include stearyl diethanolamine monolaurate, stearyl diethanolamine monomyristate, stearyl diethanolamine monopalmitate, stearyl diethanolamine monostearate, and stearyl diethanolamine monooleate, and among these, stearyl diethanolamine monostearate is preferred. Examples of stearyl diethanolamine diesters include stearyl diethanolamine dilaurate, stearyl diethanolamine dimyristate, stearyl diethanolamine dipalmitate, stearyl diethanolamine distearate, and stearyl diethanolamine diolate, and among these, stearyl diethanolamine distearate is preferred. Examples of the ethylene oxide adduct of an aliphatic amine include lauryl diethanolamine, myristyl diethanolamine, palmityl diethanolamine, stearyl diethanolamine, etc., and stearyl diethanolamine is preferable. The ethylene oxide adduct of an aliphatic amine may be used alone or in combination of two or more kinds.

[0025] The amount of the antifogging agent present in the propylene-based resin composition constituting the base layer A is preferably 0.2 to 1.0 mass%, more preferably 0.3 to 0.8 mass%, and even more preferably 0.35 to 0.6 mass%. However, as described later, the antifogging agent may migrate from the base layer A to other layers such as the intermediate layer B during the film formation process.

[0026] (others) As long as the effects of the present invention are not impaired, the polypropylene-based resin composition constituting the base layer A may contain resins other than polypropylene homopolymers, and known additives such as heat stabilizers, antioxidants, UV absorbers, nucleating agents, adhesives, flame retardants, and inorganic or organic fillers. However, the amount of these additives is preferably small, and in the polypropylene resin composition constituting the base layer A, the amount of resins other than polypropylene homopolymers is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, particularly preferably 2% by mass or less, and most preferably 1% by mass or less. In addition, in the polypropylene resin composition constituting the base layer A, the amount of additives other than resins is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less. Examples of resins other than polypropylene homopolymer include polyolefin resins other than the polypropylene homopolymer used in the base layer A, various elastomers, etc. These may be sequentially polymerized using a multi-stage reactor, blended with polypropylene resin in a Henschel mixer, master pellets prepared in advance using a melt kneader may be diluted with polypropylene to a predetermined concentration, or the entire amount may be melt kneaded in advance for use. If the surface resistance value of the polypropylene homopolymer alone used in the base layer A is too high, a surfactant may be added to reduce the surface resistance value.

[0027] [Middle layer B] The intermediate layer B made of a polypropylene-based resin composition preferably has a polypropylene copolymer containing an α-olefin other than propylene. That is, the polypropylene-based resin composition constituting the intermediate layer B preferably has a polypropylene copolymer containing an α-olefin other than propylene. By providing the intermediate layer B, the heat seal strength can be improved. In addition, in the explanation of the intermediate layer B, even if it is simply described as "polypropylene copolymer (contained in the intermediate layer B)", it refers to a polypropylene copolymer containing an α-olefin other than propylene. The intermediate layer B preferably contains 70% by mass or more of the polypropylene copolymer, more preferably contains 80% by mass or more, further preferably contains 90% by mass or more, and particularly preferably contains 95% by mass or more. In addition, as the polypropylene copolymer contained in the intermediate layer B, two or more different polypropylene copolymers can be used, and the total content is preferably within the above range. By making the polypropylene copolymer 70% by mass or more, it is easy to increase the interlayer adhesion between the intermediate layer B and the seal layer C and the interlayer adhesion between the base layer A and the intermediate layer B, and the heat seal strength of the biaxially oriented polypropylene film can be further increased. The content of α-olefin components other than propylene in the polypropylene copolymer contained in the intermediate layer B (the total amount of ethylene and α-olefins having 4 or more carbon atoms) is preferably 4.0 mol % or more (a polypropylene copolymer having constituent units of 4.0 mol % or more of α-olefin components other than propylene and 96 mol % or less of propylene), more preferably 4.0 to 12 mol %, even more preferably 5.0 to 11 mol %, and particularly preferably 6.0 to 10 mol %. Examples of α-olefin components having 4 or more carbon atoms include 1-butene, 1-pentene, 3-methyl-1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 5-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, and 1-eicosene. The α-olefin component other than propylene is preferably an α-olefin component other than propylene having 2 to 20 carbon atoms, more preferably an α-olefin component other than propylene having 2 to 10 carbon atoms, even more preferably an α-olefin component other than propylene having 2 to 6 carbon atoms, and particularly preferably an α-olefin component other than propylene having 2 to 4 carbon atoms.

[0028] Various suitable physical properties of the polypropylene resin composition are described below. When two or more different polypropylene copolymers are used, the physical properties are the mass average values ​​of the physical properties of each polypropylene copolymer (the same applies to the sealing layer C and the functional layer D described below).

[0029] The melting point of the polypropylene resin composition constituting the intermediate layer B is preferably 150°C or less, more preferably 145°C or less, and even more preferably 140°C or less. By setting the melting point within the above range, the heat seal strength can be increased. The lower limit of the melting point of the polypropylene resin composition constituting the intermediate layer B is not particularly limited, and is, for example, 120°C or more. In addition, from the viewpoint of increasing the heat seal strength, the melting point of the polypropylene resin composition constituting the intermediate layer B is preferably higher than the melting point of the polypropylene resin composition constituting the seal layer C.

[0030] The melt flow rate (MFR; 230°C, 2.16 kgf) of the polypropylene resin composition constituting the intermediate layer B is preferably 3.0 g / 10 min or more and 6.0 g / 10 min or less. It is even more preferably 3.5 g / 10 min or more and 5.5 g / 10 min or less, even more preferably 4.0 g / 10 min or more and 5.0 g / 10 min or less, and particularly preferably 4.3 g / 10 min or more and 4.8 g / 10 min or less. In addition, from the viewpoint of increasing the heat seal strength, the melt flow rate of the polypropylene resin composition constituting the intermediate layer B is preferably smaller than the melt flow rate of the polypropylene resin composition constituting the seal layer C.

[0031] The polypropylene copolymer contained in the intermediate layer B preferably contains at least one selected from the group consisting of a propylene-butene copolymer, a propylene-ethylene-butene copolymer, and a propylene-ethylene copolymer, and more preferably contains a propylene-ethylene-butene copolymer.

[0032] (propylene-ethylene-butene copolymer) The content of the α-olefin component other than propylene in the propylene-ethylene-butene copolymer is preferably 4 mol% or more. When the content of the α-olefin component other than propylene is 4 mol% or more, the interlayer adhesion between the intermediate layer B and the seal layer C is likely to be improved, and as a result, the heat seal strength and the sealability are likely to be improved. The content of the α-olefin component other than propylene is more preferably 5 mol% or more, and even more preferably 6 mol% or more. The content of the α-olefin component other than propylene is not particularly limited, and is, for example, 25 mol% or less. When there are two or more kinds of α-olefin components other than propylene, the total amount is the content of the α-olefin components other than propylene. The ethylene content is preferably 1 mol% or more, more preferably 2 mol% or more. The upper limit of the ethylene content is not particularly limited, but if the ethylene content is too high, crystallization is too suppressed, resulting in a lower crystallinity compared to a propylene homopolymer, which may result in a decrease in the stiffness of the film, so that the upper limit is, for example, 10 mol% or less. The butene content is preferably 1 mol% or more, more preferably 2 mol% or more. The upper limit of the butene content is not particularly limited, but if the butene content is too high, crystallization is too suppressed, resulting in a lower crystallinity compared to a propylene homopolymer, which may result in a decrease in the stiffness of the film, so the upper limit is, for example, 16 mol% or less. As the propylene-ethylene-butene copolymer having a total content of α-olefin components other than propylene of 4 mol % or more, a commercially available product may be used, for example, FSX66E8 manufactured by Sumitomo Chemical Co., Ltd.

[0033] (Propylene-butene copolymer) The butene content in the propylene-butene copolymer is preferably 4 mol% or more. When the butene content is 4 mol% or more, the interlayer adhesion between the intermediate layer B and the seal layer C is easily improved, and as a result, the heat seal strength and the sealability are easily improved. The butene content is more preferably 5 mol% or more, and even more preferably 6 mol% or more. There is no particular limit to the upper limit of the butene content, but if the butene content is too high, crystallization is too suppressed, and the crystallinity is lower than that of a propylene homopolymer, which may result in a decrease in the stiffness of the film. For example, the upper limit is 16 mol% or less, and preferably 12 mol% or less. As the propylene-butene copolymer having a butene content of 4 mol% or more, a commercially available product may be used, and examples of such products include SP7843 manufactured by Sumitomo Chemical Co., Ltd., SPX78J1 manufactured by Sumitomo Chemical Co., Ltd., and XR110H manufactured by Mitsui Chemical Co., Ltd.

[0034] (propylene-ethylene copolymer) The ethylene content in the propylene-ethylene copolymer is preferably 4 mol% or more. When the ethylene content is 4 mol% or more, the interlayer adhesion between the intermediate layer B and the seal layer C is likely to be improved, and as a result, the heat seal strength and sealability are likely to be improved. The ethylene content is more preferably 5 mol% or more, and even more preferably 6 mol% or more. There is no particular limit to the upper limit of the ethylene content, but if the ethylene content is too high, crystallization is too suppressed, resulting in a lower crystallinity compared to a propylene homopolymer, which may result in a decrease in the stiffness of the film, so for example, it is 12 mol% or less. As the propylene-ethylene copolymer having an ethylene content of 4 mol% or more, a commercially available product may be used, such as PC540R manufactured by Sunallomer Co., Ltd. and VM3588FL manufactured by Mitsui Chemicals, Inc.

[0035] The polypropylene resin composition constituting the intermediate layer B may or may not contain an anti-fogging agent. As the anti-fogging agent, the anti-fogging agent described in the base layer A can be used. Even if the polypropylene resin composition constituting the intermediate layer B does not contain an anti-fogging agent, the anti-fogging agent may migrate from the base layer A to the intermediate layer B in the film-forming process, and the anti-fogging agent may be contained in the intermediate layer B in the obtained biaxially oriented polypropylene film. In addition, within a range that does not impair the effects of the present invention, the polypropylene resin composition constituting the intermediate layer B may contain additives such as resins other than polypropylene copolymers, the above-mentioned anti-fogging agents, known heat stabilizers, antioxidants, ultraviolet absorbers, nucleating agents, adhesives, flame retardants, inorganic or organic fillers, etc. Examples of resins other than polypropylene copolymers include polyolefin resins other than the polypropylene copolymers used in the intermediate layer B, and various elastomers. However, the amount of these additives is preferably small, and the amount of resins other than polypropylene copolymers in the polypropylene resin composition constituting the intermediate layer B is preferably 30% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and particularly preferably 2% by mass or less. Also, the amount of additives other than resins in the polypropylene resin composition constituting the intermediate layer B is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less.

[0036] [Sealing layer C] The seal layer C made of a polypropylene-based resin composition preferably has a polypropylene copolymer containing an α-olefin other than propylene. That is, the polypropylene-based resin composition constituting the seal layer C preferably has a polypropylene copolymer containing an α-olefin other than propylene. In addition, in the explanation of the seal layer C, even if it is simply described as "polypropylene copolymer (contained in the seal layer C)", it refers to a polypropylene copolymer containing an α-olefin other than propylene. The seal layer C preferably contains 70% by mass or more of the polypropylene copolymer, more preferably contains 80% by mass or more, even more preferably contains 90% by mass or more, and particularly preferably contains 95% by mass or more. In addition, as the polypropylene copolymer contained in the seal layer C, two or more different polypropylene copolymers can be used, and the total content is preferably within the above range. By making the polypropylene copolymer 70% by mass or more, it is easy to increase the interlayer adhesion between the seal layer C and the intermediate layer B, and the heat seal strength of the biaxially oriented polypropylene film can be further increased. The content of α-olefin components other than propylene in the polypropylene copolymer contained in the sealing layer C (the total amount of ethylene and α-olefins having 4 or more carbon atoms) is preferably 4.0 mol % or more (a polypropylene copolymer having constituent units of 4.0 mol % or more of α-olefin components other than propylene and 96 mol % or less of propylene), more preferably 5.0 to 15 mol %, even more preferably 6.0 to 12 mol %, and particularly preferably 7.0 to 10 mol %. Examples of α-olefin components having 4 or more carbon atoms include 1-butene, 1-pentene, 3-methyl-1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 5-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, and 1-eicosene. The α-olefin component other than propylene is preferably an α-olefin component other than propylene having 2 to 20 carbon atoms, more preferably an α-olefin component other than propylene having 2 to 10 carbon atoms, even more preferably an α-olefin component other than propylene having 2 to 6 carbon atoms, and particularly preferably an α-olefin component other than propylene having 2 to 4 carbon atoms.

[0037] The melting point of the polypropylene resin composition constituting the seal layer C is preferably 150°C or less, more preferably 145°C or less, even more preferably 140°C or less, particularly preferably 135°C or less, and most preferably 130°C or less. By setting the melting point within the above range, it is easy to lower the heat seal start temperature and increase the heat seal strength. The lower limit of the melting point of the polypropylene resin composition constituting the seal layer C is not particularly limited, and is, for example, 110°C or more. In addition, from the viewpoint of increasing the heat seal strength, it is preferable that the melting point of the polypropylene resin composition constituting the seal layer C is lower than the melting point of the polypropylene resin composition constituting the intermediate layer B.

[0038] The melt flow rate (MFR; 230°C, 2.16 kgf) of the polypropylene resin composition constituting the seal layer C is preferably 5.0 g / 10 min or more and 8.0 g / 10 min or less. It is more preferably 5.5 g / 10 min or more and 7.5 g / 10 min or less, more preferably 6.0 g / 10 min or more and 7.0 g / 10 min or less, and particularly preferably 6.3 g / 10 min or more and 6.8 g / 10 min or less. In addition, from the viewpoint of increasing the heat seal strength, the melt flow rate of the polypropylene resin composition constituting the seal layer C is preferably higher than the melt flow rate of the polypropylene resin composition constituting the intermediate layer B.

[0039] The polypropylene copolymer contained in the sealing layer C preferably contains at least one selected from the group consisting of a propylene-butene copolymer, a propylene-ethylene-butene copolymer, and a propylene-ethylene copolymer, and more preferably contains a propylene-butene copolymer.

[0040] (propylene-ethylene-butene copolymer) The content of the α-olefin component other than propylene in the propylene-ethylene-butene copolymer is preferably 4 mol% or more. When the content of the α-olefin component other than propylene is 4 mol% or more, the interlayer adhesion between the intermediate layer B and the seal layer C is likely to be improved, and as a result, the heat seal strength and the sealability are likely to be improved. The content of the α-olefin component other than propylene is more preferably 5 mol% or more, and even more preferably 6 mol% or more. The content of the α-olefin component other than propylene is not particularly limited, and is, for example, 25 mol% or less. When there are two or more kinds of α-olefin components other than propylene, the total amount is the content of the α-olefin components other than propylene. The ethylene content is preferably 1 mol% or more, more preferably 2 mol% or more. The upper limit of the ethylene content is not particularly limited, but if the ethylene content is too high, the film surface may become sticky and the slipperiness and blocking resistance may decrease, so the upper limit is, for example, 12 mol% or less. The butene content is preferably 1 mol% or more, more preferably 2 mol% or more. Although there is no particular upper limit to the butene content, if the butene content is too high, the film surface may become sticky and the slipperiness and blocking resistance may decrease, so the upper limit is, for example, 16 mol% or less. As the propylene-ethylene-butene copolymer having a total content of α-olefin components other than propylene of 4 mol % or more, a commercially available product may be used, for example, FSX66E8 manufactured by Sumitomo Chemical Co., Ltd.

[0041] (Propylene-butene copolymer) The butene content in the propylene-butene copolymer is preferably 4 mol% or more. When the butene content is 4 mol% or more, the interlayer adhesion between the intermediate layer B and the seal layer C is easily improved, and as a result, the heat seal strength and the sealability are easily improved. The butene content is more preferably 5 mol% or more, and even more preferably 6 mol% or more. There is no particular limit to the upper limit of the butene content, but if the butene content is too high, the film surface may become sticky, and the slipperiness and blocking resistance may decrease, so for example, it is 16 mol% or less, preferably 12 mol% or less. As the propylene-butene copolymer having a butene content of 4 mol% or more, a commercially available product may be used, and examples of such products include SP7843 manufactured by Sumitomo Chemical Co., Ltd., SPX78J1 manufactured by Sumitomo Chemical Co., Ltd., and XR110H manufactured by Mitsui Chemical Co., Ltd.

[0042] (propylene-ethylene copolymer) The ethylene content in the propylene-ethylene copolymer is preferably 4 mol% or more. When the ethylene content is 4 mol% or more, the interlayer adhesion between the intermediate layer B and the seal layer C is likely to be improved, and as a result, the heat seal strength and sealability are likely to be improved. The butene content is more preferably 5 mol% or more, and even more preferably 6 mol% or more. There is no particular limit to the upper limit of the ethylene content, but if the ethylene content is too high, the film surface may become sticky and the slipperiness and blocking resistance may decrease, so for example, it is 12 mol% or less. As the propylene-ethylene copolymer having an ethylene content of 4 mol% or more, a commercially available product may be used, such as PC540R manufactured by Sunallomer Co., Ltd. and VM3588FL manufactured by Mitsui Chemicals, Inc.

[0043] The polypropylene resin composition constituting the seal layer C may or may not contain an anti-fogging agent. As the anti-fogging agent, the anti-fogging agent described in the base layer A can be used. Even if the polypropylene resin composition constituting the seal layer C does not contain an anti-fogging agent, the anti-fogging agent may migrate from the base layer A to the seal layer C in the film-forming process, and the seal layer C may contain the anti-fogging agent in the obtained biaxially oriented polypropylene film. In addition, within a range that does not impair the effects of the present invention, the polypropylene resin composition constituting the seal layer C may contain additives such as resins other than polypropylene copolymers, the above-mentioned anti-fogging agents, known heat stabilizers, antioxidants, ultraviolet absorbers, nucleating agents, adhesives, flame retardants, inorganic or organic fillers, etc. Examples of resins other than polypropylene copolymers include polyolefin resins other than the polypropylene copolymers used in the seal layer C, and various elastomers. However, the amount of these additives is preferably small, and the amount of resins other than the polypropylene copolymer in the polypropylene resin composition constituting the seal layer C is preferably 30% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and particularly preferably 2% by mass or less. Also, the amount of additives other than the resin in the polypropylene resin composition constituting the seal layer C is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less.

[0044] [Functional layer D] The functional layer D is preferably provided on the surface of the base layer A on which the seal layer C is not provided. The functional layer D is not particularly limited and may be a layer of the same composition as the intermediate layer B, or may contain an antiblocking agent, wax, a lubricant such as a metal soap, a plasticizer, a processing aid, an antistatic agent, etc., in order to impart to the functional layer D functions not present in the seal layer C, such as easy slippage between films, easy slippage between a film and a processing tool, and antistatic properties.

[0045] The functional layer D is preferably a layer made of a polypropylene-based resin composition, and more preferably has a polypropylene copolymer containing an α-olefin other than propylene. That is, the polypropylene-based resin composition constituting the functional layer D is more preferably a polypropylene copolymer containing an α-olefin other than propylene. In addition, in the explanation of the functional layer D, even if it is simply described as "polypropylene copolymer (contained in the functional layer D)", it refers to a polypropylene copolymer containing an α-olefin other than propylene. The functional layer D preferably contains 70% by mass or more of the polypropylene copolymer, more preferably contains 80% by mass or more, even more preferably contains 90% by mass or more, and particularly preferably contains 95% by mass or more. In addition, as the polypropylene copolymer contained in the functional layer D, two or more different polypropylene copolymers can be used, and the total content is preferably within the above range. By making the polypropylene copolymer 70% by mass or more, it is easy to increase the interlayer adhesion between the functional layer D and the layer adjacent to the functional layer D, and the heat seal strength of the biaxially oriented polypropylene film can be further increased. The content of α-olefin components other than propylene in the polypropylene copolymer contained in the functional layer D (the total amount of ethylene and α-olefins having 4 or more carbon atoms) is preferably 4.0 mol % or more (a polypropylene copolymer having 4.0 mol % or more of α-olefin components other than propylene and 96 mol % or less of propylene as structural units), more preferably 4.0 to 12 mol %, even more preferably 5.0 to 11 mol %, and particularly preferably 6.0 to 10 mol %. Examples of α-olefin components having 4 or more carbon atoms include 1-butene, 1-pentene, 3-methyl-1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 5-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, and 1-eicosene. The α-olefin component other than propylene is preferably an α-olefin component other than propylene having 2 to 20 carbon atoms, more preferably an α-olefin component other than propylene having 2 to 10 carbon atoms, even more preferably an α-olefin component other than propylene having 2 to 6 carbon atoms, and particularly preferably an α-olefin component other than propylene having 2 to 4 carbon atoms.

[0046] The melting point of the polypropylene resin composition constituting the functional layer D is preferably 150° C. or less, more preferably 145° C. or less, and even more preferably 140° C. or less. By setting the melting point within the above range, the heat seal strength can be increased. The lower limit of the melting point of the polypropylene resin composition constituting the functional layer D is not particularly limited, and is, for example, 120° C. or more.

[0047] The melt flow rate (MFR; 230°C, 2.16 kgf) of the polypropylene resin composition constituting the functional layer D is preferably 3.0 g / 10 min to 6.0 g / 10 min, more preferably 3.5 g / 10 min to 5.5 g / 10 min, even more preferably 4.0 g / 10 min to 5.0 g / 10 min, and particularly preferably 4.3 g / 10 min to 4.8 g / 10 min.

[0048] The polypropylene copolymer contained in the functional layer D preferably contains at least one selected from the group consisting of a propylene-butene copolymer, a propylene-ethylene-butene copolymer, and a propylene-ethylene copolymer, and more preferably contains a propylene-ethylene-butene copolymer.

[0049] (propylene-ethylene-butene copolymer) The content of the α-olefin component other than propylene in the propylene-ethylene-butene copolymer is preferably 4 mol% or more. When the content of the α-olefin component other than propylene is 4 mol% or more, the interlayer adhesion between the functional layer D and the layer adjacent to the functional layer D is easily improved, and as a result, the heat seal strength and the sealability are easily improved. The content of the α-olefin component other than propylene is more preferably 5 mol% or more, and even more preferably 6 mol% or more. The content of the α-olefin component other than propylene is not particularly limited, and is, for example, 25 mol% or less. When there are two or more kinds of α-olefin components other than propylene, the total amount is the content of the α-olefin components other than propylene. The ethylene content is preferably 1 mol% or more, more preferably 2 mol% or more. The upper limit of the ethylene content is not particularly limited, but if the ethylene content is too high, the film surface may become sticky and the slipperiness and blocking resistance may decrease, so the upper limit is, for example, 10 mol% or less. The butene content is preferably 1 mol% or more, more preferably 2 mol% or more. Although there is no particular upper limit to the butene content, if the butene content is too high, the film surface may become sticky and the slipperiness and blocking resistance may decrease, so the upper limit is, for example, 16 mol% or less. As the propylene-ethylene-butene copolymer having a total content of α-olefin components other than propylene of 4 mol % or more, a commercially available product may be used, for example, FSX66E8 manufactured by Sumitomo Chemical Co., Ltd.

[0050] (Propylene-butene copolymer) The butene content in the propylene-butene copolymer is preferably 4 mol% or more. When the butene content is 4 mol% or more, the interlayer adhesion between the functional layer D and the layer adjacent to the functional layer D is easily improved, and as a result, the heat seal strength and the sealability are easily improved. The butene content is more preferably 5 mol% or more, and even more preferably 6 mol% or more. There is no particular limit to the upper limit of the butene content, but if the butene content is too high, the film surface may become sticky, and the slipperiness and blocking resistance may decrease, so for example, it is 16 mol% or less, preferably 12 mol% or less. As the propylene-butene copolymer having a butene content of 4 mol% or more, a commercially available product may be used, and examples of such products include SP7843 manufactured by Sumitomo Chemical Co., Ltd., SPX78J1 manufactured by Sumitomo Chemical Co., Ltd., and XR110H manufactured by Mitsui Chemical Co., Ltd.

[0051] (propylene-ethylene copolymer) The ethylene content in the propylene-ethylene copolymer is preferably 4 mol% or more. When the ethylene content is 4 mol% or more, the interlayer adhesion between the functional layer D and the layer adjacent to the functional layer D is likely to be improved, and as a result, the heat seal strength and the sealability are likely to be improved. The ethylene content is more preferably 5 mol% or more, and even more preferably 6 mol% or more. There is no particular limit to the upper limit of the ethylene content, but if the ethylene content is too high, the film surface may become sticky, and the slipperiness and blocking resistance may decrease, so for example, it is 12 mol% or less. As the propylene-ethylene copolymer having an ethylene content of 4 mol% or more, a commercially available product may be used, such as PC540R manufactured by Sunallomer Co., Ltd. and VM3588FL manufactured by Mitsui Chemicals, Inc.

[0052] The polypropylene resin composition constituting the functional layer D may or may not contain an anti-fogging agent. As the anti-fogging agent, the anti-fogging agent described in the base layer A can be used. Even if the polypropylene resin composition constituting the functional layer D does not contain an anti-fogging agent, the anti-fogging agent may migrate from the base layer A to the functional layer D in the film-forming process, and the anti-fogging agent may be contained in the functional layer D in the obtained biaxially oriented polypropylene film. In addition, within a range that does not impair the effects of the present invention, the polypropylene resin composition constituting the functional layer D may contain additives such as resins other than polypropylene copolymers, the above-mentioned anti-fogging agents, known heat stabilizers, antioxidants, ultraviolet absorbers, nucleating agents, adhesives, flame retardants, inorganic or organic fillers, etc. Examples of resins other than polypropylene copolymers include polyolefin resins other than the polypropylene copolymers used in the functional layer D, and various elastomers. However, it is preferable that these are added in small amounts, and in the polypropylene resin composition constituting the functional layer D, the amount of resins other than the polypropylene copolymer is preferably 30% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and particularly preferably 2% by mass or less. Also, in the polypropylene resin composition constituting the functional layer D, the amount of additives other than the resin is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less.

[0053] [Anti-fog agent content in film] The content of the antifogging agent in the biaxially oriented polypropylene film of the present invention is preferably 0.1 to 10 mass%, more preferably 0.15 to 5 mass%, even more preferably 0.2 to 2 mass%, particularly preferably 0.25 to 1.0 mass%, and most preferably 0.3 to 0.5 mass%. Even when the antifogging agent is added only to the polypropylene resin composition constituting the base layer A, the antifogging agent migrates from the base layer A to other layers during film formation and storage after film formation, and when the antifogging agent migrates to the outermost seal layer C, the antifogging agent is present on the surface of the seal layer C, resulting in an antifogging state.

[0054] [Layer structure and thickness structure of biaxially oriented polypropylene film] The layer structure of the biaxially oriented polypropylene film of the present invention is not particularly limited, but it is preferable that the biaxially oriented polypropylene film has a base layer A and a seal layer C, and an intermediate layer B between the base layer A and the seal layer C. In other words, the layer structure of the biaxially oriented polypropylene film of the present invention preferably has a base layer A, an intermediate layer B, and a seal layer C in this order. In addition, when the seal layer C is present, it is preferable that the seal layer C is present on the outermost surface. Furthermore, another layer may be present between the base layer A and the intermediate layer B, and the intermediate layer B may be directly laminated on the base layer A. In addition, another layer may be present between the intermediate layer B and the seal layer C, and the seal layer C may be directly laminated on the intermediate layer B. Examples of biaxially oriented polypropylene films having a base layer A, an intermediate layer B, and a seal layer C include a three-layer structure of base layer A / intermediate layer B / seal layer C, a four-layer structure of seal layer C1 / base layer A / intermediate layer B / seal layer C2, a five-layer structure of seal layer C1 / intermediate layer B1 / base layer A / intermediate layer B2 / seal layer C2, and a six-layer structure of seal layer C1 / base layer A1 / intermediate layer B1 / base layer A2 / intermediate layer B2 / seal layer C. In this case, the base layer A1 and the base layer A2 may be made of different polypropylene-based resin compositions or may be the same, the intermediate layer B1 and the intermediate layer B2 may be made of different polypropylene-based resin compositions or may be the same, and the seal layer C1 and the seal layer C2 may be made of different polypropylene-based resin compositions or may be the same.

[0055] When the biaxially oriented polypropylene film of the present invention has a functional layer D, the functional layer D may be directly laminated on the surface of the base layer A, or an intermediate layer B may be interposed between the base layer A and the functional layer D. The functional layer D may also be between the base layer A and the intermediate layer B, or between the intermediate layer B and the seal layer C. In the case of having the functional layer D, the base layer A, the intermediate layer B, and the seal layer C are in this order, and as long as the seal layer C is on the outermost surface, there is no particular limitation. For example, a four-layer structure of functional layer D / base layer A / intermediate layer B / seal layer C having a functional layer D in addition to the structure of base layer A / intermediate layer B / seal layer C, and a five-layer structure of functional layer D / intermediate layer B / base layer A / intermediate layer B / seal layer C having a functional layer D in addition to the structure of intermediate layer B / base layer A / intermediate layer B / seal layer C, etc. may be mentioned.

[0056] The overall thickness of the biaxially oriented polypropylene film of the present invention varies depending on the application and method of use, but from the viewpoint of film strength, sealing property, or water vapor barrier property, it is preferably 5 to 100 μm, more preferably 10 to 80 μm, and even more preferably 18 to 50 μm. When used as a freshness-preserving packaging material, the thickness is preferably 33 μm or less, more preferably 28 μm or less, even more preferably 23 μm or less, and particularly preferably 18 μm or less.

[0057] When the base layer A is included, the thickness of the base layer A varies depending on the application and method of use, but is preferably 5 to 90 μm, more preferably 10 to 50 μm, and even more preferably 15 to 30 μm. By making the thickness 5 μm or more, the film strength, sealing property, or water vapor barrier property can be improved. In addition, by making the thickness 90 μm or less, the environmental load can be reduced by reducing the volume.

[0058] When the intermediate layer B is included, the thickness of the intermediate layer B varies depending on the application and method of use, but is preferably 0.5 to 4 μm, and more preferably 1 to 3 μm. By making the thickness 0.5 μm or more, the adhesion between the base layer A and the seal layer C can be increased, thereby increasing the seal strength. In addition, by making the thickness 4 μm or less, the environmental load can be reduced by reducing the volume.

[0059] When the seal layer C is provided, the thickness of the seal layer C varies depending on the application and method of use, but is preferably 0.3 to 2 μm, and more preferably 0.5 to 1.5 μm. By making the thickness 0.3 μm or more, the heat seal strength can be increased. In addition, by making the thickness 2 μm or less, the environmental load can be reduced by reducing the volume.

[0060] When the functional layer D is present, the thickness of the functional layer D varies depending on the purpose and method of use, but is preferably 0.3 to 2 μm, and more preferably 0.5 to 1.5 μm. By making the thickness 0.3 μm or more, the heat seal strength can be increased. In addition, by making the thickness 2 μm or less, the environmental load can be reduced by reducing the volume.

[0061] [Method for producing biaxially oriented polypropylene film] The method for producing the biaxially oriented polypropylene film of the present invention is not particularly limited, but examples thereof include a method in which melt lamination is performed by a T-die method, an inflation method, or the like using an extruder suitable for the number of layers, and then cooling is performed by a cooling roll method, a water cooling method, or an air cooling method to obtain an unstretched laminated film, and the unstretched laminated film is then stretched by a sequential biaxial stretching method, a simultaneous biaxial stretching method, a tube stretching method, or the like.

[0062] Hereinafter, an example of a film-forming method will be described in which a biaxially oriented polypropylene film having a structure of functional layer D / base layer A / intermediate layer B / sealing layer C is formed by a sequential biaxial stretching method. The polypropylene resin compositions constituting the base layer A, intermediate layer B, and sealing layer C are as described above. In addition, the amount of anti-fogging agent added to the base layer A, intermediate layer B, and sealing layer C is preferably adjusted taking into consideration the anti-fogging agent that evaporates into the atmosphere when exposed to high temperatures during the film-forming process.

[0063] The polypropylene resin composition constituting each of the functional layer D, the base layer A, the intermediate layer B, and the seal layer C is melt-extruded by one or more extruders, and the extruded multilayer sheet is cooled by a cooling roll to form an unstretched sheet. Next, the obtained unstretched sheet is stretched in the longitudinal direction (MD). Subsequently, the stretched sheet is preheated, stretched in the transverse direction (TD), and finally heat-set to obtain the biaxially oriented polypropylene film of the present invention. If necessary, at least one side of the biaxially oriented polypropylene film is surface-treated, and then wound up by a winder to obtain a film roll. The extrusion process, cooling process, stretching process, heat treatment process, and surface treatment process are described in detail below. In the following, the melting point of the polypropylene resin used in the base layer A is represented as Tma (°C), and the melting point of the polypropylene resin used in the seal layer C is represented as Tmc (°C).

[0064] <Extrusion process> The polypropylene resin compositions constituting the functional layer D, the base layer A, the intermediate layer B, and the seal layer C are melted at 200°C to 260°C, and the molten polypropylene resin compositions are sent out from different flow paths using four extruders. Each of the sent out polypropylene resin compositions is laminated in multiple layers using a multi-layer feed block, a static mixer, a multi-layer multi-manifold die, etc., and a multi-layer sheet (molten polypropylene resin composition) laminated in the order of functional layer D / base layer A / intermediate layer B / seal layer C is extruded from a T-die. It is also possible to obtain a multi-layer sheet using only one extruder by introducing a multi-layering device into the melt line from the extruder to the T-die. In addition, a method of installing a gear pump in the polymer flow path is preferable from the viewpoint of stabilizing the back pressure and suppressing thickness fluctuation.

[0065] The thickness of the multilayer sheet is preferably 3500 μm or less from the viewpoint of increasing the cooling efficiency, and more preferably 3000 μm or less, but can be appropriately adjusted according to the film thickness after successive biaxial stretching. The thickness of the unstretched sheet can be adjusted by the extrusion speed of the polypropylene resin composition and the lip width of the T-die, etc.

[0066] <Cooling process> The multilayer sheet co-extruded from the T-die into a sheet shape is brought into contact with a metal cooling roll and cooled and solidified. At this time, it is preferable to ground the seal layer C side on the cooling roll. In order to promote solidification, it is preferable to further cool the multilayer sheet cooled by the cooling roll by immersing it in a water tank. The temperature of the cooling roll is preferably 10°C or higher and lower than the crystallization temperature of the polypropylene resin composition, and when it is desired to increase the transparency of the film, it is preferable to cool and solidify with a cooling roll of 10 to 50°C. When the temperature of the cooling roll is 50°C or lower, the transparency of the unstretched sheet is likely to increase, and it is more preferably 40°C or lower, and even more preferably 30°C or lower. In order to increase the crystal orientation degree after the sequential biaxial stretching, it may be preferable to set the cooling temperature to 40°C or higher, but as described above, when using a propylene homopolymer having a mesopentad fraction of 97.0% or higher, it is preferable to set the temperature of the cooling roll to 40°C or lower, and more preferably 30°C or lower, from the viewpoint of facilitating the stretching in the next step and reducing thickness unevenness. When a water bath is used, the temperature of the water bath is also preferably 10 to 50°C, more preferably 40°C or lower, and even more preferably 30°C or lower, for the same reasons as above.

[0067] <Stretching process> The unstretched sheet that has been cooled as described above is heated to a temperature suitable for stretching, and then the unstretched sheet is stretched in the machine direction (MD) by utilizing the speed difference between the stretching rolls. Subsequently, the uniaxially stretched sheet is preheated, and then stretched in the width direction (TD) at a predetermined temperature while the sheet end is held by a tenter stretching machine, to obtain a biaxially stretched film. The longitudinal stretching step, preheating step, and width direction stretching step are described in detail below.

[0068] (Longitudinal stretching process) The stretching ratio in the longitudinal direction is preferably 4.0 to 6.0 times, and more preferably 4.2 to 5.0 times, in consideration of a stress at 5% elongation in the longitudinal direction of 35 MPa or more at 23°C and stable film formation without unevenness in stretching. The longitudinal stretching temperature is preferably Tmc-10°C to Tmc+20°C, and more preferably Tmc°C to Tmc+15°C. Within the above range, the rigidity of the film is easily increased and the heat shrinkage rate is easily reduced. In addition, the film is unlikely to adhere to the stretching rolls, making it difficult to stretch, or the quality is unlikely to decrease due to increased surface roughness. The stretching in the longitudinal direction may be performed in two or more stages using three or more pairs of stretching rolls.

[0069] (Preheating process) Prior to the width direction stretching step, the uniaxially stretched film after the longitudinal stretching must be heated at Tma to Tma+15°C (preheating temperature is Tma to Tma+15°C) to soften the polypropylene resin composition. The maximum temperature in the preheating step is the preheating temperature. By setting the preheating temperature to Tma°C or higher, softening proceeds and stretching in the width direction becomes easier. By setting the preheating temperature to Tma+15°C or lower, orientation proceeds during stretching in the width direction, and rigidity is easily developed. The preheating temperature is more preferably Tma+1 to Tma+10°C, and even more preferably Tma+2 to Tma+5°C.

[0070] (Width direction stretching process) After the preheating step, the film is stretched in the width direction. The stretching temperature in the width direction is preferably Tma-2°C to Tma+13°C, and more preferably Tma-1°C to Tma+5°C. In order to increase the stress at 5% elongation in the longitudinal and transverse directions at 23°C, it is important to increase the rigidity of the base layer A as much as possible in the transverse stretching step, so the longitudinal stretch ratio is preferably a high ratio of 12 times or more, more preferably 13 times or more, and even more preferably 13.5 times or more. In addition, from the viewpoint of suppressing the heat shrinkage rate at 120°C, it is preferably 15 times or less. This is because the seal layer C is provided to improve the heat seal strength, and in the next heat treatment step, the heat treatment and relaxation steps are also taken into consideration in order to reduce the orientation of the seal layer C, suppress the heat shrinkage rate at 120°C, and at the same time increase the tensile elongation at break, or to increase the anti-fogging properties if an anti-fogging agent is included.

[0071] (Heat treatment process) In order to suppress the thermal shrinkage rate at 120°C, it is preferable to heat treat the film stretched in the longitudinal direction at both edges held by tenter clips at Tma+7°C to Tma+13°C, and more preferably at Tma+8 to Tma+12°C. Simultaneously with the heat treatment, the film is relaxed by 3 to 8% in the width direction while both edges are held by tenter clips in order to improve heat resistance, and more preferably by 5 to 7%. By performing the relaxation in this manner, the thermal shrinkage rate in the width direction of the film can be reduced.

[0072] In this way, by using a highly crystalline polypropylene resin with high stereoregularity and a high melting point, and adopting the above-mentioned width direction stretching process, the molecules of the polypropylene resin in the base layer A are highly aligned in the main orientation direction (which corresponds to the width direction in the above-mentioned width direction stretching process), so that the crystals in the obtained biaxially oriented film have a very strong crystal orientation and are likely to have a high melting point. In addition, the orientation of the amorphous parts between the crystals is also increased in the main orientation direction (corresponding to the width direction in the width direction stretching process described above), and since there are many crystals with high melting points around the amorphous parts, the stretched polypropylene molecules in the amorphous parts are less likely to relax at temperatures lower than the melting point of the crystals, and tend to maintain their tensed state. Therefore, the entire biaxially oriented film can maintain high rigidity even at high temperatures. It should be noted that the adoption of such a process also tends to reduce the heat shrinkage rate at a high temperature of 120° C. The reason for this is that in the base layer A, since there are many crystals with high melting points around the amorphous parts, the elongated polypropylene resin molecules in the amorphous parts are less likely to relax at temperatures lower than the melting point of the crystals, and moreover, there is less entanglement between the molecules. Furthermore, when an anti-fogging agent is present, the anti-fogging properties of the final biaxially oriented film are also likely to be improved. On the other hand, since the orientation of the seal layer C can be made weak, the heat shrinkage rate at a high temperature of 120° C. can be made low, while the tensile elongation at break is likely to be improved and the heat seal strength is likely to be increased.

[0073] <Surface treatment process> In the biaxially oriented polypropylene film of the present invention, it is preferable to surface treat at least one of the seal layer C and the surface layer opposite to the seal layer C in order to improve printability, lamination properties, etc., and it is more preferable to surface treat the seal layer C from the viewpoint of increasing the surface tension of the seal layer C. Examples of the surface treatment method include corona discharge treatment, plasma treatment, flame treatment, acid treatment, etc., and there is no particular limitation. However, it is preferable to perform any one of corona discharge treatment, plasma treatment, and flame treatment from the viewpoint of enabling continuous treatment and being easily performed before the winding step in the film production process of this film, and it is more preferable to perform corona discharge treatment from the viewpoint of improving anti-fogging properties.

[0074] [Various properties of the biaxially oriented polypropylene film of the present invention] The biaxially oriented polypropylene film of the present invention preferably has the following properties. Here, the "longitudinal direction (MD)" of the biaxially oriented polypropylene film of the present invention is the direction corresponding to the flow direction in the film-forming process, and the "transverse direction (TD)" is the direction perpendicular to the flow direction in the film-forming process, and the same applies below.

[0075] (Stress at 5% elongation at 23℃) The stress (F5) of the biaxially oriented polypropylene film of the present invention at 23°C when elongated by 5% in the longitudinal direction is 35 MPa or more, preferably 35 to 70 MPa, more preferably 38 to 65 MPa, and even more preferably 40 to 50 MPa. At 35 MPa or more, the film has high rigidity, so that the film is easy to maintain the shape of a bag when it is made into a packaging bag, and the film is less likely to deform during processing such as printing. It has also been found that by increasing F5, the anti-fogging property is improved when an anti-fogging agent is present. The reason for this is presumed to be that the crystallinity of the base layer A increases, accelerating the migration of the anti-fogging agent to the seal layer C. At 70 MPa or less, the film is easy to manufacture in a practical manner.

[0076] The F5 in the width direction of the biaxially oriented polypropylene film of the present invention at 23°C is 130 MPa or more, preferably 130 to 200 MPa, more preferably 132 to 180 MPa, even more preferably 134 to 170 MPa, and particularly preferably 140 to 160 MPa. At 130 MPa or more, the film has high rigidity, so that the film is easy to maintain the shape of the bag when it is made into a packaging bag, and the film is less likely to deform during processing such as printing. It has also been found that the antifogging property is improved when an antifogging agent is present, and this is presumably because the crystallinity of the base layer A increases, accelerating the migration of the antifogging agent to the seal layer C. At 200 MPa or less, the film is easy to manufacture in a practical manner. The F5 in the longitudinal direction and the width direction can be set within the above range by adjusting the raw material composition of each layer (particularly the raw material composition of the base layer A), the stretch ratio during film formation, the relaxation rate, the temperature in each film formation process, etc.

[0077] (Heat shrinkage rate at 120℃) The thermal shrinkage rate in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 120°C is 2.0% or less, preferably 1.9% or less, and more preferably 1.8% or less. The thermal shrinkage rate in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 120°C may be set to a lower limit of 0.1%. When it is 2.0% or less, printing pitch deviation is less likely to occur when transferring printing ink. The heat shrinkage rate in the width direction of the biaxially oriented polypropylene film of the present invention at 120°C is 1.5% or less, preferably 1.3% or less, and more preferably 1.0% or less. The heat shrinkage rate in the width direction of the biaxially oriented polypropylene film of the present invention at 120°C may be set to a lower limit of 0.1%. When it is 1.5% or less, wrinkles are less likely to occur during heat sealing. The thermal shrinkage percentage in the longitudinal and transverse directions at 120°C can be within the above range by adjusting the raw material composition of each layer described above (particularly the raw material composition of the base layer A), the stretch ratio during film formation, the relaxation rate, the temperature in each film formation process, etc.

[0078] (Hayes) The haze of the biaxially oriented polypropylene film of the present invention is preferably 7.0% or less, more preferably 5.0% or less. If it is 7.0% or less, it is easy to use in applications where transparency is required. The lower limit of the haze is preferably 0%, and a practical value is 0.1%. The haze can be adjusted to within the above range by adjusting the cooling roll temperature, the longitudinal stretching temperature, the tenter preheating temperature before widthwise stretching, the widthwise stretching temperature, or the heat setting temperature, or the amount of the polypropylene resin component having a molecular weight of 100,000 or less. The haze may become large depending on the addition of an antiblocking agent or the composition of the sealing layer C.

[0079] (tensile modulus) The tensile modulus of elasticity in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 23° C. is preferably 2.0 GPa or more, more preferably 2.1 GPa or more, and even more preferably 2.2 GPa or more. There is no particular upper limit, and it is, for example, 6.0 GPa or less. When it is 2.0 GPa or more, the rigidity is high, so that the bag shape when made into a packaging bag is easily maintained, the film is less likely to deform during processing such as printing, and anti-fogging properties can also be improved. When it is 6.0 GPa or less, practical production is easy and the balance of properties in the longitudinal direction and the width direction is easily improved. The tensile modulus of elasticity in the width direction at 23° C. of the biaxially oriented polypropylene film of the present invention is preferably 5.0 GPa or more, more preferably 5.2 GPa or more, and even more preferably 5.6 GPa or more. There is no particular upper limit, and it is, for example, 10 GPa or less. When it is 5.0 GPa or more, the rigidity is high, so that the bag shape when made into a packaging bag is easily maintained, the film is less likely to deform during processing such as printing, and anti-fogging properties can also be improved. When it is 10.0 GPa or less, practical production is easy and the balance of properties in the longitudinal direction and the width direction is easily improved. The tensile modulus in the longitudinal and transverse directions can be adjusted within the above range by adjusting the stretch ratio, relaxation rate, temperature during film formation, and the like.

[0080] (Tensile breaking strength) The tensile breaking strength in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 23°C is preferably 80 to 200 MPa, more preferably 90 to 150 MPa, and even more preferably 100 to 130 MPa. If it is 80 MPa or more, printing pitch deviation is unlikely to occur when transferring printing ink, and the durability of the packaging bag is likely to be excellent. If it is 200 MPa or less, film breakage and packaging bag tearing are likely to be reduced.

[0081] The tensile breaking strength in the width direction of the biaxially oriented polypropylene film of the present invention at 23°C is preferably 320 to 500 MPa, more preferably 340 to 480 MPa, even more preferably 360 to 460 MPa, and even more preferably 380 to 440 MPa. If it is 320 MPa or more, printing pitch deviation is unlikely to occur when transferring printing ink, and the durability of the packaging bag is likely to be excellent. If it is 500 MPa or less, film breakage and packaging bag tearing are likely to be reduced. The tensile breaking strength in the longitudinal and transverse directions can be within the range by adjusting the raw material composition of each layer described above (particularly the raw material composition of the base layer A), the stretch ratio during film formation, the relaxation rate, the temperature of each film formation process, etc.

[0082] (Tensile elongation at break) The tensile breaking elongation in the longitudinal direction of the biaxially oriented polypropylene film of the present invention at 23° C. is preferably 220 to 270%, more preferably 223 to 260%, and even more preferably 228 to 250%. If it is 220% or more, the film is less likely to break and the packaging bag is less likely to break. If it is 270% or less, printing pitch deviation is less likely to occur when transferring printing ink, and the durability of the packaging bag can be increased. The tensile breaking elongation in the width direction of the biaxially oriented polypropylene film of the present invention at 23° C. is preferably 25 to 80%, more preferably 28 to 70%, and even more preferably 30 to 60%. If it is 25% or more, the film is less likely to break and the packaging bag is less likely to break. If it is 80% or less, the printing pitch deviation is less likely to occur when the printing ink is transferred, and the durability of the packaging bag can be increased. The tensile elongation at break in the longitudinal and transverse directions can be kept within the range by adjusting the raw material composition of each layer described above (particularly the raw material composition of the base layer A), the stretch ratio during film formation, the relaxation rate, the temperature of each film formation process, etc.

[0083] (Heat seal strength) In order to prevent the contents from falling out, the biaxially oriented polypropylene film of the present invention has a heat seal strength at 130°C on the seal layer C side measured by the measurement method described below of 4.0 N / 15 mm or more, preferably 4.8 N / 15 mm or more, more preferably 5.0 N / 15 mm or more, even more preferably 5.5 N / 15 mm or more, and particularly preferably 6.0 N / 15 mm or more. The upper limit is about 8.0 N / 15 mm. There is little need for it to be greater than this, and if it is too large, the bag may become difficult to open. Furthermore, when one surface of the biaxially oriented polypropylene film of the present invention is a sealing layer C and the other surface is a functional layer D, in order to maintain the packaging form, such as Z-packaging, the heat-sealed portion after bag making is folded to bond the functional layers D together. However, in order to make it easy to open the bag by hand, it is preferable that the heat seal strength at 130°C on the functional layer D side is lower than the heat seal strength at 130°C on the sealing layer C side, for example, 3.5 N / 15 mm or less, preferably 2.0 N / 15 mm or less, and more preferably 1.0 N / 15 mm or less. The biaxially oriented polypropylene film of the present invention has a heat seal strength of 4.0 N / 15 mm or more, preferably 4.8 N / 15 mm or more, more preferably 5.0 N / 15 mm or more, even more preferably 5.5 N / 15 mm or more, and particularly preferably 6.0 N / 15 mm or more, with the upper limit being about 8.0 N / 15 mm.

[0084] (Heat seal start temperature) The heat seal rising temperature of the seal layer C of the biaxially oriented polypropylene film of the present invention is preferably 90 to 130°C, more preferably 100 to 125°C, and even more preferably 110 to 120°C. When the heat seal rising temperature of the seal layer C is 130°C or less, high heat seal strength can be achieved at a relatively low temperature of about 130°C, so that the temperature of the processing tool during heat sealing can be relatively low, and high speed operation is possible during automatic packaging. In addition, since heat sealing processing can be performed at a relatively low temperature, the entire film is less likely to shrink and wrinkles are less likely to occur in the sealed portion. In addition, by setting the heat seal rising temperature of the seal layer C to 90°C or more, the film can be made less likely to fuse to the film forming device. The heat seal rise temperature can be within the range by adjusting the raw material composition of each layer (particularly the raw material composition of the base layer A), the stretch ratio during film formation, the relaxation rate, the temperature of each film formation step, and the like.

[0085] (Kinematic friction coefficient) The dynamic friction coefficient of the biaxially oriented polypropylene film of the present invention is preferably 0.50 or less on both sides (sealing layer C and the surface layer opposite to sealing layer C), more preferably 0.48 or less, and even more preferably 0.45 or less. If the dynamic friction coefficient is 0.50 or less on both sides, the film can be smoothly unwound from the roll film, making printing easier. The lower limit of the dynamic friction coefficient is not particularly limited, but is, for example, 0.10 or more.

[0086] (Wetting tension) The surface wet tension of the seal layer C of the biaxially oriented polypropylene film of the present invention is preferably 35 mN / m or more, more preferably 37 mN / m or more. If the wet tension is 35 mN / m or more, the adhesion to the surface layer opposite the seal layer C can be improved. Furthermore, if the wet tension is 35 mN / m or more, the anti-fogging properties of the film can be improved. In order to achieve a wet tension of 35 mN / m or more, it is preferable to carry out a physicochemical surface treatment such as a corona treatment or a flame treatment. In the corona treatment, it is preferable to use a preheat roll and a treatment roll and discharge in the air. If the wet tension is too high, the effect will be saturated, so it is preferable that the wet tension is 43 mN / m or less.

[0087] (Anti-fogging) The anti-fogging property of the surface of the seal layer C of the biaxially oriented polypropylene film of the present invention is preferably grade 1 to 3, more preferably grade 1 or 2, and even more preferably grade 1, as evaluated by the evaluation method described below.

[0088] [Packaging materials] The biaxially oriented polypropylene film of the present invention may be used alone or with a printed layer. Examples of packaging materials using the biaxially oriented polypropylene film of the present invention are shown below in (i) to (ix), but are not limited to these examples. (i) Biaxially oriented polypropylene film / printing layer / adhesive layer / linear low density polyethylene film sealant layer. (ii) biaxially oriented polypropylene film / printing layer / adhesive layer / unoriented polypropylene film sealant layer. (iii) biaxially oriented polyethylene terephthalate film / printing layer / adhesive layer / biaxially oriented polypropylene film / adhesive layer / unoriented polypropylene film sealant layer. (iv) biaxially oriented polyethylene terephthalate film / printing layer / adhesive layer / biaxially oriented polypropylene film / adhesive layer / linear low density polyethylene film sealant layer. (v) biaxially oriented polypropylene film / anchor coat layer / inorganic thin film layer / inorganic thin film protective layer / printing layer / adhesive layer / linear low density polyethylene film sealant layer. (vi) Linear low density polyethylene film sealant layer / adhesive layer / biaxially oriented polypropylene film / anchor coat layer / inorganic thin film layer / adhesive layer / linear low density polyethylene film sealant layer. (vii) linear low density polyethylene film layer / adhesive layer / biaxially oriented polypropylene film / anchor coat layer / inorganic thin film layer / adhesive layer / linear low density polyethylene film layer / low density polyethylene film / paper / low density polyethylene film / linear low density polyethylene film sealant layer. (viii) biaxially oriented polypropylene film / anchor coat layer / inorganic thin film layer / inorganic thin film protective layer / printing layer / adhesive layer / non-oriented polypropylene film sealant layer. (ix) Biaxially oriented PET film / inorganic thin film layer / inorganic thin film protective layer / printing layer / polyurethane-based adhesive layer / biaxially oriented polypropylene film / adhesive layer / easy-peel type unoriented polypropylene film sealant layer.

[0089] The packaging material as described above can be used to produce three-side sealed, pillow and gusset type packaging bags, which have excellent sealing strength and good appearance at the sealed parts. For example, to prepare the laminate of (i) above, the biaxially oriented polypropylene film of the present invention is printed by letterpress printing, lithographic printing, intaglio printing, stencil printing, or transfer printing according to the application. An adhesive solution is applied thereon, and an unstretched sheet, uniaxially oriented film, or biaxially oriented film made of low-density polyethylene, linear low-density polyethylene, ethylene-vinyl acetate copolymer, polypropylene, or polyester is laminated as a sealant film, and then dried (dry lamination method). Alternatively, a seal layer C is laminated while extruding a molten adhesive resin (hot melt lamination method). When it is desired to further improve the gas barrier properties and heat resistance, a packaging bag may be made which includes an unstretched sheet, uniaxially stretched film, or biaxially stretched film made of aluminum foil, polyvinylidene chloride, nylon, an ethylene-vinyl alcohol copolymer, or polyvinyl alcohol, or an inorganic oxide such as silica or alumina may be vapor-deposited onto the biaxially oriented polypropylene film of the present invention by a known method such as vacuum deposition, sputtering, or ion plating. EXAMPLES

[0090] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. The evaluation methods used in each example and comparative example are as follows. In addition, "surface (layer) opposite to the sealing layer C" refers to the base layer A in Examples 3 and 4, and refers to the functional layer D in Examples 1, 2, and Comparative Examples 1 to 4.

[0091] (1) Melt flow rate of polypropylene resin The melt flow rate (MFR) was measured in accordance with JIS K7210 at a temperature of 230° C. and a load of 2.16 kgf.

[0092] (2) Mesopentad fraction of polypropylene resin The mesopentad fraction ([mmmm]%) of polypropylene resin is measured as follows: 13 The mesopentad fraction was calculated according to the method described in Zambelli et al., Macromolecules, vol. 6, p. 925 (1973). 13 C-NMR measurements were performed using a BRUKER AVANCE500 at 110°C after dissolving 200 mg of a sample in a 8:2 mixture of o-dichlorobenzene and deuterated benzene at 135°C.

[0093] (3) Melting point Thermal measurements were performed under a nitrogen atmosphere using a TA Instruments Q1000 differential scanning calorimeter. Approximately 5 mg was cut out from a pellet of polypropylene resin and sealed in an aluminum pan for measurement. The temperature was raised to 230°C and held for 5 minutes, then cooled to 30°C at a rate of -10°C / min, held at 30°C for 5 minutes, and then raised to 230°C at a rate of 10°C / min. The main endothermic peak temperature was taken as the melting point. The melting points of the polypropylene resin compositions constituting the functional layer D, the base layer A, the intermediate layer B, and the seal layer C were also measured in the same manner.

[0094] (4) Film thickness The total thickness of the film was measured using a Millitron 1202D manufactured by Seiko EM Co., Ltd. The thickness of each layer was calculated from the total thickness measured above and the extrusion rate of each layer.

[0095] (5) Haze Measurements were performed at 23°C using Nippon Denshoku Industries' NDH5000 in accordance with JIS K7105.

[0096] (6) Stress at 5% elongation (F5), tensile modulus, tensile breaking strength, tensile breaking elongation Various physical properties were measured at 23°C during tensile testing in the longitudinal and transverse directions of the film in accordance with JIS K7127. The film was cut so that the measurement direction was 200 mm and the direction perpendicular thereto was 15 mm, and the chuck width was 100 mm and set in a tensile testing machine (Instron 5965 dual column tabletop testing machine manufactured by Instron Japan Co., Ltd.). The tensile test was performed at a tensile speed of 200 mm / min. From the obtained strain-stress curve, the tensile modulus was calculated from the slope of the linear part at the beginning of elongation, and the stress at 5% elongation was taken as F5. The tensile breaking strength and tensile breaking elongation were respectively the strength and elongation at the time when the sample broke.

[0097] (7) Heat shrinkage rate The heat shrinkage of the film in the longitudinal and transverse directions was measured according to JIS Z1712 by the following method. The film was cut so that the measurement direction was 200 mm and the direction perpendicular to this was 20 mm, and the film was hung in a hot air oven at 120°C and heated for 5 minutes. The length after heating was measured, and the heat shrinkage was calculated as the ratio of the shrunken length to the original length.

[0098] (8) Wetting tension (mN / m) The film was cut into a size of 297 mm in the longitudinal direction and 210 mm in the transverse direction, and after aging for 24 hours at a temperature of 23°C and a relative humidity of 50%, the wet tension of the surface on the seal layer C side of the sample was measured according to the following procedure in accordance with JIS K 6768. The wet tension was measured in a laboratory atmosphere in accordance with JIS K7100, at a temperature of 23°C and a relative humidity of 50%. The sample was placed on a flat substrate, and several drops of the wet tension standard liquid (a test mixture liquid described in JIS K 6768) were placed on the sealing layer C of the sample. The wet tension standard liquid was then applied to the surface of the sealing layer C by 6 cm with a cotton swab. 2 The liquid film was spread to cover an area of ​​at least 100 mm or more, and the state of the liquid film was visually observed in a bright place 3 seconds after application. If the liquid film was still in the same state as when it was applied 3 seconds after formation (no breakage of the liquid film), this meant that the film was wet, so a liquid film was formed using a wetting tension standard liquid with a surface tension one level higher than the wetting tension standard liquid used to form the liquid film. On the other hand, if the liquid film broke in less than 3 seconds, a liquid film was formed using a wetting tension standard liquid with a surface tension one level lower than the wetting tension standard liquid used to form the liquid film. A new cotton swab was used each time a liquid film was formed. The above liquid film formation was repeated, and the value of the wetting tension standard solution with the maximum value among the wetting tension standard solutions that could wet the surface of the sealing layer C in 3 seconds was taken as the wetting tension. The liquid film was formed three times using the wetting tension standard solution with the maximum value, and it was confirmed that the state at the time of application was maintained after 3 seconds had elapsed. The wetting tension of the surface layer on the opposite side to the sealing layer C was also measured using the same measuring and calculating methods as above.

[0099] (9) Anti-fogging properties Using the film, the anti-fogging property of the film surface on the seal layer C side and the anti-fogging property of the film surface on the opposite side to the seal layer C were evaluated according to the following procedure. 1) 300cc of 50°C hot water was poured into a 500cc open-top container. 2) The opening of the container was sealed with the film, with the surface of the film on which the anti-fogging properties were to be measured facing inward. 3) The film was left in a cold room at 5° C. for 30 minutes, after which the degree of dew adhesion on the film surface on the side where anti-fogging properties were to be measured was evaluated on the following 5-point scale. Grade 1: No dew on the entire surface (0 surface area) Grade 2: Dew on a small part of the surface (adhesion area is greater than 0 and less than 1 / 4) Grade 3: Dew on just under half of the surface (1 / 4 to 2 / 4 of surface area) Grade 4: Dew on most of the surface (2 / 4 to 3 / 4 of surface area) Grade 5: Dew on almost the entire surface (more than 3 / 4 of the surface area)

[0100] (10) Heat seal start temperature Two samples measuring 20 cm in the longitudinal direction and 5 cm in the width direction were cut out from the film. The seal layers C of the two cut out samples were placed face to face and then heat sealed using a Toyo Seiki Co., Ltd. heat gradient tester, and five rectangular heat seal surfaces were placed in a row in the center of the width direction of the sample and parallel to the longitudinal direction of the sample. The heat seal surfaces were placed 1 cm in the longitudinal direction of the sample and 3 cm in the width direction of the sample, with a distance of 1.5 cm between adjacent heat seal surfaces. The heat seal temperatures were different for each heat seal surface, and were 80°C, 85°C, 90°C, 95°C, and 100°C. The heat seal pressure was 1 kg / cm. 2 The time was set to 1 second. The sample was then cut to 19 cm in the longitudinal direction and 1.5 cm in the central part in the width direction so that it contained five heat-sealed surfaces. The sample was cut so that the longitudinal direction of the sample was parallel to the longitudinal direction of the cut sample, and the heat-sealed surface heat-sealed at 90°C was located in the central part in the longitudinal direction. The cut sample was attached to the upper and lower chucks of a tensile tester (Instron 5965 dual column tabletop tester), and the heat-seal strength was measured for each heat-sealed surface when pulled at a tensile speed of 200 mm / min (unit: N / 15 mm). In addition, two new cut-out samples were prepared and heat-sealed at 105°C, 110°C, 115°C, 120°C, and 125°C. Five measurement samples were prepared in the same manner as above, except that they were heat-sealed at 105°C, 110°C, 115°C, 120°C, and 125°C, and the heat seal strength was measured. A linear graph was drawn with the horizontal axis representing temperature and the vertical axis representing heat seal strength, and the temperature at which the heat seal strength reached 1N / 15mm was taken as the heat seal rise temperature. Another sample was prepared and the heat seal strength was measured two more times at 80-125°C to determine the heat seal rise temperature, and the average of the three calculated values ​​was taken as the heat seal rise temperature of the film. For the surface layer on the opposite side to the seal layer C, the heat seal rise temperature of the film was determined using the same measurement and calculation methods as above, since the surface layers on the opposite sides to the seal layer C were overlapped facing each other.

[0101] (11) Heat seal strength Two samples with a length of 29.7 cm and a width of 21.0 cm were cut out from the film. The seal layers C of the two cut out samples were placed face to face with each other, and then heat sealed at 130°C using a Toyo Seiki Co., Ltd. heat gradient tester. A rectangular heat seal surface was placed in the center of the width direction of the sample so as to be parallel to the length of the sample. The heat seal surface was placed so as to be 1.5 cm in the length direction of the sample and 3 cm in the width direction of the sample. Then, the sample was cut at 9.5 cm in the length direction and 1.5 cm in the center of the width direction. In addition, the sample was cut so that the length direction of the sample and the length direction of the cut sample were parallel to each other in the length direction, and the heat seal surface was located in the center of the length direction. The cut sample was attached to the upper and lower chucks of a tensile tester (Instron 5965 dual column tabletop tester), and the heat seal strength was measured when pulled at a tensile speed of 200 mm / min (unit: N / 15 mm). Two other samples were prepared and the heat seal strength was measured, and the average of the three calculated values ​​was regarded as the heat seal strength of the film. The heat seal strength of the film was determined by the same measuring and calculating methods as above, except that the surface layers of the two cut samples on the opposite side to the seal layer C were placed face to face with each other. Furthermore, the heat seal strength of the seal layer C and the heat seal strength of the surface layer opposite to the seal layer C were determined using the same measuring and calculation methods as above, except that the heat seal temperature was 140°C.

[0102] (12) Coefficient of kinetic friction A sample measuring 400 mm in length and 100 mm in width was cut out from the film. This was aged for 12 hours under an atmosphere of 23°C and 65% RH, and the above sample was divided into a test table sample measuring 300 mm in length x 100 mm in width for the test table and a sliding piece sample measuring 100 mm in length x 100 mm in width for the sliding piece. The test table sample was set on the test table, and the sliding piece sample was the bottom surface (area size 39.7 mm2) of a metal sliding piece with a load of 1.5 kg. 2The seal layers C were attached to the two pieces of paper (square, square) so that they were in contact with each other. In accordance with JIS K-7125, a tensile testing machine (Tensilon RTG-1210 manufactured by A&D Corporation) was used to measure the dynamic friction coefficient of the seal layer C surface under conditions of a sliding speed of the test piece of 200 mm / min, 23°C and 65% RH, and the average of three measurements was used. The dynamic friction coefficient of the surface opposite the sealing layer C was also determined in the same manner as above, except that the surfaces opposite the sealing layer C were attached so as to be in contact with each other.

[0103] (Ingredients used) The polypropylene resins constituting the layers of the films in the following examples and comparative examples are as follows. PP-1: Propylene homopolymer (FLX80H5 manufactured by Sumitomo Chemical Co., Ltd., mesopentad fraction: 98.9%, melting point: 163°C, MFR: 7.5g / 10 min, amount of components with molecular weight of 10,000 or less: 4.0% by mass, amount of components with molecular weight of 100,000 or less: 40.5% by mass) PP-2: Propylene homopolymer (EL80F5 manufactured by Sumitomo Chemical Co., Ltd., mesopentad fraction: 98.8%, melting point: 162°C, MFR: 11g / 10 min, amount of components with molecular weight of 10,000 or less: 6.9% by mass, amount of components with molecular weight of 100,000 or less: 53.1% by mass) PP-3: Propylene homopolymer (FS8051 manufactured by Sumitomo Chemical Co., Ltd., mesopentad fraction: 98.9%, melting point: 163°C, MFR: 7.5g / 10 min, amount of components with molecular weight of 10,000 or less: 4.0% by mass, amount of components with molecular weight of 100,000 or less: 40.5% by mass, contains stearyl diethanolamine monostearate, stearyl diethanolamine distearate, and stearyl diethanolamine as anti-fogging agents in total of 2.0% by mass) PP-4: Propylene-ethylene-butene copolymer (FSX66E8 manufactured by Sumitomo Chemical Co., Ltd., melting point: 138°C, MFR: 4.5g / 10min, ethylene content: 3.3mol%, butene content: 2.9mol%) PP-5: Propylene-butene copolymer (SP7843 manufactured by Sumitomo Chemical Co., Ltd., melting point: 128°C, MFR: 6.5g / 10min, butene content: 8.2mol%)

[0104] Example 1 (Base material layer A) A polypropylene-based resin composition containing 60% by mass of propylene homopolymer PP-1, 20% by mass of propylene homopolymer PP-2, and 20% by mass of propylene homopolymer PP-3 was used as the raw material. When the physical properties of each polypropylene homopolymer were averaged by mass, the polypropylene-based resin composition constituting the base layer A had a mesopentad fraction of 98.88%, a melting point of 162.8°C, an MFR of 8.2g / 10min, a content of components with a molecular weight of 10,000 or less of 4.58% by mass, and a content of components with a molecular weight of 100,000 or less of 43.02% by mass. (Middle layer B) The raw material was propylene-ethylene-butene copolymer PP-4. (Sealing layer C) The raw material was propylene-butene copolymer PP-5. (Functional Layer D) The raw material was propylene-ethylene-butene copolymer PP-4. (Film production) First, the polypropylene resin compositions constituting each of the functional layer D / base layer A / intermediate layer B / sealing layer C were heated and melted in an extruder using a multi-layer feed block at 250°C, 250°C, 250°C, and 210°C, respectively, and the molten polypropylene resin composition was laminated from a T-die at 250°C to produce a laminated molten sheet with a thickness of 1.8 mm, co-extruded so that the thickness ratio of the functional layer D / base layer A / intermediate layer B / sealing layer C was 1 / 16 / 2 / 1. The functional layer D side of the molten sheet was brought into contact with a cooling roll at 20° C., and then placed in a water bath at 20° C. Subsequently, the sheet was stretched 4.5 times in the machine direction by utilizing the difference in peripheral speed between metal rolls heated to 138° C., and then introduced into a tenter stretching machine, where, while held by clips, the sheet was stretched 13 times in the width direction at a preheating section temperature of 168° C. and a stretching section temperature of 163° C. Immediately after stretching in the width direction, the sheet was cooled to 100° C. while held by clips, and then heat-treated at 172° C. while being relaxed by 6% in the width direction. The surface of the obtained biaxially oriented polypropylene film on the side of the seal layer C was subjected to a corona treatment using a corona treatment machine manufactured by Softal Corona & Plasma GmbH under conditions of an applied current value of 0.75 A and an applied voltage of 1.8 kW, and then the film was wound up with a winder to obtain the biaxially oriented polypropylene film of the present invention. The thickness of the obtained film was 20 μm. In the obtained film, the thicknesses of the functional layer D / base layer A / intermediate layer B / seal layer C were 1 μm / 16 μm / 2 μm / 1 μm. The raw material composition of each layer and the film forming conditions are shown in Table 1, and various physical properties of the film are shown in Table 2. The biaxially oriented polypropylene film of Example 1 had high rigidity, but also had low heat shrinkage at high temperatures, high seal strength, and excellent anti-fogging properties.

[0105] Example 2 The polypropylene resin compositions constituting the base layer A, the intermediate layer B, the seal layer C, and the functional layer D were the same as those in Example 1. (Film production) First, the polypropylene resin compositions constituting each of the functional layer D / base layer A / intermediate layer B / sealing layer C were heated and melted in an extruder using a multi-layer feed block at 250°C, 250°C, 250°C, and 210°C, respectively, and the molten polypropylene resin composition was laminated from a T-die at 250°C to produce a 1mm thick laminated molten sheet, co-extruded so that the thickness ratio of the functional layer D / base layer A / intermediate layer B / sealing layer C was 1 / 12 / 2 / 1. The functional layer D side of the molten sheet was brought into contact with a cooling roll at 20°C and then placed in a water bath at 20°C. The sheet was then stretched 4.5 times in the machine direction between metal rolls heated to 133°C by utilizing the difference in peripheral speed, and then introduced into a tenter stretching machine, where it was stretched 13 times in the width direction while held by clips at a preheating section temperature of 165°C and a stretching section temperature of 162°C. Immediately after stretching in the width direction, the sheet was cooled to 100°C while held by clips, and then heat-treated at 172°C while being relaxed by 6% in the width direction. The surface of the obtained biaxially oriented polypropylene film on the side of the seal layer C was subjected to a corona treatment using a corona treatment machine manufactured by Softal Corona & Plasma GmbH under conditions of an applied current value of 0.75 A and an applied voltage of 1.8 KW, and then the film was wound up with a winder to obtain the biaxially oriented polypropylene film of Example 1. The thickness of the obtained film was 16 μm. In the obtained film, the thicknesses of the functional layer D / base layer A / intermediate layer B / seal layer C were 1 μm / 12 μm / 2 μm / 1 μm. The raw material composition of each layer and the film forming conditions are shown in Table 1, and various physical properties of the film are shown in Table 2. The biaxially oriented polypropylene film of Example 2 had high rigidity, but also had low heat shrinkage at high temperatures, high seal strength, and excellent anti-fogging properties.

[0106] Example 3 The polypropylene resin compositions constituting the base layer A, the intermediate layer B, and the seal layer C were the same as those in Example 1. The biaxially oriented polypropylene film obtained in Example 3 did not have the functional layer D. (Film production) First, the polypropylene resin compositions constituting each of the base layer A, intermediate layer B, and seal layer C were heated and melted in an extruder using a multi-layer feed block at 250°C, 250°C, and 210°C, respectively, and the molten polypropylene resin compositions were laminated from a T-die at 250°C to co-extrude a laminated molten sheet with a thickness of 1 mm such that the thickness ratio of the base layer A, intermediate layer B, and seal layer C was 1 / 12 / 2 / 1. The substrate layer A side of the molten sheet was brought into contact with a cooling roll at 20° C. and then placed in a water bath at 20° C. Subsequently, the sheet was stretched 4.5 times in the machine direction between metal rolls heated to 133° C. by utilizing the difference in peripheral speed, and then introduced into a tenter stretching machine, where the sheet was stretched 13 times in the width direction while held by clips at a preheating section temperature of 165° C. and a stretching section temperature of 162° C. Immediately after stretching in the width direction, the sheet was cooled to 100° C. while held by clips, and then heat-treated at 172° C. while being relaxed by 6% in the width direction. The surface of the obtained biaxially oriented polypropylene film on the side of the seal layer C was subjected to a corona treatment using a corona treatment machine manufactured by Softal Corona & Plasma GmbH under conditions of an applied current value of 0.75 A and an applied voltage of 1.8 KW, and then the film was wound up with a winder to obtain the biaxially oriented polypropylene film of Example 2. The thickness of the obtained film was 16 μm. In the obtained film, the thicknesses of the base layer A / intermediate layer B / seal layer C were 13 μm / 2 μm / 1 μm. The raw material composition of each layer and the film forming conditions are shown in Table 1, and various physical properties of the film are shown in Table 2. The biaxially oriented polypropylene film of Example 3 had high rigidity, but also had low heat shrinkage at high temperatures, high seal strength, and excellent anti-fogging properties.

[0107] Example 4 A biaxially oriented polypropylene film of Example 4 was obtained by the same film-forming method as in Example 3, except that the stretching ratio in the width direction was 14 times and the relaxation rate was 3%. The thickness of the obtained biaxially oriented polypropylene film was 16 μm, and the thicknesses of the base layer A / intermediate layer B / seal layer C were 13 μm / 2 μm / 1 μm. The raw material composition of each layer and the film-forming conditions are shown in Table 1, and various physical properties of the film are shown in Table 2. The biaxially oriented polypropylene film of Example 4 had a low heat shrinkage rate at high temperatures, a high seal strength, and excellent anti-fogging properties, despite its high rigidity.

[0108] Comparative Example 1 A film of Comparative Example 1 was obtained in the same manner as in Example 1, except that the thickness of the laminated molten sheet coextruded from the T-die was changed to 0.7 mm and the stretching ratio in the width direction was changed to 10. In the obtained film, the thicknesses of the functional layer D / base layer A / intermediate layer B / seal layer C were 1 μm / 16 μm / 2 μm / 1 μm. The raw material composition of each layer and the film-forming conditions are shown in Table 1, and various physical properties of the film are shown in Table 2. The biaxially oriented polypropylene film of Comparative Example 1 had low rigidity and was difficult to maintain the bag shape when made into a packaging bag.

[0109] Comparative Example 2 A film of Comparative Example 2 was obtained in the same manner as in Example 1, except that instead of performing heat treatment at 172° C. while relaxing by 6% in the width direction, heat treatment was performed at 172° C. without relaxing in the width direction. In the obtained film, the thicknesses of the functional layer D / base layer A / intermediate layer B / sealing layer C were 1 μm / 16 μm / 2 μm / 1 μm. The raw material composition of each layer and the film formation conditions are shown in Table 1, and various physical properties of the film are shown in Table 2. The biaxially oriented polypropylene film of Comparative Example 2 had a large heat shrinkage rate and was prone to wrinkles during heat sealing.

[0110] Comparative Example 3 A film of Comparative Example 3 was obtained in the same manner as in Example 1, except that the heat treatment temperature after width direction stretching was changed from 172° C. to 158° C. In the obtained film, the thicknesses of the functional layer D / base layer A / intermediate layer B / sealing layer C were 1 μm / 16 μm / 2 μm / 1 μm. The raw material composition of each layer and the film formation conditions are shown in Table 1, and various physical properties of the film are shown in Table 2. The biaxially oriented polypropylene film of Comparative Example 3 had a large heat shrinkage rate and was prone to wrinkles during heat sealing.

[0111] Comparative Example 4 A film of Comparative Example 4 was obtained in the same manner as in Example 1, except that the polypropylene-based resin composition for the base layer A was made from the following raw material. In the obtained film, the thicknesses of the functional layer D / base layer A / intermediate layer B / sealing layer C were 1 μm / 16 μm / 2 μm / 1 μm. The raw material composition of each layer and the film forming conditions are shown in Table 1, and various physical properties of the film are shown in Table 2. The biaxially oriented polypropylene film of Comparative Example 4 had low rigidity, and when made into a packaging bag, it was difficult to maintain the bag shape, and in addition, the thermal shrinkage rate was large, and wrinkles were likely to occur during heat sealing.

[0112] (Base material layer A) The raw material was a polypropylene resin composition containing 43% by mass of PP-6 (propylene homopolymer: "FY6H" manufactured by Japan Polypropylene Corporation, MFR: 1.9 g / 10 min, melting point: 163°C, mesopentad fraction: 98.9%) and 57% by mass of PP-7 (a composition obtained by adding 0.16% by mass of glycerin monostearate (TB-123 manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd.), 0.2% by mass of polyoxyethylene (2) stearylamine (TB-12 manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd.), and 0.6% by mass of polyoxyethylene (2) stearylamine monostearate (Elex 334 manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd.) to 100% by mass of the above PP-1).

[0113] [Table 1]

[0114] [Table 2] [Industrial Applicability]

[0115] The biaxially oriented polypropylene film of the present invention has excellent rigidity and heat resistance, and therefore has excellent bag-making processability, and is easy to maintain the bag shape when made into a packaging bag. Therefore, the biaxially oriented polypropylene film of the present invention can be used for packaging bags, and packaging bags containing an anti-fogging agent are particularly suitable for packaging fruits and vegetables. In addition, the biaxially oriented polypropylene film of the present invention has excellent heat sealability, and therefore can be used suitably for applications requiring high rigidity without laminating a sealant film, and can maintain its strength even when the film is thin, thereby reducing the burden on the environment.

Claims

1. A biaxially oriented polypropylene film made of a polypropylene-based resin composition, which satisfies the following (1) to (3): (1) The stress at 5% elongation at 23° C. is 35 MPa or more in the longitudinal direction and 130 MPa or more in the transverse direction. (2) The thermal shrinkage rate at 120° C. is 2.0% or less in the longitudinal direction and 1.5% or less in the transverse direction. (3) The heat seal strength at 130°C is 4.0 N / 15 mm or more.

2. 2. The biaxially oriented polypropylene film according to claim 1, wherein the haze of the biaxially oriented polypropylene film is 7.0% or less.

3. The biaxially oriented polypropylene film according to claim 1 or 2, wherein the biaxially oriented polypropylene film contains 0.2% by mass or more and 1.0% by mass or less of an anti-fogging agent.

4. 3. The biaxially oriented polypropylene film according to claim 1, wherein the thickness of the biaxially oriented polypropylene film is 10 μm or more and 50 μm or less.

Citation Information

Patent Citations

  • Biaxially oriented polypropylene resin film

    WO2018181011A1

  • Biaxially oriented polypropylene resin film, and packaging using same

    WO2022118680A1