Oxidation neutralization treatment method for aqueous nickel chloride solution
Patent Information
- Application Number
- JP2023085091
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
【0007】 本発明によれば、中和澱物の粒子径D50を16μm以下とすることで、マンガンの除去率を高くできる。
Smart Images

Figure 2024168417000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for oxidizing and neutralizing an aqueous solution of nickel chloride, and more particularly to a method for removing manganese contained in an aqueous solution of nickel chloride by an oxidizing and neutralizing method. [Background technology]
[0002] In the nickel hydrometallurgical process, nickel sulfide is leached with chlorine, impurities are removed from the resulting nickel chloride aqueous solution, and electrolytic nickel is recovered by electrowinning. The oxidation neutralization method is known as a method for removing impurities from nickel chloride aqueous solution. For example, Patent Document 1 describes the removal of impurities such as lead contained in nickel chloride aqueous solution by the oxidation neutralization method. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-171972 A Summary of the Invention [Problem to be solved by the invention]
[0004] If manganese is contained in the nickel chloride aqueous solution subjected to electrowinning, the current efficiency is deteriorated and the operating cost is increased, so it is required to remove manganese from the nickel chloride aqueous solution.
[0005] In view of the above circumstances, an object of the present invention is to provide a method for oxidizing and neutralizing an aqueous nickel chloride solution, which has a high manganese removal rate. [Means for solving the problem]
[0006] The first aspect of the oxidation neutralization treatment method for an aqueous nickel chloride solution includes an oxidation neutralization step of adding an oxidizing agent and a neutralizing agent to an aqueous nickel chloride solution containing manganese to produce a neutralized precipitate containing manganese by an oxidation neutralization reaction, and a solid-liquid separation step of performing solid-liquid separation of a slurry containing the neutralized precipitate, wherein the neutralized precipitate has a particle diameter D50 of 10 to 16 μm. The second aspect of the method for oxidizing and neutralizing an aqueous nickel chloride solution is the same as the first aspect, and is characterized in that the aqueous nickel chloride solution in the oxidizing and neutralizing step has an oxidation-reduction potential (based on an Ag / AgCl electrode) of 600 to 1,200 mV and a pH of 4 to 6. The oxidation neutralization treatment method for an aqueous nickel chloride solution of the third aspect is characterized in that in the first or second aspect, the nickel concentration of the aqueous nickel chloride solution in the oxidation neutralization step is adjusted to set the particle size D50 of the neutralized precipitate to 10 to 16 μm. Effect of the Invention
[0007] According to the present invention, by making the particle size D50 of the neutralized precipitate 16 μm or less, the manganese removal rate can be increased. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is an overall flow diagram of a nickel hydrometallurgical process. [Diagram 2] FIG. 2 is a detailed process diagram of the lead removal process. [Diagram 3] 1 is a graph showing the relationship between the particle size D50 of the neutralized precipitate and the manganese removal rate in the solid-liquid separation step. [Figure 4] 1 is a graph showing the relationship between the nickel concentration of an aqueous crude nickel chloride solution and the particle size D50 of the neutralized precipitate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Next, an embodiment of the present invention will be described with reference to the drawings. The oxidation neutralization treatment method according to one embodiment of the present invention is a method for removing manganese contained in an aqueous solution of nickel chloride by an oxidation neutralization method. The aqueous solution of nickel chloride may contain other impurities such as iron, lead, and cobalt. The aqueous solution of nickel chloride undergoes an oxidation neutralization treatment to remove the impurities.
[0010] The oxidation neutralization method of the present embodiment is preferably applied to the de-iron step and the de-leading step, particularly the de-leading step, of the nickel hydrometallurgical process described below. Therefore, the de-leading step will be described below as an example. However, the oxidation neutralization method of the present embodiment is not limited to the de-leading step, and may be applied to any process step.
[0011] As shown in Figure 1, in the nickel hydrometallurgy process, the raw material nickel sulfide is first treated in the leaching process to obtain leachate. Nickel matte and nickel-cobalt mixed sulfide can be used as nickel sulfide.
[0012] The leaching process includes a chlorine leaching process and a cementation process. In the chlorine leaching process, the metals contained in the solid matter in the raw slurry are substantially all leached into the liquid by the oxidizing power of the chlorine gas blown into the leaching tank. In the cementation process, the chlorine leaching solution is brought into contact with nickel sulfide, preferably nickel matte, to carry out a substitution reaction between copper and nickel. As a result, for example, nickel in the nickel matte is leached into the liquid, and copper ions in the liquid are precipitated in the form of copper sulfide or metallic copper. The leaching solution obtained in the leaching process is mainly composed of an aqueous nickel chloride solution, and contains impurities such as copper, iron, and lead in addition to cobalt.
[0013] In the iron removal process, impurities such as iron and arsenic are removed from the leachate (nickel chloride aqueous solution) by oxidation neutralization. In the iron removal process, an oxidizing agent is added to the leachate to adjust the oxidation-reduction potential (based on Ag / AgCl electrode, the same applies below) to 400-1,100 mV, while a neutralizing agent is added to adjust the pH to 1.5-3. Chlorine gas, for example, is used as the oxidizing agent. Nickel carbonate, for example, is used as the neutralizing agent. Impurities such as iron and arsenic contained in the leachate are precipitated as hydroxides or oxides by the oxidation neutralization reaction. The precipitate is removed by solid-liquid separation to obtain a deironization final solution from which impurities have been removed.
[0014] In the solvent extraction step, the cobalt contained in the iron-removal final solution is separated by solvent extraction to obtain an aqueous nickel chloride solution and an aqueous cobalt chloride solution. Hereinafter, for the sake of convenience, the aqueous nickel chloride solution and the aqueous cobalt chloride solution obtained in the solvent extraction step are referred to as an aqueous crude nickel chloride solution and an aqueous crude cobalt chloride solution, respectively. The nickel concentration in the aqueous crude nickel chloride solution is 160 to 200 g / L. The aqueous crude nickel chloride solution contains impurities such as lead, manganese, cobalt, and zinc. The cobalt contained in the aqueous crude nickel chloride solution is extracted into an organic solvent and selectively separated from the nickel chloride in the aqueous crude nickel chloride solution, but a very small amount of cobalt still remains in the extraction residue (aqueous crude nickel chloride solution).
[0015] The crude cobalt chloride aqueous solution is purified in a purification process to remove impurities, and the resulting high-purity cobalt chloride aqueous solution is sent to the cobalt electrolysis process, where electrolytic cobalt is produced by electrowinning.
[0016] The crude nickel chloride aqueous solution is subjected to a deleading process to remove impurities, resulting in a high-purity nickel chloride aqueous solution. The deleading process will be described in detail later. After the deleading process, other solution purification treatments may be performed as necessary. For example, trace amounts of zinc remaining in the nickel chloride aqueous solution may be removed by adsorbing them onto an anion exchange resin. The high-purity nickel chloride aqueous solution is sent to a nickel electrolysis process. In the nickel electrolysis process, electrolytic nickel is produced by electrowinning.
[0017] As shown in Fig. 2, the deleading process has three sub-processes: a dilution process, an oxidation / neutralization process, and a solid-liquid separation process. In the following description, the term "crude nickel chloride aqueous solution" is used to mean not only the starting liquid of the deleading process, but also the water to be treated in the dilution process and the oxidation / neutralization process.
[0018] In the dilution step, the crude nickel chloride aqueous solution is diluted with a diluent to reduce the nickel concentration. For example, the crude nickel chloride aqueous solution (nickel concentration 160 to 200 g / L) obtained in the solvent extraction step is diluted so that the nickel concentration becomes 90 to 130 g / L. Since the main component of the crude nickel chloride aqueous solution is nickel chloride, the nickel concentration can be used as an index showing the chloride ion concentration of the crude nickel chloride aqueous solution.
[0019] If the nickel concentration of the crude nickel chloride aqueous solution is 130 g / L or less, the chloride ion concentration is low, so the chloro complex becomes unstable, and impurities, especially cobalt, tend to precipitate in the oxidation neutralization process. Also, if the nickel concentration of the crude nickel chloride aqueous solution is 90 g / L or more, the amount of diluent added can be reduced, and a significant increase in the amount of the crude nickel chloride aqueous solution can be suppressed, so there is no need to increase the facility capacity.
[0020] It is preferable to use nickel electrolysis waste liquid as the diluent. Nickel electrolysis waste liquid is obtained as waste liquid after using a high-purity nickel chloride aqueous solution as an electrolyte in the nickel electrolysis process. By using nickel electrolysis waste liquid as a diluent, it is possible to prevent an increase in the total amount of liquid in the system of the hydrometallurgical process. Industrial water may be used as the diluent instead of nickel electrolysis waste liquid. If industrial water is used, the crude nickel chloride aqueous solution can be diluted to the target nickel concentration with a smaller amount of liquid than if nickel electrolysis waste liquid is used.
[0021] The diluted crude nickel chloride aqueous solution is sent to the oxidation neutralization step. In the oxidation neutralization step, an oxidizing agent is added to the crude nickel chloride aqueous solution to adjust the redox potential to 600 to 1,200 mV, while a neutralizing agent is added to adjust the pH to 4 to 6. Impurities such as lead, manganese, and cobalt contained in the crude nickel chloride aqueous solution are coprecipitated with nickel precipitate by the oxidation neutralization reaction. Hereinafter, the precipitate containing impurities is referred to as neutralized precipitate.
[0022] The oxidizing agent is not particularly limited as long as it can increase the redox potential of the nickel chloride aqueous solution, but chlorine gas, which does not increase impurities, is preferable. Nickel carbonate, sodium carbonate, calcium carbonate, nickel hydroxide, sodium hydroxide, calcium hydroxide, etc. can be used as the neutralizing agent. Among these, nickel carbonate and nickel hydroxide are preferable because they do not increase impurities in the nickel chloride aqueous solution.
[0023] A reaction tank is used for the oxidation neutralization treatment. A crude nickel chloride aqueous solution is continuously fed to the reaction tank. An oxidizing agent and a neutralizing agent are also continuously fed to the reaction tank. A slurry containing the neutralized precipitate is continuously discharged from the reaction tank.
[0024] In addition, a plurality of reaction tanks may be connected in series to carry out the oxidation neutralization treatment stepwise. In this case, the crude nickel chloride aqueous solution is continuously supplied to the most upstream reaction tank and flows in sequence to the downstream reaction tanks. The dilution step may be carried out in a concentration adjustment tank, or the dilution step and the oxidation neutralization step may be carried out in the same reaction tank. In the latter case, both the crude nickel chloride aqueous solution before dilution and the diluent may be supplied to the reaction tank. In this case, the dilution rate of the crude nickel chloride aqueous solution may be adjusted using the nickel concentration of the crude nickel chloride aqueous solution in the slurry continuously discharged from the reaction tank, or the nickel concentration of the crude nickel chloride aqueous solution before dilution and the nickel concentration of the diluent as an index.
[0025] The slurry containing the neutralized precipitate is separated into a high-purity nickel chloride aqueous solution and the neutralized precipitate in the solid-liquid separation process. The main components of the neutralized precipitate are nickel hydroxide and oxide. Therefore, the neutralized precipitate is used as a raw material for nickel sulfate.
[0026] The inventors of the present application have found that in such an oxidation neutralization treatment, the smaller the particle size of the neutralized precipitate, the higher the manganese removal rate. Specifically, if the particle size D50 of the neutralized precipitate is set to 16 μm or less, the manganese removal rate can be sufficiently increased.
[0027] The reason why the manganese removal rate increases as the particle size of the neutralized precipitate decreases has not been fully elucidated, but it is presumed to be as follows. When an oxidizing agent and a neutralizing agent are added to a nickel chloride aqueous solution, a nickel precipitate is generated from nickel, which is the main component of the nickel chloride aqueous solution, by an oxidation neutralization reaction. At the same time, manganese contained in the nickel chloride aqueous solution is precipitated as a hydroxide or oxide. In addition, the smaller the particle size of the nickel precipitate, the more likely it is that a substitution reaction between nickel hydroxide or nickel oxide and manganese ions remaining in the nickel chloride aqueous solution will occur, and manganese is also removed by this action. In this way, in addition to the generation of manganese precipitate by the oxidation neutralization reaction, manganese is also removed in the solid-liquid separation process. It is presumed that the smaller the particle size of the neutralized precipitate, the higher the manganese removal rate in the solid-liquid separation process.
[0028] From the viewpoint of increasing the manganese removal rate in the solid-liquid separation step, there is no lower limit to the particle size of the neutralized precipitate. However, if the particle size of the neutralized precipitate is too small, the filterability in the solid-liquid separation step deteriorates. If the particle size D50 of the neutralized precipitate is set to 10 μm or more, the filtration rate does not become too slow and productivity can be maintained. From the viewpoint of productivity, the particle size D50 of the neutralized precipitate is more preferably 12 μm or more.
[0029] The particle size of the neutralized precipitate can be adjusted by the nickel concentration of the aqueous solution of crude nickel chloride in the oxidation neutralization step. The higher the nickel concentration of the aqueous solution of crude nickel chloride, the smaller the particle size of the neutralized precipitate. This is thought to be because the degree of supersaturation of nickel increases, and nucleation becomes more dominant than nucleation growth.
[0030] Therefore, the nickel concentration of the aqueous nickel chloride solution may be adjusted so that the particle size D50 of the neutralized precipitate is 10 to 16 μm. The nickel concentration of the aqueous crude nickel chloride solution can be adjusted by the amount of diluent added in the dilution step.
[0031] The particle size of the neutralized precipitate can also be adjusted by adjusting the amount of oxidizing agent added in the oxidation neutralization step. The amount of oxidizing agent added may be adjusted so that the particle size D50 of the neutralized precipitate is 10 to 16 μm.
[0032] However, the amount of oxidizing agent added affects the redox potential of the aqueous solution of crude nickel chloride. It is preferable to adjust the amount of oxidizing agent added so that the redox potential of the aqueous solution of crude nickel chloride is in a range suitable for the oxidation neutralization treatment, that is, 600 to 1,200 mV in the deleading step. EXAMPLES
[0033] Next, an embodiment will be described. The nickel hydrometallurgical smelting process shown in Figure 1 was operated. In the deleading process shown in Figure 2, impurities contained in the crude nickel chloride aqueous solution were removed by the oxidation neutralization method. The manganese concentration in the crude nickel chloride aqueous solution at the time it was supplied to the deleading process was 1 to 20 mg / L. In the oxidation neutralization process, three reaction tanks connected in series were used. An oxidizing agent and a neutralizing agent were added to the first and second tanks. Only an oxidizing agent was added to the third tank. Chlorine gas was used as the oxidizing agent, and basic nickel carbonate was used as the neutralizing agent.
[0034] Figure 3 shows the relationship between the particle size D50 of the neutralized precipitate and the manganese removal rate in the solid-liquid separation process. The particle size of the neutralized precipitate after solid-liquid separation was measured using a Microtrac laser diffraction / scattering particle size distribution analyzer (S3500), and a volume-based frequency distribution was created to determine the particle size D50. In addition, the manganese concentration ρ1 of the filtrate obtained by sampling the slurry discharged from the first tank and filtering it through filter paper was measured. The manganese concentration ρ2 of the filtrate (high-purity nickel chloride aqueous solution) obtained in the solid-liquid separation process was measured. The manganese removal rate R in the solid-liquid separation process was calculated from these measured values based on the following formula. R = (ρ1-ρ2) / ρ1
[0035] As can be seen from the graph in FIG. 3, the smaller the particle diameter of the neutralized precipitate, the higher the manganese removal rate. Specifically, it was confirmed that if the particle diameter D50 of the neutralized precipitate is set to 16 μm or less, the manganese removal rate is 80% or more. In order to increase the manganese removal rate, it is preferable that the particle diameter of the neutralized precipitate is smaller. If the particle diameter D50 of the neutralized precipitate is set to 15 μm or less, the manganese removal rate is 85% or more. In addition, if the particle diameter D50 of the neutralized precipitate is set to 14 μm or less, the manganese removal rate is 89% or more.
[0036] The relationship between the nickel concentration of the aqueous solution of crude nickel chloride and the particle size D50 of the neutralized precipitate is shown in Figure 4. The slurry discharged from the first tank was sampled and filtered through filter paper, and the nickel concentration of the filtrate was measured, which was used as the nickel concentration of the aqueous solution of crude nickel chloride.
[0037] As can be seen from the graph in Fig. 4, the particle size of the neutralized precipitate becomes smaller as the nickel concentration of the crude nickel chloride aqueous solution becomes higher. This confirmed that the particle size of the neutralized precipitate can be adjusted by the nickel concentration of the crude nickel chloride aqueous solution.
Claims
1. an oxidation / neutralization step of adding an oxidizing agent and a neutralizing agent to an aqueous nickel chloride solution containing manganese to produce a neutralized precipitate containing manganese by an oxidation / neutralization reaction; A solid-liquid separation step of performing solid-liquid separation of the slurry containing the neutralized precipitate, The neutralized precipitate has a particle diameter D50 of 10 to 16 μm.
1. A method for oxidizing and neutralizing an aqueous nickel chloride solution, comprising:
2. The nickel chloride aqueous solution in the oxidation / neutralization step has an oxidation-reduction potential (based on an Ag / AgCl electrode) of 600 to 1,200 mV and a pH of 4 to 6.
2. The method for oxidizing and neutralizing an aqueous nickel chloride solution according to claim 1.
3. The nickel concentration of the nickel chloride aqueous solution in the oxidation neutralization step is adjusted to make the particle diameter D50 of the neutralized precipitate 10 to 16 μm.
3. The method for oxidizing and neutralizing an aqueous nickel chloride solution according to claim 1 or 2.
Citation Information
Patent Citations
Purification method of nickel chloride solution
JP2015209551A
Method for removing impurities in aqueous nickel chloride solution
JP2017171972A