Aqueous coating varnish and printed matter

The aqueous coating varnish with zinc oxide crosslinking agent and acrylic resin particles addresses the issue of steam-induced film whitening by enhancing heat and hot water resistance, ensuring stable film performance.

JP2024169024APending Publication Date: 2024-12-05SAKATA INX

Patent Information

Application Number
JP2023086193
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing water-based coating varnishes used in corrugator processing suffer from steam invasion during the dry end process, causing the coating film to whiten due to the generation of steam from water and glue at high temperatures, compromising heat resistance and storage stability.

Method used

An aqueous coating varnish containing zinc oxide crosslinking agent and acrylic resin particles with a specific glass transition temperature range, along with optional wax particles, is formulated to enhance hot water resistance and storage stability.

Benefits of technology

The formulation results in a coating varnish with improved heat resistance and storage stability, preventing film whitening and maintaining film integrity under high temperatures and water exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169024000001
    Figure 2024169024000001
Patent Text Reader

Abstract

To provide an aqueous coating varnish which has excellent hot water resistance while having heat resistance and storage stability.SOLUTION: An aqueous coating varnish contains a zinc oxide-based crosslinking agent and acrylic resin particles. The acrylic resin particles have a glass transition temperature of 50°C or higher and 130°C or lower. A content of the zinc oxide-based crosslinking agent is 0.1 mass% or more and 1.2 mass% or less in the aqueous coating varnish.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-based coating varnish and a printed matter. [Background technology]

[0002] An aqueous printing varnish composition is known that has the heat resistance required for corrugating processing used in preprinted cardboard, and is excellent in water resistance, abrasion resistance, and storage stability (Patent Document 1). This aqueous printing varnish composition contains an aqueous emulsion resin with a glass transition temperature (Tg) of 30 to 100°C, oils and fats, and a phosphoric acid ester-based activator having a specific structure. In addition, an aqueous coating varnish is known that contains a specific amount of a zinc oxide-based crosslinking agent, a specific amount of polyolefin resin particles, and a specific amount of styrene or acrylic resin particles, and has excellent blocking resistance and abrasion resistance (Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-290078 A [Patent Document 2] JP 2022-116795 A Summary of the Invention [Problem to be solved by the invention]

[0004] Meanwhile, in the corrugator processing as described above, the base paper printed with the ink and the aqueous printing varnish composition (aqueous coating varnish) is usually subjected to a wet-end process and then a dry-end process. In the dry-end process, heat of about 200°C is applied by a thermal drying process called a double facer, and the moisture in the base paper and glue is generated as steam. There was a problem that this generated steam penetrated into the coating film of the aqueous printing varnish composition (aqueous coating varnish), causing the coating film to whiten.

[0005] Therefore, the present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an aqueous coating varnish that has excellent hot water resistance while also having heat resistance and storage stability.

[0006] Another object of the present invention is to provide a printed matter obtained by printing the above-mentioned aqueous coating varnish. [Means for solving the problem]

[0007] That is, the present invention relates to an aqueous coating varnish containing a zinc oxide-based crosslinking agent and acrylic resin particles, wherein the acrylic resin particles have a glass transition temperature of 50°C or higher and 130°C or lower, and the zinc oxide-based crosslinking agent is present in an amount of 0.1% by mass or higher and 1.2% by mass or lower in the aqueous coating varnish.

[0008] The aqueous coating varnish of the present invention preferably contains wax particles.

[0009] In the aqueous coating varnish of the present invention, the acrylic resin particles preferably account for 20% by mass or more and 40% by mass or less in the aqueous coating varnish.

[0010] The present invention also relates to a printed matter obtained by printing the above-mentioned aqueous coating varnish. Effect of the Invention

[0011] The aqueous coating varnish of the present invention contains a zinc oxide-based crosslinking agent and acrylic resin particles, the acrylic resin particles having a glass transition temperature of 50° C. or higher and 130° C. or lower, and the zinc oxide-based crosslinking agent is present in an amount of 0.1% by mass or higher and 1.2% by mass or lower in the aqueous coating varnish. Since the acrylic resin particles have a glass transition temperature of 50° C. or higher and 130° C. or lower and the aqueous coating varnish contains a specific amount of zinc oxide-based crosslinking agent, a film is formed in which a high Tg resin is crosslinked, and the aqueous coating varnish has excellent hot water resistance while having heat resistance and storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] <Water-based coating varnish> The aqueous coating varnish of the present invention contains a zinc oxide-based crosslinking agent and acrylic resin particles, the acrylic resin particles having a glass transition temperature of 50°C or more and 130°C or less, and the zinc oxide-based crosslinking agent is present in an amount of 0.1% by mass or more and 1.2% by mass or less in the aqueous coating varnish.

[0013] <Zinc oxide-based crosslinking agent> The zinc oxide crosslinking agent is a crosslinking agent that reacts with an acid such as a carboxylic acid. The zinc oxide crosslinking agent is preferably used in a state of being dissolved in a basic aqueous solution, and can be used in the form of an aqueous solution in which a complex is formed using, for example, aqueous ammonia. The zinc oxide crosslinking agents can be used alone or in combination of two or more kinds.

[0014] The zinc oxide-based crosslinking agent is contained in the aqueous coating varnish at a content of 0.1% by mass or more and 1.2% by mass or less. From the viewpoint of improving heat resistance and hot water resistance in the aqueous coating varnish, the zinc oxide-based crosslinking agent is contained in the aqueous coating varnish at a content of preferably 0.2% by mass or more and more preferably 0.35% by mass or more, and from the viewpoint of improving storage stability, the zinc oxide-based crosslinking agent is contained in the aqueous coating varnish at a content of preferably 1% by mass or less and more preferably 0.6% by mass or less.

[0015] <Acrylic resin particles> The acrylic resin particles are particles in which an acrylic resin is dispersed in water, and the glass transition temperature of the resin is 50° C. or more and 130° C. or less. Examples of the acrylic resin particles include acrylic resin particles (made only of acrylic monomers), as well as styrene-acrylic resin particles containing a styrene monomer component, acrylic-maleic acid resin particles containing a maleic acid monomer component, and styrene-acrylic-maleic acid resin particles containing a styrene monomer component and a maleic acid monomer component. The acrylic resin particles can be used alone or in combination of two or more kinds.

[0016] The acrylic resin particles preferably have a glass transition temperature of 80° C. or higher from the viewpoint of improving heat resistance and hot water resistance, and preferably have a glass transition temperature of 115° C. or lower from the viewpoint of improving heat resistance and hot water resistance. If the glass transition temperature exceeds 130° C., the film-forming property becomes poor. Note that, although the glass transition temperature can be referred to the value in the manufacturer's catalog, in the case of acrylic resins, the theoretical glass transition temperature calculated by the following Wood's formula can be used. Wood's formula: 1 / Tg=W1 / Tg1+W2 / Tg2+W3 / Tg3+····+Wx / Tgx [In the formula, Tg1 to Tgx represent the glass transition temperatures of the respective homopolymers of monomers 1, 2, 3...x constituting the resin, W1 to Wx represent the respective polymerization fractions of monomers 1, 2, 3...x, and Tg represents the theoretical glass transition temperature. However, the glass transition temperature in Wood's formula is an absolute temperature.]

[0017] From the viewpoint of efficient crosslinking with a zinc oxide-based crosslinking agent, the acrylic resin particles preferably contain a carboxyl group, and the acid value is preferably 30 mgKOH / g or more and 130 mgKOH / g or less, and more preferably 40 mgKOH / g or more and 110 mgKOH / g or less.

[0018] The acrylic resin particles are contained in the aqueous coating varnish at a content of preferably 20% by mass or more and 40% by mass or less, more preferably 25% by mass or more and 40% by mass or less, and even more preferably 30% by mass or more and 40% by mass or less, from the viewpoint of improving film-forming properties.

[0019] The aqueous coating varnish preferably contains wax particles from the viewpoint of improving hot water resistance. Examples of the wax particles include polyolefins such as polyethylene, polyethylene oxide, polypropylene, and polypropylene oxide, which are simply dispersed in water together with a surfactant or other emulsions, or which are made into emulsion dispersions. The wax particles can be used alone or in combination of two or more kinds. The wax particles are preferably 0.1% by mass or more and 2.0% by mass or less, more preferably 0.3% by mass or more and 1.5% by mass or less in the aqueous coating varnish.

[0020] The aqueous coating varnish may contain an organic solvent from the viewpoint of improving film-forming properties. Examples of the organic solvent include ketones such as butyl cellosolve, and polyhydric alcohols such as ethyl diglycol, diethylene glycol, and propylene glycol, and the organic solvent is preferably present in an amount of 0.1% by mass or more and 2.0% by mass or less, and more preferably 0.5% by mass or more and 1.5% by mass or less, in the aqueous coating varnish.

[0021] The aqueous coating varnish may contain a phosphate ester from the viewpoint of imparting blocking resistance, and the content of the phosphate ester in the aqueous coating varnish is usually 0.1% by mass or more and 1.5% by mass or less.

[0022] The water content of the aqueous coating varnish is preferably 60% by mass or more and 75% by mass or less, and more preferably 60% by mass or more and 70% by mass or less.

[0023] The aqueous coating varnish may further contain additives such as leveling agents, surfactants, thickeners, antioxidants, and defoamers, as well as water-soluble resins other than the above-mentioned acrylic resin particles (e.g., alkali-soluble resins), as necessary.

[0024] The total amount of the zinc oxide crosslinking agent, acrylic resin particles, and water in the aqueous coating varnish is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. When wax particles or an organic solvent are used, the total amount of the zinc oxide crosslinking agent, acrylic resin particles, wax particles, organic solvent, and water in the aqueous coating varnish is preferably 75% by mass or more, more preferably 85% by mass or more, and even more preferably 95% by mass or more.

[0025] <Preparation method of water-based coating varnish> The method for preparing the aqueous coating varnish is not particularly limited, and for example, the above-mentioned components may be added in order or simultaneously, and the aqueous coating varnish may be prepared using a roll mill, kneader, high-speed mixer, bead mill, ball mill, sand mill, ultrasonic disperser, high-pressure disperser, or the like.

[0026] The aqueous coating varnish can be applied to a recording medium by, for example, offset inline coating printing or flexographic printing to produce a printed matter. In addition, as the recording medium, a recording medium having a coating layer such as coated paper or coated board can be suitably used. In addition, the aqueous coating varnish can be applied to a recording medium on which characters or images are printed. EXAMPLES

[0027] The present invention will be described below with reference to examples, but the present invention is not limited to these.

[0028] <Examples 1-6, Comparative Examples 1-6> <Preparation of Water-Based Coating Varnish> Each water-based coating varnish was prepared by mixing the materials according to the composition shown in Table 1. The values ​​shown in each table are the parts by mass of the active ingredient.

[0029] The following evaluations were carried out using each of the aqueous coating varnishes obtained above. The results are shown in Table 1.

[0030] <Heat resistance> Sakata Inx Gratone PCN Indigo was applied to coated paper CRC (Osaka Paper Co., Ltd.) using a 0.15 mm bar coater, and the aqueous coating varnishes of the Examples and Comparative Examples were applied on top of it using a 0.1 mm bar coater. Aluminum foil was attached to the applied surface, which had been dried using a dryer, and the evaluation was performed under the following conditions using a thermal gradient tester HG-100 (Toyo Seiki Co., Ltd.). A or B is acceptable, and A is preferable. Evaluation conditions: 200℃, 2.0kgf / cm 2 of pressure for 1 second A: There is no resistance when peeling off the aluminum foil, and no varnish adheres to the aluminum foil. B: There is resistance when peeling off the aluminum foil, but no varnish adheres to the aluminum foil C: There is resistance when peeling off the aluminum foil, and varnish is attached to the aluminum foil. D: The pressure part adheres and does not peel off.

[0031] <Hot water resistance> Sakata Inx Gratone PCN Indigo was applied to coated paper CRC (Osaka Paper Co., Ltd.) using a 0.15 mm bar coater, and the aqueous coating varnishes of the Examples and Comparative Examples were applied on top of it using a 0.1 mm bar coater. 2 cc of water was dropped onto the applied surface, which was dried with a dryer, and aluminum foil was then attached. Evaluation was performed under the following conditions using a thermal gradient tester HG-100 (Toyo Seiki Co., Ltd.). A or B is acceptable, and A is preferable. Evaluation conditions: 200℃, 2.0kgf / cm 2 of pressure for 1 second A: No change in the coating on the pressurized area B: Slight marks are visible on the coating of the pressurized area. C: The coating on the pressure area turns slightly white. D: The coating on the pressure area turns white.

[0032] <Storage stability> The aqueous coating varnishes of the Examples and Comparative Examples were placed in plastic bottles, sealed, and left at 40° C. for 7 days. The viscosity was measured before and after leaving the bottles using a B-type viscometer TVB-25L (manufactured by Toki Sangyo Co., Ltd.) to evaluate the rate of viscosity change. A or B is acceptable, and A is preferable. A: Viscosity change rate is less than 1.3 B: Viscosity change rate is 1.3 or more and less than 2 C: Viscosity change rate is 2 or more, but there is fluidity D: Solidify

[0033] [Table 1]

[0034] In Table 1, Joncryl PDX-7780 (Tg = 92°C) is an acrylic resin particle (acid value: 46 mg KOH / g, manufactured by BASF); Joncryl PDX-7177 (Tg = 113°C) is an acrylic resin particle (acid value: 104 mg KOH / g, manufactured by BASF); Joncryl PDX-7789 (Tg = 60°C) is an acrylic resin particle (acid value: 60 mg KOH / g, manufactured by BASF); Joncryl PDX-7777 (Tg = 40°C) is an acrylic resin particle (acid value: 71 mg KOH / g, manufactured by BASF); Joncryl PDX-7741 (Tg = 14°C) is an acrylic resin particle (acid value: 52 mg KOH / g, manufactured by BASF); Zinc Oxide Solution #1 (zinc oxide) is a zinc oxide-based crosslinker (manufactured by BASF); Zircosol AC-7 ((NH4)2ZrO(CO3)2) is a zirconium-based cross-linking agent (manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd.); Orgatix TC-300 (titanium lactate ammonium salt) is a titanium-based cross-linking agent (manufactured by Matsumoto Fine Chemical Co., Ltd.); SN Deformer 777 is a defoamer (manufactured by San Nopco); Chemipearl W400 is a water dispersion of polyolefin (Mitsui Chemicals); Surfynol 104DEG is a surfactant (manufactured by Nissin Chemical Industry Co., Ltd.);

Claims

1. An aqueous coating varnish containing a zinc oxide-based crosslinking agent and acrylic resin particles, The acrylic resin particles have a glass transition temperature of 50° C. or more and 130° C. or less, The aqueous coating varnish is characterized in that the zinc oxide-based crosslinking agent is contained in an amount of 0.1% by mass or more and 1.2% by mass or less in the aqueous coating varnish.

2. 2. The aqueous coating varnish according to claim 1, further comprising wax particles.

3. 3. The aqueous coating varnish according to claim 1, wherein the acrylic resin particles are contained in an amount of from 20% by mass to 40% by mass in the aqueous coating varnish.

4. A printed matter obtained by printing the aqueous coating varnish according to claim 1 or 2.

Citation Information

Patent Citations

  • Aqueous printing varnish composition and printed matter

    JP2005290078A

  • Aqueous coating varnish and printed material

    JP2022116795A

Cited By

  • Heat-resistant coating agent, coated article, laminate, and packaging material

    WO2026133759A1