Cyclic olefinic copolymer and method for producing cyclic olefinic copolymer

A cyclic olefin copolymer with controlled crystallinity and transition metal catalyst production addresses chemical resistance issues, ensuring durability in solvent-exposed environments.

JP2024169025APending Publication Date: 2024-12-05MITSUI CHEMICALS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023086194
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Cyclic olefin copolymers used in various applications face challenges in withstanding high levels of organic solvents, particularly toluene, due to inadequate chemical resistance.

Method used

A cyclic olefin copolymer with controlled crystallinity within a specific range, comprising structural units derived from acyclic and cyclic olefins, produced using a transition metal compound catalyst, enhancing chemical resistance.

Benefits of technology

The copolymer exhibits improved chemical resistance, maintaining high crystallinity and melting points, effectively resisting solvents like toluene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169025000001
    Figure 2024169025000001
  • Figure 2024169025000002
    Figure 2024169025000002
  • Figure 2024169025000003
    Figure 2024169025000003
Patent Text Reader

Abstract

To provide a cyclic olefinic copolymer with improved chemical resistance.SOLUTION: A cyclic olefinic copolymer contains a constitutional unit (A) derived from an acyclic olefin (A') and a constitutional unit (B) derived from a cyclic olefin (B'), where the cyclic olefinic copolymer has a crystallinity of 1% or more as determined under specific "X-ray diffraction measurement conditions".SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cyclic olefin copolymer and a method for producing the cyclic olefin copolymer. [Background technology]

[0002] The cyclic olefin copolymer can be used in various applications such as films, sheets, lenses, and containers.

[0003] For example, Patent Document 1 describes a cyclic olefin resin containing repeating units derived from a cyclic olefin monomer and repeating units derived from an acyclic olefin monomer, the cyclic olefin resin having a glass transition point of 150°C or higher, a ratio of the repeating units derived from the cyclic olefin monomer being 50 mol% to 80 mol%, a ratio of the repeating units derived from the acyclic olefin monomer being 20 mol% to 50 mol%, a ratio of the repeating units derived from the cyclic olefin monomer existing as dimers in the cyclic olefin component being 30 mol% or higher, and a ratio of the repeating units derived from the cyclic olefin monomer existing as trimers in the cyclic olefin component being 15 mol% or higher. Furthermore, Patent Document 1 also describes that the object of the invention described in Patent Document 1 is to provide a cyclic olefin resin suitable for producing a retardation film having high heat resistance and tensile properties, and a film using the cyclic olefin resin, in particular a retardation film. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-063629 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, cyclic olefin copolymers have come to be used in various applications and diverse environments, and there is a demand for cyclic olefin copolymers to withstand unprecedentedly harsh usage conditions, for example, to endure use in environments where there is a high probability of being exposed to highly soluble organic solvents such as toluene. Therefore, there is a demand for further improving the resistance of cyclic olefin copolymers to chemicals that can strongly damage resin products such as toluene. However, the prior art has not been able to fully meet such demands.

[0006] An object of the present invention is to provide a cyclic olefin copolymer with improved chemical resistance.

Means for Solving the Problems

[0007] The present inventors intensively studied to solve the above problems. As a result, they found that by setting the crystallinity within a predetermined numerical range, the chemical resistance of the cyclic olefin copolymer can be improved, and thus the present invention was completed.

[0008] That is, according to the present invention, there are provided the following cyclic olefin copolymer and a method for producing a cyclic olefin copolymer.

[0009] 1. A cyclic olefin copolymer having a structural unit (A) derived from a non-cyclic olefin (A') and a structural unit (B) derived from a cyclic olefin (B'), wherein the crystallinity of the cyclic olefin copolymer determined by the following <X-ray diffraction measurement conditions> is 1% or more. <X-ray diffraction measurement conditions> The powdery cyclic olefin copolymer is subjected to wide-angle X-ray diffraction measurement, and is calculated using the following formula from the crystal-derived peak area, which is the area of the peak derived from crystals, and the amorphous halo-derived area, which is the area of the halo derived from the amorphous. Crystallinity (%) = Crystal-derived peak area / (Crystal-derived peak area + Amorphous halo-derived area) × 100 結晶化度(%)=結晶由来ピーク面積 / (結晶由来ピーク面積+非晶由来ハロー面積)×100 2. When the total content of the structural units (A) and (B) is 100 mol%, the content of the structural unit (A) in the cyclic olefin copolymer is 50 mol % or more and 68 mol % or less, 2. The cyclic olefin copolymer according to 1., wherein the content of the structural unit (B) in the cyclic olefin copolymer is 32 mol % or more and 50 mol % or less. 3. The structural unit (A) has a structure represented by the following general formula (I): 3. The cyclic olefin copolymer according to 1. or 2., wherein the structural unit (B) has a structure represented by the following general formula (VI): [ka] (In the above general formula (I), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms. [ka] (In the above general formula (VI), q is 1, 2 or 3; R 32 ~R 39 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, and when q=1, R 36 and R 37 , R 37 and R 38 , R 38 and R 39 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 36 and R 36 , R 36 and R 37 , R 37 and R 38 , R 38 and R 39 , R 39 and R 39may be bonded to each other to form a monocyclic or polycyclic ring, the monocyclic or polycyclic ring may have a double bond, and the monocyclic or polycyclic ring may be an aromatic ring. 4. The structural unit (A) contains a structural unit derived from ethylene, 4. The cyclic olefin copolymer according to any one of 1. to 3., wherein the structural unit (B) contains a structural unit derived from benzonorbornadiene. 5. The cyclic olefin copolymer according to any one of 1. to 4., having a melting point of 250° C. or higher. 6. A method for producing a cyclic olefin copolymer according to any one of 1. to 5., comprising the steps of: The method includes a step of copolymerizing a non-cyclic olefin (A') and a cyclic olefin (B') in the presence of a catalyst containing a transition metal compound (X) represented by the following general formula (1), The acyclic olefin (A') has a structure represented by the following general formula (Ia): A method for producing a cyclic olefin copolymer, wherein the cyclic olefin (B') has a structure represented by the following general formula (VIa): [ka] (In the general formula (1), M 1 indicates a transition metal atom in Group 4 of the periodic table, X 1 each independently represents an atom or group selected from the group consisting of a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, and an aluminum-containing group, and substitution products thereof; n 1 represents an integer from 1 to 4, Y 1 represents a carbon atom or a silicon atom, R 1 ~R 14each independently represents an atom or group selected from the group consisting of a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, and an aluminum-containing group, and substitution products thereof; R 1 ~R 14 adjacent ones of these may be bonded to each other to form a ring, and the ring formed may have aromaticity including a conjugated double bond, R 1 ~R 14 At least one of the groups is selected from the group consisting of a hydrocarbon group having one or more carbon atoms, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, and an aluminum-containing group, and substitution products thereof. [ka] (In the above general formula (Ia), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms. [ka] (In the above general formula (VIa), q is 1, 2 or 3; R 32 ~R 39 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, and when q=1, R 36 and R 37 , R 37 and R 38 , R 38 and R 39 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 36 and R 36 , R 36 and R 37 , R 37 and R 38 , R 38 and R 39 , R 39 and R39 may be bonded to each other to form a monocyclic or polycyclic ring, the monocyclic or polycyclic ring may have a double bond, and the monocyclic or polycyclic ring may be an aromatic ring. 7. When the total content of the non-cyclic olefin (A') and the cyclic olefin (B') in the copolymerization step is taken as 100 mol%, The content of the acyclic olefin (A') is 50 mol% or more and 68 mol% or less, 7. The method for producing a cyclic olefin copolymer according to 6., wherein the content of the cyclic olefin (B') is 32 mol % or more and 50 mol % or less. 8. The acyclic olefin (A') contains ethylene, 8. The method for producing a cyclic olefin copolymer according to 6. or 7., wherein the cyclic olefin (B') contains benzonorbornadiene. 9. In the general formula (1), R 1 ~R 14 9. The method for producing a cyclic olefin copolymer according to any one of 6. to 8., wherein at least one of the groups is a hydrocarbon group having one or more carbon atoms. 10. In the general formula (1), R 1 ~R 14 The method for producing a cyclic olefin copolymer according to any one of 6. to 9., wherein at least one of the groups is a hydrocarbon group having 4 or more carbon atoms. 11. In the general formula (1), R 1 ~R 14 The method for producing a cyclic olefin copolymer according to any one of 6. to 10., wherein at least one of the groups is a t-butyl group. Effect of the Invention

[0010] According to the present invention, it is possible to provide a cyclic olefin copolymer having improved chemical resistance and a method for producing the cyclic olefin copolymer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the present invention will be described based on embodiments. In the present embodiment, "A to B" indicating a numerical range represents A or more and B or less unless otherwise specified. Moreover, each monomer constituting the cyclic olefin copolymer of the present invention may be a monomer obtained from fossil raw materials or a monomer obtained from animal and plant raw materials.

[0012] [Cyclic olefin copolymer] Hereinafter, the cyclic olefin copolymer of the present invention will be described in detail.

[0013] The cyclic olefin copolymer according to the present embodiment is a cyclic olefin copolymer having a structural unit (A) derived from an acyclic olefin (A') and a structural unit (B) derived from a cyclic olefin (B'), and the crystallinity of the cyclic olefin copolymer obtained under the following <X-ray diffraction measurement conditions> is 1% or more. <X-ray diffraction measurement conditions> The powder cyclic olefin copolymer is subjected to wide-angle X-ray diffraction measurement, and is calculated using the following formula from the crystal-derived peak area, which is the area of the peak derived from the crystal, and the amorphous halo-derived area, which is the area of the halo derived from the amorphous. Crystallinity (%) = Crystal-derived peak area / (Crystal-derived peak area + Amorphous halo-derived area) × 100

[0014] Here, the peak and the halo will be described. When the cyclic olefin copolymer contains crystals, a sharp peak derived from the crystals appears. On the other hand, when the cyclic olefin copolymer contains amorphous, a very broad pattern derived from the amorphous, so-called halo, appears. In the present embodiment, the crystallinity is calculated from the areas of the peak and the halo using the above formula.

[0015] Although the mechanism by which the above problems are solved by the cyclic olefin copolymer according to the present embodiment is not clear, it is speculated that when the crystallinity of the cyclic olefin copolymer having a specific chemical structure is a certain level or more, the molecules of the cyclic olefin copolymer are properly arranged and can resist erosion by chemicals.

[0016] The crystallinity of the cyclic olefin copolymer determined by X-ray diffraction measurement is preferably 2% or more, more preferably 5% or more, even more preferably 8% or more, even more preferably 10% or more, and even more preferably 15% or more. The upper limit of the crystallinity is not particularly limited, but is, for example, 50% or less, preferably 40% or less, more preferably 30% or less, and even more preferably 25% or less. When the crystallinity is within the range, the chemical resistance of the cyclic olefin copolymer is improved. The crystallinity can be controlled by the types and ratios of the non-cyclic olefin (A') and the cyclic olefin (B') used in the cyclic olefin copolymer, the type of catalyst used in polymerization, etc. The specific method for the X-ray diffraction measurement will be described later.

[0017] The melting point of the cyclic olefin copolymer according to this embodiment is preferably 250°C or higher, more preferably 270°C or higher, even more preferably 290°C or higher, even more preferably 310°C or higher, even more preferably 330°C or higher, and even more preferably more than 350°C. The melting point is equal to or higher than the above lower limit, thereby improving heat resistance. The upper limit of the melting point is not particularly limited, but is, for example, 800°C or lower, preferably 700°C or lower, more preferably 600°C or lower, even more preferably 500°C or lower, and even more preferably 450°C or lower.

[0018] The cyclic olefin copolymer according to this embodiment has a structural unit (A) derived from a non-cyclic olefin (A') and a structural unit (B) derived from a cyclic olefin (B').

[0019] The non-cyclic olefin (A') refers to an olefin which is not a cyclic olefin, specifically, a linear or branched olefin.

[0020] The structural unit (B) derived from the cyclic olefin (B') is not particularly limited, and examples thereof include the cyclic olefin monomers described in paragraphs 0037 to 0063 of WO 2006 / 118261.

[0021] In the cyclic olefin copolymer according to the present embodiment, from the viewpoint of improving heat resistance and improving moldability while maintaining a good balance between the transparency and refractive index of the obtained molded article, it is preferable that the structural unit (A) has a structure represented by the following general formula (I) and the structural unit (B) has a structure represented by the following general formula (VI), and it is more preferable that the structural unit (A) contains a structural unit derived from ethylene and the structural unit (B) contains a structural unit derived from benzonorbornadiene.

[0022] [ka] In the above general formula (I), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms.

[0023] [ka] In the above general formula (VI), q is 1, 2 or 3; R 32 ~R 39 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, and when q=1, R 36 and R 37 , R 37 and R 38 , R 38 and R 39 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 36 and R 36 , R 36 and R 37 , R 37 and R 38 , R 38 and R 39 , R 39 and R 39 may be bonded to each other to form a monocycle or polycycle, the monocycle or polycycle may have a double bond, and the monocycle or polycycle may be an aromatic ring.

[0024] A specific example of the acyclic olefin (A') according to this embodiment is an olefin monomer represented by the following general formula (Ia) which corresponds to the above general formula (I).

[0025] [ka] In the above general formula (Ia), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms. Examples of the olefin monomer represented by the general formula (Ia) include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. From the viewpoint of obtaining a molded product having better heat resistance, mechanical properties, and optical properties, ethylene and propylene are preferred, and ethylene is more preferred.

[0026] Two or more kinds of olefin monomers represented by the above general formula (Ia) may be used.

[0027] A specific example of the cyclic olefin (B') according to this embodiment is a cyclic olefin monomer represented by general formula (VIa) which corresponds to the above general formula (VI).

[0028] [ka] In the above general formula (VIa), q is 1, 2 or 3. q is preferably 1 or 2, and more preferably 1. R 32 ~R 39R each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom. 32 ~R 39 are each independently preferably a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and more preferably a hydrogen atom. Also, when q=1, R 36 and R 37 , R 37 and R 38 , R 38 and R 39 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 36 and R 36 , R 36 and R 37 , R 37 and R 38 , R 38 and R 39 , R 39 and R 39 may be bonded to each other to form a monocycle or polycycle, the monocycle or polycycle may have a double bond, and the monocycle or polycycle may be an aromatic ring. Examples of the hydrocarbon group having 1 to 20 carbon atoms include, independently, an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, and an aromatic hydrocarbon group. More specifically, examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, an amyl group, a hexyl group, an octyl group, a decyl group, a dodecyl group, and an octadecyl group. Examples of the cycloalkyl group include a cyclohexyl group. Examples of the aromatic hydrocarbon group include an aryl group or an aralkyl group such as a phenyl group, a tolyl group, a naphthyl group, a benzyl group, and a phenylethyl group. These hydrocarbon groups may be substituted with a halogen atom other than a fluorine atom.

[0029] Two or more kinds of cyclic olefin monomers represented by the above general formula (VIa) may be used.

[0030] When the olefin monomer represented by the general formula (Ia) and the cyclic olefin monomer represented by the general formula (VIa) are used as copolymerization components, the olefin monomer represented by the general formula (Ia) can impart flexibility to the resin composition, and the cyclic olefin monomer represented by the general formula (VIa) can increase the refractive index of the resin composition or increase the glass transition temperature, thereby improving the heat resistance.

[0031] As the cyclic olefin monomer represented by the above general formula (VIa), it is preferable to use a monomer in which q=1 in the general formula (VIa). Since these cyclic olefins have one benzene ring, they have the advantage that it is easier to obtain a resin composition that is less likely to be colored than when they have two or more benzene rings. In particular, it is preferable to use benzonorbornadiene. The advantage of using benzonorbornadiene is that it has an aromatic ring, so that the refractive index of the resin composition can be increased.

[0032] The copolymerization type of the cyclic olefin copolymer according to the present embodiment is not particularly limited, and examples thereof include random copolymers, block copolymers, etc. In the present embodiment, a random copolymer is preferable from the viewpoint of obtaining optical components with excellent optical properties such as transparency, refractive index, and birefringence, and high precision.

[0033] The cyclic olefin copolymer according to this embodiment is preferably a random copolymer of ethylene and benzonorbornadiene.

[0034] When the total content of the structural unit (A) and the structural unit (B) in the cyclic olefin copolymer is taken as 100 mol%, the content of the structural unit (A) in the cyclic olefin copolymer according to the present embodiment is preferably 50 mol% or more and 68 mol% or less, more preferably 50 mol% or more and 65 mol% or less, and even more preferably 50 mol% or more and 63 mol% or less. This allows the crystallization degree and melting point of the cyclic olefin copolymer to be adjusted to an appropriate range from the viewpoint of chemical resistance, and the chemical resistance can be further improved.

[0035] When the total content of the structural unit (A) and the structural unit (B) in the cyclic olefin copolymer is taken as 100 mol%, the content of the structural unit (B) in the cyclic olefin copolymer according to the present embodiment is preferably 32 mol% to 50 mol%, more preferably 35 mol% to 50 mol%, and even more preferably 37 mol% to 50 mol%. This allows the crystallinity and melting point of the cyclic olefin copolymer to be adjusted to an appropriate range from the viewpoint of chemical resistance, thereby further improving chemical resistance.

[0036] The above content is, when the cyclic olefin copolymer is well dissolved in the NMR heavy solvent, 13 If the solubility is poor, the measurement is performed by FT-IR. The detailed measurement method will be described later.

[0037] The cyclic olefin copolymer according to the present embodiment may have other structural units (C) derived from monomers other than the acyclic olefin (A') and the cyclic olefin (B') within the scope of not impairing the effects of the present invention. Examples of the monomers other than the acyclic olefin (A') and the cyclic olefin (B') include acrylic monomers such as acrylic acid and methacrylic acid, vinyl monomers such as vinyl chloride monomers, and styrene monomers.

[0038] The application of the cyclic olefin copolymer according to this embodiment is not particularly limited, and it can be used for films, sheets, lenses, containers, etc. Since the cyclic olefin copolymer according to this embodiment has excellent chemical resistance, it can withstand use in harsh environments where it is likely to be exposed to highly soluble organic solvents such as toluene.

[0039] The applications of the cyclic olefin copolymer according to the present embodiment include, for example, optical materials such as optical disks, optical lenses, prisms, light diffusion plates, optical cards, optical fibers, optical mirrors, liquid crystal display element substrates, light guide plates, polarizing films, and retardation films; containers for liquid, powder, or solid medicines (liquid medicine containers for injection, ampoules, vials, prefilled syringes, infusion bags, sealed medicine bags, press-through packages, solid medicine containers, eye drop containers, etc.), sampling containers (sampling test tubes for blood tests, medicine container caps, blood collection tubes, specimen containers, etc.), medical Medical equipment such as instruments (syringes, etc.), sterilized containers for medical instruments (for scalpels, forceps, gauze, contact lenses, etc.), laboratory and analytical instruments (beakers, petri dishes, flasks, test tubes, centrifuge tubes, etc.), medical optical parts (plastic lenses for medical testing, etc.), piping materials (medical infusion tubes, piping, joints, valves, etc.), artificial organs and their parts (denture bases, artificial hearts, artificial tooth roots, etc.); food containers such as bottles, returnable bottles, baby bottles, films, shrink films; processing or transport containers (tanks, trays, carriers, cases, etc.), protective materials ( Electronic component processing equipment for electronic devices (carrier tapes, separation films, etc.), piping (pipes, tubes, valves, flow meters, filters, pumps, etc.), liquid containers (sampling containers, bottles, ampoule bags, etc.); coating materials (for electric wires, cables, etc.), consumer and industrial electronic device housings (copying machines, computers, printers, televisions, video decks, video cameras, etc.), structural members (parabolic antenna structural members, flat antenna structural members, radar dome structural members, etc.); general circuit boards (rigid printed circuit boards, flexible printed circuit boards, etc.) circuit boards such as circuit boards for semiconductor devices (such as LCD substrates, multilayer printed wiring boards, etc.) and high-frequency circuit boards (such as circuit boards for satellite communication equipment); base materials for transparent conductive films (such as liquid crystal substrates, optical memory, surface heating elements, etc.); encapsulants for semiconductors (such as transistor encapsulant, IC encapsulant, LSI encapsulant, LED encapsulant, etc.) and encapsulants for electric and electronic components (such as motor encapsulant, capacitor encapsulant, switch encapsulant, sensor encapsulant, etc.); automotive interior materials such as room mirrors and meter covers; automotive exterior materials such as door mirrors, fender mirrors, beam lenses, light covers, etc.

[0040] In addition, examples of applications of the cyclic olefin copolymer according to this embodiment include circuit boards such as general circuit boards (rigid printed circuit boards, flexible printed circuit boards, multilayer printed wiring boards, etc.) and high-frequency circuit boards (circuit boards for satellite communication devices, etc.); base materials for transparent conductive films (liquid crystal substrates, optical memories, surface heating elements, etc.); encapsulants for semiconductors (transistor encapsulants, IC encapsulants, LSI encapsulants, LED encapsulants, etc.) and encapsulants for electric / electronic components (motor encapsulants, capacitor encapsulants, switch encapsulants, sensor encapsulants, etc.); automotive interior materials such as room mirrors and meter covers; and automotive exterior materials such as door mirrors, fender mirrors, beam lenses, and light covers.

[0041] The cyclic olefin copolymer according to the present embodiment can be produced by any production method. For example, it can be produced by appropriately selecting conditions according to the methods described in JP-A-60-168708, JP-A-61-120816, JP-A-61-115912, JP-A-61-115916, JP-A-61-271308, JP-A-61-272216, JP-A-62-252406, JP-A-62-252407, etc. Furthermore, the cyclic olefin copolymer according to the present embodiment, which is a ring-opening polymer of a cyclic olefin, can be produced by appropriately selecting the conditions according to the methods described in, for example, JP-A-60-26024, JP-A-9-268250, JP-A-63-145324, JP-A-2001-72839, and the like.

[0042] The cyclic olefin copolymer according to the present embodiment can be produced by the following production method.

[0043] [Method of producing cyclic olefin copolymer] The process for producing a cyclic olefin copolymer of the present invention will be described in detail below.

[0044] The method for producing a cyclic olefin copolymer according to this embodiment is the method for producing the cyclic olefin copolymer described above, and includes a step of copolymerizing a non-cyclic olefin (A') and a cyclic olefin (B') in the presence of a catalyst containing a transition metal compound (X) represented by the following general formula (1), wherein the non-cyclic olefin (A') has a structure represented by the above general formula (Ia), and the cyclic olefin (B') has a structure represented by the above general formula (VIa).

[0045] In the method for producing a cyclic olefin copolymer according to this embodiment, it is preferable that the non-cyclic olefin (A') contains ethylene, and the cyclic olefin (B') contains benzonorbornadiene.

[0046] [ka]

[0047] In the above general formula (1), M 1 indicates a transition metal atom in group 4 of the periodic table, and X 1 each independently represents an atom or group selected from the group consisting of a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, and an aluminum-containing group, and substitution products thereof; n 1 represents an integer from 1 to 4, and Y 1 represents a carbon atom or a silicon atom, and R 1 ~R 14 each independently represents an atom or group selected from the group consisting of a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, and an aluminum-containing group, and a substitution product thereof; R 1 ~R 14 adjacent ones of R may be bonded to each other to form a ring, and the ring formed may have aromaticity including a conjugated double bond; 1 ~R 14at least one of which is a group selected from the group consisting of a hydrocarbon group having one or more carbon atoms, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, and an aluminum-containing group, and substitution products thereof.

[0048] According to the production method of the present embodiment, a cyclic olefin copolymer having excellent chemical resistance can be produced. Although the detailed mechanism by which a cyclic olefin copolymer having excellent chemical resistance can be produced is unclear, the catalyst containing the transition metal compound (X) represented by the above general formula (1) has a substituent R 1 ~R 14 Among these, one or more are characterized by being a group having a certain degree of bulkiness, such as a group containing a heteroatom, such as a halogen-containing group or an oxygen-containing group, or a hydrocarbon group having one or more carbon atoms, such as a methyl group or a t-butyl group, and it is presumed that the presence of such a bulky substituent has some effect on the crystallinity of the cyclic olefin copolymer, thereby improving the chemical resistance. This effect is more pronounced when there are multiple bulky substituents.

[0049] Specific examples of the transition metal compound (X) represented by the general formula (1) are not particularly limited, but include, for example, dimethylmethylene(3-tert-butyl-cyclopentadienyl)(3,6-di-tert-butyl-fluorenyl)zirconium dichloride, dimethylmethylene(3-methyl-cyclopentadienyl)(fluorenyl)zirconium dichloride, and the like.

[0050] The production method according to this embodiment is a method for producing a cyclic olefin copolymer comprising a step of copolymerizing a non-cyclic olefin (A') and a cyclic olefin (B') (hereinafter also simply referred to as a polymerization step).

[0051] In the polymerization step of the production method according to the present embodiment, the acyclic olefin (A') may be an olefin monomer represented by the above general formula (Ia), and non-limiting specific examples thereof are as described above. Among them, from the same viewpoint as above, ethylene and propylene are preferred, and ethylene is more preferred. In the polymerization step of the production method according to the present embodiment, the cyclic olefin (B') may be a cyclic olefin monomer represented by the above general formula (VIa), and non-limiting specific examples thereof are as described above. Among them, benzonorbornadiene is preferred from the same viewpoint as above.

[0052] In the polymerization step of the production method according to the present embodiment, when the total content of the non-cyclic olefin (A') and the cyclic olefin (B') is taken as 100 mol%, from the same viewpoint as above, the content of the non-cyclic olefin (A') is preferably 50 mol% or more and 68 mol% or less, more preferably 50 mol% or more and 65 mol% or less, and even more preferably 50 mol% or more and 63 mol% or less, and further, the content of the cyclic olefin (B') is preferably 32 mol% or more and 50 mol% or less, more preferably 35 mol% or more and 50 mol% or less, and even more preferably 37 mol% or more and 50 mol% or less, from the same viewpoint as above.

[0053] The temperature of the polymerization step in the production method according to the present embodiment is preferably 20° C. or higher, more preferably 30° C. or higher, and even more preferably 40° C. or higher from the viewpoint of improving the reaction efficiency, and is preferably 100° C. or lower, more preferably 80° C. or lower, and even more preferably 60° C. or lower from the viewpoint of suppressing catalyst deactivation and side reactions.

[0054] The polymerization step of the production method according to the present embodiment may be carried out in a solvent or without a solvent. The solvent used in the polymerization step of the production method according to the present embodiment includes, for example, one or more solvents selected from the group consisting of tetrahydrofuran, toluene, cyclohexane, cyclohexanone, MEK, MIBK, PGMEA, PGME, ethyl acetate, and methyl acetate, and preferably includes toluene.

[0055] In the polymerization step of the production method according to the present embodiment, any component other than the catalyst containing the transition metal compound (X) represented by the above general formula (1) may be used. For example, an organoaluminum oxy compound described later may be used as a co-catalyst.

[0056] <Transition metal compound (X)> In the polymerization step of the production method according to this embodiment, a polymerization reaction is carried out in the presence of a transition metal compound (X) represented by the following general formula (1).

[0057] [ka]

[0058] In the above general formula (1), M 1 indicates a transition metal atom in Group 4 of the periodic table. M 1 Examples of such atoms include a titanium atom, a zirconium atom, and a hafnium atom.

[0059] M 1 is preferably a titanium atom or a zirconium atom, and more preferably a zirconium atom.

[0060] In the above general formula (1), X 1 each independently represents an atom or group selected from the group consisting of a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, and an aluminum-containing group, and substitution products thereof.

[0061] X 1 The halogen atom represented by the formula (I) can be exemplified by a fluorine atom, a chlorine atom, a bromine atom, and the like.

[0062] In the above general formula (1), X 1 Examples of the hydrocarbon group represented by the formula (I) include alkyl groups such as a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a t-butyl group, a hexyl group, an octyl group, a 2-ethylhexyl group, and a decyl group; cycloalkyl groups such as a cyclopentyl group, a cyclohexyl group, a cyclooctyl group, a norbornyl group, a bicyclononyl group, and a tricyclodecane group; aryl groups such as a phenyl group, a tolyl group, a naphthyl group, a biphenyl group, a terphenyl group, a phenanthryl group, and an anthracenyl group; aralkyl groups such as a benzyl group or a phenylethyl group; and divalent diene derivative groups such as a 1,3-butadienyl group, an isoprenyl (2-methyl-1,3-butadienyl) group, a piperylenyl (1,3-pentadienyl) group, a 2,4-hexadienyl group, a 1,4-diphenyl-1,3-pentadienyl group, and a cyclopentadienyl group.

[0063] In the above general formula (1), X 1 Examples of the halogen-containing group represented by the formula (I) include halogen-containing hydrocarbon groups such as trifluoromethyl, pentafluoroethyl, 1,1,1,3,3,3-hexafluoro-2-propyl, and nonafluoro-t-butyl; halogen-containing aryl groups such as pentafluorophenyl, pentachlorophenyl; and the like.

[0064] In the above general formula (1), X 1Examples of the oxygen-containing group represented by the formula (I) include alkoxy groups such as a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, or a t-butoxy group; aryloxy groups such as a phenoxy group, a 2,6-dimethylphenoxy group, or a 2,4,6-trimethylphenoxy group; ester groups such as an acetyloxy group, a benzoyloxy group, a methoxycarbonyl group, a phenoxycarbonyl group, or a p-chlorophenoxycarbonyl group; ether groups; acyl groups such as a formyl group, an acetyl group, a benzoyl group, a p-chlorobenzoyl group, or a p-methoxybenzoyl group; a carboxyl group; a carbonate group; a hydroxy group; a peroxy group; a carboxylic anhydride group; a furyl group; Examples include:

[0065] In the above general formula (1), X 1 Examples of the sulfur-containing group represented by the formula (I) include a mercapto group; a thioester group, such as an acetylthio group, a benzoylthio group, a methylthiocarbonyl group, or a phenylthiocarbonyl group; a dithioester group; an alkylthio group, such as a methylthio group or an ethylthio group; an arylthio group, such as a phenylthio group, a methylphenylthio group, or a naphthylthio group; a thioacyl group; a thioether group; a thiocyanate ester group; an isothiocyanate ester group; a sulfonate ester group, such as a methyl sulfonate group, an ethyl sulfonate group, or a phenyl sulfonate group; a sulfonamide group, such as a phenylsulfonamide group, an N-methylsulfonamide group, or an N-methyl-p-toluenesulfonamide group; a thiocarboxyl group; a dithiocarboxyl group; a sulfo group; a sulfonyl group; a sulfinyl group; a sulfenyl group; and the like.

[0066] In the above general formula (1), X 1Examples of the nitrogen-containing group represented by the formula (I) include an amino group; alkylamino groups such as a dimethylamino group or an ethylmethylamino group; arylamino groups such as a diphenylamino group; an imino group; alkylimino groups such as a methylimino group, an ethylimino group, a propylimino group, or a butylimino group; arylimino groups such as a phenylimino group; an amido group; alkylamido groups such as an acetamido group or an N-methylacetamido group; arylamido groups such as an N-methylbenzamido group; an imido group; alkylimido groups such as an acetimido group; arylimido groups such as a benzimido group; a pyrrolidino group; a hydrazino group; a hydrazono group; a nitro group; a nitroso group; a cyano group; an isocyano group; a cyanate ester group; an amidino group; a diazo group; and an amino group in the form of an ammonium salt. Also, X 1 Examples of the nitrogen-containing group represented by the formula (I) include a silylamide group and a phosphinoamide group.

[0067] In the above general formula (1), X 1 Examples of the phosphorus-containing group represented by the formula (I) include a phosphido group, a phosphoryl group, a thiophosphoryl group, a phosphate group, and the like.

[0068] In the above general formula (1), X 1 Examples of the silicon-containing group represented by the formula (I) include alkylsilyl groups such as a methylsilyl group, a dimethylsilyl group, a trimethylsilyl group, an ethylsilyl group, a diethylsilyl group, a triethylsilyl group, a diphenylmethylsilyl group, a triphenylsilyl group, a dimethylphenylsilyl group, and a dimethyl-t-butylsilyl group.

[0069] In the above general formula (1), X 1 Examples of the boron-containing group represented by the formula (I) include a boranediyl group, a boranetriyl group, a diboranyl group, and the like. In the above general formula (1), X 1Examples of the boron-containing group substituents represented by the formula (I) include alkyl group-substituted boron represented by (Et)B-, (iPr)B-, (iBu)B-, (Et)B, (iPr)B, (iBu)B, etc.; aryl group-substituted boron represented by (C6H5)B-, (C6H5)B, (C6F5)B, (3,5-(CF3)2C6H3)3B, etc.; boron halide represented by BCl2- or BCl3, etc.; alkyl group-substituted boron halide represented by (Et)BCl-, (iBu)BCl-, (C6H5)2BCl, etc.; and the like. Here, Et represents an ethyl group, iPr represents an isopropyl group, and iBu represents an isobutyl group.

[0070] In the above general formula (1), X 1 Examples of the aluminum-containing group substituents represented by the formula (I) include alkyl group-substituted aluminum represented by (Et)Al-, (iPr)Al-, (iBu)Al-, (Et)Al, (iPr)Al or (iBu)Al, etc.; aryl group-substituted aluminum represented by (CH)Al-, etc.; aluminum halides represented by AlCl- or AlCl, etc.; alkyl group-substituted aluminum halides represented by (Et)AlCl-, (iBu)AlCl-, etc.; and the like. Here, Et represents an ethyl group, iPr represents an isopropyl group, and iBu represents an isobutyl group.

[0071] In the above general formula (1), X 1 is a group selected from the group consisting of a hydrocarbon group, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, an aluminum-containing group, and substituted groups thereof, 1 Each of these independently preferably has 1 to 20 carbon atoms.

[0072] In the above general formula (1), X 1 are each independently preferably a halogen atom or a hydrocarbon group, and more preferably a halogen atom.

[0073] In the above general formula (1), X1 When is a halogen atom, X 1 More preferably, each independently is a chlorine atom.

[0074] In the above general formula (1), n 1 represents an integer of 1 to 4. 1 is M 1 Valence and X 1 Depending on the type of, the transition metal compound (X) represented by the above general formula (1) is selected so that the entire transition metal compound (X) is electrically neutral.

[0075] In the above general formula (1), n 1 is preferably 2 or 3, and more preferably 2.

[0076] In the above general formula (1), Y 1 represents a carbon atom or a silicon atom.

[0077] In the above general formula (1), Y 1 is preferably a carbon atom.

[0078] In the above general formula (1), R 1 ~R 14 each independently represents an atom or group selected from the group consisting of a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, and an aluminum-containing group, and substitution products thereof.

[0079] In the above general formula (1), R 1 ~R 14 Examples of the halogen atom, hydrocarbon group, halogen-containing group, oxygen-containing group, sulfur-containing group, nitrogen-containing group, phosphorus-containing group, silicon-containing group, boron-containing group and aluminum-containing group represented by X, as well as their substitutes, include 1 Examples of the halogen atom include a halogen atom, a hydrocarbon group, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group and an aluminum-containing group, as well as those exemplified as substituents thereof.

[0080] In the above general formula (1), R 1 ~R 14 Adjacent ones of these may be bonded to each other to form a ring, and the ring formed may have aromaticity by containing a conjugated double bond.

[0081] In the above general formula (1), R 1 ~R 14 Among these, adjacent ones are bonded to each other to form a ring, and the ring formed is preferably bonded to a cyclopentadienyl group. The structure in which the ring formed is bonded to a cyclopentadienyl group is, for example, the structure shown below, and is preferably a fluorenyl ring structure.

[0082] [ka]

[0083] In the above general formula (1), R 1 ~R 14 At least one of the groups is selected from the group consisting of halogen-containing groups, oxygen-containing groups, sulfur-containing groups, nitrogen-containing groups, phosphorus-containing groups, silicon-containing groups, boron-containing groups, aluminum-containing groups, and hydrocarbon groups having one or more carbon atoms, and substitution products thereof.

[0084] In the above general formula (1), R 1 ~R 14 It is preferable that at least one of R is a hydrocarbon group having one or more carbon atoms. 1 ~R 14 It is more preferable that at least one of R is a hydrocarbon group having 4 or more carbon atoms. 1 ~R 14 More preferably, one or more of R 1 ~R 14 More preferably, two or more of R 1 ~R 14It is more preferable that three or more of the groups are t-butyl groups, which further improves the chemical resistance of the resulting cyclic olefin copolymer. R 1 ~R 14 Although the detailed mechanism by which the chemical resistance of the cyclic olefin copolymer obtained by having one or more of these groups is improved is unclear, it is presumed that the catalyst having bulky groups such as methyl groups and t-butyl groups has some effect on the crystallinity of the cyclic olefin copolymer, thereby improving the chemical resistance. This effect is more pronounced when there are multiple bulky substituents.

[0085] <Organoaluminum oxy compound> In the polymerization step of the production method according to this embodiment, an organoaluminum oxy compound can be used as a co-catalyst.

[0086] As the organoaluminum oxy-compound, any of the conventionally known organoaluminum oxy-compounds can be used. Specific examples include compounds represented by the following formulas [B2-1], [B2-2], [B2-3] and [B2-4], benzene-insoluble organoaluminum oxy compounds described in JP-A-2-78687 and JP-A-2-167305, and aluminoxanes having two or more types of alkyl groups described in JP-A-3-103407.

[0087] [ka]

[0088] In the formula, R represents a hydrocarbon group having 1 to 10 carbon atoms, and n represents an integer of 2 or more.

[0089] [ka]

[0090] In the formula, R represents a hydrocarbon group having 1 to 10 carbon atoms, and n represents an integer of 2 or more.

[0091] [ka]

[0092] In the formula, R represents a hydrocarbon group having 1 to 10 carbon atoms, Me represents a methyl group, and m and n each independently represent an integer of 2 or more.

[0093] The compound represented by formula [B2-3] is called modified methylaluminoxane, and is prepared using trimethylaluminum and alkylaluminum other than trimethylaluminum. Such compounds are generally called MMAO. Such MMAO can be prepared by the methods described in U.S. Pat. No. 4,960,878 and U.S. Pat. No. 5,041,584.

[0094] [ka]

[0095] In the formula, R c R represents a hydrocarbon group having 1 to 10 carbon atoms. d may be the same or different and represent a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms.

[0096] As the organoaluminum oxy compound, methylaluminoxane, which is a commercially available product and therefore easily available, and MMAO prepared using trimethylaluminum and triisobutylaluminum are preferred.

[0097] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0098] Hereinafter, the embodiments of the present invention will be described in detail based on examples, but the embodiments of the present invention are not limited to these examples.

[0099] [Method for measuring polymerization activity] The powdered cyclic olefin copolymer obtained by the method described in each Example and Comparative Example was weighed, and the polymer yield was measured. The polymerization activity (unit: kg / (mmol hr)) was calculated by dividing the polymer yield by the amount of catalyst and the polymerization reaction time.

[0100] [Method of composition analysis] ( 13 C-NMR measurement) In principle, the composition analysis of cyclic olefin copolymers is 13 The powdered cyclic olefin copolymer obtained by the method described in each of the Examples and Comparative Examples was measured under the following measurement conditions, and the composition analysis was performed by calculating the area intensity ratio between the peak derived from BNBD appearing around 43.5 ppm and the peak derived from ethylene appearing around 30 to 32 ppm. Apparatus: Bruker Biospin AVANCEIII cryo-500 type nuclear magnetic resonance Measurement nuclei: 13 C(125MHz) Measurement mode: Single pulse proton (with inverse gate) decoupling Pulse width: 90 degrees Number of points: 64000 Measurement range: -55 to 195 ppm (total 250 ppm) Repeat time: 25 seconds Number of times accumulated: 256 Solvent: 1,1,2,2-tetrachloroethane-d2 Concentration: 20mg / 0.6mL Temperature: 120℃ Chemical shift standard: 74.2 ppm of 1,1,2,2-tetrachloroethane-d2

[0101] (FT-IR measurement) When the solubility of the cyclic olefin copolymer in the above-mentioned NMR heavy solvent was poor, composition analysis was performed by FT-IR measurement. For the measurement, a tablet sample was prepared by compressing the powdered cyclic olefin copolymer obtained by the method described in each Example and Comparative Example with a tablet press. The measurement was performed under the following conditions, and the quantitative peak of benzonorbornadiene (also called BNBD) was 1608 cm. -1 (Benzene ring C=C stretching vibration), base peak at 4257 cm -1 (The combination vibration of CH stretching vibration and CH2 bending vibration) was detected and the absorbance of each was calculated. 13 The BNBD content determined by C-NMR was plotted on the horizontal axis against the ratio of the absorbance of the quantitative peak to the absorbance of the reference peak on the vertical axis to create a linear calibration curve, and composition analysis was performed based on this calibration curve. Equipment: JASCO FT / IR-4200 Measurement method: Transmission method / Tablet sample Number of times: 32 Wavenumber resolution: 2cm -1 Measurement wave number range: 5000~400cm -1

[0102] [X-ray diffraction measurement (XRD measurement) method] The powdered cyclic olefin copolymer obtained by the method described in each Example and Comparative Example was subjected to wide-angle X-ray diffraction measurement, and the crystal-derived peak area, which is the area of ​​the peak derived from the crystal, and the amorphous halo-derived area, which is the area of ​​the halo derived from the amorphous, were calculated using the following formula. When multiple crystal-derived peaks appeared, the total area of ​​the multiple peaks was taken as the crystal-derived peak area. The X-ray diffraction pattern was analyzed using a profile fitting method. For the profile fitting, analysis software attached to the X-ray diffractometer (manufactured by Spectris Co., Ltd., product name: High Score) was used. Crystallinity (%) = crystalline peak area / (crystalline peak area + amorphous halo area) x 100 Equipment: EMPYREAN, manufactured by Spectris X-ray source: CuKα ray Output: 45kV 40mA Measurement range: 3°~35° Scan speed: 1° / min Step width: 0.026° Detector: PIXcel 3D

[0103] [DSC measurement method] The powdered cyclic olefin copolymers obtained by the methods described in the respective Examples and Comparative Examples were subjected to DSC measurement under the following measurement conditions. (1) Using a differential scanning calorimeter (Hitachi High-Tech Science, DSC7020), the cyclic olefin copolymer was heated from room temperature to 350° C. at a heating rate of 10° C. / min under a nitrogen atmosphere. (2) Held at 350°C for 5 minutes. (3) The temperature was decreased to -20°C at a rate of 10°C / min. (4) The mixture was kept at -20°C for 5 minutes. (5) The temperature was increased to 350°C at a rate of 10°C / min. The endothermic peak observed in the DSC curve obtained in the second heating step of the measurement performed according to the above procedure was taken as the melting peak, and the temperature at the apex of the melting peak was taken as the melting point.

[0104] [Chemical resistance (toluene resistance) test] The powdered cyclic olefin copolymer obtained by the method described in each Example and Comparative Example was added to toluene to a concentration of 5% by mass, and allowed to stand overnight at room temperature (23° C.). After standing, the state of the cyclic olefin copolymer added to the toluene was visually observed and evaluated according to the following criteria. +: The polymer did not dissolve and precipitated at the bottom of the container. -: The polymer does not dissolve, but is swollen with the solvent and becomes cloudy. --: The polymer is dissolved, there is no residue and it is transparent.

[0105] [Example 1] A 500 mL glass autoclave that had been thoroughly purged with nitrogen was charged with 300 mL of toluene and 23.8 g of benzonorbornadiene, and ethylene gas and nitrogen gas were passed through at flow rates of 6 L / hour and 96 L / hour, respectively. The mixture was heated to 50°C while stirring at 600 rpm, and then maintained at that temperature for 10 minutes. Next, 0.03 mmol of catalyst 1 (dimethylmethylene (3-tert-butyl-cyclopentadienyl) (3,6-di-tert-butyl-fluorenyl) zirconium dichloride) and 9.0 mmol of methylaluminoxane were charged, respectively, to initiate polymerization. After polymerization at 50°C for 10 minutes under normal pressure, an excess amount of isopropanol was added to terminate the polymerization, and a polymer solution was obtained. The copolymer was not dissolved in the solvent during the polymerization reaction and precipitated, so the polymer solution was cloudy. The obtained polymer solution was added to an excess amount of a methanol / acetone mixed solution (mixture ratio 1 / 3 (volume ratio)) to which 9 mL of hydrochloric acid had been added, and the polymer was precipitated. The precipitated polymer was taken out and dried under reduced pressure at 130°C overnight, and 1.14 g of a powdered ethylene and benzonorbornadiene copolymer was obtained. The polymerization activity was 0.23 kg / mmol·hr. The composition of the obtained ethylene-benzonorbornadiene copolymer was 52 mol% of structural unit (A) ethylene and 48 mol% of structural unit (B) benzonorbornadiene. The composition analysis was performed by FT-IR measurement because of poor solubility in NMR heavy solvents. By XRD measurement, crystal-derived peaks were observed around 2θ=7°, 14°, 16°, 17°, 21°, and 23°, and the crystallinity calculated by the above-mentioned method was 21%. In the DSC measurement, the temperature was raised from -20°C to 350°C, but no melting peak was detected, so the melting point was determined to be above 350°C. Regarding the chemical resistance to toluene, the polymer did not dissolve and precipitated at the bottom of the container (chemical resistance to toluene: +).

[0106] [Example 2] A 500 mL glass autoclave that had been thoroughly purged with nitrogen was charged with 300 mL of toluene and 19.4 g of benzonorbornadiene, and ethylene gas and nitrogen gas were passed through at flow rates of 24 L / hour and 72 L / hour, respectively. The mixture was heated to 50°C while stirring at 600 rpm, and then maintained at that temperature for 10 minutes. Next, 0.01 mmol of catalyst 1 and 3.0 mmol of methylaluminoxane were charged to initiate polymerization. After polymerization at 50°C for 10 minutes under normal pressure, an excess amount of isopropanol was added to terminate the polymerization, and a polymer solution was obtained. The copolymer was not dissolved in the solvent during the polymerization reaction and precipitated, so the polymer solution was cloudy. The obtained polymer solution was added to an excess amount of a mixed solution of methanol / acetone (mixture ratio 1 / 3 (volume ratio)) to which 3 mL of hydrochloric acid had been added, and the polymer was precipitated. The precipitated polymer was taken out and dried under reduced pressure at 130°C overnight, and 3.92 g of a powdered copolymer of ethylene and benzonorbornadiene was obtained. The polymerization activity was 2.35 kg / mmol·hr. The composition of the obtained ethylene-benzonorbornadiene copolymer was 59 mol% of structural unit (A) ethylene and 41 mol% of structural unit (B) benzonorbornadiene. The composition was analyzed by FT-IR measurement because of poor solubility in heavy solvents for NMR. By XRD measurement, crystal-derived peaks were observed around 2θ=7°, 14°, 16°, 17°, 21°, and 23°, and the crystallinity calculated by the above-mentioned method was 17%. In the DSC measurement, the temperature was raised from -20°C to 350°C, but no melting peak was detected, so the melting point was determined to be above 350°C. Regarding the chemical resistance to toluene, the polymer did not dissolve and precipitated at the bottom of the container (chemical resistance to toluene: +).

[0107] [Example 3] A 500 mL glass autoclave that had been thoroughly purged with nitrogen was charged with 300 mL of toluene and 16.0 g of benzonorbornadiene, and ethylene gas and nitrogen gas were passed through at flow rates of 24 L / hour and 72 L / hour, respectively. The mixture was heated to 50°C while stirring at 600 rpm, and then maintained at that temperature for 10 minutes. Next, 0.003 mmol of catalyst 1 and 0.9 mmol of methylaluminoxane were charged to initiate polymerization. After polymerization at 50°C for 10 minutes under normal pressure, an excess amount of isopropanol was added to terminate the polymerization, and a polymer solution was obtained. The copolymer was not dissolved in the solvent during the polymerization reaction and precipitated, so the polymer solution was cloudy. The obtained polymer solution was added to an excess amount of a mixed solution of methanol / acetone (mixture ratio 1 / 3 (volume ratio)) to which 0.9 mL of hydrochloric acid had been added, and the polymer was precipitated. The precipitated polymer was taken out and dried under reduced pressure at 130°C overnight, and 1.34 g of a powdered copolymer of ethylene and benzonorbornadiene was obtained. The polymerization activity was 2.69 kg / mmol·hr. The composition of the obtained ethylene-benzonorbornadiene copolymer is 13 C-NMR measurement revealed that the structural unit (A) was 64 mol% ethylene and the structural unit (B) was 36 mol% benzonorbornadiene. By XRD measurement, crystal-derived peaks were observed around 2θ=7°, 14°, 16°, 17°, 21°, and 23°, and the crystallinity calculated by the above-mentioned method was 6%. A melting peak was detected by DSC measurement, and the melting point was 293°C. Regarding the chemical resistance to toluene, the polymer did not dissolve and precipitated at the bottom of the container (chemical resistance to toluene: +).

[0108] [Example 4] A 500 mL glass autoclave that had been thoroughly purged with nitrogen was charged with 300 mL of toluene and 13.6 g of benzonorbornadiene, and ethylene gas and nitrogen gas were passed through at flow rates of 24 L / hour and 72 L / hour, respectively. The mixture was heated to 50°C while stirring at 600 rpm, and then maintained at that temperature for 10 minutes. Next, 0.003 mmol of catalyst 1 and 0.9 mmol of methylaluminoxane were charged to initiate polymerization. After polymerization at 50°C for 10 minutes under normal pressure, an excess amount of isopropanol was added to terminate the polymerization, and a polymer solution was obtained. The copolymer was not dissolved in the solvent during the polymerization reaction and precipitated, so the polymer solution was cloudy. The obtained polymer solution was added to an excess amount of a mixed solution of methanol / acetone (mixture ratio 1 / 3 (volume ratio)) to which 0.9 mL of hydrochloric acid had been added, and the polymer was precipitated. The precipitated polymer was taken out and dried under reduced pressure at 130°C overnight, and 1.41 g of a powdered copolymer of ethylene and benzonorbornadiene was obtained. The polymerization activity was 2.88 kg / mmol·hr. The composition of the obtained ethylene-benzonorbornadiene copolymer is 13 C-NMR measurement revealed that the structural unit (A) was 66 mol% ethylene and the structural unit (B) was 34 mol% benzonorbornadiene. By XRD measurement, peaks derived from crystals were observed at 2θ=approximately 14° and 16°, and the degree of crystallinity calculated by the above-mentioned method was 2%. A melting peak was detected by DSC measurement, and the melting point was 279°C. Regarding the chemical resistance to toluene, the polymer did not dissolve and precipitated at the bottom of the container (chemical resistance to toluene: +).

[0109] [Example 5] A 500 mL glass autoclave that had been thoroughly purged with nitrogen was charged with 300 mL of toluene and 9.2 g of benzonorbornadiene, and ethylene gas and nitrogen gas were passed through at flow rates of 24 L / hour and 72 L / hour, respectively. The mixture was heated to 50°C while stirring at 600 rpm, and then maintained at that temperature for 10 minutes. Next, 0.002 mmol of catalyst 2 (dimethylmethylene(3-methyl-cyclopentadienyl)(fluorenyl)zirconium dichloride) and 0.6 mmol of methylaluminoxane were charged to initiate polymerization. After polymerization at 50°C for 10 minutes under normal pressure, an excess amount of isopropanol was added to terminate the polymerization, and a polymer solution was obtained. The copolymer was not dissolved in the solvent during the polymerization reaction and precipitated, so the polymer solution was cloudy. The obtained polymer solution was added to an excess amount of a methanol / acetone mixed solution (mixing ratio 1 / 3 (volume ratio)) to which 0.6 mL of hydrochloric acid had been added, and the polymer was precipitated. The precipitated polymer was taken out and dried under reduced pressure at 130°C overnight, and 1.62 g of a powdered ethylene and benzonorbornadiene copolymer was obtained. The polymerization activity was 4.85 kg / mmol·hr. The composition of the obtained ethylene-benzonorbornadiene copolymer is 13 C-NMR measurement revealed that the structural unit (A) was 62 mol% ethylene and the structural unit (B) was 38 mol% benzonorbornadiene. By XRD measurement, peaks derived from crystals were observed at 2θ=approximately 14° and 16°, and the degree of crystallinity calculated by the above-mentioned method was 3%. A melting peak was detected by DSC measurement, and the melting point was 273°C. Regarding the chemical resistance to toluene, the polymer did not dissolve and precipitated at the bottom of the container (chemical resistance to toluene: +).

[0110] [Comparative Example 1] A 500 mL glass autoclave that had been thoroughly purged with nitrogen was charged with 300 mL of toluene and 9.2 g of benzonorbornadiene, and ethylene gas and nitrogen gas were passed through at flow rates of 24 L / hour and 72 L / hour, respectively. The mixture was heated to 50°C while stirring at 600 rpm, and then maintained at that temperature for 10 minutes. Next, 0.005 mmol of catalyst 1 and 1.5 mmol of methylaluminoxane were charged to initiate polymerization. After polymerization at 50°C for 10 minutes under normal pressure, an excess amount of isopropanol was added to terminate the polymerization, and a polymer solution was obtained. The resulting polymer solution was added to an excess amount of a mixed solution of methanol / acetone (mixture ratio 1 / 3 (volume ratio)) to which 1.5 mL of hydrochloric acid had been added, and the polymer was precipitated. The precipitated polymer was taken out and dried under reduced pressure at 130°C overnight, and 2.22 g of a powdered copolymer of ethylene and benzonorbornadiene was obtained. The polymerization activity was 2.67 kg / mmol·hr. The composition of the obtained ethylene-benzonorbornadiene copolymer is 13 C-NMR measurement revealed that the structural unit (A) was 70 mol % ethylene and the structural unit (B) was 30 mol % benzonorbornadiene. No peaks due to crystallinity were confirmed in the XRD measurement, indicating that the polymer was amorphous. Therefore, the crystallinity column in Table 1 shows 0%. In the DSC measurement, the temperature was raised from -20°C to 350°C, but no melting peak was detected. Regarding chemical resistance to toluene, the polymer was not dissolved, but was swollen by the solvent and became cloudy (chemical resistance to toluene: -).

[0111] [Comparative Example 2] A 500 mL glass autoclave that had been thoroughly purged with nitrogen was charged with 300 mL of a cyclohexane / hexane (9 / 1) mixed solution and 18.0 g of benzonorbornadiene, and ethylene gas and hydrogen gas were passed through at flow rates of 90 L / hour and 0.24 L / hour, respectively. The mixture was heated to 50°C while stirring at 600 rpm, and then maintained at that temperature for 10 minutes. Next, 1.5 mmol of triisobutylaluminum (TIBAL), 0.001 mmol of catalyst 3 (3,5-bis-1-methylethyl-1-pyrazolate-t-butylcyclopentadienyl titanium dichloride), and 0.004 mmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were charged to initiate polymerization. After polymerization at 50°C for 3 minutes under normal pressure, an excess amount of isopropanol was added to terminate the polymerization, and a polymer solution was obtained. The obtained polymer solution was added to an excess amount of a methanol / acetone mixed solution (mixture ratio 1 / 3 (volume ratio)) to which 1.5 mL of hydrochloric acid had been added, and the polymer was precipitated. The precipitated polymer was taken out and dried under reduced pressure at 130°C overnight, and 4.49 g of a powdered copolymer of ethylene and benzonorbornadiene was obtained. The polymerization activity was 89.8 kg / mmol·hr. The composition of the obtained ethylene-benzonorbornadiene copolymer is 13 C-NMR measurement revealed that the structural unit (A) was 57 mol% ethylene and the structural unit (B) was 43 mol% benzonorbornadiene. No peaks due to crystallinity were confirmed in the XRD measurement, indicating that the polymer was amorphous. Therefore, the crystallinity column in Table 1 shows 0%. In the DSC measurement, the temperature was raised from -20°C to 350°C, but no melting peak was detected. Regarding chemical resistance to toluene, the polymer was dissolved, leaving no residue and remaining transparent (chemical resistance to toluene: --).

[0112] [Table 1]

[0113] The chemical resistance was improved in the examples as compared with the comparative examples. From this, it is understood that the present embodiment can provide a cyclic olefin copolymer having excellent chemical resistance.

Claims

1. A structural unit (A) derived from a non-cyclic olefin (A'), A structural unit (B) derived from a cyclic olefin (B'), A cyclic olefin copolymer having the formula: The cyclic olefin copolymer has a crystallinity of 1% or more as determined by the following <X-ray diffraction measurement conditions>. <X-ray diffraction measurement conditions> A powdered cyclic olefin copolymer is subjected to wide-angle X-ray diffraction measurement, and the crystalline peak area, which is the area of ​​the peak derived from the crystals, and the amorphous halo area, which is the area of ​​the halo derived from the amorphous structure, are calculated using the following formula. Crystallinity (%)=crystalline peak area / (crystalline peak area+amorphous halo area)×100

2. When the total content of the structural units (A) and (B) is 100 mol%, the content of the structural unit (A) in the cyclic olefin copolymer is 50 mol % or more and 68 mol % or less, 2. The cyclic olefin copolymer according to claim 1, wherein the content of the structural unit (B) in the cyclic olefin copolymer is 32 mol % or more and 50 mol % or less.

3. The structural unit (A) has a structure represented by the following general formula (I): The cyclic olefin copolymer according to claim 1 or 2, wherein the structural unit (B) has a structure represented by the following general formula (VI): 【Chemistry 1】 (In the above general formula (I), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms. 【Chemistry 2】 (In the general formula (VI), q is 1, 2 or 3; R 32 ~R 39 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, and when q=1, R 36 and R 37 , R 37 and R 38 , R 38 and R 39 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 36 and R 36 , R 36 and R 37 , R 37 and R 38 , R 38 and R 39 , R 39 and R 39 may be bonded to each other to form a monocycle or polycycle, the monocycle or polycycle may have a double bond, and the monocycle or polycycle may be an aromatic ring.

4. The structural unit (A) contains a structural unit derived from ethylene, The cyclic olefin copolymer according to any one of claims 1 to 3, wherein the structural unit (B) contains a structural unit derived from benzonorbornadiene.

5. The cyclic olefin copolymer according to any one of claims 1 to 4, having a melting point of 250°C or higher.

6. A method for producing the cyclic olefin copolymer according to any one of claims 1 to 5, comprising the steps of: The method includes a step of copolymerizing a non-cyclic olefin (A') and a cyclic olefin (B') in the presence of a catalyst containing a transition metal compound (X) represented by the following general formula (1), The non-cyclic olefin (A') has a structure represented by the following general formula (Ia): The method for producing a cyclic olefin copolymer, wherein the cyclic olefin (B') has a structure represented by the following general formula (VIa): 【Chemistry 3】 (In the general formula (1), M 1 represents a transition metal atom of Group 4 of the periodic table, X 1 each independently represents an atom or group selected from the group consisting of a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, and an aluminum-containing group, and substitution products thereof; n 1 represents an integer from 1 to 4, Y 1 represents a carbon atom or a silicon atom, R 1 ~R 14 each independently represents an atom or group selected from the group consisting of a hydrogen atom, a halogen atom, a hydrocarbon group, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, and an aluminum-containing group, and substitution products thereof; R 1 ~R 14 adjacent ones of these may be bonded to each other to form a ring, and the ring formed may have aromaticity including a conjugated double bond, R 1 ~R 14 At least one of the groups is selected from the group consisting of a hydrocarbon group having one or more carbon atoms, a halogen-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a silicon-containing group, a boron-containing group, and an aluminum-containing group, and substitution products thereof. 【Chemistry 4】 (In the above general formula (Ia), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms. 【Chemistry 5】 (In the general formula (VIa), q is 1, 2 or 3; R 32 ~R 39 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, and when q=1, R 36 and R 37 , R 37 and R 38 , R 38 and R 39 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 36 and R 36 , R 36 and R 37 , R 37 and R 38 , R 38 and R 39 , R 39 and R 39 may be bonded to each other to form a monocycle or polycycle, the monocycle or polycycle may have a double bond, and the monocycle or polycycle may be an aromatic ring.

7. When the total content of the non-cyclic olefin (A') and the cyclic olefin (B') in the copolymerization step is taken as 100 mol %, The content of the non-cyclic olefin (A') is 50 mol% or more and 68 mol% or less, The method for producing a cyclic olefin copolymer according to claim 6, wherein the content of the cyclic olefin (B') is 32 mol % or more and 50 mol % or less.

8. The acyclic olefin (A') contains ethylene, The method for producing a cyclic olefin copolymer according to claim 6 or 7, wherein the cyclic olefin (B') contains benzonorbornadiene.

9. In the general formula (1), R 1 ~R 14 The method for producing a cyclic olefin copolymer according to any one of claims 6 to 8, wherein at least one of the above is a hydrocarbon group having one or more carbon atoms.

10. In the general formula (1), R 1 ~R 14 The method for producing a cyclic olefin copolymer according to any one of claims 6 to 9, wherein at least one of the above is a hydrocarbon group having 4 or more carbon atoms.

11. In the general formula (1), R 1 ~R 14 The method for producing a cyclic olefin copolymer according to any one of claims 6 to 10, wherein at least one of the groups is a t-butyl group.

Citation Information

Patent Citations

  • Production of olefinic copolymer

    JP1994271617A

  • Material of cycloolefin copolymer and its production

    JP1994336508A

  • Production of cycloolefin copolymer, and copolymer produced thereby

    JP1996003230A

  • Polyolefin manufacturing

    JP2002510358A

  • Cyclic olefin copolymer and cyclic olefin copolymer film

    JP2014224170A