Semiconductor device, memory device, and method for manufacturing semiconductor device

The transistor structure with a specific insulating and conductive layer configuration using In-M-Zn oxide materials addresses integration and power consumption challenges, enhancing electrical performance and reliability in semiconductor devices.

JP2024169350APending Publication Date: 2024-12-05SEMICON ENERGY LAB CO LTD

Patent Information

Application Number
JP2024080618
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-01
Filing Date
2024-05-17
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing semiconductor devices face challenges in achieving high integration, low power consumption, and reliable operation with large on-state current while minimizing parasitic capacitance and leakage current.

Method used

A transistor structure is developed with a specific configuration involving a first and second insulating layer, a semiconductor layer with a unique crystal orientation, and conductive layers, utilizing In-M-Zn oxide materials, which includes a gate insulating layer and a gate electrode, to enhance electrical characteristics and reduce parasitic capacitance.

Benefits of technology

The proposed transistor structure enables high integration, low power consumption, and reliable operation with large on-state current, supporting miniaturized and highly integrated semiconductor devices with improved electrical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169350000001_ABST
    Figure 2024169350000001_ABST
Patent Text Reader

Abstract

To provide a transistor having high electrical characteristics, to provide a transistor having a large on-state current, to provide a transistor having a small parasitic capacitance, and to provide a transistor, a semiconductor device, or a memory device which can be miniaturized or highly integrated.SOLUTION: In a semiconductor device, a transistor includes a first conductive layer, a second conductive layer, a semiconductor layer, a gate insulating layer over the semiconductor layer, and a gate electrode over the gate insulating layer, the first insulating layer is located between the first conductive layer and the second conductive layer, the second conductive layer is located on the first insulating layer, the first insulating layer and the second conductive layer have an opening portion reaching the first conductive layer, the semiconductor layer is in contact with a sidewall of the opening portion, and the semiconductor layer has a first oxide layer and a second oxide layer, the first oxide layer has a first region and a second region, and the second oxide layer is located between the first region and the second region.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] 1. Field of the Invention One embodiment of the present invention relates to a semiconductor device, a memory device, a display device, and an electronic device. Another embodiment of the present invention relates to a manufacturing method of a semiconductor device.

[0002] Note that one embodiment of the present invention is not limited to the above technical field. Examples of the technical field of one embodiment of the present invention include a semiconductor device, a display device, a light-emitting device, a power storage device, a memory device, an electronic device, a lighting device, an input device (e.g., a touch sensor), an input / output device (e.g., a touch panel), a driving method thereof, or a manufacturing method thereof.

[0003] In this specification and the like, a semiconductor device is a device that utilizes semiconductor characteristics, and refers to a circuit including a semiconductor element (transistor, diode, photodiode, etc.), a device having such a circuit, etc. Also, refers to any device that can function by utilizing semiconductor characteristics. For example, an integrated circuit, a chip including an integrated circuit, and an electronic component that houses a chip in a package are examples of a semiconductor device. Also, a memory device, a display device, a light-emitting device, a lighting device, and an electronic device may themselves be semiconductor devices and each may have a semiconductor device. [Background technology]

[0004] In recent years, the development of semiconductor devices has progressed, and LSIs, CPUs, memories, etc. are mainly used in semiconductor devices. A CPU is an assembly of semiconductor elements that have semiconductor integrated circuits (at least transistors and memories) that are chipped by processing a semiconductor wafer and on which electrodes that serve as connection terminals are formed.

[0005] Semiconductor circuits (IC chips) such as LSIs, CPUs, and memories are mounted on circuit boards, such as printed wiring boards, and used as components in a variety of electronic devices.

[0006] In addition, a technology for constructing a transistor using a semiconductor thin film formed on a substrate having an insulating surface is attracting attention. Such transistors are widely used in electronic devices such as integrated circuits (ICs) and display devices. Silicon-based semiconductor materials are widely known as semiconductor thin films that can be used in transistors, but oxide semiconductors are also attracting attention as other materials.

[0007] It is also known that a transistor using an oxide semiconductor has an extremely small leakage current in an off state. For example, Patent Document 1 discloses a CPU with low power consumption that utilizes the property of a transistor using an oxide semiconductor having a small leakage current. Furthermore, Patent Document 2 discloses a memory device that can retain stored data for a long period of time by utilizing the property of a transistor using an oxide semiconductor having a small leakage current.

[0008] In addition, in recent years, with the miniaturization and weight reduction of electronic devices, there is an increasing demand for further increasing the density of integrated circuits. There is also a demand for improving the productivity of semiconductor devices including integrated circuits. For example, Patent Document 3 and Non-Patent Document 1 disclose a technique for increasing the density of integrated circuits by stacking a first transistor using an oxide semiconductor film and a second transistor using an oxide semiconductor film to provide a plurality of overlapping memory cells. Patent Document 4 discloses a technique for increasing the density of integrated circuits by vertically arranging the channel of a transistor using an oxide semiconductor film. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2012-257187 A [Patent Document 2] JP 2011-151383 A [Patent Document 3] International Publication No. 2021 / 053473 [Patent Document 4] JP 2013-211537 A [Non-patent literature]

[0010] [Non-Patent Document 1] M. Oota et al., “3D-Stacked CAAC-In-Ga-Zn Oxide FETs with Gate Length of 72nm”, IEDM Tech. Dig., 2019, pp.50-53 Summary of the Invention [Problem to be solved by the invention]

[0011] An object of one embodiment of the present invention is to provide a transistor with favorable electrical characteristics. Another object of one embodiment of the present invention is to provide a transistor with high on-state current. Another object of one embodiment of the present invention is to provide a transistor with small parasitic capacitance. Another object of one embodiment of the present invention is to provide a transistor, a semiconductor device, or a memory device that can be miniaturized or highly integrated. Another object of one embodiment of the present invention is to provide a display device with high definition or a high aperture ratio. Another object of one embodiment of the present invention is to provide a highly reliable transistor, semiconductor device, display device, or memory device. Another object of one embodiment of the present invention is to provide a semiconductor device, display device, or memory device with low power consumption. Another object of one embodiment of the present invention is to provide a memory device with high operation speed. Another object of one embodiment of the present invention is to provide a manufacturing method of the transistor, semiconductor device, display device, or memory device.

[0012] Note that the description of these problems does not preclude the existence of other problems. One embodiment of the present invention does not necessarily have to solve all of these problems. Problems other than these can be extracted from the description of the specification, drawings, and claims. [Means for solving the problem]

[0013] One embodiment of the present invention includes a transistor on a first insulating layer and a second insulating layer, the transistor including a first conductive layer on the first insulating layer, a second conductive layer, a semiconductor layer, a gate insulating layer, and a gate electrode, the second insulating layer being located between the first conductive layer and the second conductive layer, the second conductive layer being located on the second insulating layer, the second insulating layer and the second conductive layer having an opening reaching the first conductive layer, the semiconductor layer being connected to a side surface of the second insulating layer in the opening, and a gate insulating layer located on the semiconductor layer; a gate electrode having a region in the opening that overlaps with the semiconductor layer with the gate insulating layer sandwiched therebetween; the semiconductor layer having a first oxide layer and a second oxide layer, the first oxide layer having a first region and a second region, each of the first region and the second region having a plurality of crystal portions, and the second oxide layer located between the first region and the second region.

[0014] In the above structure, the plurality of crystal parts preferably have a c-axis orientation.

[0015] In the above structure, the second oxide layer preferably has a crystal portion having the same crystal structure as the plurality of crystal portions.

[0016] In the above structure, the second oxide layer preferably has a crystal part connected to one of the plurality of crystal parts.

[0017] In the above structure, it is preferable that the boundary between the first oxide layer and the second oxide layer is not observed in a cross-sectional TEM image.

[0018] In the above structure, it is preferable that the first conductive layer has a recessed portion overlapping the opening portion, and the semiconductor layer has a region formed to fill the recessed portion.

[0019] Furthermore, in the above configuration, it is preferable that the opening has an eighth region having a tapered sidewall and a ninth region having a steeper sidewall than the eighth region, the eighth region including an upper end of the opening, the ninth region being located lower than the eighth region, the eighth region including a sidewall of the second conductive layer, and the ninth region including a sidewall of the second insulating layer.

[0020] In addition, in the above configuration, it is preferable that the angle between the sidewall of the eighth region and the top surface of the first insulating layer is greater than 20 degrees and less than 75 degrees, and the angle between the sidewall of the ninth region and the top surface of the first insulating layer is greater than 75 degrees and less than 90 degrees.

[0021] Alternatively, one embodiment of the present invention is a method for manufacturing a semiconductor device, comprising: forming a first insulating layer over a first conductive layer; forming a second conductive layer over the first insulating layer; removing part of the second conductive layer and part of the first insulating layer to form a first opening reaching the first conductive layer to expose an upper surface of the first conductive layer; forming a semiconductor layer so as to be in contact with the upper surface of the first conductive layer, a side surface in the first opening of the first insulating layer, a side surface in the first opening of the second conductive layer, and an upper surface of the second conductive layer; the semiconductor layer is formed through a first step of forming a first oxide layer, a second step of forming a second oxide layer, and a third step of performing heat treatment, in which the first oxide layer is formed by a sputtering method and the second oxide layer is formed by an atomic layer deposition method; forming a second insulating layer so as to be in contact with an upper surface of the semiconductor layer and an upper surface of the first insulating layer; and forming a third conductive layer over the second insulating layer.

[0022] Alternatively, one embodiment of the present invention includes a first insulating layer, a capacitor, and a transistor over the capacitor, the transistor including a first conductive layer, a second conductive layer, a semiconductor layer, a gate insulating layer, and a gate electrode, the capacitor including a third conductive layer, a second insulating layer over the third conductive layer, and a first conductive layer over the second insulating layer, the first insulating layer being located between the first conductive layer and the second conductive layer, the second conductive layer being located over the first insulating layer, and the first insulating layer and the second conductive layer having an opening reaching the first conductive layer, the semiconductor layer is in contact with a side surface of the first insulating layer in the opening and a side surface of the second conductive layer in the opening; the gate insulating layer is located on the semiconductor layer; the gate electrode has a region in the opening that overlaps with the semiconductor layer with the gate insulating layer sandwiched therebetween; the semiconductor layer has a metal oxide; and in the transistor, Id-Vgs characteristics are measured with a drain-source voltage of 0.05 V or more and 1 V or less, Id is a drain current, Vgs is a gate-source voltage, and Id in the Id-Vgs characteristics is 1×10 -12 [A], Vgs is greater than 0V and less than 0.5V.

[0023] In the above embodiment, the metal oxide is preferably an In-M-Zn oxide, and the element M is at least one selected from aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony.

[0024] In the above aspect, the retention time of the storage device is preferably 0.64 seconds or more.

[0025] In the above embodiment, when the gate of the transistor is set to 0 V, the source is set to 0 V, and a voltage of 0.05 V to 1 V is applied to the drain, the integrated amount of charge flowing through the transistor for 0.64 seconds is 3×10 -15 It is preferable that it is [F] × 0.1 [V] or less.

[0026] In the above aspect, the write time of the memory device is preferably 15 ns or less.

[0027] In the above aspect, the read time of the memory device is preferably 15 ns or less.

[0028] In the above-mentioned aspect, it is preferable that the write time is calculated using a circuit in which a first load is connected to the gate of the transistor and a second load is connected to the drain of the transistor, the first load has 256 first circuits, each of the multiple first circuits has a first resistor and a second capacitive element, the second load has 32 second circuits, each of the multiple second circuits has a second resistor and a third capacitive element, the multiple first resistors of the first circuit are connected in series, the multiple second resistors of the second circuit are connected in series, the resistance value of the first resistor is 1 Ω or more and 100 Ω or less, the resistance value of the second resistor is 1 Ω or more and 100 Ω or less, the capacitance value of the second capacitive element is 1 aF or more and 0.5 fF or less, and the capacitance value of the third capacitive element is 1 aF or more and 0.5 fF or less.

[0029] In the above aspect, the read time is calculated using a circuit in which a first load is connected to the gate of the transistor and a second load is connected to the drain of the transistor, the first load has 256 first circuits, each of the multiple first circuits has a first resistor and a second capacitive element, the second load has 32 second circuits, each of the multiple second circuits has a second resistor and a third capacitive element, the multiple first resistors of the first circuit are connected in series, the multiple second resistors of the second circuit are connected in series, and the resistance value of the first resistor is 1 Ω or more and 100 Ω or less, the resistance value of the second resistor is 1 Ω or more and 100 Ω or less, the capacitance value of the second capacitive element is 1 aF or more and 0.5 fF or less, and the capacitance value of the third capacitive element is 1 aF or more and 0.5 fF or less. Effect of the Invention

[0030] According to one embodiment of the present invention, a transistor with favorable electrical characteristics can be provided. According to another embodiment of the present invention, a transistor with large on-state current can be provided. According to another embodiment of the present invention, a transistor, a semiconductor device, or a memory device that can be miniaturized or highly integrated can be provided. According to another embodiment of the present invention, a display device with high definition or a high aperture ratio can be provided. According to another embodiment of the present invention, a highly reliable transistor, a semiconductor device, a display device, or a memory device can be provided. According to another embodiment of the present invention, a semiconductor device, a display device, or a memory device with low power consumption can be provided. According to another embodiment of the present invention, a memory device with high operation speed can be provided. According to another embodiment of the present invention, a manufacturing method of the above transistor, semiconductor device, display device, or memory device can be provided.

[0031] Note that the description of these effects does not preclude the existence of other effects. One embodiment of the present invention does not necessarily have all of these effects. Effects other than these can be extracted from the description in the specification, drawings, and claims. [Brief description of the drawings]

[0032] [Figure 1] Fig. 1(A) is a plan view showing an example of a semiconductor device, and Fig. 1(B) and Fig. 1(C) are cross-sectional views showing an example of the semiconductor device. [Diagram 2] Fig. 2A is a plan view showing an example of a semiconductor device, and Fig. 2B and Fig. 2C are cross-sectional views showing an example of the semiconductor device. [Diagram 3] Fig. 3A is a plan view showing an example of a semiconductor device, and Figs. 3B to 3D are cross-sectional views showing an example of the semiconductor device. [Figure 4] Fig. 4(A) is a plan view showing an example of a semiconductor device, and Fig. 4(B) and Fig. 4(C) are cross-sectional views showing an example of the semiconductor device. [Diagram 5] 5A to 5C are cross-sectional views showing an example of a semiconductor device. [Figure 6]6A to 6D are cross-sectional views showing an example of a semiconductor device. [Figure 7] 7(A) and 7(B) are cross-sectional views showing an example of a semiconductor device. [Figure 8] 8(A) and 8(B) are cross-sectional views showing an example of a semiconductor device. [Figure 9] 9(A) and 9(B) are cross-sectional views showing an example of a semiconductor device. [Figure 10] 10(A) and 10(B) are cross-sectional views showing an example of a semiconductor device. [Figure 11] 11A to 11D are cross-sectional views of an oxide semiconductor. [Figure 12] 12A to 12C are cross-sectional views illustrating an example of a method for manufacturing a semiconductor device. [Figure 13] Fig. 13(A) is a plan view showing an example of a memory device, and Fig. 13(B) and Fig. 13(C) are cross-sectional views showing an example of the memory device. [Figure 14] Fig. 14(A) is a plan view showing an example of a storage device, and Fig. 14(B) and Fig. 14(C) are cross-sectional views showing an example of the storage device. [Figure 15] Fig. 15(A) is a plan view showing an example of a storage device, and Fig. 15(B) is a cross-sectional view showing an example of the storage device. [Figure 16] FIG. 16 is a cross-sectional view showing an example of a storage device. [Figure 17] FIG. 17 is a cross-sectional view showing an example of a storage device. [Figure 18] FIG. 18 is a block diagram illustrating a configuration example of a semiconductor device. [Figure 19] 19A to 19H are diagrams illustrating examples of circuit configurations of memory cells. [Figure 20] 20A and 20B are perspective views illustrating a configuration example of a semiconductor device. [Figure 21] FIG. 21 is a block diagram illustrating the CPU. [Figure 22]22(A) and 22(B) are perspective views of the semiconductor device. [Diagram 23] 23(A) and 23(B) are perspective views of the semiconductor device. [Figure 24] 24(A) and 24(B) are diagrams showing various storage devices by hierarchical level. [Diagram 25] 25(A) and 25(B) are perspective views showing an example of a display device. [Figure 26] FIG. 26 is a cross-sectional view showing an example of a display device. [Figure 27] FIG. 27 is a cross-sectional view showing an example of a display device. [Figure 28] 28A to 28C are diagrams showing configuration examples of display devices. [Figure 29] 29(A) and 29(B) are diagrams showing an example of an electronic component. [Diagram 30] Fig. 30(A) to Fig. 30(C) are diagrams showing an example of a mainframe computer. Fig. 30(D) is a diagram showing an example of space equipment. Fig. 30(E) is a diagram showing an example of a storage system applicable to a data center. [Diagram 31] 31A to 31F are diagrams showing examples of electronic devices. [Diagram 32] 32A to 32G are diagrams showing examples of electronic devices. [Diagram 33] 33(A) to 33(F) are diagrams showing examples of electronic devices. [Diagram 34] 34(A) and 34(B) are diagrams showing Id-Vg characteristics. [Diagram 35] 35(A) and 35(B) are diagrams showing Id-Vd characteristics. [Diagram 36] FIG. 36 is a circuit diagram used in the circuit simulation. [Figure 37] 37(A) and 37(B) are timing charts illustrating the operation of the circuit. [Figure 38] 38(A) to 38(C) are cross-sectional TEM images according to Example 3. [Figure 39] 39(A) to 39(C) are diagrams showing the crystal orientation according to the third embodiment. [Diagram 40] FIG. 40 is a diagram showing the Id-Vgs characteristics. [Diagram 41] 41A to 41C are timing charts illustrating the operation of the circuit. [Diagram 42] 42(A) and 42(B) show the results of a circuit simulation. [Diagram 43] FIG. 43 is a cross-sectional TEM image according to Example 5. [Diagram 44] FIG. 44 is a cross-sectional TEM image according to Example 5. [Diagram 45] FIG. 45 is a circuit diagram according to the sixth embodiment. [Diagram 46] FIG. 46 is a diagram showing the measurement results of transistor current. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] The embodiments will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be easily understood by those skilled in the art that the modes and details of the present invention can be modified in various ways without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.

[0034] In the configuration of the invention described below, the same parts or parts having similar functions are denoted by the same reference numerals in different drawings, and the repeated explanations are omitted. In addition, when referring to similar functions, the same hatching pattern may be used and no particular reference numeral may be used.

[0035] In addition, for ease of understanding, the position, size, range, etc. of each component shown in the drawings may not represent the actual position, size, range, etc. Therefore, the disclosed invention is not necessarily limited to the position, size, range, etc. disclosed in the drawings.

[0036] In this specification, the ordinal numbers "first" and "second" are used for convenience and do not limit the number of components or the order of the components (e.g., the order of processes or the order of stacking). In addition, an ordinal number attached to a component in one part of this specification may not match an ordinal number attached to the same component in another part of this specification or in the claims.

[0037] A transistor is a type of semiconductor element and can realize a function of amplifying a current or voltage, a switching operation of controlling conduction or non-conduction, etc. In this specification, the term "transistor" includes an IGFET (Insulated Gate Field Effect Transistor) and a thin film transistor (TFT).

[0038] In this specification and the like, a transistor using an oxide semiconductor or a metal oxide for a semiconductor layer and a transistor having an oxide semiconductor or a metal oxide in a channel formation region may be referred to as an OS transistor, and a transistor having silicon in a channel formation region may be referred to as a Si transistor.

[0039] In this specification, a transistor is an element having at least three terminals including a gate, a drain, and a source. A region (also called a channel formation region) in which a channel is formed between the drain (drain terminal, drain region, or drain electrode) and the source (source terminal, source region, or source electrode) is provided, and a current can flow between the source and the drain through the channel formation region. In this specification, a channel formation region refers to a region through which a current mainly flows.

[0040] In addition, the functions of "source" and "drain" may be interchanged when transistors of different polarities are used, or when the direction of current flow changes during circuit operation, etc. For this reason, in this specification, the terms "source" and "drain" may be used interchangeably.

[0041] Note that impurities in a semiconductor refer to, for example, elements other than the main components constituting the semiconductor. For example, an element with a concentration of less than 0.1 atomic % can be said to be an impurity. The inclusion of impurities may, for example, increase the density of defect states in the semiconductor or reduce the crystallinity. When the semiconductor is an oxide semiconductor, impurities that change the characteristics of the semiconductor include, for example, Group 1 elements, Group 2 elements, Group 13 elements, Group 14 elements, Group 15 elements, and transition metals other than the main components of the oxide semiconductor. Specific examples include hydrogen, lithium, sodium, silicon, boron, phosphorus, carbon, and nitrogen. Note that water may also function as an impurity. For example, the inclusion of impurities may cause oxygen deficiency (V O In some cases, a junction (also referred to as a junction) may be formed.

[0042] In this specification and the like, an oxynitride refers to a material having a composition containing more oxygen than nitrogen, and a nitride oxide refers to a material having a composition containing more nitrogen than oxygen.

[0043] For example, secondary ion mass spectrometry (SIMS) or X-ray photoelectron spectroscopy (XPS) can be used to analyze the content of elements such as hydrogen, oxygen, carbon, and nitrogen contained in the film. XPS is suitable when the content of the target element is high (e.g., 0.5 atomic% or more, or 1 atomic% or more). On the other hand, SIMS is suitable when the content of the target element is low (e.g., 0.5 atomic% or less, or 1 atomic% or less). When comparing the content of elements, it is more preferable to perform a combined analysis using both SIMS and XPS analysis methods.

[0044] In addition, the words "film" and "layer" can be interchanged depending on the case or situation. For example, the term "conductive layer" can be changed to the term "conductive film". Or, for example, the term "insulating film" can be changed to the term "insulating layer".

[0045] In addition, in this specification, "parallel" refers to a state in which two straight lines are arranged at an angle of -10 degrees or more and 10 degrees or less. Therefore, it also includes the case of -5 degrees or more and 5 degrees or less. "Approximately parallel" refers to a state in which two straight lines are arranged at an angle of -30 degrees or more and 30 degrees or less. "Perpendicular" refers to a state in which two straight lines are arranged at an angle of 80 degrees or more and 100 degrees or less. Therefore, it also includes the case of 85 degrees or more and 95 degrees or less. "Approximately perpendicular" refers to a state in which two straight lines are arranged at an angle of 60 degrees or more and 120 degrees or less.

[0046] In this specification, "electrically connected" includes a case where a connection is made via "something having some electrical action". Here, "something having some electrical action" is not particularly limited as long as it allows transmission and reception of an electrical signal between the objects to be connected. For example, "something having some electrical action" includes electrodes or wiring, as well as switching elements such as transistors, resistive elements, coils, and other elements having various functions.

[0047] In this specification, unless otherwise specified, the off-state current refers to the leakage current between the source and drain when the transistor is in the off state (also called the non-conducting state or cut-off state). Unless otherwise specified, the off-state refers to the voltage V between the gate and the source in an n-channel transistor. gs is the threshold voltage V th (For p-channel transistors, V th The term "higher" refers to a state of being.

[0048] In this specification, the normally-on characteristic refers to a state in which a channel exists and a current flows through a transistor even when no voltage is applied to the gate, whereas the normally-off characteristic refers to a state in which no current flows through a transistor when no potential is applied to the gate or when a ground potential is applied to the gate.

[0049] In this specification, the top surface shape of a certain component refers to the contour shape of the component in a plan view. The plan view refers to a view from the normal direction of the surface on which the component is formed or the surface of a support (e.g., a substrate) on which the component is formed.

[0050] In this specification, the phrase "top surface shapes are approximately the same" refers to at least a portion of the contours of the stacked layers overlapping. For example, this includes cases where the upper and lower layers are processed using the same mask pattern or a portion of the same mask pattern. However, strictly speaking, the contours may not overlap, and the upper layer may be located inside the lower layer, or the upper layer may be located outside the lower layer, and in this case, it may also be said that the top surface shapes are approximately the same. In addition, when the top surface shapes are the same or approximately the same, it can also be said that the ends are aligned or approximately aligned, or that the side ends are aligned or approximately aligned.

[0051] In this specification, the term "tapered shape" refers to a shape in which at least a part of the side of the structure is inclined with respect to the substrate surface or the surface to be formed. For example, it is preferable to have a region in which the angle (also called the taper angle) between the inclined side and the substrate surface or the surface to be formed is greater than 0 degrees and less than 90 degrees. The side of the structure, the substrate surface, and the surface to be formed do not necessarily need to be completely flat, and may be approximately planar with a slight curvature or approximately planar with a slight unevenness.

[0052] In this specification and the like, when it is stated that A is in contact with B, it means that at least a part of A is in contact with B. Therefore, for example, it can be rephrased as saying that A has a region in contact with B.

[0053] In this specification and the like, when it is stated that A is located on B, at least a part of A is located on B. Therefore, for example, it can be rephrased as, A has a region located on B.

[0054] In this specification and the like, when it is stated that A covers B, at least a part of A covers B. Therefore, for example, it can be rephrased as, A has a region that covers B.

[0055] In this specification and the like, when it is stated that A overlaps with B, at least a portion of A overlaps with B. Therefore, for example, this can be rephrased as saying that A has a region that overlaps with B.

[0056] In this specification, a device fabricated using a metal mask or an FMM (fine metal mask, high-resolution metal mask) may be referred to as a device with an MM (metal mask) structure. Also, in this specification, a device fabricated without using a metal mask or an FMM may be referred to as a device with an MML (metal maskless) structure.

[0057] In this specification and the like, a structure in which light-emitting layers are separately created for light-emitting elements (also called light-emitting devices) with different emission wavelengths is sometimes referred to as an SBS (Side By Side) structure. The SBS structure allows the material and configuration to be optimized for each light-emitting element, increasing the freedom of material and configuration selection and making it easier to improve brightness and reliability.

[0058] In this specification and the like, holes or electrons may be referred to as "carriers". Specifically, a hole injection layer or an electron injection layer may be referred to as a "carrier injection layer", a hole transport layer or an electron transport layer may be referred to as a "carrier transport layer", and a hole block layer or an electron block layer may be referred to as a "carrier block layer". Note that the above-mentioned carrier injection layer, carrier transport layer, and carrier block layer may not be clearly distinguishable. Also, one layer may have two or three functions among the carrier injection layer, carrier transport layer, and carrier block layer.

[0059] In this specification etc., the light-emitting element has an EL layer between a pair of electrodes. The EL layer has at least a light-emitting layer. Here, examples of layers (also called functional layers) included in the EL layer include a light-emitting layer, a carrier injection layer (a hole injection layer and an electron injection layer), a carrier transport layer (a hole transport layer and an electron transport layer), and a carrier block layer (a hole block layer and an electron block layer). In this specification etc., the light-receiving element (also called a light-receiving device) has at least an active layer that functions as a photoelectric conversion layer between a pair of electrodes. In this specification etc., one of the pair of electrodes may be referred to as a pixel electrode, and the other as a common electrode.

[0060] In this specification and the like, a sacrificial layer (which may also be referred to as a mask layer) is located at least above a light-emitting layer (more specifically, a layer that is processed into an island shape among layers that constitute the EL layer) and has the function of protecting the light-emitting layer during the manufacturing process.

[0061] In this specification, the term "island-like" refers to a state in which two or more layers made of the same material and formed in the same process are physically separated. For example, an island-like EL layer refers to a state in which the EL layer is physically separated from the adjacent EL layer.

[0062] In this specification and the like, the term "step discontinuity" refers to a phenomenon in which a layer, a film, or an electrode is divided due to the shape of the surface on which it is formed (for example, a step or the like).

[0063] In addition, in the drawings and the like related to this specification, arrows indicating the X direction, Y direction, and Z direction may be attached. In addition, in this specification, the "X direction" is the direction along the X axis, and the forward direction and the reverse direction may not be distinguished unless explicitly stated. The same applies to the "Y direction" and the "Z direction." In addition, the X direction, the Y direction, and the Z direction are directions that intersect with each other. For example, the X direction, the Y direction, and the Z direction are directions that are perpendicular to each other.

[0064] (Embodiment 1) In this embodiment, a semiconductor device according to one embodiment of the present invention will be described.

[0065] A semiconductor device of one embodiment of the present invention includes a first conductive layer, a second conductive layer, a third conductive layer, an oxide semiconductor layer, a first insulating layer, and a second insulating layer.

[0066] The first insulating layer is located over the first conductive layer, and the second conductive layer is located over the first insulating layer. The first insulating layer and the second conductive layer have an opening that reaches the first conductive layer. The oxide semiconductor layer is in contact with at least a top surface of the first conductive layer, a side surface of the first insulating layer, and a side surface of the second conductive layer in the opening. The second insulating layer is located over the oxide semiconductor layer in the opening. The third conductive layer overlaps with the oxide semiconductor layer in the opening, with the second insulating layer sandwiched therebetween. Note that the opening is also referred to as an opening.

[0067] The first conductive layer functions as one of a source electrode and a drain electrode of the transistor, the second conductive layer functions as the other of the source electrode and the drain electrode of the transistor, the third conductive layer functions as a gate electrode of the transistor, and the second insulating layer functions as a gate insulating layer.

[0068] In this specification, the term "in a cross-sectional view" is used, but may be specifically rephrased as "in a cross-sectional view from the same direction." For example, when explaining the relationship between multiple configurations, the relationship in a cross-sectional view from the same direction is explained. In this case, the relationship between the multiple configurations can be explained using one cross-sectional view.

[0069] In a transistor according to one embodiment of the present invention, a source electrode and a drain electrode are located at different heights, and a current flows in a semiconductor layer in a height direction. In other words, it can be said that the channel length direction has a height (vertical) component, and therefore the transistor according to one embodiment of the present invention can also be called a VFET (Vertical Field Effect Transistor), a vertical transistor, a vertical channel transistor, a vertical channel transistor, or the like.

[0070] In the transistor of one embodiment of the present invention, a source electrode, a semiconductor layer, and a drain electrode can be provided in a stacked manner, and thus the occupation area can be significantly reduced as compared with a so-called planar transistor in which a semiconductor layer is arranged in a planar shape.

[0071] In this specification, the term "ends coincide" refers to at least a portion of the contours of stacked layers overlapping in a plan view. For example, this term includes cases where the upper and lower layers are processed using the same mask pattern or where a portion of the mask pattern is the same. However, strictly speaking, the contours may not overlap, and the contour of the upper layer may be located inside the contour of the lower layer, or the contour of the upper layer may be located outside the contour of the lower layer. In these cases, the term "ends coincide" is also used.

[0072] In general, it may be difficult to clearly distinguish between an "exact match" and an "approximate match." For this reason, in this specification and elsewhere, "match" may include both an exact match and an approximate match.

[0073] <Configuration Example 1 of Semiconductor Device> The structure of a semiconductor device according to one embodiment of the present invention will be described with reference to FIGS. 2A to 6D. FIG. 2A is a plan view of a semiconductor device including a transistor 200. FIG. 2B is a cross-sectional view taken along dashed line A1-A2 in FIG. 2A. FIG. 2C is a cross-sectional view taken along dashed line A3-A4 in FIG. 2A. FIG. 3A is a cross-sectional view taken along dashed line A3-A4 in FIG. 2A, including an insulating layer 280, in the XY plane. Note that some elements are omitted in the plan view of FIG. 2A for clarity. Some elements may also be omitted in the subsequent plan views.

[0074] 2A to 2C and 3A includes an insulating layer 210 over a substrate (not shown), a transistor 200 over the insulating layer 210, and an insulating layer 280 over the insulating layer 210. The insulating layer 210 and the insulating layer 280 function as interlayer films.

[0075] The transistor 200 includes a conductive layer 220, a conductive layer 240 over an insulating layer 280, an oxide semiconductor layer 230, an insulating layer 250 over the oxide semiconductor layer 230, and a conductive layer 260 over the insulating layer 250. The conductive layer 220 and the conductive layer 240 are located at different heights.

[0076] In the transistor 200, the oxide semiconductor layer 230 functions as a semiconductor layer, the conductive layer 260 functions as a gate electrode, the insulating layer 250 functions as a gate insulating layer, the conductive layer 220 functions as one of a source electrode and a drain electrode, and the conductive layer 240 functions as the other of the source electrode and drain electrode.

[0077] A region of the oxide semiconductor layer 230 which is in contact with the conductive layer 220 and the conductive layer 240 preferably functions as a low-resistance region.

[0078] As shown in FIG. 2B and FIG. 2C, the insulating layer 280 and the conductive layer 240 are provided with an opening 290 that reaches the conductive layer 220. In a configuration such as FIG. 6D described later, the bottom of the opening 290 is, for example, the upper surface of the conductive layer 220. Also, as shown in FIG. 2B and FIG. 2C, when a recess overlapping the opening 290 is provided in the conductive layer 220, the opening 290 and the recess of the conductive layer 220 may form a continuous opening. In such a case, for example, a region on the upper surface of the conductive layer 220 that overlaps with the opening 290 becomes the bottom of the continuous opening. The side walls of the opening 290 are the side surfaces of the insulating layer 280 and the side surfaces of the conductive layer 240. The opening 290 includes an opening in the insulating layer 280 and an opening in the conductive layer 240. In other words, an opening in a region where the insulating layer 280 overlaps with the conductive layer 220 is a part of the opening 290, and an opening in a region where the conductive layer 240 overlaps with the conductive layer 220 is another part of the opening 290. Note that, among the openings 290, the opening 290 provided in the insulating layer 280 is represented as opening 290a, and the opening 290 provided in the conductive layer 240 is represented as opening 290b.

[0079] At least some of the components of the transistor 200 are disposed inside the opening 290. Specifically, the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 are disposed such that at least some of them are located inside the opening 290. The oxide semiconductor layer 230 contacts an upper surface of the conductive layer 220, a side surface of the insulating layer 280, and a side surface of the conductive layer 240 within the opening 290.

[0080] Moreover, insulating layer 280 has insulating layer 280a, insulating layer 280b on insulating layer 280a, and insulating layer 280c on insulating layer 280b. Insulating layer 280a has a region in contact with the upper surface of insulating layer 210, a region in contact with the side surface of conductive layer 220, and a region in contact with the upper surface of conductive layer 220. Insulating layer 280c has a region in contact with the lower surface of conductive layer 240.

[0081] The oxide semiconductor layer 230 is provided inside an opening 290 in the insulating layer 280. The transistor 200 has a structure in which one of the source electrode and the drain electrode (the conductive layer 220 here) is located below and the other of the source electrode and the drain electrode (the conductive layer 240 here) is located above, so that a current flows in a vertical direction. That is, a channel is formed along the sidewall of the opening 290a.

[0082] The oxide semiconductor layer 230 contacts the upper surface of the conductive layer 220 and the side surface of the conductive layer 240 inside the opening 290. The oxide semiconductor layer 230 also contacts a part of the upper surface of the conductive layer 240. In this way, the oxide semiconductor layer 230 contacts not only the side surface but also the upper surface of the conductive layer 240, so that the area of ​​contact between the oxide semiconductor layer 230 and the conductive layer 240 can be made larger than, for example, a case in which the oxide semiconductor layer 230 contacts the side surface of the conductive layer 240 but does not contact the upper surface. Therefore, the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be made smaller.

[0083] The conductive layer 240 has an opening 290b in a region overlapping with the conductive layer 220. The conductive layer 240 is preferably not provided inside the opening 290a of the insulating layer 280. That is, the conductive layer 240 preferably does not have a region in contact with a side surface of the insulating layer 280 in the opening 290a. With this structure, the opening 290b of the conductive layer 240 and the opening 290a of the insulating layer 280 can be formed at the same time. Furthermore, by configuring the side surface of the conductive layer 240 in the opening 290b and the side surface of the insulating layer 280 in the opening 290a to coincide or approximately coincide, the film thickness distribution of the oxide semiconductor layer 230 provided inside the opening 290 can be made uniform. Furthermore, the oxide semiconductor layer 230 can be prevented from being divided by a step between the conductive layer 240 and the insulating layer 280.

[0084] The conductive layer 260 is preferably configured to have a laminated structure of a conductive layer 260a and a conductive layer 260b on the conductive layer 260a. Each of the conductive layer 260a and the conductive layer 260b may further have a laminated structure.

[0085] The width of the opening 290 is defined as width D. Width D may vary in the depth direction. For example, it may be the width of the upper end of the opening 290a in the insulating layer 280. Alternatively, it may be the width of the lower end. Alternatively, it may be the width at half the depth of the opening 290a in the insulating layer 280. Alternatively, the width of the opening 290b in the conductive layer 240 may be used.

[0086] The portions of the oxide semiconductor layer 230 and the insulating layer 250 that are disposed inside the opening 290 are provided to reflect the shape of the opening 290. Specifically, the oxide semiconductor layer 230 is provided so as to cover the bottom and sidewall of the opening 290, and the insulating layer 250 is provided so as to cover the oxide semiconductor layer 230. The oxide semiconductor layer 230 is preferably provided so as to contact the sidewall of the insulating layer 280 in the opening 290a. The insulating layer 250 is disposed facing the sidewall of the insulating layer 280 in the opening 290a, with the oxide semiconductor layer 230 sandwiched therebetween.

[0087] The conductive layer 260 is provided so as to fill the recess of the insulating layer 250 that reflects the shape of the opening 290. By reducing the width D, the transistor 200 can be miniaturized. However, when the width D is reduced, if the aspect ratio of the opening 290 is high, in this case, if the value obtained by dividing the depth of the opening by the width of the opening is large, there is a concern that coverage of the sidewall of the opening 290 may be reduced depending on the formation method or thickness of the components disposed inside the opening 290. In addition, when the width D is reduced and the oxide semiconductor layer 230 is thickened, there is a concern that coverage of the inside of the opening may be further reduced.

[0088] The opening 290 preferably has a tapered shape at the upper end of the opening. The opening 290 also preferably has a region having a tapered shape at the upper end of the opening and a region deeper than the tapered region, whose sidewalls are steeper than the upper end. Here, "steep" refers to, for example, that the angle of the sidewall with respect to the insulating layer 210 is perpendicular or close to perpendicular.

[0089] By forming the opening 290 in such a shape, the conductive layer 260 can be formed in a suitable shape even when the transistor 200 is made finer, the width of the opening is small, and the aspect ratio is high. Specifically, for example, in the conductive layer 260, the conductive layer 260a can have high coverage on the sidewall of the opening 290, and the conductive layer 260b can be formed to a large thickness and on the upper end of the opening 290.

[0090] The film provided inside the opening 290 can be formed using an atomic layer deposition (ALD) method, a sputtering method, a chemical vapor deposition (CVD) method, a vacuum deposition method, a pulsed laser deposition (PLD) method, or the like.

[0091] The opening 290 preferably has a tapered shape at the upper end. The sidewall of the tapered region is preferably at least partially covered with the conductive layer 260b.

[0092] Moreover, the opening 290 preferably has a region deeper than the region having the tapered shape, where the sidewall is steeper than the upper end. When the opening 290 has such a shape, for example, in the tapered region, the contact area with the conductive layer 240 increases, so that the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced. When a part of the insulating layer 280 has a tapered shape, for example, the region may function as a region for relaxing the electric field between the conductive layer 240 and the conductive layer 260.

[0093] In the transistor 200 shown in Figures 2(B) and 2(C), in the opening 290, the sidewall of the conductive layer 240 and the sidewall of the insulating layer 280c have a region having a tapered shape, and the sidewall of the insulating layer 280b and the sidewall of the insulating layer 280a have a region that is steeper than the sidewall of the conductive layer 240.

[0094] It is preferable that the insulating layer 250 has a configuration that has good coverage on the sidewall of the opening 290 and can suppress short circuits between the conductive layer 240 and the conductive layer 260.

[0095] The conductive layer 260 has a region located over the insulating layer 280. In Figures 2B and 2C, the conductive layer 260 has a region over the insulating layer 280 that covers the conductive layer 240, the oxide semiconductor layer 230, and the insulating layer 250.

[0096] Moreover, it is preferable that the conductive layer 240 has a region that is not covered with the conductive layer 260. In the region that does not overlap with the conductive layer 260, the end of the conductive layer 240 is located outside the end of the conductive layer 260. In the region of the conductive layer 240 that does not overlap with the conductive layer 260, a conductive layer can be provided thereon, and the conductive layer and the conductive layer 240 can be electrically connected to each other.

[0097] 2B shows a structure in which an end of the conductive layer 240 is located outside the opening 290, further outward than an end of the conductive layer 260. With such a structure, a plug or the like can be provided on a region of the conductive layer 240 that extends outward beyond the conductive layer 260, and the conductive layer 240 and the conductive layer 260 can be electrically connected to a conductive layer, such as a wiring or an electrode, located above the conductive layer 260.

[0098] The insulating layer 250 is provided in contact with the top surface of the oxide semiconductor layer 230. The insulating layer 250 preferably has a region in contact with the top surface of the conductive layer 240, a region in contact with a side surface of the conductive layer 240, and a region in contact with the top surface of the insulating layer 280.

[0099] 2(B) and 2(C), a part of the insulating layer 250 is located outside the opening 290, that is, on the conductive layer 240 and the insulating layer 280. At this time, it is preferable that the insulating layer 250 covers an end portion of the oxide semiconductor layer 230. This can prevent the conductive layer 260 and the oxide semiconductor layer 230 from being short-circuited. In addition, it is preferable that the insulating layer 250 covers an end portion of the conductive layer 240. This can prevent the conductive layer 260 and the conductive layer 240 from being short-circuited.

[0100] The insulating layer 250 functions as a gate insulating layer of the transistor 200. By making the gate insulating layer thin, it is possible to reduce a gate potential applied during operation of the transistor 200. In addition, it is possible to operate the transistor 200 at high speed.

[0101] Here, in FIG. 2B and FIG. 2C, a configuration is shown in which the end of the oxide semiconductor layer 230 is located inside the end of the conductive layer 240 outside the opening 290. Note that the present invention is not limited to this. For example, in the X direction, the end of the oxide semiconductor layer 230 and the end of the conductive layer 240 may coincide or approximately coincide. Alternatively, the end of the oxide semiconductor layer 230 may be located outside the end of the conductive layer 240. By making the end of the oxide semiconductor layer 230 outside the end of the conductive layer 240 and covering the end of the conductive layer 240 with the oxide semiconductor layer 230, the breakdown voltage between the conductive layer 240 and the conductive layer 260 may be further increased, and the leakage current of the insulating layer 250 located between the conductive layer 240 and the conductive layer 260 may be further reduced.

[0102] The sidewall of the opening 290 can be tapered by setting the angle between the upper surface of the insulating layer 210 and the sidewall of the opening 290 to 60 degrees or less, more preferably 50 degrees or less, and even more preferably 40 degrees or less. Furthermore, if the angle between the upper surface of the insulating layer 210 and the sidewall of the opening 290 is less than 20 degrees, the width D of the opening 290 increases, which may make it difficult to miniaturize the transistor 200. Therefore, when the sidewall of the opening 290 is tapered, for example, the angle between the upper surface of the insulating layer 210 and the sidewall of the opening 290 may be set to 20 degrees or more and 75 degrees or less, preferably 20 degrees or more and 70 degrees or less, more preferably 20 degrees or more and 60 degrees or less, and even more preferably 20 degrees or more and 50 degrees or less.

[0103] Furthermore, by making the angle between the upper surface of insulating layer 210 and the opening 290 greater than 60 degrees and less than 90 degrees, preferably greater than 70 degrees and less than 90 degrees, more preferably greater than 75 degrees and less than 90 degrees, and even more preferably greater than 80 degrees and less than 90 degrees, the sidewall of opening 290 can be made to have a steep shape, thereby enabling the miniaturization or high integration of the semiconductor device.

[0104] Alternatively, for example, the sidewall of the opening 290 may have an inverse tapered shape. In other words, the angle formed between the side surface of the insulating layer 280 at the opening 290 and the top surface of the insulating layer 210 may be greater than 90 degrees.

[0105] The sidewall of the opening 290 is preferably provided so as to be perpendicular to the upper surface of the insulating layer 210. Angles θ1a, θ1b, θ1c, and θ2, which are angles formed between the side surfaces of the insulating layer 280a, the insulating layer 280b, the insulating layer 280c, and the conductive layer 240 in the opening 290 and the upper surface of the insulating layer 210, are shown in Fig. 3(B). The angles θ1a, θ1b, θ1c, and θ2 are, for example, greater than 20 degrees and equal to or less than 90 degrees.

[0106] 3B shows an example in which the conductive layer 240 and the insulating layer 280c have a tapered shape. In FIG. 3B, the tapered portion is surrounded by a dashed line. The angle θ2 and the angle θ1c are each preferably 20 degrees or more and 75 degrees or less, more preferably 20 degrees or more and 70 degrees or less, more preferably 20 degrees or more and 60 degrees or less, and further preferably 20 degrees or more and 50 degrees or less.

[0107] Each of the angles θ1b and θ1a is preferably greater than 60 degrees and less than or equal to 90 degrees, more preferably greater than 70 degrees and less than or equal to 90 degrees, more preferably greater than 75 degrees and less than or equal to 90 degrees, and even more preferably greater than or equal to 80 degrees and less than or equal to 90 degrees.

[0108] Although the angles θ1a, θ1b, θ1c, and θ2 are herein defined as angles with the upper surface of the insulating layer 210, they may be angles with the upper surface of the conductive layer 220.

[0109] In addition, by making the thickness of the insulating layer 280c, for example, 50 nm or less, 30 nm or less, preferably 20 nm or less, and more preferably 10 nm or less, even if the insulating layer 280c is made tapered, the size of the opening 290 does not become too large, and the area occupied by the transistor can be reduced, which is preferable.

[0110] 1A to 1C show an example in which the angles θ1a, θ1b, θ1c, and θ2 in FIGS. 2A to 2C are 90 degrees.

[0111] 3(C) and 3(D) are each a modified example of FIG. 3(B).

[0112] FIG. 3C shows an example in which the sidewall of the insulating layer 280a in the opening 290 has a tapered shape in addition to the conductive layer 240 and the insulating layer 280c. In FIG. 3C, the portion having a tapered shape is surrounded by a dashed line. By making the sidewall of the insulating layer 280a in the opening 290 tapered, the coverage of the bottom of the opening 290 and its vicinity with the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260a can be improved. In addition, by making the insulating layer 280a sufficiently thin, an increase in the size of the transistor 200 can be suppressed. The insulating layer 280a may be, for example, 50 nm or less, 30 nm or less, preferably 20 nm or less, and more preferably 10 nm or less.

[0113] 3D shows an example in which the conductive layer 240 and the insulating layer 280c have regions with steep sidewalls, and the insulating layer 280b and the insulating layer 280a have regions with tapered shapes. In this way, when part of the insulating layer 280 has a tapered shape, for example, coverage of the components of the transistor 200 in the opening 290 can be improved.

[0114] Furthermore, by making the lower end of the sidewall of the conductive layer 240 and the upper end of the sidewall of the insulating layer 280c discontinuous, it is possible to provide a region in the oxide semiconductor layer 230 that is in contact with the upper surface of the insulating layer 280 and is located within the opening 290. For example, this region may function as a region for alleviating the electric field between the conductive layer 240 and the conductive layer 260. In addition, for example, it is possible to improve the coverage of the upper end of the opening 290 and its vicinity by the oxide semiconductor layer 230 and the insulating layer 250, the conductive layer 260, and the like that are thereover.

[0115] FIG. 4(A) is a plan view of a semiconductor device having a transistor 200. FIG. 4(B) is a cross-sectional view taken along dashed lines A1-A2 in FIG. 4(A). FIG. 4(C) is a cross-sectional view taken along dashed lines A3-A4 in FIG. 4(A). FIG. 5(A) is a diagram for explaining angles θ1a, θ1b, θ1c, and θ2, and corresponds to the cross section shown in FIG. 4(B). The semiconductor device shown in FIG. 4(A) to FIG. 4(C) is different from that shown in FIG. 2(A) to FIG. 2(C) in that the lower end of the sidewall of the conductive layer 240 and the upper end of the sidewall of the insulating layer 280c are discontinuous. Note that, as an example, FIG. 4(B) and FIG. 4(C) show an example in which the sidewalls of the insulating layer 280c and the conductive layer 240 at the opening 290 are steeper than those shown in FIG. 2(B) and FIG. 2(C), but each sidewall may have a tapered shape.

[0116] Fig. 5(A) shows angles θ1a, θ1b, θ1c, and θ2 formed by the side surfaces of insulating layer 280a, insulating layer 280b, insulating layer 280c, and conductive layer 240 at opening 290 in Fig. 4(B) and the upper surface of insulating layer 210. In the example shown in Fig. 5(A), the lower end of the side wall of conductive layer 240 is positioned outward by length d1 from the upper end of the side wall of insulating layer 280c.

[0117] In FIG. 5(A), the angles θ1a, θ1b, θ1c, and θ2 are each, for example, preferably greater than 60 degrees and less than 90 degrees, more preferably greater than 70 degrees and less than 90 degrees, more preferably greater than 75 degrees and less than 90 degrees, and even more preferably greater than 80 degrees and less than 90 degrees.

[0118] Moreover, Fig. 5(B) and Fig. 5(C) each show a modification of Fig. 5(A).

[0119] In Fig. 5(B), the angle θ2 and the angle θ1c are different from those in Fig. 5(A). In Fig. 5(B), the portion having a tapered shape is surrounded by a dashed line. In Fig. 5(B), the angle θ2 and the angle θ1c are, for example, preferably 20 degrees or more and 75 degrees or less, more preferably 20 degrees or more and 70 degrees or less, more preferably 20 degrees or more and 60 degrees or less, and even more preferably 20 degrees or more and 50 degrees or less.

[0120] In Fig. 5(C), the angle θ2, the angle θ1c, and the angle θ1a are different from those in Fig. 5(A). In Fig. 5(C), the portion having a tapered shape is surrounded by a dashed line. In Fig. 5(C), the angle θ2, the angle θ1c, and the angle θ1a are each, for example, preferably 20 degrees or more and 75 degrees or less, more preferably 20 degrees or more and 70 degrees or less, more preferably 20 degrees or more and 60 degrees or less, and even more preferably 20 degrees or more and 50 degrees or less.

[0121] <OSトランジスタ> The transistor 200 includes a metal oxide (also referred to as an oxide semiconductor) functioning as a semiconductor in the oxide semiconductor layer 230 including a channel formation region. That is, the transistor 200 can be said to be an OS transistor.

[0122] OS transistors have oxygen vacancies (V O ) and impurities, the electrical characteristics are likely to fluctuate and reliability may be reduced. In addition, hydrogen near the oxygen vacancy may become a defect in which hydrogen enters the oxygen vacancy (hereinafter referred to as V O H) and generate electrons that serve as carriers. For this reason, when oxygen vacancies are contained in the channel formation region in the oxide semiconductor, the OS transistor is likely to have normally-on characteristics. Therefore, it is preferable that oxygen vacancies and impurities are reduced as much as possible in the channel formation region in the oxide semiconductor. In other words, it is preferable that the carrier concentration in the channel formation region in the oxide semiconductor is reduced and the channel formation region in the oxide semiconductor is made i-type (intrinsic) or substantially i-type.

[0123] On the other hand, the source and drain regions of the OS transistor have more oxygen vacancies than the channel formation region.O It is preferable that the region has a high carrier concentration and low resistance due to a high concentration of H or a high concentration of impurities such as hydrogen, nitrogen, or metal elements. That is, the source and drain regions of the OS transistor are preferably n-type regions with a high carrier concentration and low resistance compared to the channel formation region.

[0124] A region of the oxide semiconductor layer 230 in contact with the insulating layer 280 and its vicinity function as a channel formation region of the transistor 200. One of a region of the oxide semiconductor layer 230 in contact with the conductive layer 220 and a region of the oxide semiconductor layer 230 in contact with the conductive layer 240 functions as a source region and the other functions as a drain region. That is, the channel formation region is sandwiched between the source region and the drain region.

[0125] When the oxide semiconductor layer 230 and the conductive layer 220 come into contact with each other, a metal compound or oxygen vacancy is formed, and the region of the oxide semiconductor layer 230 in contact with the conductive layer 220 has a low resistance. This makes it possible to reduce the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220. Similarly, when the oxide semiconductor layer 230 and the conductive layer 240 come into contact with each other, the region of the oxide semiconductor layer 230 in contact with the conductive layer 240 has a low resistance. This makes it possible to reduce the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240.

[0126] 3A, the insulating layer 280 is in contact with the entire outer periphery of the oxide semiconductor layer 230. Thus, the channel formation region of the transistor 200 can be formed on the entire outer periphery of the oxide semiconductor layer 230 in the opening 290 (the entire region in contact with the insulating layer 280). Note that FIG. 3A can also be considered to be a cross-sectional view in the XY plane including the channel formation region of the oxide semiconductor layer 230.

[0127] The channel length of the transistor 200 is the distance between the source region and the drain region. In other words, it can be said that the channel length of the transistor 200 is determined by the thickness of the insulating layer 280 on the conductive layer 220. In FIG. 2C, the channel length L of the transistor 200 is indicated by a dashed double-headed arrow. The channel length L is the distance between the end of the region where the oxide semiconductor layer 230 and the conductive layer 220 contact each other and the end of the region where the oxide semiconductor layer 230 and the conductive layer 240 contact each other in a cross-sectional view. In other words, the channel length L corresponds to the length of the side surface of the insulating layer 280 on the opening 290 side in a cross-sectional view.

[0128] In a planar transistor, the channel length is limited by the exposure limit of photolithography, making it difficult to further miniaturize the transistor. However, in the transistor included in the semiconductor device of one embodiment of the present invention, the channel length can be set by the thickness of the insulating layer 280. Thus, the channel length of the transistor 200 can be made to be an extremely fine structure that is equal to or less than the exposure limit of photolithography (for example, 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less, and is 0.1 nm or more, 1 nm or more, or 5 nm or more). As a result, the on-state current of the transistor 200 can be increased, and the frequency characteristics can be improved.

[0129] Furthermore, since the channel length of the transistor included in the semiconductor device of one embodiment of the present invention is determined by the thickness of the insulating layer 280 over the conductive layer 220, even when the channel length is set to be long, for example, 60 nm or more, the area occupied by the transistor, specifically, for example, the area of ​​the transistor as viewed from above, is roughly determined by the width of the opening 290. As described later, the width D of the opening 290 is, for example, 5 nm or more, 10 nm or more, or 20 nm or more, and preferably 100 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, or 30 nm or less. For example, even when the channel length is set to 150 nm, the width of the opening 290 can be made narrower than 150 nm. That is, the width of the opening can be narrower than the channel length of the transistor, which reduces the area occupied by the transistor and enables high integration of the semiconductor device.

[0130] Note that by setting the channel length of the transistor to, for example, 1 μm or less, 500 nm or less, or 300 nm or less, productivity and yield can be improved in forming the insulating layer 280, forming the opening 290 in the insulating layer 280, and the like.

[0131] Therefore, the channel length of a transistor included in a semiconductor device of one embodiment of the present invention is preferably 0.1 nm or more, 1 nm or more, or 5 nm or more, and is preferably 1 μm or less, 500 nm or less, or 300 nm or less.

[0132] Furthermore, as described above, a channel formation region, a source region, and a drain region can be formed in the opening 290. As a result, the area occupied by the transistor 200 can be reduced compared to a lateral transistor, for example, a planar transistor, in which the channel formation region, the source region, and the drain region are provided separately on the XY plane. Thus, the semiconductor device can be highly integrated. Furthermore, when the semiconductor device of one embodiment of the present invention is used for a memory device, the memory capacity per unit area can be increased.

[0133] As shown in FIG. 3A, the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 are provided concentrically. Thus, the side surface of the conductive layer 260 provided at the center faces the side surface of the oxide semiconductor layer 230 through the insulating layer 250. That is, in a plan view, the entire circumference of the oxide semiconductor layer 230 becomes a channel formation region. In this case, for example, the channel width of the transistor 200 is determined by the length of the outer periphery of the oxide semiconductor layer 230. That is, it can be said that the channel width of the transistor 200 is determined by the width of the opening 290 (the diameter when the opening 290 is circular in a plan view). In FIGS. 2C and 3A, the width D of the opening 290 is indicated by a double-headed arrow of a two-dot chain line. In FIG. 3A, the channel width W of the transistor 200 is indicated by a double-dot chain line arrow. By increasing the width D of the opening 290, the channel width per unit area can be increased, and the on-current can be increased.

[0134] When the opening 290 is formed by using a photolithography method, the width D of the opening 290 is limited by the exposure limit of the photolithography. The width D of the opening 290 is set by the film thickness of each of the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 provided in the opening 290. The width D of the opening 290 is, for example, 5 nm or more, 10 nm or more, or 20 nm or more, and is preferably 100 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, or 30 nm or less. When the opening 290 is circular in plan view, the width D of the opening 290 corresponds to the diameter of the opening 290, and the channel width W can be calculated as "D x π".

[0135] The channel length L of the transistor 200 is preferably at least shorter than the channel width W of the transistor 200. The channel length L of the transistor 200 is preferably 0.1 to 0.99 times, and more preferably 0.5 to 0.8 times, the channel width W of the transistor 200. With such a structure, a transistor with favorable electrical characteristics and high reliability can be realized.

[0136] In addition, by forming the opening 290 to have a circular shape in a plan view, the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 are provided concentrically. This makes the distance between the conductive layer 260 and the oxide semiconductor layer 230 approximately uniform, so that a gate electric field can be applied to the oxide semiconductor layer 230 approximately uniformly.

[0137] In the present embodiment, the opening 290 is circular in plan view, but the present invention is not limited to this. For example, the opening 290 may be substantially circular such as an ellipse, polygonal such as a rectangle, or polygonal such as a rectangle with rounded corners in plan view.

[0138] 6A shows an enlarged view of a part of the cross section shown in FIG. 2B. As shown in FIG. 6A, a recess overlapping with the opening 290 is formed in the conductive layer 220, and at least a part of the oxide semiconductor layer 230, the insulating layer 250, and the conductive layer 260 is formed to fill the recess. With this structure, it is possible to easily apply the gate electric field of the conductive layer 260 up to the vicinity of the conductive layer 220 of the oxide semiconductor layer 230. The recess of the conductive layer 220 is formed, for example, by overetching when the opening 290 is formed.

[0139] 6A, the opening 290 and the recess of the conductive layer 220 form a continuous opening. In this case, for example, the bottom of the continuous opening becomes the upper surface of the conductive layer 220.

[0140] 6B shows an example in which the conductive layer 220 has a three-layer structure of a conductive layer 220a, a conductive layer 220b on the conductive layer 220a, and a conductive layer 220c on the conductive layer 220b. The bottom surface of a recess in the conductive layer 220 corresponds to the upper surface of the conductive layer 220b, and the side surface of the recess corresponds to the side surface of the conductive layer 220c on the opening 290 side. Here, it is preferable that the shortest distance Tc from the upper surface of the insulating layer 210 to the upper surface of the conductive layer 220c that contacts the insulating layer 280 is longer than the shortest distance Ta from the upper surface of the insulating layer 210 to the upper surface of the insulating layer 250. This can reduce the contact resistance between the side surface of the conductive layer 220c and the oxide semiconductor layer 230. Therefore, a decrease in the on-current of the transistor 200 can be suppressed.

[0141] Fig. 6C is a modification of Fig. 6B. In Fig. 6C, the bottom surface of the recess of the conductive layer 220 is located above the top surface of the conductive layer 220b. As shown in Fig. 6C, the oxide semiconductor layer 230 is not necessarily in contact with the conductive layer 220a or the conductive layer 220b.

[0142] 6D shows an example in which the oxide semiconductor layer 230 is in contact with the upper surface of the conductive layer 220 (the upper surface of the conductive layer 220c in FIG. 6D). Depending on the conditions for forming the opening 290, there is a case in which no recess is provided in the conductive layer 220, as shown in FIG.

[0143] In FIG. 6(D), the bottom of the opening 290 becomes the upper surface of the conductive layer 220.

[0144] When the conductive layer 220 is in contact with the side surface of the oxide semiconductor layer 230, the contact area between the conductive layer 220 and the oxide semiconductor layer 230 can be increased, and the contact resistance can be reduced.

[0145] In addition, by having a region where the conductive layer 220 and the conductive layer 260 overlap each other, for example, a gate electric field is easily applied to a channel formation region of the oxide semiconductor layer 230, which can improve the electrical characteristics of the transistor. Furthermore, since a gate electric field is easily applied to a region of the oxide semiconductor layer 230 in contact with the conductive layer 220, for example, the on-current of the transistor can be increased.

[0146] <Configuration Example 2 of Semiconductor Device> The conductive layer 240 may have a stacked structure of two or more layers. Figure 7(A) is different from Figure 2(B) mainly in that the conductive layer 240 has a stacked structure of a conductive layer 240a and a conductive layer 240b on the conductive layer 240a.

[0147] Fig. 7B is a diagram for explaining angles θ1a, θ1b, θ1c, θ2a, and θ2b, and corresponds to the cross section shown in Fig. 7A. The angles θ2a and θ2b are angles corresponding to the side walls of the conductive layers 240a and 240b, respectively.

[0148] 7A shows an example in which the conductive layer 240 is a two-layer stack, the conductive layer 240 may be a three-layer stack. Each of the conductive layer 260a and the conductive layer 260b may further have a stacked structure.

[0149] 7B, the angle θ2b is larger than the angle θ2a. The angles θ2b and θ2a are each preferably 20 degrees or more and 60 degrees or less, more preferably 20 degrees or more and 50 degrees or less, and further preferably 20 degrees or more and 40 degrees or less. By making the angle θ2b larger than the angle θ2a, the tapered shape at the upper end of the opening 290 can be made into the shape of a recess, and for example, coverage of the upper end of the opening 290 and its vicinity by the oxide semiconductor layer 230 and the insulating layer 250, the conductive layer 260, and the like that are layers thereover can be improved.

[0150] 8(A) and 8(B) show modified examples of FIG. 7(A) and FIG. 7(B), respectively. FIG. 8(A) shows an example in which the lower end of the sidewall of the conductive layer 240b and the upper end of the sidewall of the conductive layer 240a are discontinuous. FIG. 8(B) is a diagram for explaining angles θ1a, θ1b, θ1c, θ2a, and θ2b, and corresponds to the cross section shown in FIG. 8(A). As shown in FIG. 8(B), the lower end of the sidewall of the conductive layer 240b on the opening 290 side is located outward by a length d2 from the upper end of the sidewall of the conductive layer 240a on the opening 290 side.

[0151] 8A, the oxide semiconductor layer 230 has a region in contact with the upper surface of the conductive layer 240a. This can increase the contact area between the oxide semiconductor layer 230 and the conductive layer 240a, thereby reducing the contact resistance. In addition, by forming a stepped shape at the upper end of the opening 290 using the conductive layer 240a and the conductive layer 240b as shown in FIG. 8A, the coverage of the upper end of the opening 290 and its vicinity by the oxide semiconductor layer 230 and the insulating layer 250, the conductive layer 260, and the like that are thereover can be improved.

[0152] <Configuration Example 3 of Semiconductor Device> 9(A) is different from FIG. 4(B) mainly in that the conductive layer 240 has a laminated structure of a conductive layer 240a and a conductive layer 240b on the conductive layer 240a. In addition, in FIG. 9(A), the end of the conductive layer 240b on the opening 290 side is located outside the end of the conductive layer 240a on the opening 290 side. Therefore, the conductive layer 240a and the conductive layer 240b form a stepped shape.

[0153] Fig. 9(B) is a diagram for explaining angles θ1a, θ1b, θ1c, θ2a, and θ2b, and corresponds to the cross section shown in Fig. 9(A). The angles θ2a and θ2b are angles corresponding to the side walls of the conductive layers 240a and 240b, respectively. The lower end of the side wall of the conductive layer 240b on the opening 290 side is located outward by a length d2 from the upper end of the side wall of the conductive layer 240a on the opening 290 side.

[0154] 9A shows an example in which the conductive layer 240 is a two-layer stack, but the conductive layer 240 may be a three-layer stack. In FIG 9B, an example in which the insulating layer 280a, the insulating layer 280b, the insulating layer 280c, the conductive layer 240a, and the conductive layer 240b each have a steep sidewall is shown, but each sidewall may have a tapered shape.

[0155] <Insulating Layer 283 and Insulating Layer 285> 10A, in the semiconductor device, an insulating layer 283 over the transistor 200 and an insulating layer 285 over the insulating layer 283 can be provided. The insulating layer 283 and the insulating layer 285 each function as an interlayer film. The insulating layer 283 is provided to cover the conductive layer 260, the insulating layer 280, and the like. The example structure shown in FIG. 10A can be manufactured, for example, by forming the insulating layer 283 using a film formation method that has high coverage and forms a film isotropically, and then forming the insulating layer 285 with a planarized upper surface over the insulating layer 283.

[0156] <Modifications of the semiconductor device> 10B includes an insulating layer 283 and an insulating layer 285 over the transistor 200, and a conductive layer 265 over the insulating layer 285. It is preferable that the height of a top surface of the conductive layer 260 and the height of a top surface of the insulating layer 285 are the same or approximately the same. The conductive layer 265 is provided over the insulating layer 285, the insulating layer 283, and the conductive layer 260. The conductive layer 260 and the conductive layer 265 are electrically connected to each other. It is preferable that the conductive layer 265 be in contact with the top surface of the conductive layer 260.

[0157] 10B, the area where the conductive layer 260 and the conductive layer 240 overlap over the insulating layer 280 is extremely small. In addition, since the insulating layer 285 is provided between the conductive layer 265 and the conductive layer 240, the parasitic capacitance between the conductive layer 265 and the conductive layer 240 can be reduced by making the insulating layer 285 thicker.

[0158] <Materials for semiconductor devices> Materials that can be used in the semiconductor device of this embodiment will be described below. Each layer constituting the semiconductor device of this embodiment may have a single layer structure or a multilayer structure.

[0159] [Insulation layer] It is preferable to use an inorganic insulating film for each of the insulating layers (insulating layer 210, insulating layer 250, insulating layer 280, insulating layer 283, insulating layer 285, etc.) included in the semiconductor device. Examples of the inorganic insulating film include an oxide insulating film, a nitride insulating film, an oxynitride insulating film, and a nitride oxide insulating film. Examples of the oxide insulating film include a silicon oxide film, an aluminum oxide film, a magnesium oxide film, a gallium oxide film, a germanium oxide film, an yttrium oxide film, a zirconium oxide film, a lanthanum oxide film, a neodymium oxide film, a hafnium oxide film, a tantalum oxide film, a cerium oxide film, a gallium zinc oxide film, and a hafnium aluminate film. Examples of the nitride insulating film include a silicon nitride film and an aluminum nitride film. Examples of the oxynitride insulating film include a silicon oxynitride film, an aluminum oxynitride film, a gallium oxynitride film, an yttrium oxynitride film, and a hafnium oxynitride film. Examples of the nitride oxide insulating film include a silicon nitride oxide film and an aluminum nitride oxide film. An organic insulating film may be used for the insulating layer of the semiconductor device.

[0160] In addition, the transistor using a metal oxide can have stable electrical characteristics by being surrounded by an insulating layer having a function of suppressing the permeation of impurities and oxygen. As the insulating layer having a function of suppressing the permeation of impurities and oxygen, for example, an insulating layer containing one or more selected from boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, and tantalum can be used in a single layer or a stacked layer. Specifically, as a material for the insulating layer having a function of suppressing the permeation of impurities and oxygen, metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide, and metal nitrides such as aluminum nitride, silicon nitride oxide, and silicon nitride can be used.

[0161] Specifically, it is preferable to use a barrier insulating layer against impurities such as water and hydrogen, and oxygen.

[0162] In this specification and the like, a barrier insulating layer refers to an insulating layer having barrier properties. The barrier properties refer to a property in which a corresponding substance is difficult to diffuse, a property in which a corresponding substance is difficult to permeate, a property in which the permeability of a corresponding substance is low, a function of suppressing the diffusion of a corresponding substance, or a function of suppressing the permeation of a corresponding substance. Note that hydrogen when described as a corresponding substance includes, for example, a hydrogen atom, a hydrogen molecule, a water molecule, and OH. - In addition, impurities when described as a corresponding substance refer to impurities in the channel formation region or semiconductor layer unless otherwise specified, and refer to at least one of, for example, hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules (NO, NO, NO, etc.), copper atoms, etc. In addition, oxygen when described as a corresponding substance refers to at least one of, for example, oxygen atoms, oxygen molecules, etc.

[0163] Examples of the insulating layer having a function of suppressing the permeation of impurities such as water and hydrogen, and oxygen include metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide. Other examples include oxides containing aluminum and hafnium (hafnium aluminate). Other examples include metal nitrides such as aluminum nitride, silicon nitride oxide, and silicon nitride.

[0164] An insulating layer, such as a gate insulating layer, that is in contact with an oxide semiconductor layer or that is provided near the oxide semiconductor layer is preferably an insulating layer having a region containing oxygen that is released by heating (hereinafter may be referred to as excess oxygen). For example, when an insulating layer having a region containing excess oxygen is in contact with an oxide semiconductor layer or is located near the oxide semiconductor layer, oxygen vacancies in the oxide semiconductor layer can be reduced. Examples of an insulating layer that is likely to form a region containing excess oxygen include silicon oxide, silicon oxynitride, and silicon oxide having vacancies.

[0165] Furthermore, for example, as transistors become finer and more highly integrated, problems such as leakage current may occur due to the thinning of the gate insulating layer. By using a material with a high relative dielectric constant (high-k) for the gate insulating layer, it is possible to reduce the voltage during transistor operation while maintaining the physical film thickness. In addition, it is possible to thin the equivalent oxide thickness (EOT) of the gate insulating layer. In addition, by using a material with a high relative dielectric constant as the dielectric layer of a capacitance element, it is possible to make the element have a larger capacitance value. On the other hand, by using a material with a low relative dielectric constant for the insulating layer that functions as an interlayer film, it is possible to reduce the parasitic capacitance generated between wirings. Therefore, it is advisable to select a material according to the function of the insulating layer. In addition, a material with a low relative dielectric constant also has a high dielectric strength.

[0166] Examples of materials having a high relative dielectric constant include aluminum oxide, gallium oxide, hafnium oxide, tantalum oxide, zirconium oxide, hafnium zirconium oxide, oxides having aluminum and hafnium, oxynitrides having aluminum and hafnium, oxides having silicon and hafnium, oxynitrides having silicon and hafnium, and nitrides having silicon and hafnium.

[0167] Examples of materials with a low relative dielectric constant include resins such as polyester, polyolefin, polyamide (nylon, aramid, etc.), polyimide, polycarbonate, and acrylic resin. Examples of other inorganic insulating materials with a low relative dielectric constant include silicon oxide with fluorine added, silicon oxide with carbon added, and silicon oxide with carbon and nitrogen added. Examples of silicon oxides include silicon oxides having vacancies. These silicon oxides may contain nitrogen.

[0168] Furthermore, for example, inorganic insulating materials such as silicon oxide, silicon oxynitride, and silicon nitride oxide can be applied to both layers in which a material with a high dielectric constant is preferably used, such as a gate insulating layer, and layers in which a material with a low dielectric constant is preferably used, such as an interlayer film. These materials have a relatively low dielectric constant compared to high-k materials such as hafnium oxide, and therefore may be referred to as materials with a low dielectric constant in this specification and the like.

[0169] Furthermore, a material capable of exhibiting ferroelectricity may be used for an insulating layer of a semiconductor device. Examples of the material capable of exhibiting ferroelectricity include hafnium oxide, zirconium oxide, and HfZrO. X(X is a real number greater than 0). Examples of materials that can have ferroelectricity include materials in which an element J1 (here, element J1 is one or more selected from zirconium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) is added to hafnium oxide. Here, the ratio of the number of hafnium atoms to the number of element J1 can be set appropriately, for example, the ratio of the number of hafnium atoms to the number of element J1 can be set to 1:1 or close thereto. Examples of materials that can have ferroelectricity include materials in which an element J2 (here, element J2 is one or more selected from hafnium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) is added to zirconium oxide. Also, the ratio of the number of zirconium atoms to the number of element J2 can be set appropriately, for example, the ratio of the number of zirconium atoms to the number of element J2 can be set to 1:1 or close thereto. In addition, lead titanate (PbTiO X Piezoelectric ceramics having a perovskite structure, such as barium strontium titanate (BST), strontium titanate, lead zirconate titanate (PZT), strontium bismuth tantalate (SBT), bismuth ferrite (BFO), and barium titanate, may also be used.

[0170] In addition, examples of materials that can have ferroelectricity include metal nitrides having elements M1, M2, and nitrogen. Here, the element M1 is one or more selected from aluminum, gallium, indium, etc. In addition, the element M2 is one or more selected from boron, scandium, yttrium, lanthanum, cerium, neodymium, europium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, etc. In addition, the ratio of the number of atoms of element M1 to the number of atoms of element M2 can be set appropriately. In addition, metal oxides having elements M1 and nitrogen may have ferroelectricity even if they do not contain element M2. In addition, examples of materials that can have ferroelectricity include materials in which element M3 is added to the above metal nitrides. In addition, element M3 is one or more selected from magnesium, calcium, strontium, zinc, cadmium, etc. In addition, the ratio of the number of atoms of element M1, the number of atoms of element M2, and the number of atoms of element M3 can be set appropriately.

[0171] Moreover, examples of materials that can have ferroelectricity include perovskite-type oxynitrides such as SrTaO2N and BaTaO2N, and GaFeO3 with a κ-alumina structure.

[0172] In the above description, metal oxides and metal nitrides are exemplified as materials that can have ferroelectricity, but the present invention is not limited thereto. For example, metal oxynitrides in which nitrogen is added to the above-mentioned metal oxides, or metal oxynitrides in which oxygen is added to the above-mentioned metal nitrides, etc. may be used.

[0173] As a material capable of having ferroelectricity, for example, a mixture or compound made of a plurality of materials selected from the materials listed above can be used. Alternatively, the insulating layer 130 can have a laminated structure made of a plurality of materials selected from the materials listed above. However, the crystal structure (characteristics) of the materials listed above may change depending on not only the film formation conditions but also various processes, so in this specification, not only materials that exhibit ferroelectricity are called ferroelectrics, but also materials capable of having ferroelectricity.

[0174] Metal oxides containing hafnium and / or zirconium can have ferroelectricity even in a thin film of a few nm. Metal oxides containing hafnium and / or zirconium can have ferroelectricity even in a small area. Therefore, by using metal oxides containing hafnium and / or zirconium, it is possible to miniaturize semiconductor devices.

[0175] In this specification, a layer of a material that can have ferroelectricity may be referred to as a ferroelectric layer. In addition, a device having such a ferroelectric layer, metal oxide film, or metal nitride film may be referred to as a ferroelectric device.

[0176] It is said that ferroelectricity is expressed by displacing oxygen or nitrogen in the crystals contained in the ferroelectric layer due to an external electric field. It is also presumed that the expression of ferroelectricity depends on the crystal structure of the crystals contained in the ferroelectric layer. Therefore, in order for the insulating layer to express ferroelectricity, the insulating layer 130 needs to contain crystals. In particular, it is preferable for the insulating layer to contain crystals having an orthorhombic crystal structure, since ferroelectricity is expressed. The crystal structure of the crystals contained in the insulating layer may be one or more selected from the cubic, tetragonal, orthorhombic, monoclinic, and hexagonal crystal systems. The insulating layer may have an amorphous structure. In this case, the insulating layer may be a composite structure having an amorphous structure and a crystalline structure.

[0177] The insulating layer 250 functions as a gate insulating layer of the transistor 200. For the insulating layer 250, a material with a high dielectric constant is preferably used.

[0178] The insulating layer 250 preferably has a function of capturing hydrogen and fixing hydrogen. This can reduce the hydrogen concentration in the oxide semiconductor layer 230 (particularly, the hydrogen concentration in the channel formation region of the transistor). OBy reducing H, the channel formation region can be made i-type or substantially i-type.

[0179] Examples of materials for the insulating layer having the function of capturing or fixing hydrogen include metal oxides such as oxides containing hafnium, oxides containing aluminum, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing magnesium. These metal oxides may further contain zirconium, and examples thereof include oxides containing hafnium and zirconium. Here, in metal oxides having an amorphous structure, some oxygen atoms have dangling bonds, so that the ability to capture or fix hydrogen is high. Therefore, these metal oxides preferably have an amorphous structure. For example, the amorphous structure may be realized by including silicon in these oxides. For example, it is preferable to use an oxide containing hafnium and silicon (hafnium silicate). Note that the metal oxide may have one or both of a crystalline region and a crystal grain boundary in a part.

[0180] The function of capturing or fixing a corresponding substance can also be said to have a property that makes it difficult for the corresponding substance to diffuse. Therefore, the function of capturing or fixing a corresponding substance can be rephrased as a barrier property.

[0181] When the insulating layer 250 has a stacked structure, it is preferable to use a layer having a function of trapping and fixing hydrogen as one of the layers (hereinafter referred to as a first insulating layer of the insulating layer 250). When the insulating layer 250 has a stacked structure of two layers, a layer having a function of trapping and fixing hydrogen is used as a layer in contact with the oxide semiconductor layer 230, and when the insulating layer 250 has a stacked structure of three or more layers, a layer having a function of trapping and fixing hydrogen is used as a layer close to the oxide semiconductor layer 230, so that hydrogen contained in the oxide semiconductor layer 230 can be more effectively trapped or fixed. Thus, the hydrogen concentration in the oxide semiconductor layer 230 can be reduced.

[0182] In addition to the first insulating layer, the insulating layer 250 preferably uses a barrier insulating layer against hydrogen as a second insulating layer. Examples of materials for the barrier insulating layer against hydrogen include aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, silicon nitride, and silicon nitride oxide.

[0183] The insulating layer 250 may be made of, for example, hafnium silicate as the first insulating layer. The insulating layer 250 may preferably have an amorphous structure as the first insulating layer. By making the structure amorphous, the formation of grain boundaries can be suppressed. By suppressing the formation of grain boundaries, the flatness of the insulating layer can be improved. This makes the film thickness distribution of the insulating layer uniform, and the extremely thin film thickness portions can be reduced, thereby improving the withstand voltage of the insulating layer. In addition, the film thickness distribution of the film provided on the insulating layer can be made uniform.

[0184] Moreover, by suppressing the formation of grain boundaries in the insulating layer, leakage current caused by defect levels in the grain boundaries can be reduced, and the insulating layer can function as an insulating film with low leakage current.

[0185] In addition, hafnium oxide is a material with a high dielectric constant, so hafnium silicate can also be a material with a high dielectric constant depending on the silicon content. Therefore, when used as a gate insulating layer, it is possible to reduce the gate potential applied during transistor operation while maintaining the physical thickness of the gate insulating layer. It also makes it possible to reduce the equivalent oxide thickness (EOT) of the gate insulating layer.

[0186] In view of the above, it is preferable to use an oxide containing one or both of aluminum and hafnium as the first insulating layer of insulating layer 250, it is more preferable to use an oxide having an amorphous structure and containing one or both of aluminum and hafnium, and it is even more preferable to use aluminum oxide having an amorphous structure.

[0187] Furthermore, by using a barrier insulating layer against hydrogen as the second insulating layer of the insulating layer 250, it is possible to suppress the diffusion of impurities contained in the conductive layer 260 into the oxide semiconductor layer 230. Silicon nitride has a high barrier property against hydrogen and is therefore suitable for the insulating layer 250. Here, the second insulating layer is preferably an upper layer of the first insulating layer.

[0188] With such a structure, a semiconductor device having good electrical characteristics, a highly reliable semiconductor device, a semiconductor device with less variation in the electrical characteristics of the transistors, and a semiconductor device with a large on-current can be provided.

[0189] Additionally, insulating layer 250 may comprise an insulating layer of a thermally stable structure, such as silicon oxide or silicon oxynitride.

[0190] The insulating layer 250 preferably includes a layer capable of supplying oxygen to the oxide semiconductor layer 230. An oxide can be used as the layer capable of supplying oxygen. When the insulating layer 250 includes silicon oxide or silicon oxynitride, oxygen can be suitably supplied from the insulating layer 250 to the oxide semiconductor layer 230.

[0191] Furthermore, the insulating layer 250 may have an insulating layer having a thermally stable structure between a pair of insulating layers having the functions of capturing and fixing hydrogen.

[0192] The insulating layer 250 preferably has a barrier insulating layer against oxygen, which can suppress oxidation of the conductive layer 240, the conductive layer 260, etc. When the insulating layer 250 has a stacked structure, each of the layer in contact with the conductive layer 240 and the layer in contact with the conductive layer 260 is preferably a barrier insulating layer against oxygen.

[0193] The layer in the insulating layer 250 that is in contact with the conductive layer 240 is preferably less permeable to oxygen than at least the insulating layer 280. When the layer has a barrier property against oxygen, the side surface of the conductive layer 240 can be prevented from being oxidized and an oxide film can be prevented from being formed on the side surface. This can prevent a decrease in the on-state current or a decrease in the field-effect mobility of the transistor 200.

[0194] For example, by using a barrier insulating layer against hydrogen and oxygen for the above-mentioned second insulating layer, it is possible to suppress oxidation of the conductive layer 260. In addition, it is possible to suppress the oxygen contained in the oxide semiconductor layer 230 from diffusing into the conductive layer 260 and the formation of oxygen vacancies in the oxide semiconductor layer 230.

[0195] Examples of the barrier insulating layer against oxygen include oxides containing hafnium, oxides containing aluminum, oxides containing aluminum and hafnium (hafnium aluminate), magnesium oxide, gallium oxide, gallium zinc oxide, silicon nitride, and silicon nitride oxide. Examples of oxides containing one or both of aluminum and hafnium include aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing hafnium and silicon (hafnium silicate).

[0196] Hafnium and silicon-containing oxides (hafnium silicate) function as a barrier insulating layer against oxygen, and as mentioned above, they are also excellent insulating layers that can easily achieve an amorphous structure and have the ability to capture or fix hydrogen.

[0197] Furthermore, silicon nitride is an excellent insulating layer that not only functions as a barrier insulating layer against oxygen, but also has high barrier properties against hydrogen, as described above.

[0198] The insulating layer 250 preferably has a two-layer structure in which a first insulating layer having a function of capturing or fixing hydrogen and a second insulating layer having a barrier property against hydrogen and oxygen are stacked in this order from the oxide semiconductor layer 230 side.

[0199] As an example, the first insulating layer may be made of an oxide containing one or both of aluminum and hafnium, and the second insulating layer may be made of silicon nitride.

[0200] In addition, it is preferable to use a three-layer structure in which, from the oxide semiconductor layer 230 side, a third insulating layer having a material with a relatively low dielectric constant, a first insulating layer having a function of capturing or fixing hydrogen, and a second insulating layer having a barrier property against hydrogen and oxygen are stacked in this order. The material with a relatively low dielectric constant of the third insulating layer refers to, for example, a material with a lower dielectric constant than any one or more of the other layers in the stacked structure. Here, silicon oxide or silicon oxynitride can be used as the third insulating layer. The third insulating layer is a layer in contact with the oxide semiconductor layer 230. By using an oxide for the third insulating layer, oxygen can be supplied to the oxide semiconductor layer 230. In addition, by providing the second insulating layer, it is possible to suppress the diffusion of oxygen contained in the third insulating layer into the conductive layer 260, and thus to suppress the oxidation of the conductive layer 260. In addition, it is possible to suppress a decrease in the amount of oxygen supplied from the third insulating layer to the oxide semiconductor layer 230.

[0201] As an example, silicon oxide or silicon oxynitride can be used as the third insulating layer, an oxide containing one or both of aluminum and hafnium can be used as the first insulating layer, and silicon nitride can be used as the second insulating layer.

[0202] The insulating layer 250 preferably has a four-layer structure in which a fourth insulating layer having a barrier property against oxygen, a third insulating layer made of a material with a relatively low dielectric constant, a first insulating layer having a function of trapping or fixing hydrogen, and a second insulating layer having a barrier property against hydrogen and oxygen are stacked in this order from the oxide semiconductor layer 230 side. The first to third insulating layers can have a similar structure to that of the layers used in the above-described three-layer structure. The fourth insulating layer is a layer in contact with the oxide semiconductor layer 230. The fourth insulating layer has a barrier property against oxygen, which can suppress desorption of oxygen from the oxide semiconductor layer 230. For example, aluminum oxide is preferably used as the fourth insulating layer. Aluminum oxide has a function of trapping or fixing hydrogen, and is therefore suitable as the fourth insulating layer in contact with the oxide semiconductor layer 230.

[0203] As an example, aluminum oxide can be used as the fourth insulating layer, silicon oxide or silicon oxynitride can be used as the third insulating layer, an oxide containing one or both of aluminum and hafnium can be used as the first insulating layer, and silicon nitride can be used as the second insulating layer.

[0204] In particular, the thickness of the insulating layer 250 in a region overlapping with the channel formation region of the oxide semiconductor layer 230 is preferably 0.1 nm to 30 nm, more preferably 0.1 nm to 20 nm, more preferably 0.1 nm to 10 nm, more preferably 0.1 nm to 8.0 nm, and still more preferably 0.5 nm to 7.0 nm.

[0205] In order to miniaturize the transistor, it is preferable that the thickness of each layer constituting the insulating layer 250 is thin. For example, the thickness of each layer constituting the insulating layer 250 is 0.1 nm to 10 nm, or 0.1 nm to 5 nm, or 0.5 nm to 5 nm, or 1 nm to less than 5 nm, or 1 nm to 3 nm. Each layer constituting the insulating layer 250 may have a region with the above thickness in at least a part thereof.

[0206] Typically, the thicknesses of the fourth insulating layer, the third insulating layer, the first insulating layer, and the second insulating layer are 1 nm, 2 nm, 2 nm, and 1 nm, respectively. With such a structure, the transistor can have good electrical characteristics even when miniaturized or highly integrated.

[0207] Since the insulating layer 210 functions as an interlayer film, it is preferable that the insulating layer 210 has a low relative dielectric constant. By using a material with a low relative dielectric constant for the interlayer film, the parasitic capacitance generated between wirings can be reduced. Silicon oxide and silicon oxynitride are both thermally stable, and therefore are suitable for the insulating layer 210.

[0208] The concentration of impurities such as water and hydrogen in the insulating layer 210 is preferably reduced. This can prevent impurities such as water and hydrogen from entering a channel formation region of the oxide semiconductor layer 230.

[0209] In addition, a barrier insulating layer against hydrogen is preferably used as the insulating layer 210. When the insulating layer 210 provided on the outer side of the oxide semiconductor layer 230 has a barrier property against hydrogen, diffusion of hydrogen into the oxide semiconductor layer 230 can be suppressed.

[0210] Examples of materials for the barrier insulating layer against hydrogen include aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, silicon nitride, and silicon nitride oxide.

[0211] For example, it is preferable to use a silicon nitride film as the insulating layer 210.

[0212] The insulating layer 210 may have a two-layer structure. For example, an insulating layer having a function of trapping or fixing hydrogen can be used as an upper layer of the insulating layer 210. In this manner, hydrogen in the oxide semiconductor layer 230 can be diffused to the upper layer of the insulating layer 210 through the conductive layer 220 and the hydrogen can be trapped or fixed. As a result, the hydrogen concentration in the oxide semiconductor layer 230 can be reduced.

[0213] For example, it is preferable to use a silicon nitride film as the lower layer of the insulating layer 210 and an oxide film containing hafnium and silicon (hafnium silicate film) as the upper layer.

[0214] A barrier insulating layer against hydrogen is preferably used for one or more of the insulating layer 283 and the insulating layer 285. This can suppress diffusion of hydrogen from above the insulating layer 283 to the oxide semiconductor layer 230. A silicon nitride film and a silicon nitride oxide film each have characteristics of releasing little impurities (for example, water and hydrogen) from themselves and being less permeable to oxygen and hydrogen, and therefore can be preferably used for the insulating layer 283.

[0215] It is particularly preferable to use silicon nitride formed by a sputtering method as one or more of the insulating layers 283 and 285. The sputtering method does not require the use of molecules containing hydrogen in a deposition gas, and therefore the hydrogen concentration in the insulating layer 283 can be reduced. Furthermore, by forming the insulating layer 283 by a sputtering method, silicon nitride with high density can be formed.

[0216] Alternatively, an insulating layer having a function of trapping or fixing hydrogen may be used as one or more of the insulating layers 283 and 285. With such a structure, diffusion of hydrogen from above the insulating layers 283 and 285 to the oxide semiconductor layer 230 can be suppressed, and hydrogen contained in the oxide semiconductor layer 230 can be trapped or fixed. Thus, the hydrogen concentration in the oxide semiconductor layer 230 can be reduced. Hafnium silicate, or the like can be used as one or more of the insulating layers 283 and 285.

[0217] Alternatively, the insulating layer 283 may have a stacked structure of an insulating layer having a function of capturing or fixing hydrogen and a barrier insulating layer against hydrogen. For example, the insulating layer 283 may be a stacked film of aluminum oxide and silicon nitride over the aluminum oxide.

[0218] In addition, the semiconductor device may have a structure in which either the insulating layer 283 or the insulating layer 285 is not provided.

[0219] In addition, for example, a material with a low relative dielectric constant can be used as the insulating layer 285. By using a material with a low relative dielectric constant as an interlayer film, parasitic capacitance occurring between wirings can be reduced.

[0220] The concentration of impurities such as water and hydrogen in the insulating layer 285 is preferably reduced. This can prevent impurities such as water and hydrogen from entering a channel formation region of the oxide semiconductor layer 230.

[0221] The insulating layer 280 preferably has the above-mentioned barrier insulating layer against hydrogen. The insulating layer 280 is provided so as to surround the oxide semiconductor layer 230. The insulating layer 280 provided on the outer side of the oxide semiconductor layer 230 has a barrier property against hydrogen, and thus can suppress diffusion of hydrogen into the oxide semiconductor layer 230. For example, the insulating layer 280 preferably has a silicon nitride film.

[0222] Silicon nitride also has a barrier property against oxygen. Therefore, by using silicon nitride for the insulating layer 280, oxygen can be prevented from being extracted from the oxide semiconductor layer 230, and an excessive amount of oxygen vacancies can be prevented from being formed in the oxide semiconductor layer 230.

[0223] Furthermore, the use of silicon nitride for the insulating layer 280 can prevent excess oxygen from being supplied to the oxide semiconductor layer 230. Thus, excess oxygen can be prevented from being contained in the channel formation region of the oxide semiconductor layer 230, which can improve the reliability of the transistor 200.

[0224] The insulating layer 280 preferably includes the above-described insulating oxide insulating film, the oxynitride insulating film, or the insulating layer having a region containing excess oxygen.

[0225] For example, an insulating layer having a region containing excess oxygen can be formed by deposition in an atmosphere containing oxygen using a sputtering method. In addition, by using a sputtering method that does not require the use of molecules containing hydrogen in the deposition gas, the hydrogen concentration in the insulating layer 280 can be reduced. By depositing at least a part of the layers constituting the insulating layer 280 in this manner, oxygen can be supplied from the insulating layer 280 to the channel formation region of the oxide semiconductor layer 230, thereby reducing oxygen vacancies and VoH.

[0226] The concentration of impurities such as water and hydrogen in the insulating layer 280 is preferably reduced. This can prevent impurities such as water and hydrogen from entering a channel formation region of the oxide semiconductor layer 230.

[0227] Since the thickness of the insulating layer 280 on the conductive layer 220 corresponds to the channel length of the transistor 200 , the thickness of the insulating layer 280 is appropriately set in accordance with the design value of the channel length of the transistor 200 .

[0228] The insulating layer 280 preferably has a laminated structure of, for example, an insulating layer 280a, an insulating layer 280b on the insulating layer 280a, and an insulating layer 280c on the insulating layer 280b.

[0229] The insulating layer 280b is a layer in contact with a channel formation region of the oxide semiconductor layer 230. When an insulating layer containing oxygen is used as the insulating layer 280b, oxygen can be supplied to the oxide semiconductor layer 230.

[0230] The insulating layer 280b preferably has a region with a higher oxygen content than at least one of the insulating layer 280a and the insulating layer 280c. In particular, the insulating layer 280b preferably has a region with a higher oxygen content than each of the insulating layer 280a and the insulating layer 280c. By increasing the oxygen content of the insulating layer 280b, it becomes easier to form an i-type region in the oxide semiconductor layer 230 near the insulating layer 280b.

[0231] It is more preferable that the insulating layer 280b be a film that releases oxygen when heated. When the insulating layer 280b releases oxygen due to heat applied during the manufacturing process of the transistor 200, oxygen can be supplied to the oxide semiconductor layer 230. When oxygen is supplied from the insulating layer 280b to the oxide semiconductor layer 230, particularly to the channel formation region of the oxide semiconductor layer 230, oxygen vacancies and V O H can be reduced, and a highly reliable transistor can be obtained that exhibits favorable electrical characteristics.

[0232] In order to improve the electrical characteristics and reliability of an OS transistor, it is important to sufficiently reduce the hydrogen concentration in the oxide semiconductor and then optimize the amount of oxygen supplied to the oxide semiconductor.

[0233] As an example, the amount of oxygen molecules released from the insulating layer 280b is 1.0×10 14 molecules / cm 2 That's it, 1.0 x 10 15 molecules / cm 2 The amount of released oxygen molecules can be measured by thermal desorption spectrometry.

[0234] In particular, when the channel length of the transistor 200 is small, oxygen vacancies in the channel formation region and V O The influence of H on the electrical characteristics and reliability is particularly large. Therefore, by optimizing the amount of oxygen supplied to the oxide semiconductor layer 230 after sufficiently reducing the hydrogen concentration in the oxide semiconductor layer 230, a transistor with a short channel length, excellent electrical characteristics, and high reliability can be realized.

[0235] The insulating layer 280b is preferably formed by a deposition method such as a sputtering method or a PECVD method. In particular, when a sputtering method is used, hydrogen gas is not required as a deposition gas, and therefore a film with an extremely low hydrogen content can be obtained. Therefore, the supply of hydrogen to the oxide semiconductor layer 230 can be suppressed, and the electrical characteristics of the transistor 200 can be stabilized.

[0236] In order to increase the amount of oxygen supplied to the oxide semiconductor layer 230, for example, heat treatment in an atmosphere containing oxygen or plasma treatment in an atmosphere containing oxygen may be performed after the insulating layer 280b is formed. Alternatively, oxygen may be supplied by forming an oxide film in an oxygen atmosphere on the top surface of the insulating layer 280b by a sputtering method. The oxide film may then be removed. By performing such treatment, oxygen can be supplied to the insulating layer 280b, and the amount of oxygen supplied to the oxide semiconductor layer 230 can be increased.

[0237] In addition, the amount of oxygen supplied to the region of the oxide semiconductor layer 230 in contact with the insulating layer 280a and the region of the oxide semiconductor layer 230 in contact with the insulating layer 280c is smaller than that to the region of the oxide semiconductor layer 230 in contact with the insulating layer 280b. Therefore, the resistance of the region of the oxide semiconductor layer 230 in contact with the insulating layer 280a and the region of the oxide semiconductor layer 230 in contact with the insulating layer 280c may be reduced. In other words, by adjusting the thickness of the insulating layer 280a, the range of the region that functions as one of the source region and the drain region can be controlled. Similarly, by adjusting the thickness of the insulating layer 280c, the range of the region that functions as the other of the source region and the drain region can be controlled. In this way, the thicknesses of the insulating layers 280a and 280c can be appropriately set according to the characteristics required for the transistor.

[0238] In addition, it is preferable to use a material with a low relative dielectric constant for the insulating layer 280b, which can reduce the parasitic capacitance between wirings. For example, silicon oxide or silicon oxynitride can be used for the insulating layer 280b.

[0239] It is preferable to use a barrier insulating layer against oxygen for each of the insulating layer 280a and the insulating layer 280c. By providing the insulating layer 280a between the insulating layer 280b and the conductive layer 220, it is possible to prevent the conductive layer 220 from being oxidized and the resistance of the conductive layer 220 from increasing. In addition, by providing the insulating layer 280c between the insulating layer 280b and the conductive layer 240, it is possible to prevent the conductive layer 240 from being oxidized and the resistance of the conductive layer 240 from increasing.

[0240] Alternatively, an insulating layer having a function of trapping or fixing hydrogen may be used as the insulating layer 280a. With such a structure, hydrogen can be prevented from diffusing from below the insulating layer 280a to the oxide semiconductor layer 230, and hydrogen contained in the oxide semiconductor layer 230 can be trapped or fixed. Thus, the hydrogen concentration in the oxide semiconductor layer 230 can be reduced. As the insulating layer 280a, magnesium oxide, aluminum oxide, hafnium oxide, or an oxide containing hafnium and silicon can be used. Alternatively, for example, a stacked film of aluminum oxide and silicon nitride on the aluminum oxide may be used as the insulating layer 280a. Similarly, an insulating layer having a function of trapping or fixing hydrogen may be used as the insulating layer 280c.

[0241] For example, the insulating layer 280a and the insulating layer 280c can be made of silicon nitride, and the insulating layer 280b can be made of silicon oxide.

[0242] [Conductive layer] For the conductive layers (conductive layer 220, conductive layer 240, conductive layer 260, etc.) of the semiconductor device, it is preferable to use a metal element selected from tungsten, copper, aluminum, chromium, silver, gold, platinum, zinc, tantalum, nickel, titanium, iron, cobalt, molybdenum, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, lanthanum, etc., or an alloy containing the above-mentioned metal elements as a component, or an alloy combining the above-mentioned metal elements, etc. As the alloy containing the above-mentioned metal elements as a component, a nitride of the alloy or an oxide of the alloy may be used. For example, it is preferable to use tantalum nitride, titanium nitride, ruthenium nitride, nitride containing molybdenum, nitride containing tungsten, titanium, and aluminum, nitride containing tantalum and aluminum, ruthenium oxide, oxide containing strontium and ruthenium, oxide containing lanthanum and nickel, etc. Furthermore, a semiconductor having high electrical conductivity, typified by polycrystalline silicon containing an impurity element such as phosphorus, or a silicide such as nickel silicide may be used.

[0243] In addition, conductive materials containing nitrogen such as nitrides containing tantalum, nitrides containing titanium, nitrides containing molybdenum, nitrides containing tungsten, nitrides containing ruthenium, nitrides containing tantalum and aluminum, or nitrides containing titanium and aluminum, conductive materials containing oxygen such as ruthenium oxide, oxides containing strontium and ruthenium, or oxides containing lanthanum and nickel, and materials containing metal elements such as titanium, tantalum, or ruthenium are preferred because they are conductive materials that are difficult to oxidize, conductive materials that have a function of suppressing oxygen diffusion, or materials that maintain conductivity even when oxygen is absorbed. Note that examples of conductive materials containing oxygen include indium oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide (also referred to as ITO), indium tin oxide containing titanium oxide, indium tin oxide with added silicon (also referred to as ITSO), indium zinc oxide (also referred to as IZO (registered trademark)), and indium zinc oxide containing tungsten oxide. In this specification and the like, a conductive film formed using a conductive material containing oxygen may be called an oxide conductive film.

[0244] Conductive materials based on tungsten, copper, or aluminum are preferred because they have high electrical conductivity.

[0245] A plurality of conductive layers formed of the above-mentioned materials may be stacked. For example, a stacked structure may be formed by combining the above-mentioned material containing a metal element and a conductive material containing oxygen. A stacked structure may be formed by combining the above-mentioned material containing a metal element and a conductive material containing nitrogen. A stacked structure may be formed by combining the above-mentioned material containing a metal element, a conductive material containing oxygen, and a conductive material containing nitrogen.

[0246] In addition, when a metal oxide is used for the channel formation region of a transistor, it is preferable to use a stacked structure in which a material containing the above-mentioned metal element and a conductive material containing oxygen are combined for the conductive layer that functions as a gate electrode. In this case, it is preferable to provide the conductive material containing oxygen on the channel formation region side. By providing the conductive material containing oxygen on the channel formation region side, oxygen desorbed from the conductive material is easily supplied to the channel formation region.

[0247] The conductive layer 260 can be made of the above-mentioned metal elements, alloys containing the above-mentioned metal elements, or alloys combining the above-mentioned metal elements. For example, it is preferable to use a material with high conductivity, such as tungsten. In addition, it is preferable to use a conductive material that is difficult to oxidize, or a conductive material that has a function of suppressing oxygen diffusion, as the conductive layer 260. As described above, examples of the conductive material include a conductive material containing nitrogen and a conductive material containing oxygen. This can suppress a decrease in the conductivity of the conductive layer 260.

[0248] In addition, the conductive layer 260 is preferably made of a conductive material containing oxygen and a metal element contained in the metal oxide in which the channel is formed. In addition, one or more of indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide to which silicon is added may be used. Indium gallium zinc oxide containing nitrogen may also be used. By using such a material, hydrogen contained in the metal oxide in which the channel is formed may be captured. Alternatively, hydrogen mixed in from an outer insulating layer may be captured.

[0249] The conductive layer 260 may have a thickness of, for example, 3 nm or more and 500 nm or less. The thickness of the conductive layer 260 may be, for example, equal to or greater than the thickness of the insulating layer 250. By making the conductive layer 260 thicker, the resistance of the conductive layer 260 can be reduced.

[0250] In addition, the conductive layer 260 preferably has a two-layer structure including a conductive layer 260a and a conductive layer 260b over the conductive layer 260a.

[0251] By using a conductive material having a function of suppressing oxygen diffusion as the conductive layer 260a, for example, release of oxygen from the oxide semiconductor layer 230 can be suppressed, and formation of oxygen vacancies in the oxide semiconductor layer 230 can be suppressed.

[0252] In addition, by using a conductive material that is not easily oxidized as the conductive layer 260a, it is possible to suppress, for example, the conductive layer 260a from being oxidized and the conductivity from being reduced due to the release of oxygen from the oxide semiconductor layer 230 or the release of oxygen from the insulating layer 250.

[0253] The material used for the conductive layer 260b preferably has a higher conductivity than the material used for the conductive layer 260a, for example. In addition, by making the conductive layer 260b thicker, the current flowing through the conductive layer 260b can be further increased.

[0254] The conductive layer 260a can be suitably formed along the sidewall of the opening 290 by using a film formation method with high coverage.

[0255] The conductive layer 260a can be, for example, a conductive material containing nitrogen, a conductive material containing oxygen, etc. In addition, the conductive layer 260a can be, for example, a conductive material containing oxygen and a metal element contained in a metal oxide in which a channel is formed.

[0256] The conductive layer 260a may be made of, for example, a conductive material containing the above-mentioned metal element and nitrogen, such as tantalum nitride, titanium nitride, ruthenium nitride, a nitride containing molybdenum, a nitride containing tungsten, titanium, and aluminum, a nitride containing tantalum and aluminum, or the like.

[0257] Furthermore, the conductive layer 260a can be made of a conductive material containing the aforementioned metal element and oxygen, such as ruthenium oxide, an oxide containing strontium and ruthenium, or an oxide containing lanthanum and nickel.

[0258] Alternatively, one or more of indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide doped with silicon may be used. Alternatively, indium gallium zinc oxide containing nitrogen may be used.

[0259] In addition, as the conductive layer 260a, materials including titanium, tantalum, ruthenium, and one or more selected from these metal elements are preferable because they are conductive materials that are resistant to oxidation, have a function of suppressing the diffusion of oxygen, or maintain their conductivity even when they absorb oxygen.

[0260] The conductive layer 260b may be made of, for example, the above-mentioned metal elements, an alloy containing the above-mentioned metal elements, or an alloy combining the above-mentioned metal elements. For example, tungsten may be used.

[0261] The conductive layer 260a may further have a stacked structure. The conductive layer 260b may further have a stacked structure. When the conductive layer 260a has a stacked structure, for example, a plurality of materials that can be used for the conductive layer 260a may be stacked. Alternatively, a plurality of materials selected from the materials that can be used for the conductive layer of one embodiment of the present invention may be stacked. When the conductive layer 260b has a stacked structure, for example, a plurality of materials that can be used for the conductive layer 260b may be stacked. Alternatively, a plurality of materials selected from the materials that can be used for the conductive layer of one embodiment of the present invention may be stacked.

[0262] Since the conductive layer 220 and the conductive layer 240 are each a conductive layer in contact with the oxide semiconductor layer 230, it is preferable to use a conductive material that is not easily oxidized, a conductive material that maintains low electrical resistance even when oxidized, an oxide conductive material, or a conductive material that has a function of suppressing oxygen diffusion, for each of them. Examples of the conductive material include a conductive material containing nitrogen and a conductive material containing oxygen. This can suppress a decrease in the conductivity of the conductive layer 220 and the conductive layer 240.

[0263] By using a conductive material containing oxygen as the conductive layer 220 or the conductive layer 240, the conductive layer 220 or the conductive layer 240 can maintain its conductivity even if it absorbs oxygen. In addition, even when an insulating layer containing oxygen such as hafnium oxide is used as the insulating layer 210, the conductive layer 220 is preferable because it can maintain its conductivity. For each of the conductive layer 220 and the conductive layer 240, it is preferable to use, for example, ITO, ITSO, IZO (registered trademark), or the like.

[0264] When the conductive layer 220 has a three-layer structure of a first conductive layer (e.g., conductive layer 220a), a second conductive layer (e.g., conductive layer 220b), and a third conductive layer (e.g., conductive layer 220c) on the insulating layer 210 in this order, it is preferable to use a conductive material that is not easily oxidized or a conductive material that has a function of suppressing oxygen diffusion as the first conductive layer, a material with high conductivity as the second conductive layer, and a conductive material containing oxygen as the third conductive layer. Specifically, it is preferable to use titanium nitride as the first conductive layer, tungsten as the second conductive layer, and ITO or ITSO as the third conductive layer. In this case, titanium nitride is in contact with the insulating layer 210, and ITO or ITSO is in contact with the oxide semiconductor layer 230. With such a structure, the conductive layer 220 can maintain conductivity even when it is in contact with the oxide semiconductor layer 230. When an oxide insulating layer is used for the insulating layer 210, excessive oxidation of the conductive layer 220 can be suppressed by the insulating layer 210. When tungsten, which has high conductivity, is used for the second conductive layer, the conductivity of the conductive layer 220 can be increased.

[0265] Furthermore, when the conductive layer 240 has a two-layer laminated structure (for example, the conductive layer 240a and the conductive layer 240b), it is preferable to use a material having a higher conductivity than the upper layer for the lower layer and a conductive material containing oxygen for the upper layer. Specifically, it is preferable to use ruthenium, tungsten, titanium nitride, or tantalum nitride for the lower layer and ITO or ITSO for the upper layer. In this case, ITO or ITSO is in contact with the oxide semiconductor layer 230. With such a structure, the conductive layer 240 can maintain its conductivity even when in contact with the oxide semiconductor layer 230. Furthermore, by using a material having a higher conductivity than the upper layer for the lower layer, it is possible to increase the conductivity of the conductive layer 240.

[0266] In addition, when the conductive layer 240 has a two-layer structure, a material having high conductivity may be used for the upper layer (e.g., the conductive layer 240b) and a conductive material containing oxygen may be used for the lower layer (e.g., the conductive layer 240a). In such a case, for example, the oxide semiconductor layer 230 is in contact with the upper surface of the conductive layer 240a, whereby the contact resistance between the conductive layer 240 and the oxide semiconductor layer 230 can be reduced.

[0267] [Oxide semiconductor layer 230] As described above, the oxide semiconductor layer 230 has a channel formation region. The channel formation region is i-type (intrinsic) or substantially i-type. The oxide semiconductor layer 230 further has a source region and a drain region. The source region and the drain region are n-type regions (low-resistance regions) having a higher carrier concentration than the channel formation region.

[0268] The crystallinity of a semiconductor material used for the oxide semiconductor layer 230 is not particularly limited, and any of an amorphous semiconductor, a single crystal semiconductor, and a semiconductor having crystallinity other than single crystal (a microcrystalline semiconductor, a polycrystalline semiconductor, or a semiconductor having a crystalline region in part) may be used. The use of a single crystal semiconductor or a semiconductor having crystallinity is preferable because deterioration of transistor characteristics can be suppressed.

[0269] The band gap of the metal oxide functioning as a semiconductor is preferably 2.0 eV or more, more preferably 2.5 eV or more. By using a metal oxide having a large band gap, the off-current of a transistor can be reduced. Since the off-current of an OS transistor is small, the power consumption of a semiconductor device can be sufficiently reduced. Furthermore, since the frequency characteristics of an OS transistor are high, the semiconductor device can operate at high speed.

[0270] The off-state current of the OS transistor is 100 zA or less per 1 μm of channel width (z: zepto, 10 -21 ), 50zA or less, 10zA or less, 1zA or less, 100yA or less (y: Yocto, 10 -24 The off-state current of an OS transistor used in a semiconductor device of one embodiment of the present invention is preferably 50 zA or less, 10 zA or less, 1 zA or less, 100 yA or less, or 10 yA or less per transistor, for example.

[0271] The temperature dependence of the off-state current can be obtained by measuring the off-state current at a plurality of temperatures and extrapolating the measured value using an Arrhenius plot. The off-state current of an OS transistor used in a semiconductor device according to one embodiment of the present invention is 1 aA (a: atto, 10 -18 ) or less, more preferably 100zA or less, and even more preferably 10zA or less. Also, at 27°C, it is preferably 1zA or less, more preferably 100yA or less, and even more preferably 10yA or less.

[0272] Examples of metal oxides that can be used for the oxide semiconductor layer 230 include indium oxide, gallium oxide, and zinc oxide. The metal oxide preferably contains at least indium (In) or zinc (Zn). The metal oxide preferably contains two or three elements selected from indium, element M, and zinc. The element M is a metal element or a metalloid element having a high bond energy with oxygen, for example, a metal element or a metalloid element having a bond energy with oxygen higher than that of indium. Specific examples of the element M include aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony. The element M of the metal oxide is preferably one or more of the above elements, more preferably one or more selected from aluminum, gallium, tin, and yttrium, and even more preferably gallium. In this specification, metal elements and metalloid elements may be collectively referred to as "metal elements", and the "metal element" described in this specification may include metalloid elements.

[0273] The oxide semiconductor layer 230 may be, for example, indium oxide (In oxide), indium zinc oxide (In-Zn oxide, also referred to as IZO (registered trademark)), indium tin oxide (In-Sn oxide), indium titanium oxide (In-Ti oxide), indium gallium oxide (In-Ga oxide), indium gallium aluminum oxide (In-Ga-Al oxide), indium gallium tin oxide (In-Ga-Sn oxide, also referred to as IGTO), gallium zinc oxide (Ga-Zn oxide, also referred to as GZO), aluminum zinc oxide (Al-Zn oxide, also referred to as AZO), Indium aluminum zinc oxide (In-Al-Zn oxide, also written as IAZO), indium tin zinc oxide (In-Sn-Zn oxide, also written as ITZO (registered trademark)), indium titanium zinc oxide (In-Ti-Zn oxide), indium gallium zinc oxide (In-Ga-Zn oxide, also written as IGZO), indium gallium tin zinc oxide (In-Ga-Sn-Zn oxide, also written as IGZTO), indium gallium aluminum zinc oxide (In-Ga-Al-Zn oxide, also written as IGAZO, IGZAO, or IAGZO), etc. can be used. Alternatively, indium tin oxide containing silicon, gallium tin oxide (Ga-Sn oxide), aluminum tin oxide (Al-Sn oxide), etc. can be used. Alternatively, the above oxides having an amorphous structure can be used. For example, indium oxide having an amorphous structure, indium tin oxide having an amorphous structure, etc. can be used.

[0274] By increasing the ratio of the number of indium atoms to the total number of atoms of all metal elements contained in the metal oxide, the field-effect mobility of the transistor can be increased, and a transistor with a large on-state current can be realized.

[0275] The metal oxide may have one or more metal elements having a large period number in the periodic table instead of or in addition to indium. The greater the overlap of the orbits of the metal elements, the greater the carrier conduction in the metal oxide. Therefore, by including a metal element having a large period number in the periodic table, the field effect mobility of the transistor may be increased. Examples of metal elements having a large period number in the periodic table include metal elements belonging to the fifth period and metal elements belonging to the sixth period. Specific examples of the metal elements include yttrium, zirconium, silver, cadmium, tin, antimony, barium, lead, bismuth, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium. Lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium are called light rare earth elements.

[0276] The metal oxide may contain one or more nonmetallic elements. When the metal oxide contains a nonmetallic element, the carrier concentration increases, the band gap decreases, and the field effect mobility of the transistor may be increased. Examples of the nonmetallic element include carbon, nitrogen, phosphorus, sulfur, selenium, fluorine, chlorine, bromine, and hydrogen.

[0277] In addition, by increasing the ratio of the number of zinc atoms to the total number of atoms of all metal elements contained in the metal oxide, the metal oxide can be made highly crystalline and the diffusion of impurities in the metal oxide can be suppressed, thereby suppressing the fluctuation of the electrical characteristics of the transistor and improving its reliability.

[0278] Moreover, by increasing the ratio of the number of atoms of element M to the sum of the number of atoms of all metal elements contained in the metal oxide, a metal oxide having a large band gap can be obtained. Furthermore, formation of oxygen vacancies in the metal oxide can be suppressed. Therefore, carrier generation due to oxygen vacancies can be suppressed, and a transistor with a small off-current can be obtained. Furthermore, a shift in the threshold voltage of the transistor can be suppressed. Furthermore, fluctuations in the electrical characteristics of the transistor can be suppressed, and reliability can be improved.

[0279] The electrical characteristics and reliability of a transistor vary depending on the composition of the metal oxide used for the oxide semiconductor layer 230. Thus, by varying the composition of the metal oxide depending on the electrical characteristics and reliability required of a transistor, a semiconductor device which has both excellent electrical characteristics and high reliability can be provided.

[0280] When the metal oxide is an In-M-Zn oxide, the atomic ratio of In in the In-M-Zn oxide is preferably equal to or greater than the atomic ratio of M. Examples of atomic ratios of metal elements in such In-M-Zn oxides include In:M:Zn=1:1:0.5, In:M:Zn=1:1:1, In:M:Zn=1:1:1.2, In:M:Zn=1:1:2, In:M:Zn=2:1:3, In:M:Zn=3:1:1, In:M:Zn=3:1:2, In:M:Zn=4:2:3, In:M:Zn=4:2:4.1, In:M:Zn=5:1:3, In:M:Zn=5:1:6, In:M:Zn=5:1:7, In:M:Zn=5:1:8, In:M:Zn=6:1:6, In:M:Zn=5:2:5, and compositions in the vicinity thereof. The term "composition in the vicinity" includes a range of ±30% of the desired atomic ratio. By increasing the atomic ratio of indium in a metal oxide, the on-state current, field-effect mobility, or the like of a transistor can be increased.

[0281] By using a metal oxide with a composition of In:M:Zn=1:1:1 [atomic ratio] or a composition close to that, the transistor can be made normally off. When the metal oxide is deposited by a sputtering method, the amount of zinc in the deposited metal oxide may decrease. Therefore, for example, it is preferable that the target composition is In:M:Zn=1:1:1.2 [atomic ratio] or a composition close to that. On the other hand, when the metal oxide is deposited by an ALD method, the amount of In in the deposited metal oxide may decrease.

[0282] In addition, the atomic ratio of In in the In-M-Zn oxide may be less than the atomic ratio of M. Examples of atomic ratios of metal elements in such In-M-Zn oxide include In:M:Zn=1:3:2, In:M:Zn=1:3:3, In:M:Zn=1:3:4, and compositions close to these. By increasing the ratio of the number of M atoms in the metal oxide, the generation of oxygen vacancies can be suppressed.

[0283] When the element M contains a plurality of metal elements, the total proportion of the atomic numbers of the metal elements can be regarded as the proportion of the atomic number of the element M.

[0284] In this specification and the like, the ratio of the number of indium atoms to the sum of the numbers of atoms of all metal elements contained may be referred to as the indium content. The same applies to other metal elements.

[0285] In addition, when the metal oxide is an In-Zn oxide, the atomic ratio of the metal elements of the In-Zn oxide may be, for example, In:Zn=1:1, In:Zn=2:1, In:Zn=4:1, or a composition close to these. The In-Zn oxide may also contain a trace amount of element M. For example, when the element M is Sn, the atomic ratio of the metal elements of the metal oxide may be, for example, In:Sn:Zn=2:0.1:1, In:Sn:Zn=4:0.1:1, or a composition close to these.

[0286] The composition of the metal oxide used in the oxide semiconductor layer 230 can be analyzed by, for example, energy dispersive X-ray spectrometry (EDX), X-ray photoelectron spectrometry (XPS), inductively coupled plasma-mass spectrometry (ICP-MS), or inductively coupled plasma-atomic emission spectrometry (ICP-AES). Alternatively, the analysis may be performed by combining a plurality of these techniques. Note that, for elements with low content, the actual content and the content obtained by analysis may differ due to the influence of analytical accuracy. For example, when the content of element M is low, the content of element M obtained by analysis may be lower than the actual content. In addition, it may be difficult to quantify element M, or element M may not be detected.

[0287] The metal oxide can be preferably formed by sputtering or ALD. When the metal oxide is formed by sputtering, the composition of the metal oxide after film formation may differ from that of the target. In particular, the content of zinc in the metal oxide after film formation may decrease to about 50% compared to that of the target. The metal oxide may also be formed by chemical vapor deposition (CVD), molecular beam epitaxy (MBE), pulsed laser deposition (PLD), or the like.

[0288] The oxide semiconductor layer 230 may have a stacked structure including two or more metal oxide layers. The two or more metal oxide layers included in the oxide semiconductor layer 230 may have the same or approximately the same composition. By using a stacked structure of metal oxide layers having the same composition, for example, the same sputtering target can be used for formation, thereby reducing manufacturing costs.

[0289] The two or more metal oxide layers in the oxide semiconductor layer 230 may have different compositions.

[0290] The oxide semiconductor layer 230 may have, for example, a two-layer structure. Hereinafter, the first layer is referred to as the oxide layer 230a, and the second layer is referred to as the oxide layer 230b. Note that the oxide layer 230a and the oxide layer 230b are not illustrated here. Note that the oxide layer 230a is, for example, a layer closer to the conductive layer 220 and the sidewall of the opening 290, and the oxide layer 230b is, for example, a layer closer to the insulating layer 250. Alternatively, the arrangement of the oxide layer 230a and the oxide layer 230b is not limited thereto.

[0291] For example, the oxide layer 230a is preferably made of a material having a higher conductivity than the oxide layer 230b. By using a material having a high conductivity for the oxide layer 230a in contact with the source and drain electrodes (the conductive layer 220 and the conductive layer 240), the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220 and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced, and a transistor with a large on-state current can be obtained.

[0292] Here, when a material having high conductivity is used for the oxide layer 230b provided on the conductive layer 260 side functioning as the gate electrode, the threshold voltage of the transistor 200 may shift, and the drain current (hereinafter also referred to as cutoff current) that flows when the gate voltage is 0 V may become large. Specifically, when the transistor 200 is an n-channel transistor, the threshold voltage may become low. Therefore, it is preferable to use a material having lower conductivity than the oxide layer 230a for the oxide layer 230b. As a result, when the transistor 200 is an n-channel transistor, the threshold voltage can be increased, and the transistor can have a small cutoff current. Note that a small cutoff current may be referred to as a normally-off transistor.

[0293] As described above, by using a material having a higher electrical conductivity than the oxide layer 230b for the oxide semiconductor layer 230 having a stacked structure, a normally-off transistor with a large on-state current can be obtained. Thus, a semiconductor device with both low power consumption and high performance can be provided.

[0294] The carrier concentration of the oxide layer 230a is preferably higher than that of the oxide layer 230b. By increasing the carrier concentration of the oxide layer 230a, the electrical conductivity is increased, and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220 and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240 can be reduced, so that a transistor with a large on-state current can be obtained. By decreasing the carrier concentration of the oxide layer 230b, the electrical conductivity is decreased, so that a normally-off transistor can be obtained.

[0295] Note that the oxide semiconductor layer 230 is not limited to the above-described structure, and the oxide layer 230a may be made of a material having a lower electrical conductivity than the oxide layer 230b. The carrier concentration of the oxide layer 230a may be lower than the carrier concentration of the oxide layer 230b.

[0296] In addition, the band gap of the first metal oxide used in the oxide layer 230a is preferably different from the band gap of the second metal oxide used in the oxide layer 230b. For example, the difference between the band gap of the first metal oxide and the band gap of the second metal oxide is preferably 0.1 eV or more, more preferably 0.2 eV or more, and even more preferably 0.3 eV or more.

[0297] The band gap of the first metal oxide used for the oxide layer 230a is preferably smaller than the band gap of the second metal oxide used for the oxide layer 230b. This can reduce the contact resistance between the oxide semiconductor layer 230 and the conductive layer 220 and the contact resistance between the oxide semiconductor layer 230 and the conductive layer 240, and can provide a transistor with a large on-state current. When the transistor 200 is an n-channel transistor, the threshold voltage can be increased, and the transistor can be a normally-off transistor. In addition, the large band gap of the second metal oxide can suppress generation and induction of carriers in the oxide layer 230b and at the interface between the oxide layer 230b and the insulating layer 250. This can improve the reliability of the transistor.

[0298] For example, the content of element M in the first metal oxide is preferably lower than the content of element M in the second metal oxide. More specifically, for example, it is preferable to use a metal oxide having a composition of In:M:Zn=1:1:1 [atomic ratio] or a composition close thereto as the oxide layer 230a, and to use a metal oxide having a composition of In:M:Zn=1:3:2 [atomic ratio] or a composition close thereto as the oxide layer 230b. In this case, it is particularly preferable to use one or more of gallium, aluminum, and tin as the element M.

[0299] Note that the oxide semiconductor layer 230 is not limited to the above-mentioned structure, and the band gap of the first metal oxide may be larger than the band gap of the second metal oxide.

[0300] Moreover, the content of element M in the first metal oxide is preferably lower than the content of element M in the second metal oxide. The first metal oxide may be configured to contain a trace amount of element M or may be configured to contain no element M. For example, it is preferable that the first metal oxide used in the oxide layer 230a is an In-Zn oxide, and the second metal oxide used in the oxide layer 230b is an In-M-Zn oxide. Specifically, the first metal oxide can be an In-Zn oxide, and the second metal oxide can be an In-Ga-Zn oxide.

[0301] For example, it is preferable to use, as the oxide layer 230a, a metal oxide having a composition of In:Zn=1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Zn=2:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Sn:Zn=2:0.1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Zn=4:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Sn:Zn=4:0.1:1 [atomic ratio] or a composition close thereto, or an indium oxide. It is also preferable to use, as the oxide layer 230b, a metal oxide having a composition of In:Ga:Zn=1:1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Ga:Zn=1:3:2 [atomic ratio] or a composition close thereto, or a metal oxide having a composition of In:Ga:Zn=1:3:4 [atomic ratio] or a composition close thereto. This allows the on-state current of the transistor 200 to be increased, and the transistor structure to have high reliability and little variation can be obtained.

[0302] Note that the oxide semiconductor layer 230 is not limited to the above-mentioned configuration, and the content of the element M in the first metal oxide may be higher than the content of the element M in the second metal oxide.

[0303] Alternatively, by using a metal oxide having an atomic ratio of In:M:Zn=1:1:1 or a composition close thereto for each of the oxide layer 230a and the oxide layer 230b, the transistor can be normally off.

[0304] The crystallinity of a semiconductor material used for the oxide semiconductor layer 230 is not particularly limited, and any of an amorphous semiconductor (a semiconductor having an amorphous structure), a single crystal semiconductor (a semiconductor having a single crystal structure), and a semiconductor having crystallinity other than single crystal (a microcrystalline semiconductor, a polycrystalline semiconductor, or a semiconductor having a crystalline region in part) may be used. Use of a single crystal semiconductor or a semiconductor having crystallinity is preferable because deterioration of transistor characteristics can be suppressed.

[0305] The oxide semiconductor layer 230 preferably has a metal oxide layer having crystallinity. Examples of the structure of the metal oxide having crystallinity include a c-axis aligned crystal (CAAC) structure, a polycrystal (Poly-crystal) structure, and a nanocrystal (nc) structure. By using a metal oxide layer having crystallinity for the oxide semiconductor layer 230, the density of defect states in the oxide semiconductor layer 230 can be reduced, and a highly reliable semiconductor device can be realized. Note that the CAAC structure is a crystal structure in which a plurality of microcrystals (typically, a plurality of IGZO microcrystals) have a c-axis alignment and are connected without being aligned in the ab plane. When a cross section of an OS film having a CAAC structure is observed using a high-resolution TEM image, it can be confirmed that metal atoms are arranged in a layered manner in the crystal portion. Therefore, the OS film having a CAAC structure can be said to have a structure having a layered crystal portion.

[0306] The polycrystalline structure has crystal grain boundaries. When a heat treatment is performed after forming an oxide semiconductor layer having a polycrystalline structure, a minute gap (also referred to as a nanocrack or a microcrack) or a minute space (also referred to as a nanospace or a microspace) may be formed between crystal parts. When a minute gap or a minute space is formed in the oxide semiconductor layer, the electric resistance of the oxide semiconductor layer increases. This is because the electric resistance of the minute gap or minute space is very high, for example, infinite. When an oxide semiconductor layer having a minute gap or minute space is used for a channel formation region of a transistor, the contact resistance between the oxide semiconductor layer and one or both of a source electrode and a drain electrode increases. This adversely affects the initial characteristics or reliability of the transistor. The CAAC structure has fewer crystal grain boundaries in the ab plane than the polycrystalline structure, and therefore a highly reliable semiconductor device can be realized.

[0307] The higher the crystallinity of the metal oxide layer used for the oxide semiconductor layer 230, the more the density of defect states in the oxide semiconductor layer 230 can be reduced. On the other hand, by using a metal oxide layer with low crystallinity, a transistor capable of passing a large current can be realized.

[0308] The higher the substrate temperature (stage temperature) during the formation of the metal oxide layer, the higher the crystallinity of the metal oxide layer that can be formed. Also, the higher the ratio of the flow rate of oxygen gas to the total deposition gas used during the formation (hereinafter, also referred to as oxygen flow rate ratio), the higher the crystallinity of the metal oxide layer that can be formed.

[0309] The crystallinity of the oxide semiconductor layer 230 can be analyzed by, for example, X-ray diffraction (XRD), a transmission electron microscope (TEM), or electron diffraction (ED). Alternatively, the analysis may be performed by combining a plurality of these techniques.

[0310] The oxide semiconductor layer 230 can have a stacked structure of two or more metal oxide layers with different crystallinity. In this case, the two or more metal oxide layers may have different compositions or may have the same or approximately the same composition. For example, a stacked structure of a first metal oxide layer and a second metal oxide layer provided over the first metal oxide layer can be used, and the second metal oxide layer can have a region with higher crystallinity than the first metal oxide layer. Alternatively, the second metal oxide layer can have a region with lower crystallinity than the first metal oxide layer. Note that when the second metal oxide layer has a region with lower crystallinity than the first metal oxide layer, the crystallinity of the second metal oxide layer can be increased by performing heat treatment (also referred to as crystallization treatment) after the second metal oxide layer is formed.

[0311] For example, it is preferable to use a metal oxide having a composition of In:M:Zn=1:3:2 [atomic ratio] or a composition close thereto as the oxide layer 230a, or a metal oxide having a composition of In:M:Zn=1:3:4 [atomic ratio] or a composition close thereto as the oxide layer 230b, and to use a metal oxide having a composition of In:M:Zn=1:1:1 [atomic ratio] or a composition close thereto as the oxide layer 230b. When a metal oxide having a high ratio of Zn to In is used for the oxide layer 230a, the crystallinity of the oxide layer 230a can be improved. Furthermore, by forming the oxide layer 230b on the oxide layer 230a having high crystallinity, it is also easy to improve the crystallinity of the oxide layer 230b. This makes it possible to improve the crystallinity of the entire oxide semiconductor layer 230, which is preferable. At this time, it is particularly preferable to use gallium, aluminum, or tin as the element M. For example, two layers of IGZO having different compositions from each other may be stacked. Also, for example, a laminated structure of any one selected from indium oxide, indium gallium oxide, and IGZO, and any one selected from IAZO, IAGZO, and ITZO (registered trademark) may be used.

[0312] The oxide semiconductor layer 230 may have a stacked structure of three or more layers. For example, the oxide semiconductor layer 230 may have a three-layer structure including an oxide layer, an oxide layer 230a on the oxide layer, and an oxide layer 230b on the oxide layer 230a.

[0313] The oxide layer 230a and the oxide layer 230b can have the same configuration as that applicable to the oxide layer 230b. The oxide layer located under the oxide layer 230a can have the same configuration as that applicable to the oxide layer 230b. In the following, they will be collectively described as a pair of oxide layers sandwiching the oxide layer 230a.

[0314] For example, it is preferable to use, as the oxide layer 230a, a metal oxide having a composition of In:Zn=1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Zn=2:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Sn:Zn=2:0.1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Zn=4:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Sn:Zn=4:0.1:1 [atomic ratio] or a composition close thereto, or an indium oxide. Also, it is preferable to use, as the pair of oxide layers sandwiching the oxide layer 230a, a metal oxide having a composition of In:Ga:Zn=1:1:1 [atomic ratio] or a composition close thereto, a metal oxide having a composition of In:Ga:Zn=1:3:2 [atomic ratio] or a composition close thereto, or a metal oxide having a composition of In:Ga:Zn=1:3:4 [atomic ratio] or a composition close thereto.

[0315] It is preferable that the pair of oxide layers sandwiching the oxide layer 230a each have a larger band gap than the oxide layer 230a. As a result, the oxide layer 230a is sandwiched between the pair of oxide layers having a larger band gap, and the oxide layer 230a mainly functions as a current path (channel). By sandwiching the oxide layer 230a between the pair of oxide layers, it is possible to reduce trap levels at the interface of the oxide layer 230a and in its vicinity. As a result, it is possible to realize a buried channel type transistor in which the channel is kept away from the insulating layer interface, and it is possible to increase the field effect mobility. In addition, the influence of the interface state that may be formed on the back channel side is reduced, and light deterioration (for example, negative bias light deterioration) of the transistor can be suppressed, and the reliability of the transistor can be improved.

[0316] The thickness of the oxide semiconductor layer 230 is preferably 3 nm or more and 200 nm or less, more preferably 3 nm or more and 100 nm or less, further preferably 5 nm or more and 100 nm or less, further preferably 10 nm or more and 100 nm or less, further preferably 10 nm or more and 70 nm or less, further preferably 15 nm or more and 70 nm or less, further preferably 15 nm or more and 50 nm or less, further preferably 20 nm or more and 50 nm or less. In a transistor used in a finer semiconductor device, the thickness of the oxide semiconductor layer 230 is preferably 1 nm or more, 3 nm or more, or 5 nm or more, and 20 nm or less, 15 nm or less, 12 nm or less, or 10 nm or less.

[0317] In addition, it is preferable to use two types of film formation methods, a sputtering method and an ALD method, when forming the oxide semiconductor layer. For example, when a first oxide semiconductor layer having a CAAC structure is formed by a sputtering method and then a second oxide semiconductor layer having a lower crystallinity than the CAAC structure is formed by an ALD method, it is expected that the atomic layer of the second oxide semiconductor layer fills or repairs the gaps in the crystal parts at the atomic level that the CAAC structure of the first oxide semiconductor layer has. In addition, it is preferable to perform a heat treatment (for example, at 100° C. to 500° C., preferably 200° C. to 450° C., more preferably 300° C. to 400° C.) after forming the second oxide semiconductor layer by the ALD method. It is expected that the heat treatment repairs the gaps in the crystal parts at the atomic level that the CAAC structure of the first oxide semiconductor layer has by the second oxide semiconductor layer (in other words, each crystal molecule formed by the ALD method). In addition, an oxide semiconductor layer formed by the above two types of film formation methods may be called a hybrid OS.

[0318] Here, the concept of heat treatment for improving the crystallinity of an oxide semiconductor layer will be described with reference to Figures 11(A), 11(B), 11(C), and 11(D). Figures 11(A), 11(B), 11(C), and 11(D) are conceptual diagrams illustrating cross sections of an oxide semiconductor layer having a CAAC structure. In each diagram, the c-axis is indicated by an arrow.

[0319] The oxide semiconductor layer 370a shown in FIG. 11A includes a region 372a and a region 372b located between the regions 372a. The region 372a corresponds to a region having a CAAC structure (i.e., a structure having layered crystal parts), and the region 372b corresponds to a region between the CAAC structures. The CAAC structure has fewer crystal grain boundaries in the ab plane than the polycrystalline structure. Thus, even in the oxide semiconductor layer 370a having the CAAC structure, there may be a minute gap or minute space (region 372b in FIG. 11A) between the crystal parts.

[0320] Therefore, in order to improve the crystallinity of the oxide semiconductor layer, in other words, to reduce the region 372b shown in FIG. 11A, an oxide semiconductor layer having a CAAC structure is formed by a sputtering method as a first oxide semiconductor layer, and then an oxide semiconductor layer having a microcrystalline structure or an amorphous structure, which has lower crystallinity than the CAAC structure, is formed by an ALD method as a second oxide semiconductor layer.

[0321] 11B, an oxide semiconductor layer having a region 372a is formed by a sputtering method as a first oxide semiconductor layer, and then an oxide semiconductor layer having a region 372c with lower crystallinity than the CAAC structure is formed by an ALD method as a second oxide semiconductor layer. Note that in FIG. 11B, the oxide semiconductor layer 370b has the region 372a and the region 372c. Since the ALD method can deposit atoms one layer at a time, the second oxide semiconductor layer can be formed to fill the region 372b.

[0322] Then, heat treatment is performed to increase the crystallinity of the region 372c of the second oxide semiconductor layer using the region 372a of the first oxide semiconductor layer as a seed. In other words, the region 372c of the second oxide semiconductor layer can be crystal-grown using the region 372a of the first oxide semiconductor layer as a seed. Alternatively, the region 372c of the second oxide semiconductor layer having an amorphous structure can be crystal-grown using the region 372a of the first oxide semiconductor layer having a CAAC structure as a nucleus. This crystal growth model can be regarded as a concept equivalent to heteroepitaxy. Note that in FIG. 11C, the oxide semiconductor layer 370c includes a region 372a and a region 372c. The region 372a shown in FIG. 11C has higher crystallinity or a higher density of crystal parts than the region 372a shown in FIG. 11B. By performing heat treatment, the crystallinity of either or both of the regions 372a and 372c can be increased. For example, the region 372c has a crystal part that has the same crystal structure as the crystal part of the region 372a. Alternatively, the region 372c has a crystal part that is connected to the crystal part of the region 372a.

[0323] 11D, the oxide semiconductor layer 370d includes a region 372a. The region 372a has improved crystallinity compared to the region 372a shown in FIGS. 11B and 11C, and the boundary between the region 372a and the region 372c disappears or the boundary between the region 372a and the region 372c is no longer observed. Therefore, the entire oxide semiconductor layer 370d has a CAAC structure. When the entire oxide semiconductor layer 370d has a CAAC structure as shown in FIG. 11D, a highly reliable semiconductor device can be realized. The presence or absence of the boundary between the region 372a and the region 372c can be confirmed by using, for example, a cross-sectional TEM, a cross-sectional STEM, or the like.

[0324] Note that even when the first oxide semiconductor layer has a small gap or a small space, the small gap or the small space in the first oxide semiconductor layer can be filled by forming a second oxide semiconductor layer over the first oxide semiconductor layer or by forming a second oxide semiconductor layer over the first oxide semiconductor layer and performing heat treatment. In this manner, by using an oxide semiconductor layer having a CAAC structure for the first oxide semiconductor layer and an oxide semiconductor layer having a microcrystalline structure or an amorphous structure for the second oxide semiconductor layer, a dense oxide semiconductor layer with improved crystallinity can be obtained. When the dense oxide semiconductor layer with improved crystallinity is used for a channel formation region of a transistor, it is expected that an increase in the electrical resistance of the oxide semiconductor layer can be suppressed or initial characteristics (particularly on-state current) of the transistor can be improved, thereby making the transistor suitable for high-speed operation.

[0325] In the case where an oxide semiconductor layer is formed by both the sputtering method and the ALD method, if the thickness of the oxide semiconductor layer formed by the ALD method is thin, the oxide semiconductor layer can be regarded as a single-layer structure, not a stacked structure of the oxide semiconductor layer formed by the sputtering method and the oxide semiconductor layer formed by the ALD method. For example, when the thickness of the oxide semiconductor layer formed by the ALD method is more than 0 nm and 3 nm or less, preferably more than 0 nm and 2 nm or less, more preferably more than 0 nm and 1 nm or less, the oxide semiconductor layer formed by the two film formation methods, the sputtering method and the ALD method, can be regarded as a single-layer structure. In such a case, for example, in a cross-sectional TEM image, a cross-sectional STEM image, or the like, the boundary between the oxide semiconductor layer formed by the sputtering method and the oxide semiconductor layer formed by the ALD method is not observed. On the other hand, when the thickness of the oxide semiconductor layer formed by the ALD method exceeds 3 nm, the oxide semiconductor layer may be regarded as having a stacked structure, a multilayer structure, or a multiple structure including an oxide semiconductor layer formed by a sputtering method and an oxide semiconductor layer formed by an ALD method.

[0326] In addition, when the oxide semiconductor layer is formed by both the sputtering method and the ALD method, it is preferable that the compositions are different from each other. Typically, a metal oxide having a composition of In:Ga:Zn=1:1:1 [atomic ratio] or a composition thereabout can be formed by the sputtering method, and then a metal oxide having a composition of In:Ga:Zn=4:0.1:1 [atomic ratio] or a composition thereabout can be formed by the ALD method. By forming the oxide semiconductor layer with the above composition, a structure having high reliability due to the metal oxide having a composition of In:Ga:Zn=1:1:1 [atomic ratio] or a composition thereabout, and a structure having high on-current or high field effect mobility due to the metal oxide having a composition of In:Ga:Zn=4:0.1:1 [atomic ratio] or a composition thereabout can be formed. In addition, instead of a metal oxide having a composition of In:Ga:Zn=4:0.1:1 [atomic ratio] or close thereto, it is possible to use a metal oxide having a composition of In:Ga:Zn=1:0:0 [atomic ratio], i.e., indium oxide or a metal oxide having a high proportion of In.

[0327] The oxide semiconductor layer formed by the above-mentioned two types of film formation methods can be regarded as a structure in which the gaps in the crystal parts of the CAAC structure are filled with atomic layers formed by the ALD method. Note that the structure can be analyzed by analytical methods such as cross-sectional SEM, cross-sectional STEM, cross-sectional TEM, SIMS, and EDX.

[0328] In addition, the oxide semiconductor layer having the CAAC structure formed by using the above two kinds of film formation methods may have higher relative dielectric constant, film density, and film hardness than an oxide semiconductor layer having the CAAC structure formed by using one kind of film formation method. In this way, by using an oxide semiconductor layer having the CAAC structure formed by using two kinds of film formation methods in a channel formation region of a transistor, a transistor having excellent characteristics (for example, a transistor with a large on-current, a transistor with a high field-effect mobility, a transistor with a small S value, a transistor with high frequency characteristics (also referred to as f characteristics), a transistor with high reliability, etc.) can be realized.

[0329] Hydrogen in the oxide semiconductor reacts with oxygen that bonds with metal atoms to form water, creating oxygen vacancies (V O In addition, defects in which hydrogen is inserted into oxygen vacancies (hereafter referred to as V O Hydrogen may function as a donor and generate electrons that serve as carriers. Some of the hydrogen may bond with oxygen that is bonded to a metal atom to generate electrons that serve as carriers. Therefore, a transistor using an oxide semiconductor that contains a lot of hydrogen tends to have normally-on characteristics (that is, a threshold voltage that has a negative value). Furthermore, hydrogen in an oxide semiconductor is easily mobile due to stress such as heat or an electric field; therefore, if an oxide semiconductor contains a lot of hydrogen, the reliability of the transistor may be deteriorated.

[0330] V in the oxide semiconductor layer 230 O It is preferable to reduce H as much as possible to make the oxide semiconductor layer 230 highly intrinsic or substantially highly intrinsic. O In order to obtain an oxide semiconductor with a sufficiently reduced amount of H, it is important to remove impurities such as water and hydrogen from the oxide semiconductor (sometimes referred to as dehydration or dehydrogenation treatment) and to supply oxygen to the oxide semiconductor to repair oxygen vacancies. O Stable electrical characteristics can be obtained by using an oxide semiconductor in which impurities such as H are sufficiently reduced for a channel formation region of a transistor. Note that supplying oxygen to an oxide semiconductor to repair oxygen vacancies is sometimes referred to as oxygen adding treatment.

[0331] The carrier concentration of the oxide semiconductor in the region functioning as the channel formation region is 1×10 18 cm -3 It is preferable that the value is less than 1×10 17 cm -3 More preferably, it is less than 1×10 16 cm -3 More preferably, it is less than 1×10 13 cm -3 More preferably, it is less than 1×10 12 cm -3Note that the lower limit of the carrier concentration of the oxide semiconductor in the region functioning as a channel formation region is not particularly limited, but is preferably, for example, 1×10 -9 cm -3 It can be said that:

[0332] Here, the influence of each impurity in a metal oxide (oxide semiconductor) will be described.

[0333] When an oxide semiconductor contains silicon or carbon, which is one of the group 14 elements, defect levels are formed in the oxide semiconductor. Therefore, the carbon concentration in the channel formation region of the oxide semiconductor measured by SIMS is 1×10 20 atoms / cm 3 Less than or equal to 5×10 19 atoms / cm 3 Less than or equal to 3×10 19 atoms / cm 3 Less than or equal to 1×10 19 atoms / cm 3 Less than or equal to 3×10 18 atoms / cm 3 Less than 1×10, more preferably 18 atoms / cm 3 The silicon concentration in the channel formation region of the oxide semiconductor measured by SIMS is 1×10 20 atoms / cm 3 Less than or equal to 5×10 19 atoms / cm 3 Less than or equal to 3×10 19 atoms / cm 3 Less than or equal to 1×10 19 atoms / cm 3 Less than or equal to 3×10 18 atoms / cm 3 Less than 1×10, more preferably 18 atoms / cm 3 The following applies.

[0334] Furthermore, when nitrogen is contained in an oxide semiconductor, electrons serving as carriers are generated, the carrier concentration increases, and the semiconductor is likely to become n-type. As a result, a transistor using an oxide semiconductor containing nitrogen as a semiconductor is likely to have normally-on characteristics. Alternatively, when nitrogen is contained in an oxide semiconductor, trap states may be formed. As a result, the electrical characteristics of the transistor may become unstable. For this reason, the nitrogen concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Less than or equal to 5×10 19 atoms / cm 3 Less than or equal to 1×10 19 atoms / cm 3 Less than or equal to 5×10 18 atoms / cm 3 Less than or equal to 1×10 18 atoms / cm 3 Less than 5×10, more preferably 17 atoms / cm 3 The following applies.

[0335] Furthermore, hydrogen contained in the oxide semiconductor reacts with oxygen bonded to metal atoms to form water, which may form oxygen vacancies. When hydrogen enters the oxygen vacancies, electrons serving as carriers may be generated. Some of the hydrogen may bond with oxygen bonded to metal atoms to generate electrons serving as carriers. Therefore, a transistor using an oxide semiconductor containing hydrogen is likely to have normally-on characteristics. For this reason, it is preferable to reduce hydrogen in the channel formation region of the oxide semiconductor as much as possible. Specifically, the hydrogen concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Less than 5 x 10 19 atoms / cm 3 less than 1×10 19 atoms / cm 3 less than 5×10 18 atoms / cm 3less than 1×10 18 atoms / cm 3 Less than.

[0336] In addition, when an oxide semiconductor contains an alkali metal or an alkaline earth metal, defect levels are formed and carriers are generated in some cases. Therefore, a transistor using an oxide semiconductor containing an alkali metal or an alkaline earth metal is likely to have normally-on characteristics. For this reason, when the concentration of the alkali metal or the alkaline earth metal in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 18 atoms / cm 3 Less than or equal to 2 x 10 16 atoms / cm 3 To the following:

[0337] When an oxide semiconductor in which impurities are sufficiently reduced is used for a channel formation region of a transistor, stable electrical characteristics can be obtained.

[0338] In addition, the semiconductor device of this embodiment may be applied to a transistor using another semiconductor material in the channel formation region. Examples of the other semiconductor material include a semiconductor made of a single element or a compound semiconductor. Examples of the semiconductor made of a single element include silicon and germanium. Examples of the compound semiconductor include gallium arsenide and silicon germanium. Other examples of the compound semiconductor include an organic semiconductor and a nitride semiconductor. The above-mentioned oxide semiconductor is also a type of compound semiconductor. These semiconductor materials may include impurities as dopants.

[0339] Silicon that can be used as a semiconductor material for a transistor includes single crystal silicon, polycrystalline silicon, microcrystalline silicon, and amorphous silicon. An example of polycrystalline silicon is low temperature polysilicon (LTPS).

[0340] The semiconductor layer of the transistor may have a layered material that functions as a semiconductor. A layered material is a general term for a group of materials that have a layered crystal structure. A layered crystal structure is a structure in which layers formed by covalent bonds or ionic bonds are stacked via bonds weaker than covalent bonds or ionic bonds, such as van der Waals bonds. A layered material has high electrical conductivity within a unit layer, that is, high two-dimensional electrical conductivity. By using a material that functions as a semiconductor and has high two-dimensional electrical conductivity in the channel formation region, a transistor with a large on-current can be provided.

[0341] Examples of the layered material include graphene, silicene, and chalcogenides. Chalcogenides are compounds containing chalcogens (elements belonging to group 16). Examples of chalcogenides include transition metal chalcogenides and group 13 chalcogenides. Specific examples of transition metal chalcogenides that can be used as the semiconductor layer of a transistor include molybdenum sulfide (representatively MoS2), molybdenum selenide (representatively MoSe2), molybdenum tellurium (representatively MoTe2), tungsten sulfide (representatively WS2), tungsten selenide (representatively WSe2), tungsten tellurium (representatively WTe2), hafnium sulfide (representatively HfS2), hafnium selenide (representatively HfSe2), zirconium sulfide (representatively ZrS2), and zirconium selenide (representatively ZrSe2).

[0342] [substrate] As the substrate on which the transistor is formed, for example, an insulating substrate, a semiconductor substrate, or a conductive substrate can be used. As the insulating substrate, for example, a glass substrate, a quartz substrate, a sapphire substrate, a stabilized zirconia substrate (such as an yttria stabilized zirconia substrate), a resin substrate, etc. are available. As the semiconductor substrate, for example, a semiconductor substrate made of silicon or germanium, or a compound semiconductor substrate made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, or gallium oxide, etc. are available. Furthermore, there is a semiconductor substrate having an insulating region inside the aforementioned semiconductor substrate, for example, an SOI (Silicon On Insulator) substrate, etc. are available. As the conductive substrate, there are a graphite substrate, a metal substrate, an alloy substrate, a conductive resin substrate, etc. are available. Alternatively, there are a substrate having a metal nitride, a substrate having a metal oxide, etc. are available. Furthermore, there are a substrate in which a conductor or semiconductor is provided on an insulating substrate, a substrate in which a conductor or insulator is provided on a semiconductor substrate, a substrate in which a semiconductor or insulator is provided on a conductive substrate, etc. are available. Alternatively, these substrates on which elements are provided may be used. The elements provided on the substrate include a capacitor element, a resistor element, a switch element, a light-emitting element, a memory element, and the like.

[0343] <Example 1 of manufacturing method of semiconductor device> A method for manufacturing a semiconductor device will be described with reference to Figures 12(A) to 12(C). Here, as an example, a method for manufacturing the structure shown in Figure 7(A) will be described. Note that, regarding the materials and formation methods of each element, descriptions of parts similar to those described above may be omitted.

[0344] Thin films (insulating films, semiconductor films, conductive films, etc.) constituting a semiconductor device can be formed by a sputtering method, a CVD method, a vacuum deposition method, a PLD method, an ALD method, or the like.

[0345] Sputtering methods include RF sputtering, which uses a high-frequency power source as the sputtering power source, DC sputtering, which uses a direct current power source, and pulsed DC sputtering, which changes the voltage applied to the electrode in a pulsed manner. There is also RF-superimposed DC sputtering, which superimposes RF and DC. RF sputtering is preferably used for film formation using an insulating target. DC sputtering is mainly used when forming a film using a conductive target. In addition to forming a conductive film, DC sputtering can also form an insulating film by performing reactive sputtering. Pulsed DC sputtering is mainly used when forming a film of compounds such as oxides, nitrides, and carbides using reactive sputtering. RF-superimposed DC sputtering allows control of ion energy during film formation and control of the target side potential. Therefore, compared to RF sputtering, damage caused by film formation is reduced. Also, a high-quality film can be obtained.

[0346] Examples of sputtering methods that can be used include ionization sputtering and long-throw sputtering. Ionization sputtering is a method in which sputtering particles generated from a target are ionized by RF or the like, and anisotropic film formation is performed by self-bias or the like. In addition, long-throw sputtering can form anisotropic film by increasing the distance between the sputtering target and the substrate.

[0347] CVD methods can be classified into PECVD, thermal CVD (TCVD) that uses heat, photo CVD (Photo CVD) that uses light, etc. They can also be further classified into metal CVD (MCVD) and metal organic CVD (MOCVD) based on the source gas used.

[0348] The PECVD method can obtain a high-quality film at a relatively low temperature. Moreover, the thermal CVD method is a film formation method that can reduce plasma damage to the object to be processed because it does not use plasma. For example, wiring, electrodes, elements (transistors, capacitive elements, etc.) included in a semiconductor device may be charged up by receiving electric charge from plasma. At this time, the wiring, electrodes, elements, etc. included in the semiconductor device may be destroyed by the accumulated electric charge. On the other hand, in the case of the thermal CVD method that does not use plasma, such plasma damage does not occur, so the yield of the semiconductor device can be increased. Furthermore, in the thermal CVD method, plasma damage does not occur during film formation, so a film with few defects can be obtained.

[0349] As the ALD method, a thermal ALD method in which a reaction between a precursor and a reactant is carried out using only thermal energy, a plasma enhanced ALD method in which a plasma excited reactant is used, or the like can be used.

[0350] In addition, the ALD method can deposit atoms one layer at a time, which has the advantages of enabling extremely thin films to be formed, films to be formed on structures with high aspect ratios, films with fewer defects such as pinholes, films with excellent coverage, and films at low temperatures. In the PEALD (Plasma Enhanced ALD) method, the use of plasma allows films to be formed at lower temperatures, which may be preferable. Note that some precursors used in the ALD method contain impurities such as carbon. For this reason, films formed by the ALD method may contain more impurities such as carbon than films formed by other film formation methods. Note that the amount of impurities can be quantified using X-ray photoelectron spectroscopy (XPS).

[0351] The CVD method and the ALD method are different from the film formation method in which particles emitted from a target or the like are deposited, and are film formation methods in which a film is formed by a reaction on the surface of a workpiece. Therefore, they are film formation methods that are not easily affected by the shape of the workpiece and have good step coverage. In particular, the ALD method has excellent step coverage and excellent thickness uniformity, so it is suitable for coating the surface of an opening with a high aspect ratio. However, since the ALD method has a relatively slow film formation speed, it may be preferable to use it in combination with other film formation methods such as the CVD method, which has a fast film formation speed.

[0352] In the CVD method and the ALD method, the composition of the film obtained can be controlled by the flow rate ratio of the raw material gas. For example, in the CVD method and the ALD method, a film of any composition can be formed by changing the flow rate ratio of the raw material gas. In addition, for example, in the CVD method and the ALD method, a film whose composition changes continuously can be formed by changing the flow rate ratio of the raw material gas while forming the film. When forming a film while changing the flow rate ratio of the raw material gas, the time required for film formation can be shortened compared to the case of forming a film using multiple film formation chambers because no time is required for transport and pressure adjustment. Therefore, the productivity of semiconductor devices can be increased in some cases.

[0353] In addition, in the CVD method, a film of any composition can be formed by changing the flow rate ratio of the raw material gases. For example, in the CVD method, a film with a continuously changing composition can be formed by changing the flow rate ratio of the raw material gases while forming a film. When forming a film while changing the flow rate ratio of the raw material gases, the time required for film formation can be shortened compared to the case of forming a film using multiple film formation chambers because no time is required for transportation or pressure adjustment. Therefore, the productivity of semiconductor devices can be increased in some cases.

[0354] In addition, in the ALD method, a film of any composition can be formed by simultaneously introducing multiple different precursors, or by controlling the number of cycles of each precursor when multiple different precursors are introduced.

[0355] Furthermore, the thin films (insulating films, semiconductor films, conductive films, etc.) constituting the semiconductor device can be formed by a wet film formation method such as spin coating, dip coating, spray coating, inkjet printing, dispensing, screen printing, offset printing, doctor knife method, slit coating, roll coating, curtain coating, or knife coating.

[0356] Furthermore, when processing a thin film constituting a semiconductor device, a photolithography method or the like can be used. Alternatively, the thin film may be processed by a nanoimprint method, a sandblasting method, a lift-off method, or the like. Furthermore, an island-shaped thin film may be directly formed by a film formation method using a shielding mask such as a metal mask.

[0357] There are two typical photolithography methods. One is a method in which a resist mask is formed on the thin film to be processed, the thin film is processed by etching or the like, and the resist mask is then removed. The other is a method in which a photosensitive thin film is formed, and then exposed and developed to process the thin film into the desired shape.

[0358] In the photolithography method, the light used for exposure may be, for example, i-line (wavelength 365 nm), g-line (wavelength 436 nm), h-line (wavelength 405 nm), or a mixture of these. In addition, ultraviolet light, KrF laser light, ArF laser light, or the like may be used. Exposure may also be performed by immersion exposure technology. Extreme ultraviolet (EUV) light or X-rays may also be used as the light used for exposure. An electron beam may also be used instead of the light used for exposure. Extreme ultraviolet light, X-rays, or an electron beam are preferable because they enable extremely fine processing. When exposure is performed by scanning a beam such as an electron beam, a photomask is not required.

[0359] For etching the thin film, a dry etching method, a wet etching method, a sandblasting method, or the like can be used.

[0360] First, the conductive layer 220 is formed over the insulating layer 210, the insulating layer 280 is formed over the conductive layer 220, and the conductive layer 240 is formed over the insulating layer 280. Note that the insulating layer 280 here has a three-layer structure of an insulating layer 280a, an insulating layer 280b, and an insulating layer 280c.

[0361] Note that after the insulating layer 280 is formed, a planarization treatment (also referred to as a CMP treatment) using a chemical mechanical polishing (CMP) method is preferably performed to planarize the top surface of the insulating layer 280. By performing the planarization treatment on the insulating layer 280, the surface on which the conductive layer 240, which functions as a wiring, is formed can be made flat, and discontinuity of the conductive layer 240 can be suppressed. Note that the planarization treatment is not necessarily performed, and in that case, the manufacturing cost can be reduced.

[0362] Next, an opening 290 is formed in the conductive layer 240 and the insulating layer 280 at a position overlapping the conductive layer 220 (FIG. 12(A)). At this time, a recess is formed in the conductive layer 220 at a position overlapping the opening 290.

[0363] Since the opening 290 has a large aspect ratio, it is preferable to process a part of the conductive layer 240 and a part of the insulating layer 280 by anisotropic etching. In particular, processing by a dry etching method is preferable because it is suitable for fine processing. In addition, the processing may be performed under different conditions depending on the layer.

[0364] Here, it is preferable to use processing conditions that give the side walls of the conductive layer 240 and the insulating layer 280c a tapered shape, and it is also preferable to use processing conditions that give the side walls of the insulating layer 280b a steep shape.

[0365] Furthermore, the insulating layer 280a may be formed using processing conditions that result in a tapered sidewall, or may be formed using processing conditions that result in a steep sidewall.

[0366] Here, by devising the materials of the insulating layers 280c and 280b, it is possible to form the insulating layer 280c in a tapered shape and the insulating layer 280b in a steep shape using the same dry etching conditions.

[0367] Subsequently, a heat treatment may be performed, for example, at a temperature of 250° C. or higher and 650° C. or lower, preferably 300° C. or higher and 500° C. or lower, and more preferably 320° C. or higher and 450° C. or lower.

[0368] The heat treatment is performed in an atmosphere of nitrogen gas or an inert gas, or an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more. For example, when the heat treatment is performed in a mixed atmosphere of nitrogen gas and oxygen gas, the oxygen gas content is preferably about 20%. The heat treatment may be performed under reduced pressure. Alternatively, after the heat treatment in the nitrogen gas or inert gas atmosphere, the heat treatment may be performed in an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more to compensate for the desorbed oxygen. By performing the above-described heat treatment, impurities such as water contained in the insulating layer 280 and the like can be reduced before the formation of the oxide semiconductor layer 230.

[0369] In addition, the gas used in the heat treatment is preferably highly purified. For example, the amount of moisture contained in the gas used in the heat treatment is preferably 1 ppb or less, more preferably 0.1 ppb or less, and even more preferably 0.05 ppb or less. By using a highly purified gas to perform the heat treatment, it is possible to prevent moisture and the like from being taken into the insulating layer 280 as much as possible.

[0370] The conductive layer 240 and the insulating layer 280 may be opened using the same mask or different masks.

[0371] Next, the oxide semiconductor layer 230 is formed so as to cover the opening 290. The oxide semiconductor layer 230 is formed in contact with the upper surface of the conductive layer 220, the side surface of the insulating layer 280, and the upper surface and side surface of the conductive layer 240.

[0372] The oxide semiconductor layer 230 can be formed by, for example, a sputtering method, a CVD method, an MBE method, a PLD method, or an ALD method.

[0373] The oxide semiconductor layer 230 is preferably formed as a film with as uniform a thickness as possible within the opening 290 along the upper surface of the conductive layer 220, the side surface of the insulating layer 280, and the side surface of the conductive layer 240. By forming the film using the ALD method, a thin film can be formed with good controllability. Therefore, it is preferable to form the oxide semiconductor layer 230 using the ALD method.

[0374] In addition, when the oxide semiconductor layer 230 has high crystallinity, diffusion of impurities in the oxide semiconductor layer 230 is suppressed, so that the electrical characteristics of the transistor are less likely to fluctuate and the reliability can be improved. When the oxide semiconductor layer 230 is formed by a sputtering method, it is easier to form a layer with high crystallinity than when an ALD method is used, which is preferable.

[0375] When the oxide semiconductor layer 230 is formed by a sputtering method, oxygen or a mixed gas of oxygen and a noble gas is used as a sputtering gas. By increasing the ratio of oxygen contained in the sputtering gas, the amount of excess oxygen in the oxide film to be formed can be increased. When the oxide film is formed by a sputtering method, an In-M-Zn oxide target or the like can be used.

[0376] When the oxide semiconductor layer 230 is formed by a sputtering method, an oxygen-excessive oxide semiconductor is formed when the ratio of oxygen contained in a sputtering gas is set to more than 30% and less than or equal to 100%, preferably greater than or equal to 70% and less than or equal to 100%. A transistor using an oxygen-excessive oxide semiconductor for a channel formation region can have relatively high reliability. However, one embodiment of the present invention is not limited thereto. An oxygen-deficient oxide semiconductor is formed when the ratio of oxygen contained in a sputtering gas is set to more than or equal to 1% and less than or equal to 30%, preferably greater than or equal to 5% and less than or equal to 20%. A transistor using an oxygen-deficient oxide semiconductor for a channel formation region can have relatively high field-effect mobility. Furthermore, the crystallinity of the oxide semiconductor layer can be improved by performing the film formation while heating the substrate.

[0377] Next, the conductive layer 240 and the oxide semiconductor layer 230 are processed into an island shape (FIG. 12B). Here, the conductive layer 240 and the oxide semiconductor layer 230 can be processed at the same time by using the same mask.

[0378] Note that the step of processing the conductive layer 240 into an island shape and the step of processing the oxide semiconductor layer 230 into an island shape may be performed independently. In this case, for example, the step of processing the conductive layer 240 into an island shape and the step of providing the opening 290 in the conductive layer 240 can be performed independently, and the order of the steps does not matter. In addition, the island shape processing and the formation of the opening may be performed at the same time by performing exposure using a mask for processing into a square island shape and exposure using a mask for providing a circular opening, and then performing etching. In addition, exposure using a multi-tone mask (typically a half-tone mask or a gray-tone mask) may be used.

[0379] Subsequently, the insulating layer 250 is formed on the oxide semiconductor layer 230 and the insulating layer 280. The insulating layer 250 is formed in contact with the oxide semiconductor layer 230.

[0380] Next, heat treatment is preferably performed. The heat treatment is preferably performed within a temperature range in which the oxide semiconductor layer 230 is not polycrystallized. The temperature of the heat treatment is preferably from 100° C. to 650° C., more preferably from 250° C. to 600° C., and further preferably from 350° C. to 550° C. For details of the heat treatment, refer to the above description.

[0381] In addition, a gas used in the heat treatment is preferably highly purified. When the heat treatment is performed using a highly purified gas, moisture and the like can be prevented from being introduced into the oxide semiconductor layer 230 as much as possible.

[0382] In this embodiment, the heat treatment is performed at a temperature of 450° C. for one hour with a flow rate ratio of nitrogen gas and oxygen gas set to 4:1. Such heat treatment including oxygen gas can reduce impurities such as carbon, water, and hydrogen in the oxide semiconductor layer 230. Reducing the impurities in the film in this manner can improve the crystallinity of the oxide semiconductor layer 230 and provide a denser and more compact structure. This can increase the crystalline regions in the oxide semiconductor layer 230 and reduce in-plane variations in the crystalline regions in the oxide semiconductor layer 230. Thus, in-plane variations in electrical characteristics of the transistor can be reduced.

[0383] In addition, in the case where the insulating layer 280 contains oxygen, it is preferable to supply oxygen from the insulating layer 280 to the channel formation region of the oxide semiconductor layer 230 by heat treatment. O H can be reduced.

[0384] Next, a conductive layer to become the conductive layer 260a is formed over the insulating layer 250. The conductive layer to become the conductive layer 260a is formed so as to cover an upper surface of the conductive layer 220, a side surface of the insulating layer 280, and an upper surface and a side surface of the conductive layer 240, with the oxide semiconductor layer 230 and the insulating layer 250 sandwiched therebetween. Next, a conductive layer to become the conductive layer 260b is formed.

[0385] The conductive layer 260a and the conductive layer 260b are formed in contact with the insulating layer 250 provided in the opening 290 having a large aspect ratio. Therefore, the conductive layer that becomes the conductive layer 260a and the conductive layer that becomes the conductive layer 260b are preferably formed by a film formation method having good coverage, and more preferably, the ALD method, the metal CVD method, or the like.

[0386] Next, the conductive layer to be the conductive layer 260b and the conductive layer to be the conductive layer 260a are partly removed using a mask to form the conductive layer 260b and the conductive layer 260a (FIG. 12C).

[0387] In the above manner, a semiconductor device of one embodiment of the present invention can be manufactured.

[0388] <Example 2 of manufacturing method of semiconductor device> An example of a method for manufacturing the semiconductor device shown in FIG. 10B will be described below.

[0389] 12B is fabricated. Then, a dummy structure is formed in the region where the insulating layer 250 and the conductive layer 260 are to be provided. After that, an insulating layer 283 and an insulating layer 285 are formed outside the dummy structure.

[0390] Subsequently, the dummy structure is removed, and an insulating layer 250 and a conductive layer 260 are formed.

[0391] Subsequently, a conductive layer 265 is formed on the conductive layer 260 and on the insulating layer 285 .

[0392] In this manner, the semiconductor device shown in Fig. 10B can be manufactured. Note that the method for manufacturing the semiconductor device shown in Fig. 10B is not limited to this.

[0393] This embodiment mode can be combined with other embodiment modes as appropriate. In addition, in the case where a plurality of configuration examples are shown in one embodiment mode in this specification, the configuration examples can be combined as appropriate.

[0394] (Embodiment 2) In this embodiment, a memory device of one embodiment of the present invention will be described with reference to FIGS. 14 to 17. The memory device of one embodiment of the present invention includes a memory cell. The memory cell includes a transistor and a capacitor.

[0395] <Storage device configuration example 1> The structure of a memory device including a transistor and a capacitor will be described with reference to Figures 14(A) to 14(C). Figure 14(A) is a plan view of a memory device including a transistor 200 and a capacitor 100. Figure 14(B) is a cross-sectional view taken along dashed line A1-A2 in Figure 14(A). Figure 14(C) is a cross-sectional view taken along dashed line A3-A4 in Figure 14(A).

[0396] 14A to 14C includes an insulating layer 140 over a substrate (not shown), a conductive layer 110 over the insulating layer 140, a memory cell 150 over the conductive layer 110, an insulating layer 180 over the conductive layer 110, an insulating layer 280, and an insulating layer 283 over the memory cell 150. The insulating layer 140, the insulating layer 180, the insulating layer 280, and the insulating layer 283 function as interlayer films. The conductive layer 110 functions as a wiring.

[0397] The memory cell 150 includes a capacitor 100 over a conductive layer 110 and a transistor 200 over the capacitor 100 .

[0398] The capacitor 100 includes a conductive layer 115 on the conductive layer 110, an insulating layer 130 on the conductive layer 115, and a conductive layer 120 on the insulating layer 130. The conductive layer 120 functions as one of a pair of electrodes (sometimes referred to as an upper electrode), the conductive layer 115 functions as the other of the pair of electrodes (sometimes referred to as a lower electrode), and the insulating layer 130 functions as a dielectric. In other words, the capacitor 100 constitutes a MIM (Metal-Insulator-Metal) capacitor.

[0399] As shown in FIG. 14(B) and FIG. 14(C), the insulating layer 180 has an opening 190 reaching the conductive layer 110. At least a part of the conductive layer 115 is disposed in the opening 190. The conductive layer 115 has a region in contact with the upper surface of the conductive layer 110 in the opening 190, a region in contact with the side surface of the insulating layer 180 in the opening 190, and a region in contact with at least a part of the upper surface of the insulating layer 180. The insulating layer 130 is disposed so that at least a part of it is located in the opening 190. The conductive layer 120 is disposed so that at least a part of it is located in the opening 190. As shown in FIG. 14(B) and FIG. 14(C), the conductive layer 120 is preferably provided so as to fill the opening 190. The films provided inside the opening 190 are preferably formed using a method with high coverage such as the ALD method. This improves the coverage of the film. For example, the conductive layer 115, the insulating layer 130, and the conductive layer 120 are preferably formed using an ALD method, a metal CVD method, or the like.

[0400] In the opening 190, the capacitive element 100 has an upper electrode and a lower electrode facing each other with a dielectric sandwiched therebetween, not only on the bottom surface but also on the side surface, so that the capacitance per unit area can be increased. Therefore, the deeper the opening 190, the larger the capacitance of the capacitive element 100 can be. Increasing the capacitance per unit area of ​​the capacitive element 100 in this way can stabilize the read operation of the memory device. In addition, miniaturization or high integration of the memory device can be promoted.

[0401] 14B and 14C show an example in which the sidewall of the opening 190 is perpendicular to the top surface of the conductive layer 110. In this case, the opening 190 has a cylindrical shape. With such a structure, miniaturization or high integration of the memory device can be achieved.

[0402] A conductive layer 115 and an insulating layer 130 are laminated along the sidewall of the opening 190 and the upper surface of the conductive layer 110. A conductive layer 120 is provided on the insulating layer 130 so as to fill the opening 190. The capacitive element 100 having such a configuration may be called a trench type capacitor or a trench capacitor.

[0403] An insulating layer 280 is disposed on the capacitive element 100. That is, the insulating layer 280 is disposed on the conductive layer 115, the insulating layer 130, and the conductive layer 120. In other words, the conductive layer 120 is disposed below the insulating layer 280.

[0404] The transistor 200 includes a conductive layer 120 (corresponding to the conductive layer 220 in FIG. 2B etc.), a conductive layer 240 over an insulating layer 280, an oxide semiconductor layer 230, an insulating layer 250 over the oxide semiconductor layer 230, and a conductive layer 260 over the insulating layer 250. The oxide semiconductor layer 230 functions as a semiconductor layer, the conductive layer 260 functions as a gate electrode, the insulating layer 250 functions as a gate insulating layer, the conductive layer 120 functions as one of a source electrode and a drain electrode, and the conductive layer 240 functions as the other of the source electrode and drain electrode.

[0405] The transistor 200 can be described in detail in the first embodiment (FIGS. 2 and 3, etc.), and therefore will not be described in detail here. The transistor included in the memory cell 150 is not limited to the transistor 200 in the memory cell 150 shown in FIGS. 2 to 3, etc., and any of the transistors exemplified in the first embodiment can be used.

[0406] As shown in FIG. 14A to FIG. 14C, the transistor 200 is provided so as to overlap with the capacitor 100. An opening 290 in which part of the structure of the transistor 200 is provided has a region overlapping with an opening 190 in which part of the structure of the capacitor 100 is provided. In particular, the conductive layer 120 functions as one of the source electrode and drain electrode of the transistor 200 and as the upper electrode of the capacitor 100, so that the transistor 200 and the capacitor 100 share part of their structures. With this structure, the transistor 200 and the capacitor 100 can be provided without significantly increasing the occupied area in a plan view. This can reduce the occupied area of ​​the memory cell 150, and therefore the memory cells 150 can be arranged at a high density, thereby increasing the memory capacity of the memory device. In other words, the memory device can be highly integrated.

[0407] Furthermore, by providing the transistor 200 above the capacitor 100, the transistor 200 is not affected by heat treatment during manufacturing of the capacitor 100. Therefore, in the transistor 200, deterioration of electrical characteristics such as a change in threshold voltage and an increase in parasitic resistance, as well as an increase in variation in electrical characteristics due to the deterioration of the electrical characteristics, can be suppressed.

[0408] A circuit diagram of the memory device described in this embodiment is shown in Fig. 19(A). As shown in Fig. 19(A), the configurations shown in Fig. 14(A) to Fig. 14(C) function as memory cells. The memory cell 951 includes a transistor M1 and a capacitor CA. Here, the transistor M1 corresponds to the transistor 200, and the capacitor CA corresponds to the capacitor 100.

[0409] One of the source and drain of the transistor M1 is connected to one of a pair of electrodes of the capacitance element CA. The other of the source and drain of the transistor M1 is connected to a wiring BIL. The gate of the transistor M1 is connected to a wiring WOL. The other of the pair of electrodes of the capacitance element CA is connected to a wiring CAL.

[0410] Here, the wiring BIL corresponds to the conductive layer 240, the wiring WOL corresponds to the conductive layer 260, and the wiring CAL corresponds to the conductive layer 110. As shown in Figs. 14(A) to 14(C), it is preferable that the conductive layer 260 is provided extending in the X direction, and the conductive layer 240 is provided extending in the Y direction. With this configuration, the wiring BIL and the wiring WOL are provided so as to cross each other. Also, in Fig. 14(A), the wiring CAL (conductive layer 110) is provided in a planar shape, but the present invention is not limited to this. For example, the wiring CAL may be provided parallel to the wiring WOL (conductive layer 260) or parallel to the wiring BIL (conductive layer 240).

[0411] The memory cells will be described in detail in a later embodiment.

[0412] 13A to 13C illustrate an example in which the structure shown in FIGS. 1A to 1C is used as the structure of the transistor 200 in FIGS. 14A to 14C.

[0413] [Capacitive element 100] The capacitor 100 includes a conductive layer 115, an insulating layer 130, and a conductive layer 120. In addition, a conductive layer 110 is provided under the conductive layer 115. The conductive layer 115 has a region in contact with the conductive layer 110.

[0414] The conductive layer 110 is provided on the insulating layer 140. The conductive layer 110 functions as a wiring CAL and can be provided in a planar shape, for example. The conductive layer 110 can be formed as a single layer or a stacked layer using the conductive material described in the [Conductive Layer] section of Embodiment 1. For example, a conductive material with high conductivity, such as tungsten, can be used as the conductive layer 110. By using such a conductive material with high conductivity, the conductivity of the conductive layer 110 can be improved, and the conductive layer 110 can function sufficiently as a wiring CAL.

[0415] The conductive layer 115 is preferably made of a conductive material that is not easily oxidized or a conductive material that has a function of suppressing diffusion of oxygen, and is used in a single layer or a stacked layer. For example, titanium nitride or indium tin oxide to which silicon is added may be used. Alternatively, for example, a structure in which titanium nitride is stacked on tungsten may be used. Alternatively, for example, a structure in which tungsten is stacked on a first titanium nitride, and a second titanium nitride is stacked on the tungsten may be used. With such a structure, when an oxide is used for the insulating layer 130, the conductive layer 110 can be prevented from being oxidized by the insulating layer 130. Furthermore, when an oxide is used for the insulating layer 180, the conductive layer 110 can be prevented from being oxidized by the insulating layer 180.

[0416] The insulating layer 130 is provided on the conductive layer 115. The insulating layer 130 is provided so as to contact the upper surface and side surfaces of the conductive layer 115. In other words, the insulating layer 130 is preferably structured to cover the side end portions of the conductive layer 110. This can prevent the conductive layer 115 and the conductive layer 120 from shorting out.

[0417] Alternatively, a structure may be used in which the side ends of the insulating layer 130 coincide with the side ends of the conductive layer 115. With such a structure, the insulating layer 130 and the conductive layer 115 can be formed using the same mask, and the manufacturing process of the memory device can be simplified.

[0418] It is preferable to use a material having a high relative dielectric constant (high-k) for the insulating layer 130. By using a high-k material for the insulating layer 130, the insulating layer 130 can be made thick enough to suppress leakage current, and the capacitance of the capacitive element 100 can be sufficiently ensured.

[0419] The insulating layer 130 is preferably made of a laminate of insulating layers made of a high-k material, and preferably has a laminate structure of a high dielectric constant (high-k) material and a material having a higher dielectric strength than the high-k material. For example, the insulating layer 130 may be made of an insulating film laminated in the order of zirconium oxide, aluminum oxide, and zirconium oxide. Alternatively, the insulating film may be made of an insulating film laminated in the order of zirconium oxide, aluminum oxide, zirconium oxide, and aluminum oxide. Alternatively, the insulating film may be made of an insulating film laminated in the order of hafnium zirconium oxide, aluminum oxide, hafnium zirconium oxide, and aluminum oxide. By using a laminate of insulating layers having a relatively high dielectric strength, such as aluminum oxide, the dielectric strength is improved, and electrostatic breakdown of the capacitance element 100 can be suppressed.

[0420] Moreover, a material that can have ferroelectricity may be used as the insulating layer 130. For details about the material that can have ferroelectricity, the description in the first embodiment can also be referred to.

[0421] Metal oxides containing one or both of hafnium and zirconium can have ferroelectricity even when they are as thin as a few nm, and are therefore preferable for the insulating layer 130. The film thickness of the insulating layer 130 is preferably 100 nm or less, more preferably 50 nm or less, even more preferably 20 nm or less, and even more preferably 10 nm or less (typically, 2 nm or more and 9 nm or less). In addition, for example, the film thickness is preferably 8 nm or more and 12 nm or less. By using a ferroelectric layer that can be thinned, the capacitive element 100 can be combined with a semiconductor element such as a miniaturized transistor to form a semiconductor device.

[0422] Furthermore, a metal oxide containing one or both of hafnium and zirconium can have ferroelectricity even in a small area, and is therefore preferable as the insulating layer 130. For example, when the area (occupancy area) of the ferroelectric layer in a plan view is 100 μm 2 Below, 10μm 2 Below, 1μm 2 Less than or equal to 0.1μm2 Even if the thickness is less than 10,000 nm, the material can have ferroelectric properties. 2 or less than 1000nm 2 Even if the thickness is less than 100 nm, the ferroelectric layer may have ferroelectricity. By using a ferroelectric layer with a small area, the area occupied by the capacitor 100 can be reduced.

[0423] A ferroelectric is an insulator, and has a property that polarization occurs inside when an electric field is applied from the outside, and the polarization remains even when the electric field is made zero. Therefore, a nonvolatile memory element can be formed by using a capacitance element (hereinafter, sometimes referred to as a ferroelectric capacitor) using this material as a dielectric. A nonvolatile memory element using a ferroelectric capacitor is sometimes called a FeRAM (Ferroelectric Random Access Memory), a ferroelectric memory, etc. For example, a ferroelectric memory has a transistor and a ferroelectric capacitor, and one of the source and drain of the transistor is electrically connected to one terminal of the ferroelectric capacitor. Therefore, when a ferroelectric capacitor is used as the capacitance element 100, the memory device shown in this embodiment functions as a ferroelectric memory.

[0424] The conductive layer 120 is provided in contact with a part of the upper surface of the insulating layer 130. The side end of the conductive layer 120 is preferably located inside the side end of the conductive layer 115 in both the X direction and the Y direction. In a structure in which the insulating layer 130 covers the side end of the conductive layer 115, the side end of the conductive layer 120 may be located outside the side end of the conductive layer 115.

[0425] The conductive layer 120 can be formed as a single layer or a stacked layer using the conductive material described in the section [Conductive Layer] of Embodiment 1. It is preferable to use a conductive material that is not easily oxidized or a conductive material that has a function of suppressing diffusion of oxygen as the conductive layer 120. For example, titanium nitride or tantalum nitride can be used. For example, a structure in which tantalum nitride is stacked on titanium nitride may be used. In this case, titanium nitride is in contact with the insulating layer 130, and tantalum nitride is in contact with the oxide semiconductor layer 230. With such a structure, excessive oxidation of the conductive layer 120 by the oxide semiconductor layer 230 can be suppressed. Furthermore, when an oxide is used for the insulating layer 130, excessive oxidation of the conductive layer 120 by the insulating layer 130 can be suppressed. Alternatively, for example, a structure in which tungsten is stacked on titanium nitride may be used as the conductive layer 120.

[0426] In addition, since the conductive layer 120 has a region in contact with the oxide semiconductor layer 230, it is preferable to use a conductive material containing oxygen. By using a conductive material containing oxygen for the conductive layer 120, the conductive layer 120 can maintain its conductivity even if it absorbs oxygen. In addition, even when an insulating layer containing oxygen such as zirconium oxide is used for the insulating layer 130, the conductive layer 120 is preferable because it can maintain its conductivity. For example, ITO, ITSO, IZO (registered trademark), or the like can be used as the conductive layer 120 in a single layer or a stacked layer.

[0427] Since the insulating layer 180 functions as an interlayer film, it is preferable that the insulating layer 180 has a low relative dielectric constant. By using a material with a low relative dielectric constant as the interlayer film, the parasitic capacitance generated between wirings can be reduced. As the insulating layer 180, an insulating layer containing a material with a low relative dielectric constant can be used in a single layer or a multilayer structure. Silicon oxide and silicon oxynitride are preferable because they are thermally stable.

[0428] 14B and 14C, the insulating layer 180 is shown as a single layer, but the present invention is not limited to this. The insulating layer 180 may have a laminated structure of two layers, or a laminated structure of three or more layers.

[0429] <Storage device configuration example 2> The memory cell 150 including the transistor 200 and the capacitor 100 described in this embodiment can be used as a memory cell of a storage device. The transistor 200 is a transistor in which a channel is formed in a semiconductor layer including an oxide semiconductor. The transistor 200 has a small off-state current; therefore, when used in a storage device, stored data can be retained for a long time. That is, a refresh operation is not required or is performed extremely infrequently; therefore, the power consumption of the storage device can be sufficiently reduced. Furthermore, the high frequency characteristics of the transistor 200 enable high-speed reading and writing of data from and to the storage device.

[0430] A memory cell array can be configured by arranging the memory cells 150 three-dimensionally in a matrix.

[0431] 15A is a plan view of a memory device, and shows an example in which 2×2 memory cells (memory cells 150a to 150d) are arranged in the X and Y directions.

[0432] Fig. 15(B) is a cross-sectional view taken along dashed line A3-A4 in Fig. 15(A). In Fig. 15(A) and Fig. 15(B), two memory cells (memory cell 150a and memory cell 150b in Fig. 15(B)) are connected to a common wiring (conductive layer 246).

[0433] Here, each of the memory cells 150a and 150b shown in FIG. 15A and FIG. 15B has a similar configuration to the memory cell 150. The memory cell 150a includes a capacitor 100a and a transistor 200a, and the memory cell 150b includes a capacitor 100b and a transistor 200b. The memory cells 150c and 150d shown in FIG. 15A also have a similar configuration to the memory cell 150. Therefore, in the memory device shown in FIG. 15A and FIG. 15B, structures having the same functions as those of the structures constituting the memory device shown in FIG. 14 are denoted by the same reference numerals. For details of the memory cells 150a to 150d, the description of the memory cell 150 in <Structure example 1 of memory device> can be referred to.

[0434] As shown in FIG. 15A and FIG. 15B, the conductive layer 260 functioning as the wiring WOL is provided in each of the memory cells 150a and 150b. As shown in FIG. 15A, one conductive layer 260 is provided in common to the memory cells 150a and 150c, and another conductive layer 260 is provided in common to the memory cells 150b and 150d. One conductive layer 240 functioning as a part of the wiring BIL is provided in common to the memory cells 150a and 150b. That is, the conductive layer 240 is in contact with the oxide semiconductor layer 230 of the memory cell 150a and the oxide semiconductor layer 230 of the memory cell 150b. The other conductive layer 240 is provided in common to the memory cells 150c and 150d.

[0435] 15A and 15B includes a conductive layer 245 and a conductive layer 246 which are electrically connected to the memory cell 150a and the memory cell 150b and function as plugs (which can also be referred to as connection electrodes). The conductive layer 245 is disposed in an opening formed in the insulating layer 140, the insulating layer 180, the insulating layer 130, and the insulating layer 280, and is in contact with a lower surface of the conductive layer 240. The conductive layer 246 is disposed in an opening formed in the insulating layer 285, the insulating layer 283, and the insulating layer 250, and is in contact with an upper surface of the conductive layer 240. Note that the conductive layer 245 and the conductive layer 246 can be formed using a conductive material that can be used for the conductive layer 240, or the like.

[0436] The conductive layer 245 and the conductive layer 246 function as plugs or wirings for electrically connecting a circuit element, such as a switch, a transistor, a capacitor, an inductor, a resistor, and a diode, a wiring, an electrode, or a terminal, to the memory cell 150a and the memory cell 150b. For example, the conductive layer 245 can be electrically connected to a sense amplifier (not shown) provided under the memory device shown in FIG. 15B, and the conductive layer 246 can be electrically connected to a similar memory device (not shown) provided over the memory device shown in FIG. 15B. In this case, the conductive layer 245 and the conductive layer 246 function as part of the wiring BIL. In this way, by providing a memory device or the like above or below the memory device shown in FIG. 15B, the memory capacity per unit area can be increased.

[0437] The memory cell 150a and the memory cell 150b are configured to be symmetrical with respect to the perpendicular bisector of the dashed line A3-A4. Thus, the transistor 200a and the transistor 200b are also arranged symmetrically with the conductive layer 245 and the conductive layer 246 sandwiched therebetween. Here, the conductive layer 240 functions as the other of the source electrode and the drain electrode of the transistor 200a and as the other of the source electrode and the drain electrode of the transistor 200b. The transistor 200a and the transistor 200b share the conductive layer 245 and the conductive layer 246 that function as plugs. In this way, by configuring the connection between the two transistors and the plugs as described above, a memory device that can be miniaturized or highly integrated can be provided.

[0438] Note that the conductive layer 110 functioning as the wiring CAL may be provided in each of the memory cells 150a and 150b, or may be provided in common to the memory cells 150a and 150b. However, as shown in FIG. 15B, the conductive layer 110 is provided apart from the conductive layer 245 so that the conductive layer 110 and the conductive layer 245 are not short-circuited.

[0439] 16 shows an example in which the four memory cells shown in FIG. 15A are stacked in n layers (n is an integer of 3 or more) in the Z direction. FIG. 16 is a cross-sectional view taken along dashed line A3-A4 shown in FIG. 15A.

[0440] The memory device shown in FIG. 16 has n memory layers 160. Specifically, a memory layer 160[2] is provided on the memory layer 160[1], and (n-2) memory layers are further provided on the memory layer 160[2], with the memory layer 160[n] provided at the top. The number of memory cells in one memory layer 160 is not particularly limited, and two or more memory cells may be included. The memory cells in the n memory layers 160 are electrically connected to a sense amplifier (not shown) provided under the n memory layers 160 by the conductive layers 245, 246, 247, and 248, etc.

[0441] As shown in Fig. 16, by stacking multiple memory cells, the cells can be integrated and arranged without increasing the area occupied by the memory cell array. In other words, a 3D memory cell array can be configured.

[0442] FIG. 17 shows an example of a cross-sectional configuration of a memory device in which a layer having memory cells is stacked over a layer in which a driver circuit including a sense amplifier is provided.

[0443] In FIG. 17, a memory cell 150 (a transistor 200 and a capacitor 100) is provided above a transistor 300.

[0444] The transistor 300 is one of the transistors included in the sense amplifier.

[0445] For the memory cell 150 illustrated in FIG. 17, the description of the memory cell 150 in <Structure example 1 of memory device> can be referred to. Note that FIG. 17 illustrates an example in which the capacitor 100 includes a conductive layer 120a and a conductive layer 120b over the conductive layer 120a, instead of the conductive layer 120. Here, for example, a material that can be used for the conductive layer 220c can be used as the conductive layer 120b. For example, a material that can be used for the conductive layer 220a and the conductive layer 220b can be used as the conductive layer 120a. Although FIG. 17 illustrates an example in which the oxide semiconductor layer 230 is in contact with the top surface of the conductive layer 120a, the oxide semiconductor layer 230 does not necessarily need to be in contact with the top surface of the conductive layer 120a.

[0446] 17, the bit line can be shortened by providing a sense amplifier so as to overlap the memory cell 150. This reduces the bit line capacitance and enables high-speed operation of the memory device.

[0447] 17 can correspond to the semiconductor device 900 described in Embodiment 3. Specifically, the transistor 300 corresponds to a transistor included in a sense amplifier 927 in the semiconductor device 900. The memory cell 150 corresponds to a memory cell 950.

[0448] The transistor 300 is provided over a substrate 311 and includes a conductive layer 316 functioning as a gate, an insulating layer 315 functioning as a gate insulating layer, a semiconductor region 313 formed of a part of the substrate 311, and a low-resistance region 314a and a low-resistance region 314b functioning as a source region or a drain region. The transistor 300 may be either a p-channel type or an n-channel type.

[0449] Here, in the transistor 300 shown in FIG. 17, a semiconductor region 313 (a part of a substrate 311) in which a channel is formed has a convex shape. A conductive layer 316 is provided so as to cover the side and top surface of the semiconductor region 313 with an insulating layer 315 interposed therebetween. Note that the conductive layer 316 may be made of a material that adjusts the work function. Such a transistor 300 is also called a FIN type transistor because it uses a convex portion of a semiconductor substrate. Note that an insulating layer that is in contact with an upper portion of the convex portion and functions as a mask for forming the convex portion may be provided. Note that, although a case where a convex portion is formed by processing a part of a semiconductor substrate has been shown here, a semiconductor film having a convex shape may be formed by processing an SOI substrate.

[0450] Note that the transistor 300 illustrated in FIG. 17 is just an example, and the present invention is not limited to this structure. Any appropriate transistor can be used depending on the circuit configuration or driving method.

[0451] Between each structure, a wiring layer having an interlayer film, wiring, plugs, etc. may be provided. Also, a plurality of wiring layers may be provided according to the design. Here, the conductive layer functioning as a plug or wiring may be given the same reference symbol as a plurality of structures. Also, in this specification, the wiring and the plug electrically connected to the wiring may be integrated. That is, there are cases where a part of the conductive layer functions as the wiring, and cases where a part of the conductive layer functions as the plug.

[0452] For example, an insulating layer 320, an insulating layer 322, an insulating layer 324, and an insulating layer 326 are stacked in this order as an interlayer film over the transistor 300. A conductive layer 328 is embedded in the insulating layer 320 and the insulating layer 322, and a conductive layer 330 is embedded in the insulating layer 324 and the insulating layer 326. Note that the conductive layer 328 and the conductive layer 330 function as a plug or a wiring.

[0453] In addition, the insulating layer functioning as an interlayer film may also function as a planarizing film that covers the uneven shape below it. For example, the top surface of the insulating layer 322 may be planarized by a planarization process using a CMP method or the like to improve the planarity.

[0454] A wiring layer may be provided over the insulating layer 326 and the conductive layer 330. For example, in FIG. 17, an insulating layer 350, an insulating layer 352, and an insulating layer 354 are stacked in this order. A conductive layer 356 is formed in the insulating layer 350, the insulating layer 352, and the insulating layer 354. The conductive layer 356 functions as a plug or a wiring.

[0455] The insulating layer 352, the insulating layer 354, and the like which function as an interlayer film can be the above-mentioned insulating layer which can be used in a semiconductor device or a memory device.

[0456] A conductive layer functioning as a plug or a wiring, such as the conductive layer 328, the conductive layer 330, and the conductive layer 356, can be formed using a conductive material applicable to the conductive layer 240. A high melting point material having both heat resistance and conductivity, such as tungsten or molybdenum, is preferably used, and tungsten is preferably used. Alternatively, it is preferably formed using a low resistance conductive material, such as aluminum or copper. By using a low resistance conductive material, the wiring resistance can be reduced.

[0457] The conductive layer 240 of the transistor 200 is electrically connected to the low-resistance region 314b functioning as a source region or drain region of the transistor 300 through a conductive layer 643, a conductive layer 642, a conductive layer 644, a conductive layer 645, a conductive layer 646, a conductive layer 356, a conductive layer 330, and a conductive layer 328.

[0458] The conductive layer 643 is embedded in the insulating layer 280. The conductive layer 642 is provided on the insulating layer 130 and embedded in the insulating layer 641. The conductive layer 642 can be manufactured using the same material and in the same process as the conductive layer 120a. The conductive layer 644 is embedded in the insulating layer 180 and the insulating layer 130. The conductive layer 645 is embedded in the insulating layer 647. The conductive layer 645 can be manufactured using the same material and in the same process as the conductive layer 110. The conductive layer 646 is embedded in the insulating layer 648. The transistor 300 and the conductive layer 110 are electrically insulated by the insulating layer 648.

[0459] As described above, the memory device of this embodiment has a transistor with reduced parasitic capacitance, and therefore the operating speed can be increased. In addition, the memory device of this embodiment has a capacitor and a transistor stacked on top of each other, and therefore the area occupied by the memory cell in a plan view can be reduced, and a memory device with high integration can be realized.

[0460] This embodiment mode can be combined with other embodiment modes as appropriate.

[0461] (Embodiment 3) In this embodiment, a semiconductor device 900 according to one embodiment of the present invention will be described. The semiconductor device 900 can function as a memory device.

[0462] Fig. 18 shows a block diagram illustrating a configuration example of a semiconductor device 900. The semiconductor device 900 shown in Fig. 18 has a driver circuit 910 and a memory cell array 920. The memory cell array 920 has one or more memory cells 950. Fig. 18 shows an example in which the memory cell array 920 has a plurality of memory cells 950 arranged in a matrix.

[0463] The memory cell 950 can be the memory device described in the second embodiment (such as the memory cell 150).

[0464] The drive circuit 910 includes a PSW 931 (power switch), a PSW 932, and a peripheral circuit 915. The peripheral circuit 915 includes a peripheral circuit 911, a control circuit 912, and a voltage generating circuit 928.

[0465] In the semiconductor device 900, each circuit, each signal, and each voltage can be appropriately selected or omitted as necessary. Alternatively, other circuits or other signals may be added. The signals BW, CE, GW, CLK, WAKE, ADDR, WDA, PON1, and PON2 are input signals from the outside, and the signal RDA is an output signal to the outside. The signal CLK is a clock signal.

[0466] Moreover, signals BW, CE, and GW are control signals. Signal CE is a chip enable signal, signal GW is a global write enable signal, and signal BW is a byte write enable signal. Signal ADDR is an address signal. Signal WDA is write data, and signal RDA is read data. Signals PON1 and PON2 are power gating control signals. Signals PON1 and PON2 may be generated by the control circuit 912.

[0467] The control circuit 912 is a logic circuit having a function of controlling the overall operation of the semiconductor device 900. For example, the control circuit 912 performs a logical operation on the signals CE, GW, and BW to determine an operation mode (e.g., a write operation, a read operation) of the semiconductor device 900. Alternatively, the control circuit 912 generates a control signal for the peripheral circuit 911 so that this operation mode is executed.

[0468] The voltage generating circuit 928 has a function of generating a negative voltage. The signal WAKE has a function of controlling the input of the signal CLK to the voltage generating circuit 928. For example, when an H-level signal is provided as the signal WAKE, the signal CLK is input to the voltage generating circuit 928, and the voltage generating circuit 928 generates a negative voltage.

[0469] The peripheral circuit 911 is a circuit for writing and reading data to and from the memory cells 950. The peripheral circuit 911 has a row decoder 941, a column decoder 942, a row driver 923, a column driver 924, an input circuit 925, an output circuit 926, and a sense amplifier 927.

[0470] The row decoder 941 and the column decoder 942 have a function of decoding the signal ADDR. The row decoder 941 is a circuit for specifying a row to be accessed, and the column decoder 942 is a circuit for specifying a column to be accessed. The row driver 923 has a function of selecting a row specified by the row decoder 941. The column driver 924 has a function of writing data to the memory cell 950, a function of reading data from the memory cell 950, a function of holding the read data, and the like.

[0471] The input circuit 925 has a function of holding a signal WDA. The data held by the input circuit 925 is output to the column driver 924. The output data of the input circuit 925 is data (Din) to be written to the memory cell 950. The data (Dout) read from the memory cell 950 by the column driver 924 is output to the output circuit 926. The output circuit 926 has a function of holding Dout. In addition, the output circuit 926 has a function of outputting Dout to the outside of the semiconductor device 900. The data output from the output circuit 926 is a signal RDA.

[0472] PSW931 is the V to the peripheral circuit 915 DD The PSW 932 has the function of controlling the supply of V HM In this embodiment, the high power supply voltage of the semiconductor device 900 is V DD and the low power supply voltage is GND (ground potential). Also, V HM is the high power supply voltage used to drive the word line high, and V DD 18, in the peripheral circuit 915, V DD Although the number of power domains to which the power is supplied is set to one, it is also possible to set it to multiple. In this case, a power switch may be provided for each power domain.

[0473] A configuration example of a memory cell that can be used as the memory cell 950 will be described with reference to FIGS.

[0474] In the following, when it is stated that two components are connected, this includes being electrically connected via a circuit element (such as a transistor, a switch, a diode, or a resistive element). Electrical connection means that a state in which a current can flow between two components. Note that when two components are connected via a switch or a transistor, this is also included in the electrical connection because a state in which a current can flow when these are in the on state is possible.

[0475] [DOSRAM] 19A shows an example of a circuit configuration of a memory cell of a DRAM. In this specification and the like, a DRAM using an OS transistor is referred to as a dynamic oxide semiconductor random access memory (DOSRAM). The memory cell 951 includes a transistor M1 and a capacitor CA.

[0476] The transistor M1 may have a front gate (sometimes simply referred to as a gate) and a back gate. In this case, the back gate may be connected to a wiring that supplies a constant potential or a signal, or the front gate and the back gate may be connected to each other.

[0477] A first terminal of the transistor M1 is connected to a first terminal of the capacitance element CA, a second terminal of the transistor M1 is connected to the wiring BIL, a gate of the transistor M1 is connected to the wiring WOL, and a second terminal of the capacitance element CA is connected to the wiring CAL.

[0478] The wiring BIL functions as a bit line, and the wiring WOL functions as a word line. The wiring CAL functions as a wiring for applying a predetermined potential to the second terminal of the capacitance element CA. When writing and reading data, it is preferable to apply a low-level potential (sometimes called a reference potential) to the wiring CAL.

[0479] Data is written and read by applying a high-level potential to the wiring WOL, turning on the transistor M1, and bringing the wiring BIL and the first terminal of the capacitor CA into a conductive state (a state in which a current can flow).

[0480] Further, a memory cell that can be used as the memory cell 950 is not limited to the memory cell 951, and the circuit configuration can be changed. For example, a memory cell 952 shown in FIG. 19B may be used. The memory cell 952 is an example of a memory cell that does not include a capacitor CA and a wiring CAL. The first terminal of the transistor M1 is in an electrically floating state.

[0481] In the memory cell 952, the potential written through the transistor M1 is held in a capacitance (also referred to as a parasitic capacitance) between the first terminal and the gate, which is indicated by a dashed line. With this configuration, the configuration of the memory cell can be significantly simplified.

[0482] Note that it is preferable to use an OS transistor as the transistor M1. An OS transistor has a characteristic that its off-state current is extremely small. By using an OS transistor as the transistor M1, the leakage current of the transistor M1 can be made extremely low. That is, since written data can be held by the transistor M1 for a long time, the frequency of refreshing the memory cell can be reduced. Alternatively, the refresh operation of the memory cell can be made unnecessary. Furthermore, since the leakage current is extremely low, multi-level data or analog data can be held in the memory cell 951 and the memory cell 952.

[0483] [NOSRAM] 19C shows an example of a circuit configuration of a gain cell type memory cell having two transistors and one capacitor. The memory cell 953 includes a transistor M2, a transistor M3, and a capacitor CB. In this specification and the like, a memory device having a gain cell type memory cell using an OS transistor as the transistor M2 is referred to as a nonvolatile oxide semiconductor RAM (NOSRAM).

[0484] A first terminal of the transistor M2 is connected to a first terminal of the capacitance element CB, a second terminal of the transistor M2 is connected to the wiring WBL, and a gate of the transistor M2 is connected to the wiring WOL. A second terminal of the capacitance element CB is connected to the wiring CAL. A first terminal of the transistor M3 is connected to the wiring RBL, a second terminal of the transistor M3 is connected to the wiring SL, and a gate of the transistor M3 is connected to the first terminal of the capacitance element CB.

[0485] The line WBL functions as a write bit line, the line RBL functions as a read bit line, and the line WOL functions as a word line. The line CAL functions as a line for applying a predetermined potential to the second terminal of the capacitance element CB. When writing data, while holding data, and when reading data, it is preferable to apply a low-level potential (sometimes called a reference potential) to the line CAL.

[0486] Data is written by applying a high-level potential to the wiring WOL, turning on the transistor M2, and bringing the wiring WBL and the first terminal of the capacitor CB into electrical continuity. Specifically, when the transistor M2 is on, a potential corresponding to the information to be recorded is applied to the wiring WBL, and the potential is written to the first terminal of the capacitor CB and the gate of the transistor M3. After that, a low-level potential is applied to the wiring WOL to turn off the transistor M2, thereby holding the potential of the first terminal of the capacitor CB and the potential of the gate of the transistor M3.

[0487] Data is read by applying a predetermined potential to the wiring SL. The current flowing between the source and drain of the transistor M3 and the potential of the first terminal of the transistor M3 are determined by the potential of the gate of the transistor M3 and the potential of the second terminal of the transistor M3. Therefore, the potential held in the first terminal of the capacitance element CB (or the gate of the transistor M3) can be read by reading the potential of the wiring RBL connected to the first terminal of the transistor M3. In other words, information written in this memory cell can be read from the potential held in the first terminal of the capacitance element CB (or the gate of the transistor M3).

[0488] Further, for example, the wiring WBL and the wiring RBL may be integrated into a single wiring BIL. An example of the circuit configuration of the memory cell is shown in Fig. 19(D). The memory cell 954 is configured such that the wiring WBL and the wiring RBL of the memory cell 953 are integrated into a single wiring BIL, and the second terminal of the transistor M2 and the first terminal of the transistor M3 are connected to the wiring BIL. In other words, the memory cell 954 is configured to operate the write bit line and the read bit line as a single wiring BIL.

[0489] 19E is an example of a memory cell 955 in which the capacitor CB and the wiring CAL are omitted in the memory cell 953. Also, FIG 19F is an example of a memory cell 956 in which the capacitor CB and the wiring CAL are omitted in the memory cell 954. With such a configuration, the integration degree of the memory cells can be increased.

[0490] Note that at least the transistor M2 is preferably an OS transistor, and in particular, the transistors M2 and M3 are preferably OS transistors.

[0491] Since the OS transistor has a characteristic that the off-state current is extremely small, the written data can be held for a long time by the transistor M2, so that the frequency of refreshing the memory cell can be reduced. Alternatively, the refresh operation of the memory cell can be eliminated. In addition, since the leakage current is extremely low, multi-level data or analog data can be held in the memory cell 953, the memory cell 954, the memory cell 955, and the memory cell 956.

[0492] The memory cell 953, the memory cell 954, the memory cell 955, and the memory cell 956 in which an OS transistor is used as the transistor M2 are one aspect of NOSRAM.

[0493] Note that a Si transistor may be used as the transistor M3. The Si transistor can increase the field effect mobility and can also be a p-channel transistor, which increases the degree of freedom in circuit design.

[0494] When an OS transistor is used as the transistor M3, the memory cell can be configured as a unipolar circuit.

[0495] 19G shows a three-transistor, one-capacitor gain cell type memory cell 957. The memory cell 957 includes transistors M4 to M6 and a capacitor CC.

[0496] A first terminal of the transistor M4 is connected to a first terminal of the capacitance element CC, a second terminal of the transistor M4 is connected to the wiring BIL, and a gate of the transistor M4 is connected to the wiring WOL. A second terminal of the capacitance element CC is connected to a first terminal of the transistor M5 and the wiring GNDL. A second terminal of the transistor M5 is connected to a first terminal of the transistor M6, and a gate of the transistor M5 is connected to the first terminal of the capacitance element CC. A second terminal of the transistor M6 is connected to the wiring BIL, and a gate of the transistor M6 is connected to the wiring RWL.

[0497] The wiring BIL functions as a bit line, the wiring WOL functions as a write word line, and the wiring RWL functions as a read word line. The wiring GNDL is a wiring that applies a low level potential.

[0498] Data is written by applying a high-level potential to the wiring WOL, turning on the transistor M4, and connecting the wiring BIL and the first terminal of the capacitor CC. Specifically, when the transistor M4 is on, a potential corresponding to the information to be recorded is applied to the wiring BIL, and the potential is written to the first terminal of the capacitor CC and the gate of the transistor M5. After that, a low-level potential is applied to the wiring WOL to turn off the transistor M4, thereby holding the potential of the first terminal of the capacitor CC and the potential of the gate of the transistor M5.

[0499] Data is read by precharging the wiring BIL with a predetermined potential, then putting the wiring BIL in an electrically floating state and applying a high-level potential to the wiring RWL. Since the wiring RWL is at a high-level potential, the transistor M6 is turned on, and the wiring BIL and the second terminal of the transistor M5 are in a conductive state. At this time, the potential of the wiring BIL is applied to the second terminal of the transistor M5, and the potential of the second terminal of the transistor M5 and the potential of the wiring BIL change depending on the potential held in the first terminal of the capacitance element CC (or the gate of the transistor M5). Here, by reading the potential of the wiring BIL, the potential held in the first terminal of the capacitance element CC (or the gate of the transistor M5) can be read. In other words, information written in this memory cell can be read from the potential held in the first terminal of the capacitance element CC (or the gate of the transistor M5).

[0500] Note that it is preferable to use an OS transistor for at least the transistor M4.

[0501] Note that Si transistors may be used as the transistors M5 and M6. As described above, a Si transistor may have higher field-effect mobility than an OS transistor depending on the crystal state of silicon used in a semiconductor layer.

[0502] When OS transistors are used as the transistors M5 and M6, the memory cell can be configured as a unipolar circuit.

[0503] [OS-SRAM] FIG. 19H shows an example of a static random access memory (SRAM) using OS transistors. In this specification and the like, an SRAM using OS transistors is referred to as an oxide semiconductor SRAM (OS-SRAM). Note that a memory cell 958 shown in FIG. 19H is a memory cell of an SRAM capable of backing up data.

[0504] The memory cell 958 includes transistors M7 to M10, transistors MS1 to MS4, and capacitors CD1 and CD2. Note that the transistors MS1 and MS2 are p-channel transistors, and the transistors MS3 and MS4 are n-channel transistors.

[0505] A first terminal of the transistor M7 is connected to the wiring BIL, and a second terminal of the transistor M7 is connected to a first terminal of the transistor MS1, a first terminal of the transistor MS3, a gate of the transistor MS2, a gate of the transistor MS4, and a first terminal of the transistor M10. A gate of the transistor M7 is connected to the wiring WOL. A first terminal of the transistor M8 is connected to the wiring BILB, and a second terminal of the transistor M8 is connected to a first terminal of the transistor MS2, a first terminal of the transistor MS4, a gate of the transistor MS1, a gate of the transistor MS3, and a first terminal of the transistor M9. A gate of the transistor M8 is connected to the wiring WOL.

[0506] A second terminal of the transistor MS1 is connected to the wiring VDL. A second terminal of the transistor MS2 is connected to the wiring VDL. A second terminal of the transistor MS3 is connected to the wiring GNDL. A second terminal of the transistor MS4 is connected to the wiring GNDL.

[0507] A second terminal of the transistor M9 is connected to a first terminal of the capacitance element CD1, and a gate of the transistor M9 is connected to the wiring BRL. A second terminal of the transistor M10 is connected to a first terminal of the capacitance element CD2, and a gate of the transistor M10 is connected to the wiring BRL.

[0508] A second terminal of the capacitance element CD1 is connected to the wiring GNDL, and a second terminal of the capacitance element CD2 is connected to the wiring GNDL.

[0509] The wirings BIL and BILB function as bit lines, the wiring WOL functions as a word line, and the wiring BRL is a wiring that controls the on / off state of the transistors M9 and M10.

[0510] The line VDL is a line that applies a high-level potential, and the line GNDL is a line that applies a low-level potential.

[0511] Data is written by applying a high-level potential to the wiring WOL and a high-level potential to the wiring BRL. Specifically, when the transistor M10 is on, a potential corresponding to information to be recorded is applied to the wiring BIL, and the potential is written to the second terminal of the transistor M10.

[0512] Incidentally, since the memory cell 958 forms an inverter loop with the transistors MS1 and MS2, an inverted signal of the data signal corresponding to the potential is input to the second terminal of the transistor M8. Since the transistor M8 is in an on state, the potential applied to the wiring BIL, i.e., the inverted signal of the signal input to the wiring BIL, is output to the wiring BILB. Since the transistors M9 and M10 are in an on state, the potential of the second terminal of the transistor M7 and the potential of the second terminal of the transistor M8 are held in the first terminal of the capacitor CD2 and the first terminal of the capacitor CD1, respectively. After that, a low-level potential is applied to the wiring WOL and a low-level potential is applied to the wiring BRL to turn off the transistors M7 to M10, thereby holding the potential of the first terminal of the capacitor CD1 and the first terminal of the capacitor CD2.

[0513] Data is read by precharging the wirings BIL and BILB to a predetermined potential in advance, and then applying a high-level potential to the wiring WOL and a high-level potential to the wiring BRL, so that the potential of the first terminal of the capacitor CD1 is refreshed by the inverter loop of the memory cell 958 and output to the wiring BILB. Also, the potential of the first terminal of the capacitor CD2 is refreshed by the inverter loop of the memory cell 958 and output to the wiring BIL. In the wirings BIL and BILB, the potentials change from the precharged potentials to the potential of the first terminal of the capacitor CD2 and the potential of the first terminal of the capacitor CD1, respectively, so that the potential held in the memory cell can be read from the potential of the wiring BIL or wiring BILB.

[0514] Note that it is preferable to use OS transistors as the transistors M7 to M10. In this case, written data can be held for a long time by the transistors M7 to M10, so that the frequency of refreshing the memory cells can be reduced. Alternatively, the refresh operation of the memory cells can be eliminated.

[0515] Note that Si transistors may be used as the transistors MS1 to MS4.

[0516] The driver circuit 910 and the memory cell array 920 included in the semiconductor device 900 may be provided on the same plane. Alternatively, as shown in Fig. 20A, the driver circuit 910 and the memory cell array 920 may be provided so as to overlap each other. By providing the driver circuit 910 and the memory cell array 920 so as to overlap each other, the signal propagation distance can be shortened. Alternatively, as shown in Fig. 20B, the memory cell array 920 may be provided in multiple layers on the driver circuit 910.

[0517] Next, an example of a processing device that can include a semiconductor device such as the memory device will be described.

[0518] Fig. 21 shows a block diagram of the arithmetic device 960. The arithmetic device 960 shown in Fig. 21 can be applied to, for example, a CPU (Central Processing Unit). The arithmetic device 960 can also be applied to processors such as a GPU (Graphics Processing Unit), a TPU (Tensor Processing Unit), and an NPU (Neural Processing Unit) that have a large number (tens to hundreds) of processor cores capable of parallel processing compared to a CPU.

[0519] 21 has an ALU 991 (ALU: Arithmetic logic unit, arithmetic circuit), an ALU controller 992, an instruction decoder 993, an interrupt controller 994, a timing controller 995, a register 996, a register controller 997, a bus interface 998, a cache 999, and a cache interface 989 on a substrate 990. The substrate 990 uses a semiconductor substrate, an SOI substrate, a glass substrate, or the like. It may have a rewritable ROM and a ROM interface. The cache 999 and the cache interface 989 may be provided on a separate chip.

[0520] The cache 999 is connected to a main memory provided on a separate chip via a cache interface 989. The cache interface 989 has a function of supplying a portion of the data held in the main memory to the cache 999. The cache interface 989 also has a function of outputting a portion of the data held in the cache 999 to the ALU 991, register 996, etc. via the bus interface 998.

[0521] As described later, a memory cell array 920 can be provided by stacking it on the arithmetic device 960. The memory cell array 920 can be used as a cache. In this case, the cache interface 989 may have a function of supplying data held in the memory cell array 920 to the cache 999. In this case, it is preferable that a part of the cache interface 989 has a drive circuit 910.

[0522] It is also possible to use only the memory cell array 920 as a cache without providing the cache 999.

[0523] The arithmetic device 960 shown in FIG. 21 is merely an example of a simplified configuration, and the actual arithmetic device 960 has a wide variety of configurations depending on its application. For example, it is preferable to use a configuration including the arithmetic device 960 shown in FIG. 21 as one core, and to use a so-called multi-core configuration in which the cores are included and each core operates in parallel. The more cores there are, the higher the arithmetic performance can be. The more cores there are, the more preferable it is, but for example, 2, preferably 4, more preferably 8, even more preferably 12, and even more preferably 16 or more. In addition, when very high arithmetic performance is required for server applications, it is preferable to use a multi-core configuration having 16 or more cores, preferably 32 or more, and even more preferably 64 or more. In addition, the number of bits that the arithmetic device 960 can handle in its internal arithmetic circuit, data bus, etc. can be, for example, 8 bits, 16 bits, 32 bits, 64 bits, etc.

[0524] An instruction input to the arithmetic unit 960 via the bus interface 998 is input to an instruction decoder 993 , decoded, and then input to an ALU controller 992 , an interrupt controller 994 , a register controller 997 , and a timing controller 995 .

[0525] The ALU controller 992, the interrupt controller 994, the register controller 997, and the timing controller 995 perform various controls based on the decoded instructions. Specifically, the ALU controller 992 generates a signal for controlling the operation of the ALU 991. Furthermore, the interrupt controller 994 judges and processes interrupt requests from external input / output devices, peripheral circuits, etc. based on their priority and mask state while the arithmetic device 960 is executing a program. The register controller 997 generates an address for a register 996, and reads and writes data from and to the register 996 depending on the state of the arithmetic device 960.

[0526] Furthermore, the timing controller 995 generates signals that control the timing of the operations of the ALU 991, the ALU controller 992, the instruction decoder 993, the interrupt controller 994, and the register controller 997. For example, the timing controller 995 includes an internal clock generating unit that generates an internal clock signal based on a reference clock signal, and supplies the internal clock signal to the various circuits described above.

[0527] In the arithmetic device 960 shown in FIG. 21, the register controller 997 selects a holding operation in the register 996 in accordance with an instruction from the ALU 991. That is, the register controller 997 selects whether data is to be held by a flip-flop or by a capacitive element in the memory cell of the register 996. When holding data by a flip-flop is selected, a power supply voltage is supplied to the memory cell in the register 996. When holding data in a capacitive element is selected, data is rewritten to the capacitive element, and the supply of power supply voltage to the memory cell in the register 996 can be stopped.

[0528] The memory cell array 920 and the arithmetic device 960 can be provided overlapping each other. FIGS. 22A and 22B are perspective views of a semiconductor device 970A. The semiconductor device 970A includes a layer 930 in which a memory cell array is provided over an arithmetic device 960. A memory cell array 920L1, a memory cell array 920L2, and a memory cell array 920L3 are provided in the layer 930. The arithmetic device 960 and each memory cell array have an overlapping region. To make the configuration of the semiconductor device 970A easier to understand, the arithmetic device 960 and the layer 930 are shown separately in FIG. 22B.

[0529] By overlapping the layer 930 having the memory cell array and the arithmetic device 960, the connection distance between them can be shortened. Therefore, the communication speed between them can be increased. In addition, the short connection distance can reduce power consumption.

[0530] As a method for stacking the layer 930 having the memory cell array and the arithmetic device 960, a method of stacking the layer 930 having the memory cell array directly on the arithmetic device 960 (also called monolithic stacking) may be used, or a method of forming the arithmetic device 960 and the layer 930 on different substrates, bonding the two substrates, and electrically connecting them using a through via or conductive film bonding technology (Cu-Cu bonding, etc.) may be used. Since the former does not require consideration of misalignment during bonding, it is possible to reduce not only the chip size but also the manufacturing cost.

[0531] Here, the arithmetic device 960 does not have a cache 999, and the memory cell arrays 920L1, 920L2, and 920L3 provided in the layer 930 can be used as caches. In this case, for example, the memory cell array 920L1 can be used as an L1 cache (also called a level 1 cache), the memory cell array 920L2 can be used as an L2 cache (also called a level 2 cache), and the memory cell array 920L3 can be used as an L3 cache (also called a level 3 cache). Of the three memory cell arrays, the memory cell array 920L3 has the largest capacity and is accessed the least frequently. Also, the memory cell array 920L1 has the smallest capacity and is accessed the most frequently.

[0532] When the cache 999 provided in the arithmetic device 960 is used as an L1 cache, each memory cell array provided in the layer 930 can be used as a lower-level cache or a main memory. The main memory has a larger capacity than the cache and is accessed less frequently.

[0533] 22B, a driving circuit 910L1, a driving circuit 910L2, and a driving circuit 910L3 are provided. The driving circuit 910L1 is connected to the memory cell array 920L1 via a connection electrode 940L1. Similarly, the driving circuit 910L2 is connected to the memory cell array 920L2 via a connection electrode 940L2, and the driving circuit 910L3 is connected to the memory cell array 920L3 via a connection electrode 940L3.

[0534] Although the number of memory cell arrays functioning as a cache is three in this embodiment, the number may be one or two, or four or more.

[0535] When the memory cell array 920L1 is used as a cache, the drive circuit 910L1 may function as a part of the cache interface 989, or the drive circuit 910L1 may be configured to be connected to the cache interface 989. Similarly, the drive circuit 910L2 and the drive circuit 910L3 may also function as a part of the cache interface 989, or may be configured to be connected thereto.

[0536] Whether the memory cell array 920 is caused to function as a cache or as a main memory is determined by a control circuit 912 included in each drive circuit 910. The control circuit 912 can cause some of the multiple memory cells 950 included in the semiconductor device 900 to function as a RAM based on a signal supplied from the arithmetic device 960.

[0537] The semiconductor device 900 can cause some of the memory cells 950 to function as a cache and the other memory cells to function as a main memory. That is, the semiconductor device 900 can have both a function as a cache and a function as a main memory. The semiconductor device 900 according to one embodiment of the present invention can function as, for example, a universal memory.

[0538] Furthermore, a layer 930 having one memory cell array 920 may be provided overlapping with the arithmetic device 960. Figure 23A shows a perspective view of a semiconductor device 970B.

[0539] In the semiconductor device 970B, one memory cell array 920 can be divided into multiple areas, and each area can be used for different functions. Fig. 23(A) shows an example in which the area L1 is used as an L1 cache, the area L2 is used as an L2 cache, and the area L3 is used as an L3 cache.

[0540] In addition, in the semiconductor device 970B, the capacity of each of the areas L1 to L3 can be changed according to the situation. For example, if it is desired to increase the capacity of the L1 cache, this can be achieved by increasing the area of ​​the area L1. With this configuration, it is possible to improve the efficiency of the calculation process and the processing speed.

[0541] Moreover, a plurality of memory cell arrays may be stacked. FIG 23B shows a perspective view of a semiconductor device 970C.

[0542] The semiconductor device 970C has a layer 930L1 having a memory cell array 920L1, a layer 930L2 having a memory cell array 920L2 thereon, and a layer 930L3 having a memory cell array 920L3 thereon. The memory cell array 920L1, which is physically closest to the arithmetic device 960, can be used as a higher-level cache, and the memory cell array 920L3, which is the furthest away, can be used as a lower-level cache or main memory. With this configuration, the capacity of each memory cell array can be increased, thereby further improving the processing power.

[0543] This embodiment mode can be combined with other embodiment modes as appropriate.

[0544] (Embodiment 4) In this embodiment, application examples of a storage device according to one embodiment of the present invention will be described.

[0545] Generally, various storage devices are used in semiconductor devices such as computers depending on the purpose. FIG. 24(A) shows various storage devices used in semiconductor devices by hierarchy. The higher the storage device is located in the hierarchy, the faster the operation speed is required, and the lower the storage device is located in the hierarchy, the larger the storage capacity and the higher the recording density are required. In FIG. 24(A), from the top layer, there are a memory integrated as a register in an arithmetic processing device such as a CPU, an L1 cache, an L2 cache, an L3 cache, a main memory, a storage, and the like. Note that, although an example having up to an L3 cache is shown here, a lower cache may also be included.

[0546] The memory embedded as a register in a processor such as a CPU is used for temporary storage of calculation results, and is accessed frequently by the processor. Therefore, a faster operating speed is required rather than a larger memory capacity. The register also has the function of storing setting information for the processor.

[0547] A cache has the function of duplicating and storing a portion of the data stored in the main memory. By duplicating frequently used data and storing it in the cache, the access speed to the data can be increased. The storage capacity required for a cache is smaller than that of the main memory, but it is required to operate faster than the main memory. In addition, data that is rewritten in the cache is duplicated and supplied to the main memory.

[0548] The main memory has a function of holding programs, data, etc. read from storage.

[0549] Storage has the function of storing data that needs to be stored for a long time, various programs used by the processing unit, etc. Therefore, storage requires a large memory capacity and high recording density rather than an operating speed. For example, a high-capacity, non-volatile storage device such as 3D NAND can be used.

[0550] A storage device using an oxide semiconductor according to one embodiment of the present invention (OS memory) has a high operating speed and can retain data for a long period of time. Therefore, as shown in FIG. 24A, the storage device according to one embodiment of the present invention can be preferably used in both a tier where a cache is located and a tier where a main memory is located. The storage device according to one embodiment of the present invention can also be applied to a tier where a storage is located.

[0551] As the OS memory, the above-mentioned DOSRAM, NOSRAM, and OS-SRAM can be suitably used.

[0552] Among these memories, caches are required to have faster operating speeds.

[0553] On the other hand, since the main memory has a larger capacity than the cache, it is preferable that the memory element used for the main memory has a structure capable of further reducing power consumption. The OS memory of one embodiment of the present invention can realize a memory having a long retention time by utilizing the characteristics of the extremely small off-current of the OS transistor. By using the OS memory as the main memory, a long retention time can be realized, and power consumption of the storage device can be reduced. For example, a DOSRAM having an operation speed of 15 ns or less and a long retention time can be used as the main memory. In the case of a DRAM formed of transistors using silicon, the retention time is about 64 ms (milliseconds). In the case of a DOSRAM using an OS transistor, a retention time of about 10 times that can be realized. By increasing the retention time, the refresh frequency can be reduced, and power consumption of the storage device can be reduced. By setting the write time and read time of the DOSRAM to 15 ns (nanoseconds) or less, respectively, the DOSRAM can be suitably used as the main memory. In addition, the retention time of the DOSRAM is preferably 0.64 s (seconds) or more. The write time and read time of the DOSRAM of one embodiment of the present invention are preferably 15 ns or less. At least one of the write time and read time of the DOSRAM according to one embodiment of the present invention is, for example, 1 ns or more and less than 15 ns. Or, for example, it is more than 2 ns and less than 15 ns. The retention time of the DOSRAM according to one embodiment of the present invention is preferably 0.16 s or more, more preferably 0.32 s or more, and even more preferably 0.64 s or more. The memory is preferably operable in an environmental temperature range of, for example, -40°C or more and 110°C or less.

[0554] 2, 1, etc., in the OS memory, the area occupied by the transistors can be made smaller than that of the planar type, and further, by using the configuration of the DOSRAM shown in Figures 14, 15, etc., the memory cells can be arranged at a high density by providing the transistors over the capacitors. In addition, the use of OS transistors makes it possible to realize high operating speed and long-term data retention.

[0555] FIG. 24B shows an example in which an SRAM is used as part of a cache, and an OS memory according to one embodiment of the present invention is used as the other part.

[0556] The lowest level cache can be called a Last Level cache (LLC). Although an LLC is not required to operate faster than higher level caches, it is desirable for the LLC to have a large storage capacity. The OS memory of one embodiment of the present invention has a high operating speed and is capable of retaining data for a long period of time, and therefore can be suitably used for an LLC. Note that the OS memory of one embodiment of the present invention can also be applied to a Final Level cache (FLC).

[0557] For example, as shown in Fig. 24(B), a configuration can be adopted in which an SRAM is used for a higher-level cache (such as an L1 cache or an L2 cache) and an OS memory according to one embodiment of the present invention is used for an LLC. Also, as shown in Fig. 24(B), not only an OS memory but also a DRAM can be applied to the main memory.

[0558] This embodiment mode can be combined with other embodiment modes as appropriate.

[0559] (Embodiment 5) In this embodiment, a display device according to one embodiment of the present invention will be described.

[0560] The semiconductor device of one embodiment of the present invention can be used for a display device or a module having the display device. Examples of the module having the display device include a module in which a connector such as a flexible printed circuit (hereinafter, referred to as FPC) or a TCP (Tape Carrier Package) is attached to the display device, and a module in which an integrated circuit (IC) is mounted by a chip on glass (COG) method, a chip on film (COF) method, or the like.

[0561] The display device of this embodiment may have a function as a touch panel. For example, various detection elements (also referred to as sensor elements) capable of detecting the proximity or contact of a detection target such as a finger can be applied to the display device.

[0562] Examples of sensor types include a capacitance type, a resistive film type, a surface acoustic wave type, an infrared type, an optical type, and a pressure sensitive type.

[0563] The capacitance type includes, for example, a surface capacitance type and a projected capacitance type. The projected capacitance type includes, for example, a self-capacitance type and a mutual capacitance type. The mutual capacitance type is preferable because it enables simultaneous multi-point detection.

[0564] Examples of touch panels include an out-cell type, an on-cell type, and an in-cell type. Note that an in-cell type touch panel refers to a configuration in which electrodes constituting a detection element are provided on one or both of a substrate supporting a display element and an opposing substrate.

[0565] [Display module] 25A shows a perspective view of the display module 170. The display module 170 includes a display device 600A and an FPC 298. Note that the display device included in the display module 170 is not limited to the display device 600A, and may be a display device 600B described later.

[0566] The display module 170 includes a substrate 291 and a substrate 299. The display module 170 includes a display unit 297. The display unit 297 is a region that displays an image in the display module 170, and is a region where light from each pixel provided in a pixel unit 294 described later can be viewed.

[0567] 25(B) shows a perspective view that typically illustrates the configuration on the substrate 291 side. A circuit portion 292, a pixel circuit portion 293 on the circuit portion 292, and a pixel portion 294 on the pixel circuit portion 293 are laminated on the substrate 291. A terminal portion 295 for connecting to an FPC 298 is provided in a portion of the substrate 291 that does not overlap with the pixel portion 294. The terminal portion 295 and the circuit portion 292 are electrically connected by a wiring portion 296 that is composed of a plurality of wirings.

[0568] The semiconductor device of one embodiment of the present invention can be used for one or both of the circuit portion 292 and the pixel circuit portion 293.

[0569] The pixel section 294 has a plurality of pixels 294a arranged periodically. An enlarged view of one pixel 294a is shown on the right side of Fig. 25(B). Fig. 25(B) shows an example in which one pixel 294a has a sub-pixel 130R that emits red light, a sub-pixel 130G that emits green light, and a sub-pixel 130B that emits blue light.

[0570] The subpixel has a display element. Various elements can be used as the display element, for example, a liquid crystal element and a light emitting element. In addition, a shutter type or optical interference type MEMS (Micro Electro Mechanical Systems) element, a display element using a microcapsule type, an electrophoresis type, an electrowetting type, or an electronic liquid powder (registered trademark) type can also be used. In addition, a QLED (Quantum-dot LED) using a light source and a color conversion technology using a quantum dot material may be used.

[0571] Examples of the light-emitting element include self-luminous light-emitting elements such as LEDs (Light Emitting Diodes), OLEDs (Organic LEDs), semiconductor lasers, etc. Examples of the LED that can be used include mini LEDs and micro LEDs.

[0572] The pixel arrangement in the display device of this embodiment is not particularly limited, and various methods can be applied. Examples of the pixel arrangement include a stripe arrangement, an S-stripe arrangement, a matrix arrangement, a delta arrangement, a Bayer arrangement, and a Pentile arrangement. Figure 25(B) shows an example in which a stripe arrangement is applied to the pixel arrangement.

[0573] The pixel circuit section 293 has a plurality of pixel circuits 293a that are periodically arranged.

[0574] One pixel circuit 293a is a circuit that controls the driving of multiple elements included in one pixel 294a. One pixel circuit 293a can be configured to have three circuits that control the emission of one light-emitting element. For example, the pixel circuit 293a can be configured to have at least one selection transistor, one current control transistor (drive transistor), and a capacitance for each light-emitting element. At this time, a gate signal is input to the gate of the selection transistor, and a source signal is input to the source. This realizes an active matrix display device.

[0575] The circuit portion 292 includes a circuit for driving each pixel circuit 293a of the pixel circuit portion 293. For example, it is preferable that the circuit portion 292 includes one or both of a gate line driver circuit and a source line driver circuit. In addition, the circuit portion 292 may include at least one of an arithmetic circuit, a memory circuit, a power supply circuit, and the like.

[0576] The FPC 298 functions as wiring for supplying a video signal, a power supply potential, or the like from the outside to the circuit portion 292. In addition, an IC may be mounted on the FPC 298.

[0577] The display module 170 can be configured such that one or both of the pixel circuit portion 293 and the circuit portion 292 are provided overlappingly below the pixel portion 294, and therefore the aperture ratio (effective display area ratio) of the display portion 297 can be made extremely high. In addition, the pixels 294a can be arranged at an extremely high density, and the resolution of the display portion 297 can be made extremely high.

[0578] Such a display module 170 is extremely high-definition and can be suitably used in VR devices such as HMDs or glasses-type AR devices. For example, even in a configuration in which the display unit of the display module 170 is viewed through a lens, the display module 170 has an extremely high-definition display unit 297, so that even if the display unit is enlarged with a lens, pixels are not visible, and a highly immersive display can be performed. In addition, the display module 170 is not limited to this, and can be suitably used in electronic devices having a relatively small display unit. For example, it can be suitably used in the display unit of a wearable electronic device such as a wristwatch.

[0579] [Display device configuration example 1] 26 shows a cross-sectional view of a display device 600A. The display device 600A is an example of a display device to which an MML (metal maskless) structure is applied. In other words, the display device 600A has light-emitting elements manufactured without using a fine metal mask.

[0580] The island-shaped light-emitting layer in the light-emitting element of the display device to which the MML structure is applied is formed by forming a film of the light-emitting layer on one surface and then processing it using a photolithography method. Therefore, it is possible to realize a high-definition display device or a display device with a high aperture ratio, which has been difficult to realize until now. Furthermore, since the light-emitting layer can be made separately for each color, it is possible to realize a display device that is extremely vivid, has high contrast, and has high display quality. For example, if a display device is composed of three types of light-emitting elements, namely, a light-emitting element that emits blue light, a light-emitting element that emits green light, and a light-emitting element that emits red light, the film formation of the light-emitting layer and the processing by photolithography can be repeated three times to form three types of island-shaped light-emitting layers.

[0581] Devices with the MML structure can be manufactured without using a metal mask, and therefore exceed the upper limit of definition resulting from the alignment accuracy of the metal mask. Furthermore, when devices are manufactured without using a metal mask, the equipment for manufacturing the metal mask and the process of cleaning the metal mask can be eliminated. Furthermore, since the same or similar equipment as that used to manufacture transistors can be used for photolithography processing, there is no need to introduce special equipment to manufacture devices with the MML structure. In this way, the MML structure makes it possible to keep manufacturing costs low, making it suitable for mass production of devices.

[0582] In a display device to which the MML structure is applied, there is no need to artificially increase the resolution by applying a special pixel arrangement such as a PenTile arrangement, so it is possible to realize a display device with high resolution (for example, 500 ppi or more, 1000 ppi or more, 2000 ppi or more, 3000 ppi or more, or 5000 ppi or more) by using a so-called stripe arrangement in which the R, G, and B sub-pixels are each arranged in one direction.

[0583] Furthermore, by providing a sacrificial layer on the light-emitting layer, damage to the light-emitting layer during the manufacturing process of the display device can be reduced, and the reliability of the light-emitting element can be improved. Note that the sacrificial layer may remain in the completed display device, or may be removed during the manufacturing process. For example, the sacrificial layer 618a shown in Figures 26 and 27 is a part of the sacrificial layer provided on the light-emitting layer.

[0584] Furthermore, by employing a film formation step using an area mask and a processing step using a resist mask, a light-emitting element can be manufactured through a relatively simple process.

[0585] 26 is a schematic cross-sectional view of a display device 600A (semiconductor device) of one embodiment of the present invention. The display device 600A has a configuration in which a pixel circuit, a driver circuit, and the like are provided over a substrate 410. Note that in the display device 600A in FIG. 26, a wiring layer 670 is also illustrated in addition to an element layer 620, an element layer 630, and an element layer 660. The wiring layer 670 is a layer in which wirings are provided.

[0586] A pixel circuit of a display device is preferably provided in the element layer 630. A driver circuit of the display device (either or both of a gate driver and a source driver) is preferably provided in the element layer 620. The element layer 620 may be provided with one or more types of circuits such as an arithmetic circuit and a memory circuit.

[0587] The element layer 620 includes, for example, a substrate 410 on which a transistor 400d is formed. A wiring layer 670 is provided above the transistor 400d, and the wiring layer 670 includes a wiring that electrically connects the transistor 400d to a conductive layer or a transistor (conductive layer 514 in FIG. 26) provided in the element layer 630. An element layer 630 and an element layer 660 are provided above the wiring layer 670, and the element layer 630 includes, for example, a transistor MTCK. The element layer 660 includes a light-emitting element 650 (light-emitting element 650R, light-emitting element 650G, and light-emitting element 650B in FIG. 26).

[0588] The transistor 400d is an example of a transistor included in the element layer 620. The transistor MTCK is an example of a transistor included in the element layer 630. The light-emitting elements (light-emitting element 650R, light-emitting element 650G, and light-emitting element 650B) are an example of a light-emitting element included in the element layer 660.

[0589] The transistor MTCK can be, for example, an OS transistor. FIG 26 illustrates an example in which the transistor 200 described in the above embodiment is used as the transistor MTCK.

[0590] The substrate 410 may be, for example, a semiconductor substrate (for example, a single crystal substrate made of silicon or germanium). In addition, the substrate 410 may be, for example, a silicon on insulator (SOI) substrate, a glass substrate, a quartz substrate, a plastic substrate, a sapphire glass substrate, a metal substrate, a stainless steel substrate, a substrate having stainless steel foil, a tungsten substrate, a substrate having tungsten foil, a flexible substrate, a laminated film, a paper containing a fibrous material, or a base film, in addition to a semiconductor substrate. In this embodiment, the substrate 410 is described as a semiconductor substrate having silicon as a material. Therefore, the transistor included in the element layer 620 may be a Si transistor.

[0591] The transistor 400d includes an element isolation layer 412, a conductive layer 416, an insulating layer 415, an insulating layer 417, a semiconductor region 413 formed of a part of a substrate 410, and a low-resistance region 414a and a low-resistance region 414b functioning as a source region and a drain region. For this reason, the transistor 400d is a Si transistor. Note that although one of the source and the drain of the transistor 400d is electrically connected to the conductive layer 514 provided in the element layer 630 through the conductive layer 428, the conductive layer 430, and the conductive layer 456 in FIG. 26, the electrical connection structure of the display device of one embodiment of the present invention is not limited thereto.

[0592] The transistor 400d can be a fin type by, for example, covering the top surface and the side surface in the channel width direction of the semiconductor region 413 with the conductive layer 416 interposed therebetween, the insulating layer 415 functioning as a gate insulating layer. By making the transistor 400d a fin type, the effective channel width can be increased, and the on characteristics of the transistor 400d can be improved. In addition, the contribution of the electric field of the gate electrode can be increased, and the off characteristics of the transistor 400d can be improved. The transistor 400d may be a planar type instead of a fin type.

[0593] Note that the transistor 400d may be either a p-channel type or an n-channel type. Alternatively, a plurality of transistors 400d may be provided, and both p-channel type and n-channel type transistors may be used.

[0594] The region in which the channel of the semiconductor region 413 is formed, the region in the vicinity thereof, and the low resistance region 414a and the low resistance region 414b which become the source region or drain region preferably contain a silicon-based semiconductor, specifically, preferably contain single crystal silicon. Alternatively, each of the above-mentioned regions may be formed using, for example, germanium, silicon germanium, gallium arsenide, aluminum gallium arsenide, or gallium nitride. A configuration using silicon in which the effective mass is controlled by applying stress to the crystal lattice and changing the lattice spacing may be used. Alternatively, the transistor 400d may be, for example, a HEMT (High Electron Mobility Transistor) using gallium arsenide and aluminum gallium arsenide.

[0595] The conductive layer 416 functioning as a gate electrode can be made of a semiconductor material such as silicon containing an element that imparts n-type conductivity, such as arsenic or phosphorus, or an element that imparts p-type conductivity, such as boron or aluminum, or can be made of a conductive material such as a metal material, an alloy material, or a metal oxide material.

[0596] Since the work function is determined by the material of the conductive layer, the threshold voltage of the transistor can be adjusted by selecting the material of the conductive layer. Specifically, it is preferable to use one or both of titanium nitride and tantalum nitride for the conductive layer. Furthermore, in order to achieve both conductivity and embeddability, it is preferable to use one or both of tungsten and aluminum as a stacked metal material for the conductive layer, and in particular, tungsten is preferable in terms of heat resistance.

[0597] The element isolation layer 412 is provided to isolate a plurality of transistors formed on the substrate 410. The element isolation layer can be formed by using, for example, a local oxidation of silicon (LOCOS) method, a shallow trench isolation (STI) method, or a mesa isolation method.

[0598] 26, an insulating layer 420 and an insulating layer 422 are stacked in this order from the substrate 410 side over a transistor 400d.

[0599] The insulating layer 420 and the insulating layer 422 can be formed using, for example, one or more selected from silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, aluminum oxide, aluminum oxynitride, aluminum nitride oxide, and aluminum nitride.

[0600] The insulating layer 422 may function as a planarizing film that planarizes steps generated by the insulating layer 420 and the transistor 400d covered by the insulating layer 422. For example, the top surface of the insulating layer 422 may be planarized by planarization treatment using a CMP method or the like in order to improve the planarity.

[0601] A conductive layer 428 that connects to a transistor MTCK and the like provided above the insulating layer 422 is buried in the insulating layer 420 and the insulating layer 422. Note that the conductive layer 428 functions as a plug or a wiring.

[0602] In the display device 600A, a wiring layer 670 is provided over the transistor 400d. The wiring layer 670 includes, for example, an insulating layer 424, an insulating layer 426, a conductive layer 430, an insulating layer 450, an insulating layer 452, an insulating layer 454, and a conductive layer 456.

[0603] An insulating layer 424 and an insulating layer 426 are stacked in this order over the insulating layer 422 and the conductive layer 428. An opening is formed in the insulating l...

Claims

1. a transistor on a first insulating layer and a second insulating layer; the transistor includes a first conductive layer on the first insulating layer, a second conductive layer, a semiconductor layer, a gate insulating layer, and a gate electrode; the second insulating layer is located between the first conductive layer and the second conductive layer; the second conductive layer is located on the second insulating layer; the second insulating layer and the second conductive layer have an opening reaching the first conductive layer; the semiconductor layer is in contact with a side surface of the second insulating layer in the opening and a side surface of the second conductive layer in the opening; the gate insulating layer is located on the semiconductor layer; the gate electrode has a region in the opening that overlaps with the semiconductor layer with the gate insulating layer interposed therebetween, the semiconductor layer includes a first oxide layer and a second oxide layer; the first oxide layer has a first region and a second region; each of the first region and the second region has a plurality of crystal parts; the second oxide layer is located between the first region and the second region. Semiconductor device.

2. 2. The semiconductor device according to claim 1, wherein the plurality of crystal portions have a c-axis orientation.

3. In claim 1 or 2, The second oxide layer has a plurality of crystal portions having the same crystal structure as the crystal portions.

4. In claim 1 or 2, The second oxide layer has a crystal portion connected to one of the plurality of crystal portions.

5. In claim 1 or 2, A semiconductor device, wherein a boundary between the first oxide layer and the second oxide layer is not observed in a cross-sectional TEM image.

6. In claim 1 or 2, the first conductive layer has a recess overlapping the opening, The semiconductor device includes a semiconductor layer having a region formed to fill the recess.

7. In claim 1 or 2, the opening has an eighth region having a tapered sidewall and a ninth region having a steeper sidewall than the eighth region; the eighth region includes an upper end of the opening, the ninth region is located below the eighth region, the eighth region includes a side surface of the second conductive layer; The ninth region includes a side surface of the second insulating layer.

8. In claim 7, an angle between a sidewall of the eighth region and a top surface of the first insulating layer is equal to or greater than 20 degrees and equal to or less than 75 degrees; A semiconductor device, wherein an angle between a sidewall of the ninth region and an upper surface of the first insulating layer is greater than 75 degrees and is equal to or smaller than 90 degrees.

9. forming a first insulating layer on the first conductive layer; forming a second conductive layer on the first insulating layer; forming a first opening reaching the first conductive layer by removing a portion of the second conductive layer and a portion of the first insulating layer to expose an upper surface of the first conductive layer; forming a semiconductor layer so as to be in contact with an upper surface of the first conductive layer, a side surface of the first insulating layer within the first opening, a side surface of the second conductive layer within the first opening, and an upper surface of the second conductive layer; the semiconductor layer is formed by a first step of forming a first oxide layer, a second step of forming a second oxide layer, and a third step of performing a heat treatment; The first oxide layer is formed by using a sputtering method; the second oxide layer is formed using atomic layer deposition; forming a second insulating layer in contact with an upper surface of the semiconductor layer and an upper surface of the first insulating layer; forming a third conductive layer on the second insulating layer; A method for manufacturing a semiconductor device.

10. a first insulating layer, a capacitance element, and a transistor on the capacitance element; the transistor includes a first conductive layer, a second conductive layer, a semiconductor layer, a gate insulating layer, and a gate electrode; the capacitive element includes a third conductive layer, a second insulating layer on the third conductive layer, and the first conductive layer on the second insulating layer; the first insulating layer is located between the first conductive layer and the second conductive layer; the second conductive layer is located on the first insulating layer; the first insulating layer and the second conductive layer have an opening reaching the first conductive layer; the semiconductor layer is in contact with a side surface of the first insulating layer in the opening and a side surface of the second conductive layer in the opening; the gate insulating layer is located on the semiconductor layer; the gate electrode has a region in the opening that overlaps with the semiconductor layer with the gate insulating layer interposed therebetween, the semiconductor layer comprises a metal oxide; In the transistor, the Id-Vgs characteristics are measured with a drain-source voltage of 0.05 V or more and 1 V or less, where Id is the drain current and Vgs is the gate-source voltage, In the Id-Vgs characteristic, Id is 1×10 -12 [A], Vgs is greater than 0 V and less than 0.5 V; storage device.

11. In claim 10, the metal oxide is In-M-Zn oxide, The element M is at least one selected from aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony; storage device.

12. In claim 10, The retention time of the storage device is 0.64 seconds or more. storage device.

13. In claim 10, When the gate of the transistor is set to 0 V, the source is set to 0 V, and a voltage of 0.05 V to 1 V is applied to the drain, the integrated amount of charge flowing through the transistor for 0.64 seconds is 3×10 -15 [F] × 0.1 [V] or less, storage device.

14. In claim 10, The write time of the memory device is 15 ns or less. storage device.

15. In claim 10, The read time of the memory device is 15 ns or less. storage device.

16. In claim 14, The write time is calculated using a circuit in which a first load is connected to the gate of the transistor and a second load is connected to the drain of the transistor; the first load has 256 first circuits; Each of the first circuits includes a first resistor and a second capacitive element; the second load includes 32 second circuits; Each of the second circuits includes a second resistor and a third capacitive element, the first resistors of the first circuit are connected in series; the second resistors of the second circuit are connected in series; The resistance value of the first resistor is equal to or greater than 1 Ω and equal to or less than 100 Ω, The resistance value of the second resistor is 1 Ω or more and 100 Ω or less, The capacitance value of the second capacitive element is equal to or greater than 1 aF and equal to or less than 0.5 fF, The capacitance value of the third capacitive element is equal to or greater than 1 aF and equal to or less than 0.5 fF. storage device.

17. In claim 15, The read time is calculated using a circuit in which a first load is connected to the gate of the transistor and a second load is connected to the drain of the transistor; the first load has 256 first circuits; Each of the first circuits includes a first resistor and a second capacitive element; the second load includes 32 second circuits; Each of the second circuits includes a second resistor and a third capacitive element, the first resistors of the first circuit are connected in series; the second resistors of the second circuit are connected in series; The resistance value of the first resistor is equal to or greater than 1 Ω and equal to or less than 100 Ω, The resistance value of the second resistor is 1 Ω or more and 100 Ω or less, The capacitance value of the second capacitive element is equal to or greater than 1 aF and equal to or less than 0.5 fF, The capacitance value of the third capacitive element is equal to or greater than 1 aF and equal to or less than 0.5 fF. storage device.

Citation Information

Patent Citations

  • Semiconductor device

    JP2011151383A

  • Semiconductor integrated circuit

    JP2012257187A

  • Semiconductor device

    JP2013211537A

  • Semiconductor device and method for manufacturing semiconductor device

    WO2021053473A1

Cited By

  • Oxide semiconductor film, transistor, and method for manufacturing oxide semiconductor film