Negative electrode for power storage device

A silicon-titanium composite electrode addresses capacity degradation in lithium-ion batteries by enhancing conductivity and stability, improving battery performance through the use of particulate composites with controlled atomic ratios and sizes.

JP2024169576AActive Publication Date: 2024-12-05SEMICON ENERGY LAB CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024161233
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2016-05-12
Filing Date
2024-09-18
Publication Date
2024-12-05
Estimated Expiration
2036-12-05

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries face issues with capacity degradation due to the expansion and contraction of silicon-based negative electrode materials during charge and discharge cycles, leading to poor conductivity, peeling, and reduced cycle life.

Method used

A negative electrode composed of particulate composites containing silicon as the active material and titanium as the functional material, with a specific atomic ratio and particle size, is used to enhance conductivity and stability, mitigating the effects of volume changes.

Benefits of technology

The composite structure improves the capacity, charge/discharge efficiency, and cycle characteristics of the battery by maintaining electrical conductivity and preventing material degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169576000001_ABST
    Figure 2024169576000001_ABST
Patent Text Reader

Abstract

To provide a power storage device with high capacity, a power storage device with an excellent cycle characteristic, a power storage device with high charge-discharge efficiency, or a power storage device including a negative electrode with low resistance.SOLUTION: A negative electrode for a power storage device includes a number of composite bodies with a particulate shape. The composite body includes a negative electrode active material, a first functional material, and a compound. The compound includes a constituent element of a negative electrode active material, and a constituent element of the first functional material. The negative electrode active material includes a region in contact with at least one of the first functional material and the compound.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an article, a method, or a manufacturing method. , manufacture, or composition of matter. One embodiment of the present invention is a semiconductor device, a display device, a light-emitting device, a power storage device, and a driving method thereof. In particular, one embodiment of the present invention relates to an electrode for a power storage device and a manufacturing method thereof. It relates to a manufacturing method. [Background technology]

[0002] In recent years, the number of portable devices such as mobile phones, smartphones, electronic books (e-books), and portable game consoles has increased. Electronic devices are becoming more and more common. As a result, the lithium-ion secondary battery that drives these devices is becoming more and more popular. In addition, research and development of energy storage devices such as solar power plants is being actively carried out. With the growing interest in the issue of hybrid and electric vehicles, Electricity storage devices are becoming increasingly important in applications.

[0003] Lithium-ion secondary batteries are widely used among energy storage devices due to their high energy density. The battery is made of lithium cobalt oxide (LiCoO2) or lithium iron phosphate (LiFePO4). The positive electrode contains the active material and the negative electrode is made of carbon materials such as graphite that can absorb and release lithium. In organic solvents such as ethylene carbonate and diethyl carbonate, LiBF4 and Li It is composed of an electrolyte solution in which an electrolyte made of lithium salt such as PF6 is dissolved. The charging and discharging of lithium-ion secondary batteries is carried out by the lithium ions in the lithium-ion secondary battery passing through the electrolyte. Lithium ions move between the positive and negative electrodes, and are inserted and removed from the positive and negative active materials. This is done by:

[0004] On the other hand, lithium-ion secondary batteries are widely used as power sources for portable electronic devices and electric vehicles. Therefore, there is a strong demand for smaller, larger capacity lithium-ion secondary batteries.

[0005] Therefore, instead of carbon materials such as graphite that were used in the conventional negative electrode active material, There is active development of forming electrodes using alloy materials such as silicon and tin. The negative electrode used in the secondary battery is formed by forming an active material on at least one surface of a current collector. Conventionally, the negative electrode active material has been produced by using carrier ions (hereinafter, carrier ions Graphite, which is a material capable of absorbing and releasing hydrogen, has been used as the negative electrode active material. Graphite, carbon black as a conductive agent, and resin as a binder are mixed together to make a slurry. The negative electrode was manufactured by forming a conductive layer, applying it onto a current collector, and drying it.

[0006] In response to this, the negative electrode active material is silicon, a material that undergoes alloying and dealloying reactions with lithium. When used, it is possible to increase the capacity compared to carbon. Theoretical capacity of carbon (graphite) anode The theoretical capacity of the silicon anode is 4200mAh / g, which is significantly higher than the 372mAh / g. For this reason, it is an optimal material for increasing the capacity of lithium-ion secondary batteries.

[0007] However, in materials that form alloys with lithium, such as silicon, as the amount of carrier ions absorbed increases, The expansion and contraction caused by the absorption and release of carrier ions during the charge and discharge cycles is large, so the active Contact between the active material and the conductive additive, between the active material itself, or between the active material and the current collector becomes poor, resulting in poor conductivity. The electrical path may be damaged. This can cause problems during the charge and discharge cycle. In addition, the capacity decreases. In some cases, the silicon may deform or collapse, causing the current collector to By peeling off or pulverizing the battery, it will maintain its functionality as a lithium-ion secondary battery. It becomes difficult.

[0008] In Patent Document 1, a silicon layer is formed on a current collector, and a conductive layer is formed on the silicon layer. This allows the silicon to expand and contract repeatedly, causing the silicon layer to separate from the current collector. Even if the battery is peeled off, current can be collected through the conductive layer, so deterioration of the battery characteristics is reduced. In addition, impurities such as phosphorus and boron are added to the silicon layer to form a conductive layer. The use of a layer having a thickness of 100 nm or less is also disclosed. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2012-009429 A Summary of the Invention [Problem to be solved by the invention]

[0010] An object of one embodiment of the present invention is to provide a power storage device with high capacity. An object of one embodiment of the present invention is to provide a power storage device with excellent cycle characteristics. An object of one embodiment of the present invention is to provide a power storage device with high charge and discharge efficiency. An object of one embodiment of the present invention is to provide a novel power storage device or the like.

[0011] The description of these problems does not preclude the existence of other problems. It is not necessary for the embodiment to solve all of these problems. The above will become apparent from the description in the specification, drawings, claims, etc. It is possible to extract other issues from the descriptions in the patent, claims, etc. [Means for solving the problem]

[0012] One aspect of the present invention is a composite material having a large number of particles, the composite material comprising a negative electrode active material and a first functional material. a negative electrode active material having a region in contact with a first functional material, be.

[0013] The composite material includes a plurality of particulate composites, the composites including a negative electrode active material, a first functional material, and a compound. and a compound including a constituent element of the negative electrode active material and a constituent element of the functional material, The active material is a negative electrode for a power storage device having a region in contact with at least one of a functional material and a compound. The poles are also an aspect of the present invention.

[0014] The composite has a plurality of particles, the composite having the negative electrode active material and a first functional material. and a composite having the negative electrode active material, the first functional material, and the compound. A negative electrode for a power storage device is also one embodiment of the present invention.

[0015] In addition, the first functional material has a higher Young's modulus than the negative electrode active material. This is one aspect of the invention.

[0016] The above-described negative electrode for a power storage device in which the negative electrode active material contains silicon is also one embodiment of the present invention.

[0017] The above-described negative electrode for a power storage device in which the first functional material contains titanium is also one embodiment of the present invention.

[0018] In addition, the atomic ratio of silicon to titanium is 2 to 8 times the aforementioned material for use in an electric storage device. The negative electrode is also an aspect of the present invention.

[0019] The present invention also provides the above-mentioned negative electrode for a power storage device, in which the particle size of the composite is 0.1 μm or more and 20 μm or less. This is one aspect of the invention.

[0020] The present invention also provides the above-mentioned negative electrode for a power storage device, in which the surface of the composite is coated with a second functional material. This is one aspect of clarity.

[0021] In one aspect of the present invention, the film thickness of the second functional material is 10 nm or more and 200 nm or less. , the negative electrode for the power storage device.

[0022] In one aspect of the present invention, the second functional material contains a common constituent element with the first functional material. This is the aforementioned negative electrode for the power storage device.

[0023] A power storage device including the above-described negative electrode for a power storage device is also one embodiment of the present invention.

[0024] Further, an electric device equipped with the above-described power storage device is also one embodiment of the present invention. Effect of the Invention

[0025] According to one embodiment of the present invention, a power storage device with high capacity can be provided. According to one embodiment, a power storage device with excellent cycle characteristics can be provided. According to one embodiment of the present invention, a power storage device with high charge and discharge efficiency can be provided. In this manner, it is possible to provide an electricity storage device using a negative electrode with low resistance. According to one embodiment, a novel power storage device or the like can be provided.

[0026] The description of these effects does not preclude the existence of other effects. An embodiment does not necessarily have to have all of these effects. Effects other than these may also be included. The above is self-evident from the description, drawings, claims, etc. Other effects can be extracted from the claims and other descriptions. [Brief description of the drawings]

[0027] [Figure 1] FIG. [Diagram 2] 4A to 4C are diagrams illustrating composite particles contained in a negative electrode active material layer. [Diagram 3] 4A to 4C are diagrams illustrating composite particles contained in a negative electrode active material layer. [Figure 4] 4A to 4C are diagrams illustrating composite particles contained in a negative electrode active material layer. [Diagram 5] FIG. [Figure 6] FIG. 1 is a diagram illustrating a coin-type storage battery. [Figure 7] FIG. 1 is a diagram illustrating a cylindrical storage battery. [Figure 8] FIG. 1 is a diagram illustrating a thin storage battery. [Figure 9] 1A and 1B are diagrams illustrating a thin, flexible storage battery. [Figure 10] FIG. 1 is a diagram illustrating a thin storage battery. [Figure 11] FIG. 1 is a diagram illustrating a thin storage battery. [Figure 12] 1A and 1B are diagrams illustrating examples of power storage devices. [Figure 13] 1A and 1B are diagrams illustrating examples of power storage devices. [Figure 14] 1A and 1B are diagrams illustrating examples of power storage devices. [Figure 15] 1A and 1B are diagrams illustrating examples of power storage devices. [Figure 16] 1A and 1B are diagrams illustrating examples of power storage devices. [Figure 17] 1A and 1B are diagrams illustrating examples of power storage devices. [Figure 18] 1A to 1C are diagrams illustrating application modes of a power storage device. [Figure 19] 4 is a cross-sectional STEM image of electrode A in Example 1. [Figure 20] 4 is a STEM-EDX analysis result of the electrode A in Example 1. [Figure 21] 4 is a cross-sectional STEM image of electrode B in Example 1. [Figure 22] 3 shows a connection configuration of half cells according to the first embodiment. [Figure 23] 3 shows a connection configuration of half cells according to the first embodiment. [Figure 24] 3 shows a connection configuration of half cells according to the first embodiment. [Diagram 25] 3 shows a connection configuration of half cells according to the first embodiment. [Figure 26] 4 is a graph showing the change in capacity retention rate of each half-cell over time according to Example 1. [Figure 27] 6 shows the initial charge / discharge characteristics of each sample according to Example 2. [Figure 28] 1 is a graph showing the change in capacity retention rate of each sample over time according to Example 2. [Figure 29] 11 is a graph showing the change in capacity retention rate of each sample over time according to Example 3. [Diagram 30] 11A to 11C are cross-sectional images of the samples after charging and discharging in accordance with Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Hereinafter, the embodiments will be described with reference to the drawings. It is possible to carry out the present invention in various forms without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that various modifications may be made to the details of the present invention. However, the present invention should not be construed as being limited to the description of the following embodiments.

[0029] (Embodiment 1) In this embodiment, a negative electrode for use in a power storage device according to one embodiment of the present invention will be described. A method for producing the negative electrode will be described.

[0030] [Negative electrode structure 1] FIG. 1(A) is a bird's-eye view of the negative electrode, and FIG. 1(B) is an enlarged view of the cross section enclosed by the dashed line in FIG. 1(A). The negative electrode 100 is provided with a negative electrode active material layer 102 in contact with a negative electrode current collector 101. In the figure, negative electrode active material layers 102 are provided on both sides of a negative electrode current collector 101. However, the negative electrode active material layer 102 may be provided on only one surface of the negative electrode current collector 101 .

[0031] The negative electrode active material layer 102 includes a large number of particulate composites. The negative electrode for an electrochemical device includes a composite. The composite includes a negative electrode active material and a functional material. The specific structure of the body will be described later.

[0032] The active material refers to a material involved in the insertion and removal of ions, which are carriers. When preparing the negative electrode, the active material is mixed with other materials such as conductive additives, binders, and solvents. The mixture of the above materials is formed on the current collector as an active material layer. are distinguished.

[0033] The negative electrode current collector 101 is made of a metal such as gold, platinum, zinc, iron, copper, titanium, tantalum, or manganese. and their alloys (such as stainless steel), which have high electrical conductivity and can carry lithium ions, etc. Materials that do not alloy with ions can be used. Also, materials that react with silicon to form silicide can be used. The metal may be a metal element that reacts with silicon to form a silicide. The elements are zirconium, titanium, hafnium, vanadium, niobium, tantalum, and chromium. The negative electrode current collector 101 is made of, for example, chromium, molybdenum, tungsten, cobalt, or nickel. Foil, plate (sheet), net, cylinder, coil, punched metal, expanded The negative electrode current collector 101 may be in the form of a metal or the like. The thickness is preferably 8 μm to 15 μm. In addition, the negative electrode current collector 101 may have a thickness of 5 μm or more over the entire area, for example. The thickness is preferably 30 μm or less, and more preferably 8 μm to 15 μm. However, one aspect of the embodiment of the present invention is not limited to this. For example, the negative electrode current collector 101 At least in a part, the thickness is 5 μm or more and 30 μm or less, more preferably Alternatively, the negative electrode current collector 101 may have a region having a diameter of 8 μm or more and 15 μm or less. Preferably, the thickness is 5 μm or more and 30 μm or less in 50% or more of the negative electrode current collector 101. It is more desirable that the thickness of the region is 8 μm or more and 15 μm or less.

[0034] The negative electrode active material undergoes charge and discharge reactions through alloying and dealloying reactions with carrier ions. The carrier ion is a lithium ion. In this case, the metal may be, for example, Mg, Ca, Al, Si, Ge, Sn, Pb, As , Sb, Bi, Ag, Au, Zn, Cd, Hg, etc. can be used. has a large capacity compared to graphite, and Si (silicon) in particular has a theoretical capacity of 4200mAh / g. Therefore, it is preferable to use silicon as the negative electrode active material. Examples of compound materials using elements include SiO, Mg2Si, Mg2Ge, SnO, and S nO2, Mg2Sn, SnS2, V2Sn3, FeSn2, CoSn2, Ni3Sn2, Cu6Sn5, Ag3Sn, Ag3Sb, Ni2MnSb, CeSb3, LaSn3, L Examples include a3Co2Sn7, CoSb3, InSb, and SbSn.

[0035] In addition, titanium dioxide (TiO2) and lithium titanium oxide (Li4T i5O 12 ), niobium pentoxide (Nb2O5), tungsten oxide (WO2), molybdenum oxide The negative electrode active material can be an oxide such as lithium-ion (MoO2). Graphite intercalation compound (Li x C6) may also be used.

[0036] In addition, the negative electrode active material is a nitride of lithium and a transition metal, Li3N type structure L i 3-x M x N (M=Co, Ni, Cu) can be used. For example, Li 2.6 C o 0.4 N3 is preferable because it exhibits a large charge / discharge capacity (900 mAh / g).

[0037] When a nitride of lithium and a transition metal is used, the negative electrode active material contains lithium ions, so the positive electrode Combine with materials such as V2O5 and Cr3O8 that do not contain lithium ions as electrode active materials In addition, even when a material containing lithium ions is used as the positive electrode active material, By first removing the lithium ions from the positive electrode active material, As the lithium-transition metal nitride, a lithium-transition metal nitride can be used.

[0038] In a negative electrode for a power storage device according to one embodiment of the present invention, silicon is used as a negative electrode active material. Amorphous silicon, microcrystalline silicon, polycrystalline silicon, or a combination of these Generally, the higher the crystallinity, the higher the electrical conductivity of silicon. Highly crystalline silicon can be used as an electrode with high electrical conductivity in an energy storage device. When silicon is amorphous, more ions such as lithium ions are trapped in it than in crystalline silicon. Since the carrier ions can be absorbed, the discharge capacity can be increased.

[0039] In addition, by increasing the electrical conductivity of silicon through the addition of impurities, it is possible to prevent uneven battery reactions in the electrodes. The doping impurity can be reduced by, for example, impurities that give n-type conductivity. The impurities that give the p-type conductivity include phosphorus (P) and arsenic (As), and the impurities that give the p-type conductivity include boron (B). (B), aluminum (Al), gallium (Ga), etc. The resistivity of the silicon is preferably 10 -4 [Ω·cm] or more and 50 [Ω·cm] or less, more preferable Preferably 10 -3 [Ω·cm] or more and 20 [Ω·cm] or less.

[0040] The composite includes a functional material. The functional material is formed in contact with the negative electrode active material. The functional material is It is preferable that the adhesion to the substance is high. For example, at the interface between the functional material and the negative electrode active material, A chemical bond such as a metallic bond or a covalent bond may be formed between the constituent atoms of both. Even if a compound such as an alloy of the functional material and the negative electrode active material is formed near the interface between the two, good.

[0041] The functional material is formed in contact with the negative electrode active material, which prevents deformation and shrinkage caused by the expansion and contraction of the negative electrode active material. Therefore, it is preferable for a functional material to have a high Young's modulus. Specifically, it is preferable that the functional material has a higher Young's modulus than the negative electrode active material. The functional material is designed to absorb and release carrier ions so that the carrier ions can be absorbed and released even when the substrate is covered with the functional material. It is preferable that the material does not form an alloy with rear ions and has high permeability to carrier ions. Preferably, the functional material is highly conductive.

[0042] The Young's modulus of the negative electrode active material may change depending on the charge / discharge state of the power storage device. For example, when silicon is used as the negative electrode active material, the active material contains almost no lithium. The Young's modulus is higher in the charged state than in the charged state where lithium is contained in the active material. It is preferable that the Young's modulus be higher than that of the active material in the discharged state.

[0043] As the functional material, it is preferable to use a material containing titanium. Specifically, titanium, Titanium silicides such as Ti3Si, Ti5Si3, TiSi, and TiSi2, and titanium-containing TiO x ), titanium nitride (TiN x ), titanium-containing oxynitride (T iO x N y ), lithium titanate (L4Ti5O 12 (also written as LTO) Titanium has a high Young's modulus and is highly permeable to lithium ions, Materials containing tan can be suitably used as functional materials. Alternatively, tin, aluminum oxide, etc. may be used.

[0044] The negative electrode for a power storage device according to one embodiment of the present invention includes a functional material such as titanium or TiN. x or TiO x for There are.

[0045] In addition, the negative electrode active material layer 102 preferably contains a conductive assistant. The conductive auxiliary improves the electronic conductivity of the negative electrode active material layer 102. , acetylene black particles, Ketjen Black (registered trademark) particles, carbon nanofibers Various conductive additives can be used, such as carbon particles such as carbon bars, graphene, etc.

[0046] The negative electrode active material layer 102 may also contain a binder. By using the above, the binding property between the negative electrode active material and the conductive additive, etc., and the binding property between the negative electrode active material and the current collector can be improved. The typical binder is polyvinylidene fluoride (PVDF). ), polyimide, polytetrafluoroethylene, polyvinyl chloride, ethylene polypropene, Propylene diene polymer, butadiene rubber, styrene-butadiene rubber, butyl rubber, Crylonitrile-butadiene rubber, fluororubber, polyvinyl acetate, polymethyl methacrylate For example, cellulose acetate, polyethylene, polypropylene, nitrocellulose, etc. may be used. When silicon or the like, which undergoes significant volumetric changes during charging and discharging, is used as the negative electrode active material, the battery has excellent binding properties. By using polyimide, it is possible to improve the adhesion between the negative electrode active materials, between the negative electrode active materials and the conductive additive, and between the negative electrode active materials and the aggregates. This can improve the adhesion between the current collector and the graphene, and between the current collector and the current collector. This makes it possible to suppress the peeling and pulverization of the negative electrode active material, thereby achieving good charge-discharge cycle characteristics.

[0047] Next, a cross-sectional structure of a particulate composite that can be used for the negative electrode active material layer 102 will be described with reference to FIGS. 2 to 4 show an example of the structure of the complex. 1 is a cross-sectional view corresponding to a cut surface passing near the core.

[0048] <Example 1 of cross-sectional structure of composite particle> The composite 110 shown in FIG. 2(A) includes a negative electrode active material 115, a functional material 116, a compound 117, and Compounds 117 and 118 include negative electrode active material 115 and functional material 11 That is, compounds 117 and 118 are the same as the constituent elements of the negative electrode active material 115 and and the constituent elements of the functional material 116.

[0049] The functional material 116 has a function of relieving stress caused by the expansion and contraction of the composite 110. In addition, the compounds 117 and 118, which contain the elements constituting the functional material 116, also relax the stress. In the configuration shown in FIG. 2(A), the ability to relieve the stress is The order of increasing efficiency is material 116, compound 117, and compound 118.

[0050] Compound 117 and compound 118 are each a compound of the elements constituting the negative electrode active material 115. The weight ratio of the functional material 116 is different from that of the compound 117. In comparison, the compound 118 has a larger weight ratio of the elements constituting the negative electrode active material 115 .

[0051] The negative electrode active material 115 is in contact with at least one of the functional material 116, the compound 117, and the compound 118. With this structure, the cracks generated on the surface of the negative electrode active material 115 can be prevented. Therefore, the power storage device of one embodiment of the present invention can have excellent cycle characteristics. The surface of the negative electrode active material 115 may be a functional material 116, a compound 117, or the like. , 118, the surface of the negative electrode active material 115 is covered with one or more of the above. The functional material 116 has a function of transmitting carrier ions. In order to achieve this, the negative electrode active material 115 is one or more of the functional material 116, the compound 117, and the compound 118. In FIG. 2(A), the negative electrode can absorb and release carrier ions even when it is covered with An example is shown in which an active material 115 is covered with a functional material 116 and a compound 117 .

[0052] Negative electrode active material 115 and compounds 117 and 118, and functional material 116 and compounds 117 and 11 8 have common constituent atoms, so there are chemical bonds (e.g., metal The formation of the bond is facilitated by the use of compound 117 and / or compound 118. In this way, the adhesion between the negative electrode active material 115 and the functional material 116 can be improved.

[0053] The negative electrode active material 115 has a function of absorbing and releasing carrier ions. Compounds 117 and 118 also absorb and release carrier ions because they contain the elements that make up 115. In the configuration shown in FIG. 2(A), the ability to absorb and release carrier ions The negative electrode active material 115 has the highest electrochemical activity, followed by compound 118 and compound 117.

[0054] In addition, the greater the weight ratio of the functional material 116, the compounds 117, and the compounds 118 in the composite 110, the For example, the capacity of the power storage device including the negative electrode active material layer 102 is reduced. By making the weight ratio of the compounds 117 and 118 as small as possible, the battery storage device according to one embodiment of the present invention can be The weight ratio can provide a power storage device with high capacity and excellent cycle characteristics. The cycle time can be determined according to the cycle characteristics required for the battery.

[0055] In this embodiment, the negative electrode active material 115 and the functional material 116 are silicon and In this case, compounds 117 and 118 are titanium silicides. There is no limitation on the composition of the silicon silicide, but for example, Ti:Si=1:2, 1:3, 1:4, etc. Some examples include:

[0056] In addition, the vicinity of the boundaries of the negative electrode active material 115, the functional material 116, and the compounds 117 and 118 In the region, the elements constituting the negative electrode active material 115 and / or the functional material 116 are The weight ratio of the elements may change continuously. It may be difficult to clearly determine the boundaries of compounds 116, 117, and 118. do.

[0057] In addition, the complex 110 may not have the compound 117 or the compound 118. The composite 110 is a composite of an element constituting the negative electrode active material 115 and an element constituting the functional material 116. The negative electrode active material may contain one or more compounds having a different ratio of amounts from the compounds 117 and 118. A portion of the substance 115 or / and the functional material 116 is not covered by the compound 117, and The combined body 110 may be exposed on the surface.

[0058] The surface of the complex 110 may be covered with a thin film of the functional material 116A (FIG. 2(B) By adopting such a structure, the stress applied to the surface of the composite 110A is further reduced. This can further improve the cycle characteristics of the power storage device of one embodiment of the present invention. 116A may be a different material than functional material 116, but is preferably a similar material. It is preferable that the functional material 116A and the functional material 116 have a common constituent element, so that the functional material 116A and the functional material 116 have a common constituent element. When the body 110A has an area where the functional material 116 and the functional material 116A are in contact with each other, This can improve the adhesion between the material 116 and the functional material 116A.

[0059] <Example 2 of cross-sectional structure of composite particle> The composite 111 shown in FIG. 3(A) includes a negative electrode active material 115 and a functional material 116. The composite 111 includes one or more masses of negative electrode active material 115 and one or more functional materials 116. The negative electrode active material 115 has a region in contact with the functional material 116.

[0060] Since the composite 111 does not contain the compound 117, etc., the negative electrode active material 115 in the composite 111 is Therefore, the power storage device of one embodiment of the present invention can have a higher capacity. It can be something like that.

[0061] The functional material 116 is formed in contact with the negative electrode active material 115, and the negative electrode active material 115 expands. The negative electrode active material 115 and the functional material 116 can be used to relieve stress caused by the shrinkage of the negative electrode. At the interface with 116, it is preferable that a chemical bond is formed between the constituent atoms of both. stomach.

[0062] The greater the weight ratio of the functional material 116 in the composite 111, the greater the amount of the negative electrode active material layer 102. The weight ratio of the functional material 116 should be as small as possible because this reduces the capacity of the resulting power storage device. The weight ratio can be determined depending on the cycle characteristics required for the power storage device. do.

[0063] A thin film of functional material 116A may be provided on the surface of the composite 111 (FIG. 3(B) )). By adopting such a configuration, the stress applied to the surface of the composite 111A is relieved and accumulated. The cycle characteristics of the battery can be further improved. The functional material 11 may be a different material from that of the functional material 116, but is preferably a similar material. Since the functional material 116 and the functional material 6A have a common constituent element, the functional material 116 and the functional material The adhesion of 116A can be improved.

[0064] <Example 3 of cross-sectional structure of composite particle> The composite 112 shown in FIG. 4 includes a negative electrode active material 115 and a functional material 116B. 15 has a region in contact with the functional material 116B. Specifically, the surface of the negative electrode active material 115 is covered with functional material 116B.

[0065] The functional material 116B is formed in contact with the negative electrode active material 115, and the expansion of the negative electrode active material 115 is suppressed. The negative electrode active material 115 and the functional material 116 can relieve the stress caused by the tension and contraction. At the interface with the material 116B, it is preferable that a chemical bond is formed between the constituent atoms of both. I wish.

[0066] The cracks and peeling caused by the absorption and release of carrier ions in the negative electrode active material 115 are caused by the negative electrode active material 11 In most cases, cracks start from the surface of the 5. Therefore, it is important to cover only the area where the cracks start. By providing the functional material 116B in the composite 112, the power storage device of one embodiment of the present invention can be realized. , and can have even higher capacity.

[0067] The functional material 116B is the same as the functional material 116 or the functional material 116A. It is possible.

[0068] The above negative electrode can be used for the power storage device which is one embodiment of the present invention.

[0069] [Method of manufacturing negative electrode structure 1] In this embodiment, silicon is used as the negative electrode active material 115, and titanium is used as the functional material 116. A method for producing the above-mentioned negative electrode 100 will be described below.

[0070] First, granular silicon and granular titanium are prepared, weighed, and mechanically mixed. For example, the molar ratio of silicon should be between 2 and 8 times that of titanium. Specifically, the mechanical mixing is carried out by mixing each material weighed out in a metal container with a mixture of A number of metal balls are placed in the container and the container is rotated. The amount of balls is determined by, for example, the total weight of each material. The amount should be at least 10 times the amount of the mixture. Adjust the rotation speed of the container, the number of balls, the processing time of mechanical mixing, etc. By doing so, it is possible to obtain the composite 110 and / or the composite 111 having an appropriate particle size. That is, fine particles of a mixture or compound of an active material and a functional material having an appropriate particle size, or an active Mixtures of active materials and functional materials, and fine particles made of compounds of active materials and functional materials, etc. It can be generated.

[0071] In addition, on the surface of the complex 110 and / or complex 111 obtained as described above, barrels The functional material 116A is deposited by sputtering, whereby the composite 110A and / or the composite Alternatively, the surface of the granular silicon may be subjected to barrel sputtering. The functional material 116B is formed into a film by the above method, thereby obtaining the composite 112. Sputtering is a process in which a target is fixed in a container with a polygonal or circular cross section, and a film is formed on the target. This is a deposition method in which particulate samples are placed in a rotating container in a vacuum and sputtered. Barrel sputtering is used to deposit the target's constituent elements onto the surface of each particle. The thickness of the functional material 116A formed by barrel sputtering is It is preferable that the thickness is 10 nm or more and 200 nm or less.

[0072] Alternatively, a functional material is formed on the surface of the composite 110 and / or the composite 111 by a sol-gel method. 116A may be formed.

[0073] The complexes listed below are complexes 110, 111, 110A, 111A, and 112. It shall include at least one.

[0074] Here, the particle size of the complex will be described. If the complex particles are large compared to the conductive additive, It may be difficult to mix uniformly with the agent, and a good conductive path may not be formed. In addition, when the particle size is large, the surface area is small relative to the volume expansion, so stress occurs on the surface. On the other hand, the particle size of the composite may become large, and cracks may easily occur in the particles. If the surface area of ​​the composite increases, the decomposition reaction of the electrolyte increases, resulting in a decrease in the charge / discharge efficiency. The rate may decrease and the capacity may decrease. Therefore, the particle size of the composite has a certain optimum value. For example, the particle size of the complex is preferably 0.001 μm or more and 20 μm or less, more preferably 0. Use a thickness of 0.1 μm or more and 20 μm or less, and more preferably 0.5 μm or more and 5 μm or less. It is good.

[0075] The silicon to be prepared to obtain the composite having the above-mentioned particle size is, for example, a granular silicon wafer. It can be obtained by crushing silicon that is not of a large particle size. The silicon may be crushed to obtain silicon of a desired particle size. The grinding method includes grinding in a mortar or grinding in a ball mill. After crushing, the powder may be pulverized using a ball mill. A solvent is added to one or more weighed raw materials, and the mixture is then mixed with a metal or ceramic material. The mixture is rotated using balls made of a material called a ball mill. The raw materials can be finely divided at the same time as mixing the materials, and the electrode material after preparation can be In addition, the ball mill process allows the raw materials to be homogenized. The materials can be mixed together.

[0076] The conductive assistant, the particulate complex, and the binder are added to a solvent and mixed. The mixing ratio of these is The amount may be appropriately adjusted according to the desired battery characteristics.

[0077] The solvent may be a liquid in which the raw material does not dissolve but in which the raw material disperses. The solvent is preferably a polar solvent, for example, water, methanol, ethanol, acetone, tetrahydrofuran, etc. Tetrahydrofuran (THF), dimethylformamide (DMF), N-methyl-2-pyrrolidone One or more of NMP and DMSO A mixture of liquids may be used.

[0078] In addition, as the binder, a binder having high heat resistance, such as polyimide, is used. The material mixed in the mixing step is a polyimide precursor, and the precursor is heated in the subsequent heating step. The precursor is imidized to form a polyimide.

[0079] The above-mentioned compounds may be mixed, for example, using a kneader. The aggregate and the solvent are combined and stirred using a kneader to produce a slurry (mixture).

[0080] Next, the slurry is applied onto the negative electrode current collector 101, and the negative electrode current collector on which the slurry is applied is The solvent is removed by drying. The drying step is, for example, performed at room temperature in a dry atmosphere. It is possible to remove the solvent by a subsequent heating step. In this case, the drying step is not necessarily required.

[0081] Next, the negative electrode current collector coated with the slurry is heated. The temperature is set to 0° C. or lower, preferably about 300° C., and the temperature is maintained for 1 hour to 2 hours, preferably about The heating is continued for 1 hour. The slurry is baked by the heating, and the polyimide precursor is imidized. This results in polyimide.

[0082] In this embodiment, the heating step for firing the slurry is performed at a temperature at which the binder is not decomposed, e.g. The temperature is preferably 200° C. or higher and 400° C. or lower, and more preferably 300° C. Decomposition can be prevented, and a decrease in the reliability of the power storage device can be prevented.

[0083] By the above-mentioned manufacturing process, a negative electrode 1 having a negative electrode active material layer 102 on a negative electrode current collector 101 is obtained. 00 can be manufactured.

[0084] [Negative electrode structure 2] Next, a negative electrode current collector is placed on the negative electrode of the electricity storage device together with the particulate composite, A negative electrode active material layer including graphene and a binder will be described.

[0085] Graphene functions as a conductive additive that forms an electronic conduction path between the composite and the current collector. In this specification, graphene refers to a single-layer graphene or a graphene having 2 to 100 layers. This includes multi-layer graphene. Single-layer graphene is a single atomic layer of carbon with π bonds. Graphene is a sheet of molecules. When this graphene is formed by reducing graphene oxide, In this study, the oxygen in graphene oxide was not completely released, but some of it remained in the graphene. When oxygen is contained in graphene, the oxygen ratio can be measured by XPS (X-ray photoelectron spectroscopy). For example, the content is 2 atomic % or more and 20 atomic % or less of the total graphene, preferably The content is 3 atomic % or more and 15 atomic % or less. Note that graphene oxide is a material in which the graphene is oxidized. This refers to a compound that has been

[0086] As the binder, the materials described above as the binder can be used. In particular, the negative electrode active material that constitutes the composite uses silicon, which exhibits a significant volume change during charging and discharging. In this case, by using polyimide with excellent binding properties, the particle-shaped composites can be easily bonded to each other and to the particle-shaped composites. The adhesion between the particle and graphene, between the particle composite and the current collector, and between the graphene and the current collector was This can improve the charge / discharge characteristics by suppressing the exfoliation and pulverization of the composite. You can obtain the Ikuru trait.

[0087] In this way, when a negative electrode active material layer including a particulate composite, graphene, and a binder is used, The graphene sheets are in two-dimensional contact with the alloy material particles, so as to encase them. The graphenes are in two-dimensional contact with each other so that they overlap, and therefore the giant nanoparticles are formed in the negative electrode active material layer. A large three-dimensional network of electron conduction paths is constructed. The granular acetylene black (AB) and ketjen black ( When using a KB, electrical contacts are made at points, whereas the negative electrode active material has high electronic conductivity. A layer of solid can be formed.

[0088] In addition, graphene is bonded to each other to form a mesh-like graphene (hereafter referred to as graphene network). When the composite is covered with a graphene net, Fennet can also function as a binder to bind particles together. This allows the amount of binder to be reduced or even eliminated, making it possible to improve the electrode structure. The ratio of the composite to the volume and weight of the electrode can be improved. The capacity can be increased.

[0089] FIG. 5(A) is a bird's-eye view of the negative electrode, and FIG. 5(B) is an enlarged view of the cross section enclosed by the dashed line in FIG. 5(A). The negative electrode 200 has a structure in which a negative electrode active material layer 202 is provided on a negative electrode current collector 201. In the figure, the negative electrode active material layer 202 is provided on both sides of the negative electrode current collector 201. Alternatively, the negative electrode active material layer 202 may be provided on only one surface of the negative electrode current collector 201 .

[0090] For the negative electrode current collector 201, the current collector shown as the negative electrode current collector 101 can be used.

[0091] FIG. 5C shows a composite 203 and a sheet-like graphene 2 covering a plurality of the composites 203. FIG. 2 is a top view of a negative electrode active material layer 202 having a plurality of composite particles 204 and a binder (not shown). The surface of the composite 203 is covered with different graphenes 204. The complex 203 may be the complex 110 or / and the complex 110. The combined total is 111.

[0092] Graphene 204 is a thin film having a thickness of a single layer or multiple layers of carbon molecules. The granules 204 are arranged to surround or cover the composite 203 in the form of a plurality of particles. Since they are formed so as to be attached to the surface of the composite 203, they are in surface contact with each other. In addition, the graphenes 204 are in surface contact with each other, so that the graphenes 204 are This forms a three-dimensional electrical conduction network.

[0093] As will be described later, the formation of graphene 204 requires the use of an acid that is highly dispersible in a polar solvent. This is because the graphene oxide is used in the dispersion medium containing uniformly dispersed graphene oxide. The solvent is removed by volatilization, and the graphene oxide is reduced to graphene. The graphene 204 remaining on the substrate 2 is partially overlapped and dispersed to such an extent that it is in surface contact with each other. This creates a pathway for electrical conduction.

[0094] Therefore, unlike conventional granular conductive additives such as acetylene black, which come into point contact with the active material, Since Raphene 204 enables surface contact with low contact resistance, the amount of conductive additive is increased. The electrical conductivity between the granular composite 203 and the graphene 204 is improved without adding any other material. Therefore, the ratio of the composite 203 in the negative electrode active material layer 202 can be increased. This allows the capacity of the power storage device to be increased. The weight of the graphene 204 used is preferably, for example, 30% or less of the weight of the composite 203. , more preferably 15% or less, and further preferably 3% or less. After that, the weight of the graphene is almost halved.

[0095] As described above, in order to improve the characteristics of the electron conduction path in the negative electrode active material layer 202, The negative electrode active material layer 202 contains graphene, and in addition, acetylene black. black particles, ketjen black particles, carbon particles such as carbon nanofibers, etc. The conductive layer may contain various conductive assistants.

[0096] The complex 203 is at least one of the complexes 110, 111, 110A, and 111A described above. Includes one.

[0097] FIG. 5(D) is a cross-sectional view of a part of the negative electrode active material layer 202. The composite 203 is covered with graphene 204. The graphene 204 is The multiple complexes 203 are observed to be linear. The graphene 204 is sandwiched between the graphene 204. In some cases, the nanoparticles may contain multiple complexes 203. In addition, the nanoparticles may not be covered with graphene 204. A portion of the complex 203 may be exposed.

[0098] The graphene 204 forms a three-dimensional network. Therefore, it functions as a conductive additive. In addition, the graphene network is a complex that can absorb and release carrier ions. It has the function of holding the 203. Therefore, it can also serve as a binder. Therefore, the amount of the binder used can be reduced, and the number of composites per negative electrode active material layer 202 can be reduced. It is possible to increase the proportion of 03, thereby increasing the discharge capacity of the power storage device.

[0099] In addition, in the composite 203, the volume of which expands due to the occlusion of carrier ions, the negative electrode The active material layer 202 may become brittle, causing a portion of the negative electrode active material layer 202 to collapse. If a part of the negative electrode active material layer 202 collapses, the reliability of the power storage device decreases. Even if the volume of the composite 203 increases or decreases due to charging and discharging, the graphene 204 covers the composite. Therefore, the graphene 204 prevents the dispersion of the composite 203 and the collapse of the negative electrode active material layer 202. That is, the graphene 204 increases the volume of the composite 203 during charging and discharging. Even if the amount of the complex 203 increases or decreases, the complex 203 has a function of maintaining the bond between the complexes 203.

[0100] In addition, when applied to flexible display devices and electronic devices, the flexible parts (casing A storage device such as a secondary battery is provided in the whole or part of the Even in this case, repeated bending or other deformation of the storage device can cause the negative electrode current collector inside the storage device to deteriorate. There is a possibility that peeling may occur between the body 201 and the composite body 203, accelerating the deterioration of the electricity storage device. .

[0101] Here, the graphene is in surface contact with each other, forming a plurality of graphenes. Graphene forms a three-dimensional electrical conduction network. It also has the advantage that the network is not easily broken down even when subjected to deformation such as bending. Therefore, a good conductive path can be maintained even after repeated deformation. If the phenanthrene is bag-shaped and contains the complex 203, the complex 203 may be detached due to bending. The electrode layer is less likely to collapse.

[0102] The above negative electrode can be used for the power storage device which is one embodiment of the present invention.

[0103] [Method of manufacturing negative electrode structure 2] The negative electrode active material layer 202 in the negative electrode 200 according to one embodiment of the present invention is made of graphite as described above. Graphene includes, for example, graphene oxide, which is the raw material of graphene, and The aggregate 203 is kneaded with a binder and then thermally reduced to obtain the above-mentioned product. An example of a method for producing such a negative electrode will be described.

[0104] First, graphene oxide, the raw material for graphene, is prepared. Various synthesis methods, such as the Hummers method, the modified Hummers method, or oxidation of graphite It can be prepared using the method.

[0105] For example, the Hummers method involves oxidizing flake graphite to produce oxidized graphite. This is a method to form graphite. The graphite oxide formed is In fact, functional groups such as carbonyl groups, carboxyl groups, and hydroxyl groups are oxidized. The crystallinity of graphite is impaired and the distance between layers is increased. Therefore, the layers can be easily separated by ultrasonic treatment to obtain graphene oxide. The length of one side of the graphene oxide to be produced (also called the flake size) is several μm. It is preferable that the thickness is not less than several tens of μm.

[0106] Next, the graphene oxide obtained by the above method or the like is bound to a particulate composite 203. The mixing ratio of these is appropriately adjusted according to the desired battery characteristics. For example, the ratio of the particulate negative electrode active material, graphene oxide, and binder to be added may be , can be weighed out to give a ratio of 80:5:15 by weight.

[0107] The solvent may be a liquid in which the raw material does not dissolve but in which the raw material disperses. The solvent is preferably a polar solvent, for example, water, methanol, ethanol, acetone, tetrahydrofuran, etc. Tetrahydrofuran (THF), dimethylformamide (DMF), N-methyl-2-pyrrolidone One or more of NMP and DMSO A mixture of liquids may be used.

[0108] In addition, a binder having high heat resistance, such as polyimide, is used as the binder. The material mixed in the mixing step is a polyimide precursor, and the precursor is heated in the subsequent heating step. The precursor is imidized to form a polyimide.

[0109] In addition, in a solution having polarity, the functional groups of graphene oxide Because the graphene oxide is negatively charged, it is difficult for different graphene oxides to aggregate together. In a liquid having polarity, graphene oxide is likely to be uniformly dispersed. By adding the compound to the solvent and mixing it in the early stages of the mixing process, the compound is more uniformly distributed in the solvent. As a result, graphene is uniformly dispersed in the negative electrode active material, and electrical conductivity is improved. Thus, a highly conductive negative electrode active material can be produced.

[0110] The above-mentioned compounds may be mixed, for example, using a kneader. The binder, the active material, and the solvent are mixed together in a kneader. Stir using a stirrer to create a slurry (mixture).

[0111] Here, the order of adding the graphene oxide, the particulate composite 203, and the binder to the solvent is as follows: For example, the particulate composite 203 is added to a solvent and mixed. After mixing, graphene oxide is added and mixed, and then a binder is added and mixed. In each mixing step, a solvent may be added as appropriate to adjust the viscosity of the mixture. stomach.

[0112] An example of the mixing method will be described. First, a solvent is added to the composite 203, and the mixture is mixed in a kneader. For example, NMP may be used as the solvent. Next, graphene oxide is added and kneaded. Kneading is a process that involves kneading with high viscosity, and by kneading the mixture with high viscosity, the graphene oxide aggregates. This allows the aggregation of the composite 203 and graphene oxide to be dispersed more uniformly. The solvent may be added during the kneading process. For example, the amount of the electrolyte is preferably 0.46 ml or more and 0.80 ml or less per 1 g of the active material. Next, a binder is added and mixed in a kneader. A solvent is then added and the mixture is mixed in a kneader.

[0113] Through the above steps, the particulate composite 203, the graphene oxide, the binder, and the solvent are mixed. A slurry (mixture) is formed.

[0114] Next, the slurry is applied onto the negative electrode current collector 201, and the negative electrode current collector on which the slurry is applied is The solvent is removed by drying. The drying step is, for example, performed at room temperature in a dry atmosphere. It is possible to remove the solvent by a subsequent heating step. In this case, the drying step is not necessarily required.

[0115] Next, the negative electrode current collector coated with the slurry is heated. The temperature is set to 0° C. or lower, preferably about 300° C., and the temperature is maintained for 1 hour to 2 hours, preferably about The heating is continued for 1 hour. The slurry is baked by the heating, and the polyimide precursor is imidized. At the same time, the graphene oxide is reduced to form graphene. In this way, both the heating for slurry sintering and the heating for graphene oxide reduction can be achieved by a single heating process. Since the heating for the purpose of the heating can be performed simultaneously with the heating for the purpose of the heating, there is no need to perform the heating step twice. This makes it possible to reduce the number of steps required for manufacturing the negative electrode.

[0116] In this embodiment, the heating process for firing the slurry and reducing the graphene oxide is performed in a manner that the binder is The reaction is carried out at a temperature at which decomposition does not occur, for example, at a temperature of 200°C to 400°C, preferably at 300°C. This makes it possible to prevent the binder from being decomposed, and to prevent a decrease in the reliability of the electricity storage device. The weight of graphene oxide can be reduced by almost half through reduction treatment.

[0117] In addition, the reduced graphene oxide has low dispersibility due to the loss of functional groups, and the composite 20 3) Graphene oxide (i.e., graphene) that has been reduced before being mixed with a binder is used. If the mixture is mixed with the composite 203, the resulting electricity storage device will have poor electrical properties. This is because graphene oxide has oxygen-containing functional groups on its surface. The graphene oxide particles are negatively charged by bonding with each other, and are dispersed by repelling each other and the polar solvent. In contrast, reduced graphene loses many of these functional groups upon reduction. This is due to the reduced dispersibility of the particles.

[0118] Therefore, after mixing the graphene oxide with the composite 203, the mixture was heated to form In the negative electrode active material layer, graphene oxide was dispersed before the functional groups were reduced. Therefore, the reduced graphene is uniformly dispersed in the negative electrode active material layer. Therefore, by dispersing graphene oxide and then carrying out a reduction process, it is possible to create a highly electrically conductive battery. You can get a position.

[0119] By the above-mentioned manufacturing process, a negative electrode 202 having a negative electrode active material layer 202 on a negative electrode current collector 201 is obtained. 00 can be manufactured.

[0120] Note that various power storage devices can be formed using the above negative electrode. Examples of such batteries include batteries, secondary batteries, and lithium-ion secondary batteries. As another example of the device, the present invention can be applied to a capacitor. The material is used as the negative electrode, and this is combined with an electric double layer positive electrode to create a lithium-ion capacitor. It is also possible to configure a capacitor such as a capacitor.

[0121] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0122] (Embodiment 2) In this embodiment, a power storage device using a negative electrode manufactured by the manufacturing method shown in Embodiment 1 The structure of the storage battery will be described with reference to FIGS. 6 to 9. 10 to 14. An example of an electric device will be described with reference to FIG. This will be explained using:

[0123] [Coin-type battery] FIG. 6(A) is an external view of a coin-type (single-layer flat) storage battery, and FIG. 6(B) is a cross-sectional view of the battery. FIG.

[0124] The coin-type storage battery 300 is made up of a positive electrode can 301 that also serves as a positive electrode terminal and a negative electrode can 302 that also serves as a negative electrode terminal. 02 is insulated and sealed by a gasket 303 made of polypropylene or the like. Here, the negative electrode for a power storage device described in Embodiment 1 is used as the negative electrode 307.

[0125] The positive electrode 304 is composed of a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector 305. The positive electrode active material layer 306 is formed by the positive electrode active material, and also by improving the adhesion of the positive electrode active material. and a conductive assistant to increase the conductivity of the positive electrode active material layer. As the conductive additive, a material with a large specific surface area is preferable. Carbon black (AB) and the like can be used. Carbon nanotubes, graphene Carbon materials such as fluorene and fullerene can also be used.

[0126] The negative electrode 307 is composed of a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector. The negative electrode 307 is formed using the negative electrode for a power storage device described in Embodiment 1. .

[0127] Between the positive electrode active material layer 306 and the negative electrode active material layer 309, a separator 310 and an electrolyte (FIG. (not shown).

[0128] The separator 310 may be made of cellulose (paper), or perforated polypropylene, poly An insulator such as ethylene may be used.

[0129] The electrolyte solution uses a material having carrier ions as an electrolyte. Representative examples of electrolytes Examples include LiPF6, LiClO4, LiAsF6, LiBF4, LiCF3SO3, Lithium salts include Li(CF3SO2)2N and Li(C2F5SO2)2N. The electrolyte may be used alone or in any combination and ratio of two or more. Good too.

[0130] In addition, the carrier ions are alkali metal ions other than lithium ions, alkaline earth metal ions, etc. In the case of metal ions, an alkali metal ion is used instead of lithium in the above lithium salt as an electrolyte. Alkaline metals (e.g., sodium and potassium), alkaline earth metals (e.g., calcium, Strontium, barium, beryllium, magnesium, etc.) may also be used.

[0131] As the solvent for the electrolyte, a material that allows the movement of carrier ions is used. The solvent is preferably an aprotic organic solvent. Representative examples of the aprotic organic solvent include , Ethylene carbonate (EC), Propylene carbonate, Dimethyl carbonate, Di Ethyl carbonate (DEC), γ-butyrolactone, acetonitrile, dimethoxyethane tetrahydrofuran, etc., and one or more of these can be used. By using a polymer material that gels as a solvent for the electrolyte, safety against leakage, etc. is improved. In addition, it is possible to make the storage battery thinner and lighter. Examples include silicone gel, acrylic gel, acrylonitrile gel, and polyethylene glycol. Examples of gels include oxide-based gels, polypropylene oxide-based gels, and fluorine-based polymer gels.

[0132] In addition, a flame-retardant and non-volatile ionic liquid (room-temperature molten salt) was used as the solvent for the electrolyte. By using multiple batteries, the battery can withstand an internal short circuit or an increase in internal temperature due to overcharging. This can prevent the battery from exploding or catching fire. Ionic liquids are made up of cations and anions. The electrolyte solution contains organic cations and anions. fatty cations such as monium cations, tertiary sulfonium cations, and quaternary phosphonium cations aromatic onium cations, imidazolium cations and pyridinium cations In addition, examples of anions used in the electrolyte include monovalent amide anions, Monovalent methide anion, fluorosulfonate anion, perfluoroalkylsulfone Acid anion, tetrafluoroborate anion, perfluoroalkylborate anion , hexafluorophosphate anion, or perfluoroalkylphosphate anion On etc.

[0133] In particular, when an aliphatic quaternary ammonium cation is used, the reduction resistance is high, so that the This is particularly effective in suppressing the decomposition of the electrolyte during charging and discharging. This can suppress the charge-discharge current and provide good cycle characteristics. It can be improved.

[0134] In addition, instead of the electrolyte, solid electrolytes containing inorganic materials such as sulfides and oxides, and P A solid electrolyte containing a polymer material such as EO (polyethylene oxide) can be used. When a solid electrolyte is used, the installation of a separator or spacer becomes unnecessary. Since the entire pond can be solidified, there is no risk of leakage, and safety is improved dramatically.

[0135] The positive electrode can 301 and the negative electrode can 302 are made of nickel or aluminum, which are resistant to corrosion by the electrolyte. Metals such as titanium, or their alloys or alloys of these with other metals (e.g. stainless steel In order to prevent corrosion by the electrolyte, nickel or aluminum can be used. The positive electrode can 301 is preferably covered with a positive electrode 304, and the negative electrode can 302 is preferably covered with a negative electrode 305. 07 and electrically connect them to each other.

[0136] The negative electrode 307, the positive electrode 304 and the separator 310 are impregnated with an electrolyte, and as shown in FIG. As shown, the positive electrode can 301 is placed downward, and the positive electrode 304, the separator 310, the negative electrode 307, and the negative electrode The cans 302 are stacked in this order, and the positive electrode can 301 and the negative electrode can 302 are secured together with a gasket 303 interposed therebetween. The coin-shaped storage battery 300 is manufactured by crimping.

[0137] Here, the flow of current during charging of the power storage device will be described with reference to FIG. When the secondary battery used is considered as a closed circuit, the movement of lithium ions and the flow of current are the same. In secondary batteries that use lithium ions, the anode (positive electrode) ) and the cathode (negative electrode) are switched, and the oxidation and reduction reactions are switched. The electrode with the higher reaction potential is called the positive electrode, and the electrode with the lower reaction potential is called the negative electrode. In the specification, it is said that the reverse pulse current flows whether during charging or discharging. Even when a charging current is applied, the positive pole is called the "positive pole" or "+ pole (plus pole)". The negative electrode is called the "negative electrode" or "-electrode (minus electrode)". The terms anode and cathode, which are related to the reaction, are used to distinguish between charging and discharging. When the current is applied, the anode is turned on, which can cause confusion. The terms cathode and cathode are not used in this specification. When using the terms anode and cathode, specify whether they are being used during charging or discharging. In addition, it is also necessary to indicate whether it corresponds to a positive electrode (plus electrode) or a negative electrode (minus electrode). do.

[0138] A charger is connected to the two terminals shown in FIG. 6C, and the storage battery 400 is charged. As the charging of the battery 400 progresses, the potential difference between the electrodes increases. From the external terminal, it flows toward the positive electrode 402, and inside the storage battery 400, it flows from the positive electrode 402 to the negative electrode The direction of the current flowing from the negative electrode to the external terminal of the storage battery 400 is called positive. In other words, the direction of the charging current is the direction of the current.

[0139] [Cylindrical storage battery] Next, an example of a cylindrical storage battery will be described with reference to FIG. As shown in FIG. 7(A), the battery has a positive electrode cap (battery cover) 601 on the top surface and The positive electrode cap and the battery can (external can) 602 are are insulated from each other by a gasket (insulating packing) 610.

[0140] FIG. 7(B) is a schematic diagram showing a cross section of a cylindrical storage battery. On the inside of 02, a strip-shaped positive electrode 604 and a negative electrode 606 are wound with a separator 605 sandwiched between them. Although not shown, the battery element is wound around a center pin. The battery can 602 is closed at one end and open at the other end. Metals such as nickel, aluminum, titanium, etc. that are resistant to corrosion by the electrolyte, or Alloys and alloys of these with other metals (e.g., stainless steel, etc.) can be used. In addition, it is preferable to coat the material with nickel, aluminum, etc. to prevent corrosion by the electrolyte. Inside the battery can 602, the battery element in which the positive electrode, the negative electrode, and the separator are wound is The battery element is sandwiched between a pair of insulating plates 608 and 609. The inside of the battery can 602 is filled with a non-aqueous electrolyte (not shown). A storage battery similar to that of the above type can be used.

[0141] The negative electrode for a power storage device described in Embodiment 1 is used for the negative electrode 606. 06 may be manufactured in the same manner as the positive and negative electrodes of the coin-type storage battery described above, but The positive and negative electrodes used in the storage battery are wound, so active materials are formed on both sides of the current collector. The positive electrode 604 is connected to a positive electrode terminal (positive electrode current collector lead) 603, and the negative electrode 606 is connected to A negative electrode terminal (negative electrode current collecting lead) 607 is connected to the positive electrode terminal 603 and the negative electrode terminal 607. The positive terminal 603 is a safety valve. The negative terminal 607 is resistance welded to the bottom of the battery can 602 via the mechanism 612. The structure 612 is a PTC element (Positive Temperature Coefficient The positive electrode cap 601 is electrically connected to the positive electrode cap 601 via the safety valve mechanism 611. 12 is a circuit diagram showing a structure of a positive electrode cap 601 and a positive electrode 604 when the internal pressure of the battery increases beyond a predetermined threshold value. The PTC element 611 cuts off the electrical connection between the This is a thermal resistor element whose resistance increases over time, and the increase in resistance limits the amount of current to prevent abnormal heat generation. The PTC element is made of barium titanate (BaTiO3) based semiconductor ceramic. etc. can be used.

[0142] [Thin storage battery] Next, an example of a thin storage battery will be described with reference to FIG. If the structure has the above, when the device is mounted on an electronic device having at least a part having flexibility, This allows the battery to bend in accordance with the deformation of the electronic device.

[0143] FIG. 8 shows an external view of a thin storage battery 500. Also, FIG. 9(A) and FIG. 9(B) show the external view of FIG. 5 shows a cross section taken along the line A1-A2 and a cross section taken along the line B1-B2, which are indicated by dashed lines. A positive electrode 503 having a positive electrode current collector 501 and a positive electrode active material layer 502, and a negative electrode current collector 504 and a negative electrode 506 having a negative electrode active material layer 505; a separator 507; and an electrolyte solution 508. The battery has an exterior body 509. A positive electrode 503 and a negative electrode 506 are disposed in the exterior body 509. A separator 507 is disposed between the battery 501 and the battery 502. The inside of the exterior body 509 is filled with an electrolyte 508. The negative electrode for a power storage device described in Embodiment 1 is used as the negative electrode 506.

[0144] The separator 507 is processed into a bag shape so as to enclose either the positive electrode 503 or the negative electrode 506. For example, as shown in FIG. 10(A), the positive electrode 503 is sandwiched between the positive electrode 503 and the positive electrode 504. The separator 507 is folded in half as shown in FIG. 1, and the sealing portion 51 is formed on the outer side of the area overlapping with the positive electrode 503. By sealing with 4, the positive electrode 503 can be reliably supported within the separator 507. Then, as shown in FIG. 10(B), the positive electrode 503 and the negative electrode 504 are wrapped in a separator 507. 506 are alternately stacked and placed inside an exterior body 509 to form a thin storage battery 500. It is advisable to form a

[0145] FIG. 11B shows an example in which a current collector is welded to a lead electrode. For example, a positive electrode current collector 501 is welded to a lead electrode. The positive electrode current collector 501 is welded to the positive electrode lead electrode 510 by ultrasonic welding or the like. The positive electrode current collector 501 is welded to the positive electrode lead electrode 510 at a welding area 512. By having the curved portion 513 shown in FIG. 11(B), it is possible to prevent the storage battery 500 from being subjected to an external force after it is manufactured. This can reduce the stress caused by the application of heat, thereby improving the reliability of the storage battery 500. Cut.

[0146] In the thin storage battery 500 shown in FIGS. 8 and 9, the positive electrode lead electrode 510 is a positive electrode current collector. 501 and the negative electrode lead electrode 511 are ultrasonically bonded to the negative electrode current collector 504. The positive electrode current collector 501 and the negative electrode current collector 504 serve as terminals for electrical contact with the outside. In that case, the positive electrode current collector 501 and the negative electrode current collector 502 are not used as lead electrodes. A portion of the electric conductor 504 may be arranged so as to be exposed to the outside from the exterior body 509 .

[0147] In the thin storage battery 500, the exterior body 509 is made of, for example, polyethylene, polypropylene, etc. A film made of a material such as polycarbonate, ionomer, or polyamide is coated with aluminum. A thin metal film made of a material having excellent flexibility, such as stainless steel, copper, or nickel, is then formed on the thin metal film. The outer surface of the exterior body is provided with an insulating synthetic resin film such as polyamide resin or polyester resin. A three-layer film having such a structure can be used.

[0148] In addition, in FIG. 8, the number of electrode layers is set to three as an example, but the number of electrode layers is of course not limited to three. The number of electrode layers may be large or small. When the number of electrode layers is large, the capacity is increased. In addition, when the number of electrode layers is small, the battery can be made thin and flexible. This can be an excellent storage battery.

[0149] In this embodiment, a coin type, a cylindrical type, and a thin type storage battery are shown as the storage battery. However, other types of batteries, such as sealed batteries and rectangular batteries, can be used. In addition, a structure in which a positive electrode, a negative electrode, and a separator are laminated in multiple layers, It may also be of a wound structure.

[0150] The negative electrodes of the storage batteries 300, 500, and 600 shown in this embodiment are The negative electrode active material layer according to the embodiment is used. The discharge capacity of the battery 600 can be increased, or the cycle characteristics can be improved. Cut.

[0151] The thin storage battery is not limited to that shown in FIG. 8. Another example of a thin storage battery is shown in FIG. 12. The wound body 993 shown in FIG. 9 has a negative electrode 994, a positive electrode 995, and a separator 996. .

[0152] The wound body 993 is formed by stacking a negative electrode 994 and a positive electrode 995 with a separator 996 in between. The laminated sheet is then wound. This wound body 993 is placed in a square sealed container or the like. A square secondary battery is produced by covering the battery with a material such as a polyester.

[0153] The number of layers of the negative electrode 994, the positive electrode 995, and the separator 996 is determined based on the required capacity. The negative electrode 994 is connected to the lead electrode 997 and the lead electrode 998. The positive electrode 995 is connected to a lead electrode 996. 97 and the other of the lead electrodes 998 are connected to a positive electrode current collector (not shown).

[0154] The power storage device 980 shown in FIGS. 12B and 12C includes a film 981 and a filter having a recess. The above-mentioned wound body 993 is inserted into the space formed by bonding the film 982 to the film 982 by thermocompression or the like. The winding body 993 has a lead electrode 997 and a lead electrode 998. The insides of film 981 and film 982 having the recesses are impregnated with an electrolyte.

[0155] The film 981 and the film 982 having the recesses are made of a metal material such as aluminum. The film 981 and the film 982 having the recesses can be made of a material such as a resin material. If a resin material is used as the material, when an external force is applied, the film 981 and the recessed portion are formed. The film 982 can be deformed to produce a flexible storage battery. Cut.

[0156] In addition, although two films are used in FIG. 12(B) and (C), one film may be used. The film is folded to form a space, and the above-mentioned wound body 993 is stored in the space. You may do so.

[0157] In addition, the exterior body of the power storage device and the sealing container are made of a resin material, etc., so that the device has flexibility. However, when the exterior body or the sealing container is made of a resin material, The parts that are connected to the outside are made of conductive material.

[0158] For example, an example of a flexible rectangular storage battery is shown in FIG. 13. The wound body 993 in FIG. 13(A) is , is the same as that shown in FIG. 12(A), so a detailed description will be omitted.

[0159] The power storage device 990 shown in FIGS. 13B and 13C includes the above-described wound body inside an outer casing 991. The winding body 993 contains a lead electrode 997 and a lead electrode 998. The exterior bodies 991 and 992 are impregnated with an electrolyte inside. For example, a metal material such as aluminum or a resin material can be used. If a resin material is used as the material of 92, the exterior bodies 991 and 99 2 can be deformed to produce a flexible rectangular storage battery.

[0160] In addition, examples of the structure of the power storage device (power storage unit) will be described with reference to FIGS. 14, 15, and 16. .

[0161] 14A and 14B are diagrams showing the external appearance of a power storage device. The device includes a substrate 900 and a power storage unit 913. A label 910 is attached to the power storage unit 913. As shown in FIG. 14B, the power storage device includes a terminal 951 and a terminal 952. It has an antenna 914 and an antenna 915.

[0162] The circuit board 900 includes a terminal 911 and a circuit 912. The terminal 911 is connected to a terminal 951. , a terminal 952, an antenna 914, an antenna 915, and a circuit 912. A plurality of terminals 911 are provided, and each of the plurality of terminals 911 is used as a control signal input terminal, a power supply terminal, etc. may also be used.

[0163] The circuit 912 may be provided on the back surface of the circuit board 900. The antenna 915 is not limited to a coil shape, but may be, for example, a wire shape or a plate shape. Planar antenna, aperture antenna, traveling wave antenna, EH antenna, magnetic field antenna, dielectric Alternatively, the antenna 914 or the antenna 915 may be The flat conductor may function as one of the conductors for electric field coupling. In other words, the annulus can be used as one of the two conductors of the capacitor. In this way, the electromagnetic field, the magnetic field, and the like can be detected by the antenna 914 or the antenna 915. Alternatively, power can be exchanged using an electric field.

[0164] The line width of antenna 914 is preferably larger than the line width of antenna 915. This allows the amount of power received by the antenna 914 to be increased.

[0165] The power storage device includes an antenna 914 and an antenna 915, and a layer 916 between the power storage body 913. The layer 916 has a function of shielding an electromagnetic field generated by the power storage unit 913, for example. The layer 916 may be made of, for example, a magnetic material.

[0166] The structure of the power storage device is not limited to that shown in FIG.

[0167] For example, as shown in FIG. 15(A-1) and FIG. 15(A-2), In the power storage unit 913 shown in FIG. 1(B), an antenna may be provided on each of a pair of opposing surfaces. FIG. 15(A-1) is an external view seen from one side of the pair of faces. 14(A) and 14(B) are external views of the pair of surfaces as viewed from the other side. 14(A) and 14(B) are the same as those in the power storage device shown in FIG. The description of the power storage device can be used as appropriate.

[0168] As shown in FIG. 15(A-1), a layer 916 is sandwiched between one of a pair of surfaces of a power storage unit 913. 15(A-2), a tenon 914 is provided on the other of the pair of surfaces of the power storage unit 913. An antenna 915 is provided between the layers 917. The layer 917 is, for example, The layer 917 has a function of blocking electromagnetic fields. It is possible.

[0169] By adopting the above structure, the size of both the antenna 914 and the antenna 915 can be increased. It is possible.

[0170] 14(A) and 14(B), as shown in FIG. 15(B-1) and FIG. 15(B-2). In the case of the power storage unit 913 shown in FIG. 9B, a separate antenna may be provided on each of a pair of opposing surfaces. FIG. 15(B-1) is an external view seen from one side of the pair of faces. FIG. 14(A) and FIG. 14(B) are external views seen from the other side of the pair of surfaces. The same parts as those in the power storage device shown in FIG. 14B are shown in FIGS. The description of the power storage device can be used as appropriate.

[0171] As shown in FIG. 15(B-1), a layer 916 is sandwiched between one of a pair of surfaces of a power storage unit 913. 15B-2, a capacitor 91 An antenna 918 is provided on the other of the pair of surfaces of the substrate 3 with a layer 917 interposed therebetween. The antenna 918 is For example, the antenna 918 has a function of performing data communication with an external device. For example, an antenna having a shape applicable to antenna 914 and antenna 915 may be applied. As a method for communication between the power storage device and other devices via the antenna 918, NFC is used. It is possible to apply a response method that can be used between the storage device and other devices, such as the above. do.

[0172] 16A, the power storage unit 913 shown in FIG. 14A and FIG. A display device 920 may be provided. The display device 920 is connected to the terminal 911 via the terminal 919. The label 910 is not provided on the portion where the display device 920 is provided. Note that the same parts as those in the power storage device shown in FIG. The description of the power storage device in FIGS. 14(A) and 14(B) can be used as appropriate.

[0173] The display device 920 displays, for example, an image indicating whether charging is in progress, an image indicating the amount of stored power, etc. The display device 920 may be, for example, an electronic paper, a liquid crystal display device, an electrophotographic display device, or the like. For example, an electroluminescence (EL) display device can be used. By using the par, the power consumption of the display device 920 can be reduced.

[0174] 16B, the power storage unit 913 shown in FIG. 14A and FIG. A sensor 921 may be provided. The sensor 921 is electrically connected to the terminal 911 via a terminal 922. Note that the same parts as those of the power storage device shown in FIG. The description of the power storage device in FIGS. 14A and 14B can be used as appropriate.

[0175] The sensor 921 may be, for example, a force, a displacement, a position, a velocity, an acceleration, an angular velocity, a rotation speed, a distance, etc. , light, liquid, magnetism, temperature, chemicals, sound, time, hardness, electric field, current, voltage, power, radiation The equipment may include a function to measure flow rate, humidity, gradient, vibration, odor, or infrared rays. By providing the sensor 921, for example, it is possible to detect the environment in which the power storage device is placed. Data (such as temperature) can also be sensed and stored in memory within the circuit 912 .

[0176] In addition, examples of mounting the flexible storage battery shown in FIG. 8, FIG. 12, and FIG. 13 on an electronic device are shown. FIG. 17 shows an example of an electronic device that uses a flexible power storage device. For example, television equipment (also called television or television receiver), computer Any monitor, digital camera, digital video camera, digital photo frame, mobile phone Mobile phones (also called mobile phones or mobile phone devices), portable game machines, portable information terminals, audio playback equipment Examples include large gaming machines such as pachinko machines.

[0177] In addition, the flexible energy storage device can be mounted on the inner or outer walls of a house or building, or on the inside or outside of a car. It is also possible to incorporate it along the curved surfaces of the interior or exterior of the vehicle.

[0178] FIG. 17A shows an example of a mobile phone. A mobile phone 7400 includes a housing 7401. In addition to the display unit 7402, operation buttons 7403, an external connection port 7404, The mobile phone 7400 is equipped with a speaker 7405, a microphone 7406, and the like. It has device 7407.

[0179] FIG. 17B shows the mobile phone 7400 in a curved state. When the 0 is deformed by an external force and curved as a whole, the storage device installed inside The bent power storage device 7407 is also bent. The power storage device 7407 is a thin storage battery. The power storage device 7407 is fixed to the current collector 7409. For example, the current collector 7409 is made of copper foil, some of which is alloyed with gallium. The adhesion between the current collector 7409 and the active material layer in contact therewith is improved, and the power storage device 7407 This structure is highly reliable even when bent.

[0180] FIG. 17D shows an example of a bangle-type display device. The portable display device 7100 is The device includes a housing 7101 , a display portion 7102 , operation buttons 7103 , and a power storage device 7104 . FIG. 17E shows a bent state of the power storage device 7104. When the device is worn on the user's arm in a buckled state, the housing may deform and cause damage to part of the power storage device 7104 or The total curvature changes. Note that the degree of curvature at any point on the curve is expressed as the radius of the corresponding circle. The value expressed is the radius of curvature, and the inverse of the radius of curvature is called the curvature. A part of the main surface of the housing or the power storage device 7104 within the range of R of 40 mm to 150 mm Or the entire surface of the power storage device 7104 changes. If the distance is within 50 mm, high reliability can be maintained. The lead electrode 7105 is electrically connected to the collector 7106. 06 is copper foil, which is partially alloyed with gallium to form a layer of the active material in contact with the current collector 7106. The adhesion is improved, and the power storage device 7104 has high reliability even if it is bent many times by changing the curvature. It is a structure that can maintain reliability.

[0181] FIG. 17F shows an example of a wristwatch-type portable information terminal. The portable information terminal 7200 is , a housing 7201, a display unit 7202, a band 7203, a buckle 7204, and an operation button 72 05, input / output terminal 7206, etc.

[0182] The portable information terminal 7200 is capable of carrying out mobile telephone calls, e-mails, viewing and creating documents, playing music, and using the Internet. - It can run various applications such as internet communication and computer games. do.

[0183] The display unit 7202 has a curved display surface, and displays images along the curved display surface. The display portion 7202 is provided with a touch sensor, and can be used to input a touch signal to the screen using a finger or a stylus. For example, the icon 72 displayed on the display unit 7202 can be operated by touching it. You can launch the application by touching 07.

[0184] The operation button 7205 is used to set the time, turn the power on and off, and turn wireless communication on and off. It has various functions such as operation, silent mode activation and deactivation, power saving mode activation and deactivation, etc. For example, an operating system installed in the portable information terminal 7200 can The function of the operation button 7205 can also be freely set using the stem.

[0185] In addition, the mobile information terminal 7200 is capable of performing short-distance wireless communication according to a communication standard. For example, by communicating with a wireless headset, You can also make calls.

[0186] The portable information terminal 7200 also includes an input / output terminal 7206, and can communicate with other information terminals via connectors. It is also possible to charge the device via the input / output terminal 7206. The charging operation can be performed by wireless power supply without going through the input / output terminal 7206. This is also fine.

[0187] The display portion 7202 of the portable information terminal 7200 includes a power storage device having the electrode member of one embodiment of the present invention. For example, the power storage device 7104 in FIG. 17E is included in a housing 7201. It can be installed in a curved state in the part of the band 7203 or in a curved state inside the band 7203. Cut.

[0188] [Example of electrical equipment: Installed in a vehicle] Next, an example of installing a storage battery in a vehicle will be shown. Hybrid electric vehicles (HEV), electric vehicles (EV), plug-in hybrid vehicles (PHEV), etc. This will make the next generation of clean energy vehicles a reality.

[0189] FIG. 18 illustrates an example of a vehicle using one embodiment of the present invention. 100 is an electric vehicle that uses an electric motor as a power source for running; or A hybrid vehicle that can select between an electric motor and an engine as a power source for driving. By using one embodiment of the present invention, a vehicle with a long driving range can be realized. The automobile 8100 also has a power storage device. The power storage device can be used to power the electric motor 8 It not only drives the 106, but also the headlights 8101 and room lights (not shown). The light emitting device can be supplied with power.

[0190] In addition, the power storage device may be used for displaying information such as a speedometer and a tachometer of the automobile 8100. The power storage device can supply power to the navigation device of the automobile 8100. The present invention can provide power to semiconductor devices such as power distribution systems.

[0191] The automobile 8100 shown in FIG. 18B is a power storage device of the automobile 8100. The device can be charged by receiving power from an external charging facility using a contactless power supply method or other methods. FIG. 18B shows a diagram of a charging device 8021 installed on the ground and a storage device 8100 installed in the vehicle. The charging device is shown being charged via a cable 8022. The power supply method and connector standards are specified as appropriate, such as CHAdeMO (registered trademark) or Combo. The charging device 8021 may be a charging station installed in a commercial facility. For example, plug-in technology allows the The battery storage device mounted on the automobile 8100 can be charged by the AC / DC converter. This can be achieved by converting AC power into DC power via a conversion device such as an inverter.

[0192] Although not shown, a power receiving device is mounted on the vehicle and receives power from a ground power transmitting device in a non-contact manner. In this non-contact power supply method, a power transmission device is installed on the road or exterior wall. By incorporating this technology, charging can be done not only when the vehicle is stopped but also while it is moving. Using this method, electric power may be transmitted between vehicles. A solar cell may be provided to charge the power storage device while the vehicle is stopped or running. The power can be supplied using an electromagnetic induction method or a magnetic resonance method.

[0193] According to one embodiment of the present invention, the cycle characteristics of a power storage device can be improved and the reliability can be improved. Furthermore, according to one embodiment of the present invention, the characteristics of a power storage device can be improved. Therefore, the storage device itself can be made smaller and lighter. This contributes to reducing the weight of the vehicle, improving the cruising distance. The power storage device can be used as a power supply source for something other than a vehicle. It is possible to avoid using commercial power during peak hours.

[0194] This embodiment mode can be implemented in appropriate combination with other embodiment modes. EXAMPLES

[0195] In the following examples, a half cell was prepared using the negative electrode shown in the first embodiment, and cycle characteristics were Sexuality was evaluated.

[0196] (Preparation of Complex) The composite particles were prepared. First, titanium powder with a particle size of 45 μm and silicon powder with a particle size of 5 μm were used. The silicon powder was weighed out so that the molar ratio of Ti:Si=1:2 and the total weight was about 20 g. The grinding container (C) attached to the planetary rotation type ball mill grinder (LP-4, Ito Seisakusho) Put the weighed titanium powder, silicon powder and media into a 500ml container (manufactured by ROM). The media is chrome steel balls with a diameter of 10 mm, and the amount of the balls is 1 / 3 of the total amount of the grinding container. The crushing container had an Ar atmosphere and the rotation speed was 200. A composite of sample A was produced by rotating and revolving at rpm. The rotation / revolution stirring was further performed at 250 rpm to obtain a composite of samples B to D. For each of Samples B to D, the processing time of the stirring at a rotation speed of 250 rpm was That is, sample B was stirred for 18 hours, sample C for 38 hours, and sample D for 50 hours. The results are shown in Table 1. Processing conditions by the crusher, and the average particle size and The particle size was measured using a laser diffraction particle size distribution analyzer (SALD-2200, Shima The particle size was measured using a laser diffraction / scattering method. Although the average particle size and D90 of sample A were not measured, they are considered to be larger than those of sample B. can be.

[0197] [Table 1]

[0198] (Preparation of negative electrode) Using the obtained samples A to D and comparative sample E, negative electrodes were produced by the following method. That is, a 10 μm thick stainless steel foil with nickel coating on the surface was used as the negative electrode current collector. The composite particles or Si particles, acetylene black, and polyimide ( More precisely, the mixing ratio of the polyimide precursor was 80:5:15 (wt%). The mixture was mixed using a planetary mixer to prepare a slurry. NMP was used as the solvent. First, a solvent was added to the composite particles or Si particles, and the mixture was mixed in a kneader. Acetylene black and NMP were added and the mixture was kneaded. Next, the polyimide precursor and Finally, NMP was added again and mixed in the kneader. The kneading conditions were a rotation speed of 2000 rpm and 5 minutes, including hard kneading. The slurry was then applied to the current collector using the blade method. The operation speed was 10 mm / sec. The mixture was dried in air at 50°C for 1 hour to evaporate NMP. In order to imidize the polyimide precursor, the polyimide precursor was heated at 400°C for 5 hours in a N2 atmosphere. Heat treatment was carried out.

[0199] The negative electrodes prepared using the samples A to D and the comparative sample E in the above manner were designated as negative electrode A. to negative electrode D, and comparative negative electrode E.

[0200] FIG. 19 shows a cross section of electrode A made using sample A, photographed by STEM (Scanning Transform). The results were obtained by observing the Sample A in FIG. 19 contains a composite 111. STEM-EDX (Energy Dispersive X-ray Spectroscopy) of electrode A Fig. 20(A) shows the results of elemental analysis by ectroscopy. FIG. 20(B) is a STEM image of the Ti-based structure 111, and FIG. 20(C) is a mapping image of Ti. 19 and 20, the composite 111 is a silicon The negative electrode active material 115 contains titanium, and the functional material 116 contains titanium. 5 is in contact with the functional material 116 .

[0201] Figure 21 shows the cross-section of electrode B, which was fabricated using sample B, observed by STEM. The composite 110 shown in FIG. 1 is a negative electrode active material 115 containing silicon, a functional material 116 containing titanium, and , Compound 117 and Compound 118, which contain titanium silicide. The substrate 115 is in contact with at least one of the functional material 116, the compound 117, and the compound 118. The weight ratio of silicon to titanium in compound 118 is higher than that in compound 117. The weight ratio of silicon and titanium in Compound 117 and Compound 118 is It is not constant within 111.

[0202] (Cell Preparation) Next, negative electrodes A to D (hereinafter collectively referred to as composite electrodes) prepared as described above were A half cell was prepared using the negative electrode E (hereinafter also referred to as the silicon electrode) for comparison. The characteristics were evaluated using a CR2032 type (diameter 20 mm, height 3.2 mm) coin-type battery. The counter electrode was made of metallic lithium, and the separator was made of polypropylene. The solution contained 1M / l LiPF6 as the solute and EC (ethylene carbonate) as the solvent. The mixture used was a mixture of ethyl acetate (ETA) and diethyl carbonate (DEC) in a volume ratio of 3:7. The half cells prepared using negative electrodes A to D are called cells A to D, respectively, and the comparative negative electrodes are called cells B to D. The half cell made using pole E is designated as cell E.

[0203] Here, the charge and discharge of the half cell using the composite electrode or the silicon electrode is performed using the formula: FIG. 22 shows a half cell using a composite electrode or a silicon electrode and a Li counter electrode. 1 shows a connection configuration between a half cell 121A and a load 122 when discharging. When discharging the Fusel 121A, the reaction of formula (1) occurs at the composite electrode or silicon electrode. happen.

[0204] Si + xLi + +xe - → SiLi x (1)

[0205] Furthermore, at the Li electrode, the reaction represented by formula (2) occurs.

[0206] xLi → xLi + +xe - (2)

[0207] Figure 23 shows the case of charging a half cell using a composite electrode or a silicon electrode and a Li counter electrode. 1 shows a connection configuration between a half cell 121A and a charger 123 in the half cell 121. When A is charged, the reaction of formula (3) occurs at the composite electrode or silicon electrode.

[0208] SiLi x → Si + xLi + +xe - (3)

[0209] Furthermore, at the Li electrode, the reaction represented by formula (4) occurs.

[0210] xLi + +xe - → xLi (4)

[0211] Here, in the formulas (1) to (4), x satisfies x≦4.4.

[0212] As shown in formulas (1) to (4), Li is inserted into silicon during discharge and is removed from silicon during charging. Li is released from the

[0213] In addition, if part of the titanium contained in the composite particles in the composite electrode is oxidized, the oxidation Titanium oxide may also contribute to charging and discharging. The following reaction may occur. When discharging a half cell using a composite electrode with titanium dioxide and a Li counter electrode, The figure shows a connection configuration between the half cell 121B and the load 122. In this case, the reaction of equation (5) occurs at the composite electrode.

[0214] Si + TiO2 + (x+y)Li + + (x+y)e - → SiLi x + Li y TiO2(5)

[0215] Furthermore, at the Li electrode, the reaction represented by formula (6) occurs.

[0216] (x+y)Li → (x+y)Li + + (x+y)e - (6)

[0217] FIG. 25 shows the case where a half cell using a composite electrode having titanium oxide and a Li counter electrode is charged. 1 shows a connection configuration between the half cell 121B and the charger 123 in the half cell 121. When B is charged, the reaction of equation (7) occurs at the composite electrode.

[0218] SiLi x + Li y TiO2 → Si + TiO2+ (x+y)Li + + (x+y)e - (7)

[0219] Furthermore, at the Li electrode, the reaction represented by formula (8) occurs.

[0220] (x+y)Li + + (x+y)e - → (x+y)Li (8)

[0221] Here, in formulas (5) to (8), x satisfies x≦4.4, and y satisfies y<0.7. Add.

[0222] As shown in formulas (5) to (8), Li is inserted into silicon and titanium oxide by discharge. Lithium is released from silicon and titanium oxide upon charging.

[0223] (Cell Measurement) Next, the results of measuring the charge / discharge characteristics and cycle characteristics of the cells A to E prepared as described above were The results are presented.

[0224] The measurement conditions for the half-cell are explained below. The charge and discharge method is a constant current at a rate of 0.2C. The battery was charged at a constant voltage and discharged at a constant current at a rate of 0.2 C. The upper limit of the charge and discharge voltage was 1.5 V. The lower limit voltage was set to 0.01 V. The measurement temperature was 25°C. The calculations are based on the theoretical capacity of 4200mAh / g.

[0225] Table 2 shows the initial discharge capacity obtained as a result of charging and discharging cells A to E, and the The capacity retention rate after 10 cycles and the capacity after 20 cycles compared to the initial discharge capacity Figure 26 shows the change in the capacity retention rate when the initial discharge capacity is taken as 100%. The results of cell A are shown as a solid line, the results of cell B as a dashed line, the results of cell C as a dashed line, and the results of cell The results of cell D are shown by the two-dot chain line, and the results of cell E are shown by the dotted line. The amount maintenance rate is not listed because it is still being measured.

[0226] [Table 2]

[0227] As shown in Table 2 and FIG. 26, the composite was used as a negative electrode active material for a power storage device negative electrode according to one embodiment of the present invention. The cells A to D using the particles were more efficient than the cell E using silicon particles as the negative electrode active material. This is because the titanium is in contact with the silicon in the composite particles. The presence of silicon oxide reduces the stress that occurs when silicon expands and contracts during charging and discharging. This is thought to be because it is possible to suppress cracks and peeling of the silicon.

[0228] In addition, the longer the mixing time in the preparation of the composite microparticles, the lower the initial volume tends to be. This is because the amount of titanium silicide formed in the composite particles changes depending on the stirring time. This is thought to be because the amount of silicon, which mainly contributes to the absorption and release of lithium ions, increases and the amount of silicon decreases. On the other hand, there is no simple proportional relationship between the stirring time and the cell capacity maintenance rate. Therefore, in order to obtain a high-capacity, high-cycle electricity storage device, the stirring time is It is preferable to determine it appropriately. EXAMPLES

[0229] In this example, a power storage device was manufactured to confirm the performance of a negative electrode for a power storage device according to one embodiment of the present invention. The results of evaluating the characteristics are then explained.

[0230] The power storage device prepared in this example is a coin-type battery (coin cell). There are four samples in total: sample G, sample H, and comparison sample I. Each sample has an electrode, a counter electrode, an electrolyte, and a separator. The structure other than the electrodes is the same for all samples. The method for fabricating the electrodes will be described below. The electrodes used for Sample F, Sample G, Sample H, and Comparative Sample I are referred to as Electrode F and Electrode G, respectively. , electrode H and electrode I.

[0231] (Method of manufacturing electrodes) An active material layer and a functional layer are formed on a titanium substrate, which serves as a current collector, using a sputtering device. The silicon target used for forming the active material layer was the same for electrodes F to I. The titanium target used for forming the functional layer is common to electrodes F to H. be.

[0232] Electrode F is a titanium substrate with a 90 nm silicon film and titanium nitride (TiN x ) membrane to 30 nm The deposition conditions for the titanium nitride film were Ar gas flow rate of 9 sccm, N2 gas flow rate of 1 s It was decided as ccm.

[0233] Electrode G is a titanium substrate with a 90 nm silicon film and titanium oxide (TiO x ) membrane to 30 nm The deposition conditions for the titanium oxide film were Ar gas flow rate of 9 sccm, O2 gas flow rate of 1 s It was decided as ccm.

[0234] Electrode H was made by depositing a 90 nm thick silicon film and a 30 nm thick titanium film on a titanium substrate. The film was formed under conditions of an Ar gas flow rate of 9 sccm.

[0235] Electrode I was prepared by depositing a silicon film to a thickness of 90 nm on a titanium substrate.

[0236] The nitrogen content of the titanium nitride film of electrode F is about 18 atomic %, and the oxygen content is The concentration of the oxide in electrode G was approximately 0.1 atomic % to 0.3 atomic %. The oxygen content of the titanium film is about 40 atomic %, and the nitrogen content is about 0.3 atomic %. The titanium nitride film and titanium oxide film were For quantitative analysis of titanium films, secondary ion mass spectrometry (SIMS) was used. Mass spectrometry was used.

[0237] (Sample Preparation) In Samples F to H and Comparative Sample I, a Li foil having a thickness of 600 μm was used as the counter electrode. The electrolyte was a mixture of EC and DEC in a volume ratio of 3:7 as a solvent, and LiPF6 was used. Polypropylene with a thickness of 25 μm was used as the separator.

[0238] In this manner, each sample was prepared.

[0239] (Sample Measurement) Next, the initial charge / discharge characteristics of each sample of this example at 25° C. were evaluated. The measurement was performed using a charge measuring device (manufactured by Toyo Systems Co., Ltd.). Constant current charging was performed with an upper limit of 1.5 V. The charge / discharge rate was 0.2 C and the lower limit was 0.01 V. The rate is calculated based on the theoretical capacity of silicon, which is 4200mAh / g.

[0240] FIG. 27(A) shows the results of the specimen F, FIG. 27(B) shows the results of the specimen G, FIG. 27(C) shows the results of the specimen H, and FIG. Fig. 27 shows the initial charge / discharge curve of comparative sample I. The horizontal axis is capacity (mAh / g). The vertical axis is voltage (V). The servings are different.

[0241] The initial discharge capacity obtained was 2645mAh / g for sample F and 2955mAh / g for sample G. The capacity of sample H was 2158mAh / g, and that of comparative sample I was 4518mAh / g. The initial charge-discharge efficiency of sample F was 84.8%, and the initial charge-discharge efficiency of sample G was 79.9%.

[0242] Next, the cycle characteristics of each sample of this example at 25° C. were evaluated. The charging conditions were the same as those in the initial charge-discharge characteristic evaluation described above.

[0243] FIG. 28 shows the change in the capacity retention rate when the initial discharge capacity is taken as 1. F, sample H and comparative sample I are overlapped. 28(C) and (D) are graphs in which the capacity retention rates of sample H and comparative sample I are superimposed. are graphs in which the vertical axis of FIG. 28(A) and (B) is enlarged, respectively. ), Samples F and G are shown with thick solid lines, Sample H is shown with a thin solid line, and Comparative Sample I is shown with a thin dashed line. The capacity retention rate for samples F and G up to 20 cycles is shown, and the capacity retention rate for sample H and Comparative Sample I show a capacity retention rate up to 50 cycles.

[0244] From FIG. 28, it can be seen that samples F and G exhibit good cycle characteristics similar to sample H. Therefore, titanium nitride and titanium oxide, like titanium, are also one aspect of the present invention. It has been shown to be suitable as a functional material contained in composite particles in negative electrodes for power storage devices. . EXAMPLES

[0245] In this example, a negative electrode for a power storage device according to one embodiment of the present invention was prepared in a manner different from that in Example 2. A power storage device was manufactured and its characteristics were evaluated. The results are described below.

[0246] The power storage device prepared in this example is a coin-type battery (coin cell). Each sample contains an electrode, a counter electrode, an electrolyte, and a separator. The structure is the same for all samples. The method for fabricating the electrodes is explained below. The electrodes used for the sample J and the comparative sample K are referred to as electrode J and electrode K, respectively.

[0247] (Method of manufacturing electrodes) An active material layer and a functional layer are formed on a titanium substrate, which serves as a current collector, using a sputtering device. The silicon target used for forming the active material layer was the same for electrodes J and K. It is common.

[0248] Electrode J was made by depositing a 70 nm silicon film and a 30 nm titanium film on a titanium substrate. The deposition conditions for the titanium film were an Ar gas flow rate of 9 sccm.

[0249] The electrode K was formed by depositing a silicon film of 70 nm on a titanium substrate.

[0250] (Sample Preparation) A half cell was made using electrode J and electrode K. The characteristics were evaluated using a CR2032 type. A coin-type storage battery with a diameter of 20 mm and a height of 3.2 mm was used. The separator was polypropylene. The electrolyte used was a mixture of EC and DEC as a solvent. The mixture was mixed in a volume ratio of 3:7 and LiPF6 was used as the solute. This was dissolved to prepare an electrolyte with a LiPF6 concentration of 1.0 mol / L.

[0251] In this manner, each sample was prepared.

[0252] (Sample Measurement) Next, the cycle characteristics of each sample of this example at 25° C. were evaluated. The test was performed using a constant current / constant voltage charger (manufactured by Toyo Systems Co., Ltd.). The charge / discharge rate was 0.2C, and the constant voltage discharge was performed with a lower limit of 0.01V. The theoretical capacity of the active material, including silicon and titanium, is 4190mAh / g. The calculation is based on the relationship between any one charge / discharge cycle and the next charge / discharge cycle. There was a 30-minute or 2-hour break between sessions.

[0253] Figure 29 shows the change in capacity of each sample during cycle evaluation. The broken line shows the capacity change of sample I and the broken line shows the capacity change of sample J for comparison. 2122mAh / g, and comparative sample K is 3814mAh / g.

[0254] From FIG. 29, it can be seen that sample J exhibits better cycle characteristics than comparative sample K. Light.

[0255] (Cross-section observation of sample) FIG. 30 shows the results of STEM observation of the cross sections of sample J and comparative sample K after charging and discharging. FIG. 30(A) shows the results of a sample prepared under the same conditions as sample J after 10 charge / discharge cycles. FIG. 30(B) is a cross-sectional image of a sample fabricated under the same conditions as comparative sample K after 10 cycles. The cross-sectional images of the cell after charging and discharging are shown in Fig.

[0256] In the comparative sample K, protuberances and depressions were generated in the silicon film 715 on the titanium substrate 705, On the other hand, the surface unevenness is large (see FIG. 30(B)). In the case of sample J, in which the silicon film 715 is covered with the titanium film 716, the silicon No significant irregularities were observed in the titanium film 715 (see FIG. 30(A)). It was confirmed that this material is suitable as a functional material that can suppress deformation caused by the expansion and contraction of silicon. . [Explanation of symbols]

[0257] 100 negative electrode 101 Negative electrode current collector 102 Negative electrode active material layer 110 Complex 110A complex 111 Complex 111A complex 112 Complex 115 Anode active material 116 Functional Materials 116A Functional materials 116B Functional materials 117 Compound 118 compounds 121A Half Cell 121B Half Cell 122 Load 123 Charger 200 negative electrode 201 Negative electrode current collector 202 Negative electrode active material layer 203 Complex 204 Graphene 300 Battery 301 Positive electrode can 302 Anode can 303 Gasket 304 Positive electrode 305 Positive electrode current collector 306 Positive electrode active material layer 307 Negative electrode 308 Negative electrode current collector 309 Negative electrode active material layer 310 Separator 372mAh theoretical capacity 400 Battery 402 Positive electrode 404 Negative electrode 500 Battery 501 Positive electrode current collector 502 Positive electrode active material layer 503 Positive electrode 504 Negative electrode current collector 505 Negative electrode active material layer 506 negative electrode 507 Separator 508 Electrolyte 509 Exterior body 510 Positive lead electrode 511 Negative lead electrode 512 Welding Area 513 Curved section 514 Sealing part 600 Battery 601 Positive electrode cap 602 Battery Can 603 Positive terminal 604 Positive electrode 605 Separator 606 negative electrode 607 Negative terminal 608 Insulating plate 609 Insulating plate 611 PTC element 612 Safety valve mechanism 705 Titanium Substrate 715 Silicone membrane 716 Titanium Film 900 Circuit Board 910 Label 911 Terminal 912 Circuit 913 Electricity storage unit 914 Antenna 915 Antenna 916 layers 917 layers 918 Antenna 919 Terminal 920 Display device 921 Sensor 922 Terminal 951 Terminal 952 Terminal 981 Film 982 Film 990 Power storage device 991 Exterior body 992 Exterior body 993 Wound body 994 negative electrode 995 positive electrode 996 Separator 997 Lead Electrode 998 Lead Electrode 7100 Portable display devices 7101 Case 7102 Display section 7103 Operation button 7104 Energy storage devices 7105 Lead electrode 7106 Current collector 7200 Portable Information Terminal 7201 Case 7202 Display section 7203 Band 7204 Buckle 7205 Operation button 7206 Input / output terminal 7207 Icon 7400 Mobile Phone 7401 Case 7402 Display section 7403 Operation button 7404 External connection port 7405 Speaker 7406 Mike 7407 Energy storage devices 7408 Lead electrode 7409 Current collector 8021 Charging device 8022 Cable 8100 Automobiles 8101 Headlight 8106 Electric Motor

Claims

1. a negative electrode active material layer including a particulate composite, a conductive additive, and a binder on a current collector; The composite has an active material containing silicon, a material containing titanium, a first compound containing silicon and titanium, and a second compound containing silicon and titanium, the second compound has a higher weight ratio of silicon to titanium than the first compound; The conductive additive comprises a particulate conductive additive and a sheet-like conductive additive.

2. a negative electrode active material layer including a particulate composite, a conductive additive, and a binder on a current collector; The composite has an active material containing silicon, a material containing titanium, a first compound containing silicon and titanium, and a second compound containing silicon and titanium, the second compound has a higher weight ratio of silicon to titanium than the first compound; The conductive assistant has a region where it is attached to the surface of the composite.

3. a negative electrode active material layer including a particulate composite, a conductive additive, and a binder on a current collector; The composite has an active material containing silicon, a material containing titanium, a first compound containing silicon and titanium, and a second compound containing silicon and titanium, the second compound has a higher weight ratio of silicon to titanium than the first compound; The conductive assistant has a region in two-dimensional contact with the composite.

4. a negative electrode active material layer including a particulate composite, a conductive additive, and a binder on a current collector; The composite has an active material containing silicon, a material containing titanium, a first compound containing silicon and titanium, and a second compound containing silicon and titanium, the second compound has a higher weight ratio of silicon to titanium than the first compound; the active material has a region in contact with at least one of the material, the first compound, and the second compound; The conductive additive comprises a particulate conductive additive and a sheet-like conductive additive.

5. a negative electrode active material layer including a particulate composite, a conductive additive, and a binder on a current collector; The composite has an active material containing silicon, a material containing titanium, a first compound containing silicon and titanium, and a second compound containing silicon and titanium, the second compound has a higher weight ratio of silicon to titanium than the first compound; the active material has a region in contact with at least one of the material, the first compound, and the second compound; The conductive assistant has a region where it is attached to the surface of the composite.

6. a negative electrode active material layer including a particulate composite, a conductive additive, and a binder on a current collector; The composite has an active material containing silicon, a material containing titanium, a first compound containing silicon and titanium, and a second compound containing silicon and titanium, the second compound has a higher weight ratio of silicon to titanium than the first compound; the active material has a region in contact with at least one of the material, the first compound, and the second compound; The conductive assistant has a region in two-dimensional contact with the composite.

Citation Information

Patent Citations

  • Negative film for lithium ion secondary battery as well as preparation method and application of negative film

    CN103996821A

  • Powder for negative electrode material of lithium ion secondary battery and negative electrode material of lithium ion secondary battery including the same

    JP2014120247A

  • Negative electrode active material for electrical device

    WO2013099441A1

  • Electric storage device and manufacturing method thereof

    JP2012009429A