Separation or concentration method of mixture gas containing carbon dioxide

The zeolite membrane composite maintains high carbon dioxide permeability after a propane contact treatment, addressing the challenge of high-pressure gas separation and concentration, enabling efficient carbon dioxide separation in actual gas applications.

JP2024169593AInactive Publication Date: 2024-12-05MITSUBISHI CHEM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024162081
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-05-29
Filing Date
2024-09-19
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional methods for separating and concentrating carbon dioxide using zeolite membranes face challenges in maintaining high permeability under high-pressure conditions, making it difficult to identify suitable zeolite membrane composites for actual gas applications.

Method used

A method involving a zeolite membrane composite with a zeolite membrane formed on a porous support, where the permeability of carbon dioxide is maintained at 0.7 or more after a propane contact treatment, ensuring high permeability even in high-pressure gas mixtures.

Benefits of technology

The method allows for effective separation and concentration of carbon dioxide in high-pressure gas mixtures, maintaining high permeability and reducing impurities, suitable for applications such as natural gas processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169593000001_ABST
    Figure 2024169593000001_ABST
Patent Text Reader

Abstract

To solve the problem that a zeolite membrane composite cannot maintain high permeance, when separating or concentrating mixture gas containing carbon dioxide and hydrocarbons.SOLUTION: Mixture gas is separated or concentrated by using a zeolite membrane composite in which P2 / P1 is 0.7 or more, when expressing a permeance of carbon dioxide as P1 in a carbon dioxide permeability test (1) before performing a prescribed propane contact treatment, and expressing permeance of carbon dioxide as P2 in a carbon dioxide permeability test (2) after performing the prescribed propane contact treatment.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses a method for separating or concentrating a gas mixture containing carbon dioxide. [Background technology]

[0002] Conventionally, separation and concentration of mixed gases containing organic and inorganic compounds have been carried out by adsorption separation, absorption separation, distillation separation, cryogenic separation, etc., depending on the properties of the target substances. However, these methods have drawbacks such as requiring a lot of energy or being limited in the scope of application of the separation and concentration targets.

[0003] In recent years, a method using membranes has been proposed as an alternative to these methods. Membrane separation involves almost no phase change during the separation process, and is a technique that separates by using the difference in speed of gas passing through a membrane, using the pressure difference as the driving energy. Compared to other gas separation and purification methods, membrane separation is easy to handle and the equipment scale is relatively small, so it can separate and concentrate the target gas at low cost and with little energy.

[0004] As a method for gas separation using membranes, methods using polymer membranes have been proposed since the 1970s. However, while polymer membranes are characterized by their excellent processability, many of them are subject to degradation and loss of performance due to heat, chemicals, and pressure, and the range of applications for separation and concentration is limited.

[0005] In recent years, various inorganic membranes with good chemical resistance, oxidation resistance, heat resistance, and pressure resistance have been proposed to solve these problems. Among them, zeolite has regular pores of sub-nanometer size and acts as a molecular sieve, allowing specific molecules to selectively pass through and demonstrating high separation performance.

[0006] Zeolite membranes are usually used for separation and concentration as a zeolite membrane composite in which zeolite is formed in a membrane shape on a support. Because zeolite membranes are made of inorganic materials, they can be used for separation and concentration over a wider temperature range than polymer membranes, and can also be used to separate mixtures containing organic compounds.

[0007] Examples of separation targets using the zeolite membrane composite include hydrogen, oxygen, carbon dioxide, nitrogen, and hydrocarbons. Among them, carbon dioxide is a greenhouse gas, so it is required to separate and capture it without discharging it into the atmosphere, and to store it or use it as a chemical raw material. For example, separation of carbon dioxide and methane is desired in natural gas refining plants and plants that generate biogas by methane fermentation of food waste. In addition, application to separation of carbon dioxide from combustion exhaust gas, such as separation of carbon dioxide and nitrogen emitted from thermal power plants, is also being considered. In particular, in thermal power generation using coal, coal is inexpensive, so power generation can be performed at low cost, but the exhaust gas contains a lot of carbon dioxide, and separation of carbon dioxide using a low-energy membrane has been desired. Zeolite membranes that can separate these well include DDR (Patent Document 1), SAPO-34 (Non-Patent Document 1), and SSZ-13 (Non-Patent Document 2). In addition, FAU membrane (Non-Patent Document 3) is also known as a zeolite membrane that can separate carbon dioxide well. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2004-105942 A [Non-patent literature]

[0009] [Non-Patent Document 1] Shiguang Li et al., "Improved SAPO-34 Membranes for CO2 / CH4 Separation", AIChE Journal. 2004, Vol. 50, No. 1, 127-135 [Non-Patent Document 2] Halil Kalipcilar et al., "Synthesis and Separation Performance of SSZ-13 Zeolite Membranes on Tubular Supports", Chem. Mater. 2002, 14, 3458-3464 [Non-Patent Document 3] Xuehong Gu et al., "Synthesis of Defect-Free FAU-Type Zeolite Membranes and Separation for Dry and Moist CO2 / N2 Mixtures", Ind. Eng. Chem. Res. 2005, 44, 937-944 Summary of the Invention [Problem to be solved by the invention]

[0010] The above-mentioned natural gas has a high pressure of several MPa to several tens of MPa. It is expected that the zeolite membrane composite can be used to separate and concentrate such high-pressure mixed gases. However, separation tests of high-pressure mixed gases such as natural gas cannot usually be performed in a laboratory, and a special large-scale high-pressure gas processing facility must be used. This high-pressure gas processing facility must also be used to judge the quality of a zeolite membrane composite, but evaluation in a high-pressure gas processing facility may be difficult due to the need for high safety confirmation. On the other hand, according to the new findings of the present inventors, even if a zeolite membrane composite shows high permeance in a low-pressure test performed in a laboratory, the permeance may not be maintained when it is applied to the separation and concentration of real gas.

[0011] As described above, in the conventional technology, there is a problem that it is difficult to distinguish and select a zeolite membrane composite that can maintain high permeance in the separation and concentration process of real gas. [Means for solving the problem]

[0012] The present application discloses the following as one of the means for solving the above problems. The first invention is a method for separating or concentrating a mixed gas, which comprises contacting a mixed gas containing at least carbon dioxide and a hydrocarbon and having a pressure of 1 MPa or more at a normal temperature or at 35°C with a zeolite membrane composite having a zeolite membrane formed on a porous support, and allowing a gas component having high permeability to permeate from the mixed gas, wherein the zeolite membrane composite has a P2 / P1 ratio of 0.7 or more, where P1 is the carbon dioxide permeance in a carbon dioxide permeation test (1) before the following propane contact treatment, and P2 is the carbon dioxide permeance in a carbon dioxide permeation test (2) after the following propane contact treatment.

[0013] Carbon dioxide permeation test (1): When a single-component gas of 100% carbon dioxide is supplied to the surface of the zeolite membrane under the conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C, the permeance of carbon dioxide that permeates the zeolite membrane is defined as P1.

[0014] Propane contact treatment: After the carbon dioxide permeation test (1), the supply gas is changed from a single component gas of 100% carbon dioxide to propane, and propane is supplied to the surface of the zeolite membrane under conditions of a supply gas pressure of 0.1 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C to replace the carbon dioxide with the propane, and then propane is supplied to the surface of the zeolite membrane for 30 minutes under conditions of a supply gas pressure of 0.4 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C.

[0015] Carbon dioxide permeation test (2): After the propane contact treatment, the supply gas is changed from propane to a single-component gas of 100% carbon dioxide, and the permeance of carbon dioxide permeating the zeolite membrane when a single-component gas of 100% carbon dioxide is supplied to the surface of the zeolite membrane under the conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C is defined as P2.

[0016] The second invention of the present invention is a method for separating or concentrating a mixed gas, which includes at least carbon dioxide and a hydrocarbon and has a pressure of 1 MPa or more at a normal temperature or at 35° C., and causes a gas component with high permeability to permeate from the mixed gas, and the zeolite membrane composite has a zeolite membrane formed on a porous support, and has a permeance of methane of P under conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 40° C. CH4 , the permeance of sulfur hexafluoride is P SF6 In this case, P CH4 ≦3.02×P SF6 +8.19×10 -9 The present invention relates to a method for separating or concentrating a mixed gas, which satisfies the above requirements. The second invention may be dependent on the first invention.

[0017] In the first and second aspects of the present invention, the zeolite constituting the zeolite membrane preferably has a pore structure with eight or fewer oxygen ring members. Effect of the Invention

[0018] According to the new findings of the present inventors, when propane is supplied to a zeolite membrane surface under specified conditions, a zeolite membrane composite in which the carbon dioxide permeance after the supply of propane is 70% or more of the carbon dioxide permeance before the supply of propane has a high carbon dioxide permeance retention rate even in an actual gas test. Also, a zeolite membrane composite in which the methane permeance and sulfur hexafluoride permeance under specified conditions satisfy a specified relationship has a high carbon dioxide permeance retention rate even in an actual gas test. In other words, according to the method for separating or concentrating a mixed gas disclosed herein, high permeance can be maintained even in actual gas tests. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a schematic diagram of a measurement device used for gas separation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The following describes in more detail the embodiments of the present invention. However, the description of the components disclosed below is an example of an embodiment, and the present invention is not limited to these contents, and can be implemented in various modifications within the scope of the gist of the present invention.

[0021] In the following explanation, permeance (also called "permeability") is the amount of permeating substance divided by the product of the membrane area, time, and the partial pressure difference between the supply side and the permeation side of the permeating substance, and its unit is [mol (m 2 s Pa) -1 ].

[0022] 1. Method for separating or concentrating mixed gases The method for separating or concentrating a mixed gas disclosed herein is a method for separating or concentrating a mixed gas, which includes at least carbon dioxide and a hydrocarbon, and has a pressure of 1 MPa or more at a normal temperature or 35°C, and allows a gas component with high permeability to permeate from the mixed gas. A mixed gas having a pressure of 1 MPa or more at a normal temperature or 35°C is defined as a high-pressure gas as defined in the High Pressure Gas Safety Act, and the normal temperature refers to a temperature in a state in which a container, device, etc. is normally used. One feature of the method disclosed herein is that a specific zeolite membrane composite is used. That is, in the method disclosed herein, the zeolite membrane composite has a P2 / P1 ratio of 0.7 or more, where P1 is the carbon dioxide permeance in a carbon dioxide permeation test (1) before the following propane contact treatment, and P2 is the carbon dioxide permeance in a carbon dioxide permeation test (2) after the following propane contact treatment. It is more preferably 0.74 or more, even more preferably 0.75 or more, even more preferably 0.78 or more, and particularly preferably 0.8 or more.

[0023] Carbon dioxide permeation test (1): When a single-component gas of 100% carbon dioxide is supplied to the surface of the zeolite membrane under the conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C, the permeance of carbon dioxide that permeates the zeolite membrane is defined as P1.

[0024] Propane contact treatment: After the carbon dioxide permeation test (1), the supply gas is changed from a single component gas of 100% carbon dioxide to propane, and propane is supplied to the surface of the zeolite membrane under conditions of a supply gas pressure of 0.1 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C to replace the carbon dioxide with the propane, and then propane is supplied to the surface of the zeolite membrane for 30 minutes under conditions of a supply gas pressure of 0.4 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C.

[0025] Carbon dioxide permeation test (2): After the propane contact treatment, the supply gas is changed from propane to a single-component gas of 100% carbon dioxide, and the permeance of carbon dioxide permeating the zeolite membrane when a single-component gas of 100% carbon dioxide is supplied to the surface of the zeolite membrane under the conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C is defined as P2.

[0026] 1.1.Zeolite membrane composite The zeolite membrane composite used in the method of the present disclosure has a zeolite membrane formed on a porous support. Preferred embodiments of the porous support and the zeolite membrane are described below.

[0027] 1.1.1. Porous support The porous support may be any support (inorganic porous support) that is chemically stable enough to crystallize zeolite into a membrane on its surface, etc. and is made of inorganic porosity. Examples of the porous support include sintered ceramics (ceramic supports) such as silica, α-alumina, γ-alumina, mullite, zirconia, titania, yttria, silicon nitride, and silicon carbide, sintered metals such as iron, bronze, and stainless steel, glass, and carbon molded bodies.

[0028] Among these porous supports, inorganic porous supports (ceramic supports) containing sintered ceramics, which are solid materials whose basic components or most of which are composed of inorganic nonmetallic substances, are preferred. The use of such supports is expected to enhance adhesion through bonding with zeolite.

[0029] Specifically, examples of the ceramic sintered body (ceramic support) include silica, alumina such as α-alumina and γ-alumina, mullite, zirconia, titania, yttria, silicon nitride, silicon carbide, etc. Among them, inorganic porous supports containing at least one of alumina, silica, and mullite are preferred. If these supports are used, partial zeolite formation is easy, so that the bond between the support and zeolite is strong, and a dense membrane with high separation performance is easily formed.

[0030] The shape of the porous support is not particularly limited as long as it has a zeolite membrane that can effectively separate and concentrate the mixed gas. Specific examples of the shape of the porous support include flat, tubular, honeycomb, and monolithic supports having a large number of cylindrical, columnar, or prismatic holes.

[0031] In the zeolite membrane composite of the present disclosure, zeolite is formed in a membrane on such a porous support, i.e., on the surface of the support. The surface of the porous support may be polished with a file or the like as necessary. The surface of the porous support means the surface portion where zeolite is crystallized, and may be any surface or multiple surfaces depending on the shape of the support. For example, in the case of a cylindrical support, it may be the outer surface or the inner surface, or in some cases, both the outer and inner surfaces.

[0032] The average pore size of the porous support surface is not particularly limited, but it is preferable that the pore size is controlled. The average pore size of the support surface is usually 0.02 μm or more, preferably 0.05 μm or more, more preferably 0.1 μm or more, and usually 20 μm or less, preferably 10 μm or less, more preferably 5 μm or less. When the average pore size is equal to or more than the lower limit, the permeation amount tends to be large, and when it is equal to or less than the upper limit, the strength of the support itself is less problematic, and the proportion of pores on the support surface is small, and a dense zeolite membrane tends to be formed. The porous support does not substantially have adsorption performance for gas. That is, the gas passes through the pores in the porous support.

[0033] The average thickness (wall thickness) of the porous support is usually 0.1 mm or more, preferably 0.3 mm or more, more preferably 0.5 mm or more, and usually 7 mm or less, preferably 5 mm or less, more preferably 4 mm or less, and even more preferably 3 mm or less. The support is used for the purpose of imparting mechanical strength to the zeolite membrane, and when the average thickness of the support is equal to or greater than the lower limit, the zeolite membrane composite has sufficient strength and tends to be resistant to impact, vibration, and the like. When the average thickness of the support is equal to or less than the upper limit, the diffusion of the permeated substance tends to be good, and the permeability tends to be high.

[0034] The porosity of the porous support is usually 20% or more, preferably 25% or more, more preferably 30% or more, and usually 70% or less, preferably 60% or less, more preferably 50% or less. The porosity of the support affects the permeation flow rate when separating gas, and if it is above the lower limit, the diffusion of the permeant tends to be less hindered, while if it is below the upper limit, the strength of the support tends to be improved.

[0035] 1.1.2.Zeolite membrane The components constituting the zeolite membrane may include, as necessary, inorganic binders such as silica and alumina, organic compounds such as polymers, or materials containing Si atoms (silylation agents) that modify the zeolite surface as described below in detail. The zeolite membrane of the present invention may also include a portion of amorphous components. Furthermore, it may include a metal that is applied to the zeolite surface as described below in detail.

[0036] As the zeolite, aluminosilicates are preferable from the viewpoint that they can be synthesized in a wide range and tend to form a membrane with a composition suitable for separation.

[0037] The thickness of the zeolite membrane is not particularly limited, but is usually 0.1 μm or more, preferably 0.6 μm or more, more preferably 1.0 μm or more, and is usually 100 μm or less, preferably 60 μm or less, more preferably 20 μm or less. If the membrane thickness is too large, the permeation amount tends to decrease, and if it is too small, the selectivity and membrane strength tend to decrease. The particle size of the zeolite is not particularly limited, but if it is too small, the number of grain boundaries increases, which tends to reduce the permeability selectivity. It is usually 30 nm or more, preferably 50 nm or more, more preferably 100 nm or more, and the upper limit is equal to or less than the thickness of the membrane. Furthermore, it is particularly preferable that the particle size of the zeolite is the same as the thickness of the membrane.

[0038] The method for measuring the particle size is not particularly limited, but for example, the particle size can be measured by observing the surface of the zeolite membrane with an SEM, observing the cross section of the zeolite membrane with an SEM, or observing the zeolite membrane with a TEM.

[0039] The SiO2 / Al2O3 molar ratio of the zeolite membrane itself is usually 2 or more, preferably 5 or more, more preferably 8 or more, even more preferably 10 or more, even more preferably 15 or more, particularly preferably 20 or more, especially preferably 25 or more, especially preferably 30 or more, and preferably 2000 or less, more preferably 1000 or less, even more preferably 500 or less, especially preferably 100 or less, especially preferably 70 or less. When the SiO2 / Al2O3 molar ratio of the zeolite membrane is within this range, the membrane is excellent in separating the above-mentioned mixed gas from the viewpoint of hydrophilicity and hydrophobicity.

[0040] The SiO2 / Al2O3 molar ratio of the zeolite membrane itself is a value obtained by scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX). In SEM-EDX, by measuring with an electron beam acceleration voltage of about 10 kV, information on the membrane of only a few microns can be obtained. Since the zeolite membrane is formed uniformly, the SiO2 / Al2O3 molar ratio of the membrane itself can be obtained by this measurement.

[0041] The zeolite constituting the zeolite membrane preferably contains a zeolite having a pore structure of 12 or less oxygen rings, more preferably contains a zeolite having a pore structure of 10 or less oxygen rings, even more preferably contains a zeolite having a pore structure of 8 or less oxygen rings, and particularly preferably contains a zeolite having a pore structure of 6 to 8 oxygen rings. The value of n of the zeolite having n oxygen rings here indicates the zeolite with the largest number of oxygen atoms among the pores composed of oxygen and T elements (elements other than oxygen constituting the framework) that form the zeolite framework. For example, when pores of 12 oxygen rings and 8 oxygen rings exist as in the case of MOR type zeolite, it is considered to be a zeolite having 12 oxygen rings.

[0042] Examples of zeolites having a pore structure with 12 or less oxygen ring members include AEI, AEL, AFI, AFG, ANA, ATO, BEA, BRE, CAS, CDO, CHA, CON, DDR, DOH, EAB, EPI, ERI, ESV, EUO, FAR, FAU, FER, FRA, HEU, GIS, GIU, GME, GOO, ITE, KFI, LEV, LIO, LOS, LTA, LTL, LTN, MAR, MEP, MER, MEL, MON, MOR, MSO, MTF, MTN, MTW, MWF, MWW, NON, NES, OFF, PAU, PHI, RHO, RTE, RTH, RUT, SGT, SOD, STI, STT, TOL, TON, TSC, UFI, VNI, WEI, and YUG.

[0043] Among these, examples of zeolites having a pore structure with 10 or less oxygen ring members include AEI, AEL, AFG, ANA, BRE, CAS, CDO, CHA, DDR, DOH, EAB, EPI, ERI, ESV, EUO, FAR, FER, FRA, HEU, GIS, GIU, GOO, ITE, KFI, LEV, LIO, LOS, LTA, LTN, MAR, MEP, MER, MEL, MON, MSO, MTF, MTN, MWF, MWW, NON, NES, PAU, PHI, RHO, RTE, RTH, RUT, SGT, SOD, STI, STT, TOL, TON, TSC, UFI, VNI, WEI, and YUG.

[0044] Furthermore, examples of zeolites having a pore structure with 8 or less oxygen ring members include AEI, AFG, ANA, BRE, CAS, CDO, CHA, DDR, DOH, EAB, EPI, ERI, ESV, FAR, FRA, GIS, GIU, GOO, ITE, KFI, LEV, LIO, LOS, LTA, LTN, MAR, MEP, MER, MON, MSO, MTF, MTN, MWF, NON, PAU, PHI, RHO, RTE, RTH, RUT, SGT, SOD, TOL, TSC, UFI, VNI, and YUG.

[0045] Among these, examples of zeolites having an oxygen 6- to 8-membered ring structure include AEI, AFG, ANA, CHA, EAB, ERI, ESV, FAR, FRA, GIS, ITE, KFI, LEV, LIO, LOS, LTA, LTN, MAR, MWF, PAU, RHO, RTH, SOD, TOL, and UFI.

[0046] In the zeolite membrane composite of the present disclosure, from the viewpoint of adjusting the zeolite pore size so that carbon dioxide can easily diffuse in the zeolite pores and hydrocarbons are unlikely to enter the pores, a structure having an oxygen 6- to 8-membered ring structure and three-dimensionally connected pores is preferred. That is, preferred structures of the main zeolite constituting the zeolite membrane are AEI, AFG, CHA, EAB, ERI, ESV, FAR, FRA, GIS, ITE, KFI, LEV, LIO, LOS, LTN, MAR, PAU, RHO, RTH, SOD, TOL, and UFI, more preferred structures are AEI, CHA, ERI, KFI, LEV, PAU, RHO, RTH, and UFI, even more preferred structures are CHA, RHO, and MWF, particularly preferred structures are CHA and MWF, and most preferred structure is CHA.

[0047] In this specification, the structure of zeolite is shown by the code defining the structure of zeolite defined by the International Zeolite Association (IZA) as described above.

[0048] In addition, the framework density (T / 1000Å) of the main zeolite constituting the zeolite membrane was 3 ) is not particularly limited, but is usually 17 or less, preferably 16 or less, more preferably 15.5 or less, particularly preferably 15 or less, and is usually 10 or more, preferably 11 or more, more preferably 12 or more.

[0049] The framework density is the density of 1000Å of zeolite. 3This means the number of elements (T elements) other than oxygen that make up the framework per unit area, and this value is determined by the structure of the zeolite. The relationship between framework density and the structure of zeolite is shown in ATLAS OF ZEOLITE FRAMEWORK TYPES Sixth Revised Edition 2007 ELSEVIER.

[0050] By having a framework density of at least the lower limit, the zeolite structure is prevented from becoming fragile, the durability of the zeolite membrane is increased, and the membrane can be easily applied to various applications. On the other hand, by having a framework density of at most the upper limit, the diffusion of substances in the zeolite is not hindered, and the permeation flux of the zeolite membrane tends to be high, which is economically advantageous.

[0051] The extent of penetration of the zeolite membrane into the porous support, as a weighted average value of the distance from the support surface, is usually 4 μm or less, preferably 3.5 μm or less, more preferably 3.0 μm or less, even more preferably 2.7 μm or less, particularly preferably 2.5 μm or less, especially preferably 2.2 μm or less, and is preferably 0.01 μm or more, more preferably 0.02 μm or more, even more preferably 0.03 μm or more.

[0052] The distance between the end of the zeolite membrane, which penetrates from the surface into the support as a continuum, and the support surface is calculated using an SEM image of a cross section smoothed with a cross-section polisher. The support surface is determined by distinguishing the zeolite from the support using one of the following methods, and the boundary between them is determined to be the support surface. 1) Contrast difference in SEM images 2) Difference in Si and Al signal intensity ratio in EDS mapping 3) Differences in shape change due to etching rate

[0053] The end of the zeolite membrane that penetrates as a continuum is the part where the support void first appears on the perpendicular line from the support surface to the inside of the membrane. If possible, it is desirable to calculate the distance for the maximum number of pixel units relative to the support surface. For simplicity, it is also possible to calculate the distance at 1 μm pitch relative to the support surface.

[0054] As long as such a porous support-zeolite membrane composite can be obtained, any method may be used for production, but it is preferable to apply the following method.

[0055] The composite with suppressed penetration can be obtained by a method of synthesizing a zeolite membrane after adhering inorganic particles on a porous support. The elements constituting the adhering inorganic particles are not particularly limited, but preferably contain Si or Al. Si and Al are constituent elements of zeolite, and are thought to have little effect on the composition of the obtained zeolite membrane and to cause no inhibition of membrane growth. The adhering material may function as a raw material for the zeolite membrane during the membrane formation process and become part of the zeolite membrane. Preferred types of inorganic particles to be adhering include fumed silica, colloidal silica, amorphous aluminum silicate gel, alumina sol, sodium aluminate, aluminum hydroxide, aluminum sulfate, aluminum nitrate, aluminum oxide, amorphous aluminosilicate gel, etc., more preferred are fumed silica, colloidal silica, and alumina sol, and most preferred is fumed silica.

[0056] The zeolite membrane can be produced by a conventionally known method, but in order to produce a uniform membrane, it is particularly preferred to produce it by hydrothermal synthesis.

[0057] For example, a zeolite membrane can be prepared by placing a reaction mixture for hydrothermal synthesis (hereinafter sometimes referred to as an "aqueous reaction mixture"), the composition of which has been adjusted and made uniform, into a heat-resistant and pressure-resistant vessel such as an autoclave with a porous support loosely fixed inside, sealing the vessel, and heating for a certain period of time.

[0058] The aqueous reaction mixture contains a Si element source, an Al element source, an alkali source, and water, and may further contain an organic template as necessary.

[0059] Examples of the silicon source that can be used in the aqueous reaction mixture include amorphous silica, colloidal silica, silica gel, sodium silicate, amorphous aluminum silicate gel, tetraethoxysilane (TEOS), and trimethylethoxysilane.

[0060] Examples of the Al element source that can be used include sodium aluminate, aluminum hydroxide, aluminum sulfate, aluminum nitrate, aluminum oxide, amorphous aluminosilicate gel, etc. In addition to the Al element source, other element sources, such as Ga, Fe, B, Ti, Zr, Sn, and Zn, may also be included.

[0061] In the crystallization of zeolite, an organic template (structure directing agent) can be used as necessary. By synthesizing using an organic template, the ratio of silicon atoms to aluminum atoms in the crystallized zeolite increases, improving acid resistance and water vapor resistance.

[0062] The organic template may be of any type as long as it can form a desired zeolite membrane. In addition, one type of organic template may be used, or two or more types may be used in combination.

[0063] When the zeolite is a CHA type, the organic template is usually an amine or a quaternary ammonium salt. For example, the organic templates described in U.S. Pat. No. 4,544,538 and U.S. Patent Publication No. 2008 / 0075656 are preferred.

[0064] The alkali source used in the aqueous reaction mixture may be a hydroxide ion of the counter anion of the organic template, an alkali metal hydroxide such as NaOH or KOH, or an alkaline earth metal hydroxide such as Ca(OH)2. The type of alkali counter cation is not particularly limited, and Na, K, Li, Rb, Cs, Ca, Mg, Sr, Ba, or the like is usually used. Among these, Li, Na, and K are preferred, and it is more preferred to contain at least K. In addition, two or more types of alkali may be used in combination, and specifically, it is preferred to use Na and K, or Li and K in combination. The counter cation added here contributes to the growth of zeolite crystals, and is incorporated into the entire zeolite membrane as the zeolite membrane grows.

[0065] The ratio of the Si element source to the Al element source in the aqueous reaction mixture is usually expressed as the molar ratio of the oxides of each element, that is, the SiO2 / Al2O3 molar ratio. The SiO2 / Al2O3 molar ratio is not particularly limited, but is usually 5 or more, preferably 8 or more, more preferably 10 or more, and even more preferably 15 or more. In addition, it is usually 10,000 or less, preferably 1,000 or less, more preferably 300 or less, and even more preferably 100 or less.

[0066] When the SiO2 / Al2O3 molar ratio is within this range, the zeolite membrane is dense and has high separation performance. Furthermore, since the zeolite has a moderate amount of Al atoms, separation performance is improved for gas and liquid components that are adsorbed by Al. Furthermore, when Al is within this range, a zeolite membrane with high resistance to acid and water vapor is obtained.

[0067] The ratio of the silica source to the organic template in the aqueous reaction mixture, expressed as the molar ratio of the organic template to SiO (organic template / SiO molar ratio), is usually 0.005 or more, preferably 0.01 or more, more preferably 0.02 or more, and is usually 1 or less, preferably 0.4 or less, more preferably 0.2 or less.

[0068] When the organic template / SiO2 molar ratio is within the above range, a dense zeolite membrane can be produced, and the produced zeolite has high resistance to acid and water vapor. In the present invention, "dense" means "few defects", and a zeolite having gaps between crystal particles even if highly crystalline, particularly a zeolite having particle gaps larger than the pore size of the zeolite, in which the gaps are the main permeation path for the gas to be separated in the zeolite membrane, and therefore the separation effect due to the molecular sieve action cannot be fully obtained in the separation of a gas mixture, does not fall under the category of "dense membrane" according to the present invention. On the other hand, even if the crystallinity is somewhat low, if the crystal particles are densely packed together, it can be considered a "dense film."

[0069] The ratio of the Si element source to the alkali source is M (2 / n) The molar ratio of O / SiO2 (wherein M represents an alkali metal or an alkaline earth metal, and n represents its valence of 1 or 2) is usually 0.02 or more, preferably 0.04 or more, more preferably 0.05 or more, and usually 0.5 or less, preferably 0.4 or less, more preferably 0.3 or less. M (2 / n) The preferred range of O / SiO2 is desirably adjusted as appropriate depending on the SiO2 / Al2O3 molar ratio in the aqueous mixture, and the upper limit when the SiO2 / Al2O3 molar ratio is greater than 30 is 0.20 or less, more preferably 0.12 or less, even more preferably 0.09 or less, even more preferably 0.08 or less, and even more preferably 0.07 or less. When expressed as an M / Si molar ratio (M is an alkali metal or alkaline earth metal), the monovalent alkali metal has a value twice the above value, and the divalent alkaline earth metal has the same value as above.

[0070] The ratio of the Si element source to water, in terms of the molar ratio of water to SiO (H2O / SiO2 molar ratio), is usually 10 or more, preferably 30 or more, more preferably 40 or more, and particularly preferably 50 or more, and is usually 1000 or less, preferably 500 or less, more preferably 200 or less, and particularly preferably 150 or less.

[0071] When the molar ratios of the materials in the aqueous reaction mixture are within these ranges, dense zeolite membranes can be produced. The amount of water is particularly important in producing dense zeolite membranes, and conditions in which the water content is higher relative to the silica content than those typically used in powder synthesis methods tend to produce dense membranes.

[0072] Furthermore, in hydrothermal synthesis, it is not necessary to have seed crystals in the reaction system, but adding seed crystals can promote the crystallization of zeolite on the support. The method of adding seed crystals is not particularly limited, and can include a method of adding seed crystals to an aqueous reaction mixture, as in the synthesis of powdered zeolite, or a method of attaching seed crystals to a support.

[0073] When producing a zeolite membrane composite, it is preferable to attach seed crystals to the support in advance, which facilitates the production of a dense zeolite membrane with good separation performance.

[0074] The method for attaching the seed crystals to the support is not particularly limited, and examples of methods that can be used include a dip method in which the seed crystals are dispersed in a solvent such as water and the support is immersed in the dispersion to attach the seed crystals, and a method in which the seed crystals are mixed with a solvent such as water to form a slurry or the seed crystals themselves are applied to the support. The dip method is desirable in order to control the amount of attached seed crystals and produce a membrane composite with good reproducibility.

[0075] The solvent in which the seed crystals are dispersed is not particularly limited, and water or various organic solvents can be used. The pH may be adjusted by adding an acid or alkali to water. When the ratio of the Si element source to the Al element source in the aqueous reaction mixture is relatively low, i.e., when SiO2 / Al2O3 is 30 or less, it is preferable to use seed crystals to which an alkali has been added in order to obtain a zeolite membrane with good gas permeability. When SiO2 / Al2O3 is greater than 30, there is no particular limit, but water is particularly preferable in terms of ease of handling.

[0076] The amount of seed crystals to be dispersed is not particularly limited, and is usually 0.01 mass% or more, preferably 0.1 mass% or more, more preferably 0.3 mass% or more, relative to the total mass of the dispersion, and is usually 20 mass% or less, preferably 10 mass% or less, more preferably 5 mass% or less, even more preferably 4 mass% or less, and particularly preferably 3 mass% or less.

[0077] If the amount of dispersed seed crystals is too small, the amount of seed crystals attached to the support is small, so that there are some areas on the support where zeolite is not generated during hydrothermal synthesis, which may result in a defective film. Since the amount of seed crystals attached to the support by the dipping method becomes almost constant when the amount of seed crystals in the dispersion liquid is equal to or exceeds a certain level, if the amount of seed crystals in the dispersion liquid is too large, a lot of seed crystals are wasted, which is disadvantageous in terms of cost.

[0078] It is preferable to attach seed crystals to a support by dipping or by applying a slurry, and then dry the support before forming the zeolite membrane.

[0079] The amount of seed crystals to be attached to the support in advance is not particularly limited. 2 The mass per unit area is usually 0.01 g or more, preferably 0.05 g or more, more preferably 0.1 g or more, and usually 100 g or less, preferably 50 g or less, more preferably 10 g or less, and even more preferably 8 g or less.

[0080] If the amount of seed crystals is less than the lower limit, crystals are difficult to form, and the membrane may grow insufficiently or unevenly. If the amount of seed crystals exceeds the upper limit, the seed crystals may increase the surface unevenness, or the seed crystals that fall off the support may easily cause spontaneous nuclei to grow, inhibiting membrane growth on the support. In either case, it tends to be difficult to produce a dense zeolite membrane.

[0081] When forming a zeolite membrane on a support by hydrothermal synthesis, there is no particular limitation on the method of immobilizing the support, and any form can be used, such as vertical placement, horizontal placement, etc. In this case, the zeolite membrane may be formed by a static method, or the zeolite membrane may be formed by stirring the aqueous reaction mixture.

[0082] The temperature for forming the zeolite membrane is not particularly limited, but is usually 100° C. or higher, preferably 120° C. or higher, more preferably 150° C. or higher, and usually 200° C. or lower, preferably 190° C. or lower, more preferably 180° C. or lower. If the reaction temperature is too low, the zeolite may be difficult to crystallize. If the reaction temperature is too high, a type of zeolite different from the zeolite of the present invention may be easily produced.

[0083] The heating time is not particularly limited, but is usually 1 hour or more, preferably 5 hours or more, more preferably 10 hours or more, and usually 10 days or less, preferably 5 days or less, more preferably 3 days or less, and more preferably 2 days or less. If the reaction time is too short, the zeolite may be difficult to crystallize. If the reaction time is too long, a type of zeolite different from the desired zeolite may be easily produced.

[0084] The pressure during the formation of the zeolite membrane is not particularly limited, and the autogenous pressure that occurs when the aqueous reaction mixture placed in a sealed container is heated to this temperature range is sufficient. Furthermore, an inert gas such as nitrogen may be added as necessary.

[0085] The zeolite membrane composite obtained by hydrothermal synthesis is washed with water, and then heat-treated and dried. Here, the heat treatment means drying the zeolite membrane composite by applying heat, or calcining the organic template when an organic template is used.

[0086] The temperature of the heat treatment, when aimed at drying, is usually 50° C. or higher, preferably 80° C. or higher, more preferably 100° C. or higher, and usually 200° C. or lower, preferably 150° C. or lower. When aimed at calcining the organic template, the temperature is usually 350° C. or higher, preferably 400° C. or higher, more preferably 430° C. or higher, even more preferably 480° C. or higher, and usually 900° C. or lower, preferably 850° C. or lower, more preferably 800° C. or lower, even more preferably 750° C. or lower.

[0087] If the purpose is to calcinate the organic template, if the heat treatment temperature is too low, the proportion of the organic template remaining will tend to be high, resulting in fewer pores in the zeolite, which may reduce the permeability during separation and concentration. If the heat treatment temperature is too high, the difference in thermal expansion coefficient between the support and the zeolite will be large, which may lead to the zeolite membrane being more susceptible to cracks, causing the zeolite membrane to lose its denseness and reducing its separation performance.

[0088] The heating time is not particularly limited as long as the zeolite membrane is sufficiently dried or the organic template is calcined, and is preferably 0.5 hours or more, more preferably 1 hour or more. The upper limit is not particularly limited, and is usually within 200 hours, preferably within 150 hours, more preferably within 100 hours. When the purpose is to calcinate the organic template, the heat treatment may be performed in an air atmosphere, but may also be performed in an atmosphere containing an inert gas such as N2 or oxygen.

[0089] When the hydrothermal synthesis is carried out in the presence of an organic template, it is appropriate to wash the obtained zeolite membrane composite with water and then remove the organic template by, for example, a heat treatment or extraction, preferably by a heat treatment, i.e., calcination.

[0090] The heating rate during the heat treatment for calcining the organic template is desirably as slow as possible to reduce the difference in thermal expansion coefficient between the support and the zeolite that causes cracks in the zeolite membrane. The heating rate is usually 5°C / min or less, preferably 2°C / min or less, more preferably 1°C / min or less, and particularly preferably 0.5°C / min or less. In consideration of workability, the heating rate is usually 0.1°C / min or more.

[0091] In addition, the rate of temperature drop after firing must also be controlled to avoid cracking of the zeolite membrane. As with the rate of temperature rise, the slower the better. The rate of temperature drop is usually 5°C / min or less, preferably 2°C / min or less, more preferably 1°C / min or less, and particularly preferably 0.5°C / min or less. In consideration of workability, the rate is usually 0.1°C / min or more.

[0092] The zeolite membrane may be ion-exchanged as necessary. When the membrane is synthesized using an organic template, the ion exchange is usually carried out after removing the organic template. By carrying out ion exchange, the effective pore size, effective volume, and adsorption characteristics can be adjusted according to the size of the ions used. The ions to be exchanged can be selected according to the zeolite pore size, the amount of ion exchange sites, and the size of the target separation gas. Examples of ions to be exchanged include protons, Na + , K + , Li + Alkali metal ions such as Ca 2+ , Mg 2+ , Sr 2+ , B.A. 2+ ions of Group 2 elements such as Fe and Cu, ions of transition metals such as Al, Ga, and Zn, and ions of other metals such as Al, Ga, and Zn. Preferred are Group 2 element ions, and more preferred are Ca 2+ The metal ions introduced by ion exchange and the metals attached to the zeolite membrane surface to enhance the carbon dioxide adsorption performance described below have different effects. The Al that forms the zeolite framework is Si 4+ Al 3+Since Al has a low valence, a negative charge is generated, but the metal ions introduced by ion exchange exist in the zeolite pores near the Al atoms introduced into the zeolite framework to keep the charge neutral. After the ion exchange treatment, the treatment solution remaining on the zeolite membrane surface is washed, and metal ions that do not have electrostatic interactions with the zeolite framework are removed. Therefore, when gas molecules diffuse inside the zeolite membrane, it affects the size of the zeolite pore size and the adsorption of gas molecules, and affects the molecular sieving ability and permeability coefficient of the zeolite membrane, but has little effect on the adsorption and desorption of gas molecules on the zeolite membrane surface. On the other hand, the metal attached to the zeolite membrane surface described later is attached to the zeolite membrane surface by coating or the like, and is uniformly held on the zeolite membrane surface regardless of whether the charge of the zeolite framework is compensated for or not. Although it does not affect the behavior of gas molecules inside the zeolite, by adsorbing and desorbing specific gas molecules on the surface of the zeolite membrane, it is expected that in the separation of mixed gases containing multiple gas species, it will contribute to the adsorption of specific gas molecules onto the zeolite membrane surface, thereby improving the permeability of those gas species.

[0093] Ion exchange may be performed by treating the zeolite membrane after calcination (when an organic template is used, for example) with an aqueous solution containing ammonium salts such as NH4NO3 and NaNO3 or ions to be exchanged, or in some cases with an acid such as hydrochloric acid, usually at room temperature to 100°C, followed by washing with water. The degree of ion exchange can be controlled by appropriately selecting the ion concentration of the aqueous solution, the treatment temperature, and the treatment time. Since ion exchange occurs at the point where ions come into contact, it is considered that ion exchange occurs near the surface of the membrane in a short treatment, and ion exchange progresses inside the membrane, i.e., in the membrane thickness direction, as the treatment time is extended. The degree of ion exchange can be appropriately adjusted depending on the desired membrane performance. The SiO2 / Al2O3 molar ratio of the zeolite membrane to be ion-exchanged is not particularly limited, but the lower the SiO2 / Al2O3 molar ratio, the more likely it is that the effect of ion exchange can be obtained from the viewpoint of the number of ions exchanged. After ion exchange, the membrane is usually dried, but may be further calcined at 200°C to 500°C as necessary. By calcining, chemical species derived from anions that could not be completely removed by washing, such as NO3 - If the remaining anion-derived chemical species are causing permeation resistance, they can be removed by calcination, improving the permeation performance. In addition, when ion exchange is performed with NH4NO3, the NH4 + Ion to H + It can be changed to ion. H + By changing to an ion, the ions inside the pores become smaller, and the effective pore volume increases, which can improve permeability. When removing remaining anions, a gas containing oxygen is preferable from the viewpoint of being able to remove them by oxidation, and air is preferable from the viewpoint of ease of handling.

[0094] The air permeability [L / (m 2 ·h)] is usually 1400L / (m 2 ·h) or less, preferably 1000 L / (m 2 ·h), and more preferably 700L / (m 2 ·h), and more preferably 600L / (m2 ·h), and more preferably 500 L / (m 2 ·h), and particularly preferably 300 L / (m 2 ·h), most preferably 200 L / (m 2 The lower limit of the permeation amount is not particularly limited, but is usually 0.01 L / (m 2 ·h) or more, preferably 0.1L / (m 2 ·h), and more preferably 1L / (m 2 h) or more.

[0095] Here, the air permeability is the amount of air permeated [L / (m 2 ·h).

[0096] In the present invention, from the viewpoint of high gas permeability, it is preferable that the zeolite membrane composite has an X-ray diffraction pattern obtained by irradiating the membrane surface with X-rays in which the peak intensity at about 2θ=17.9° is less than 0.5 times the peak intensity at about 2θ=20.8°.

[0097] Here, the peak intensity refers to the measured value minus the background value. In terms of the peak intensity ratio (hereinafter sometimes referred to as "peak intensity ratio A") expressed as (peak intensity around 2θ=17.9°) / (peak intensity around 2θ=20.8°), it is usually less than 0.5, preferably 0.45 or less. There is no particular lower limit, but it is usually 0.001 or more.

[0098] In addition, in the present invention, from the viewpoint of high gas permeability, it is preferable that the peak intensity at about 2θ=9.6° in the X-ray diffraction pattern is 2.0 to 4.0 times the peak intensity at about 2θ=20.8°.

[0099] The peak intensity ratio (hereinafter sometimes referred to as "peak intensity ratio B"), expressed as (peak intensity around 2θ=9.6°) / (peak intensity around 2θ=20.8°), is usually 2.0 or more, preferably 2.1 or more, more preferably 2.3 or more, and particularly preferably 2.5 or more. The upper limit is usually less than 4.0, preferably 3.9 or less, more preferably 3.7 or less, and particularly preferably 3.5 or less.

[0100] The X-ray diffraction pattern referred to here is obtained by irradiating the surface on which the zeolite is mainly attached with X-rays from a CuKα radiation source, with the scanning axis set to θ / 2θ. The shape of the sample to be measured may be any shape that allows X-ray irradiation to the surface on which the zeolite of the membrane composite is mainly attached, and it is preferable to use the membrane composite as it is or cut it to an appropriate size limited by the apparatus, as it clearly shows the characteristics of the membrane composite.

[0101] The X-ray diffraction pattern here may be measured by fixing the irradiation width using an automatic variable slit when the surface of the zeolite membrane composite is curved. The X-ray diffraction pattern when an automatic variable slit is used refers to a pattern that has been subjected to variable-to-fixed slit correction.

[0102] Here, the peak near 2θ=17.9° refers to the maximum peak that is not derived from the substrate and exists in the range of 17.9°±0.6°.

[0103] The peak near 2θ=20.8° refers to the maximum peak that is not derived from the substrate and exists in the range of 20.8°±0.6°.

[0104] The peak near 2θ=9.6° refers to the maximum peak that is not derived from the substrate and exists in the range of 9.6°±0.6°.

[0105] In the X-ray diffraction pattern, the peak at 2θ=9.6° is due to the plane with indices (1,0,0) in the CHA structure, and the peak at 2θ=17.9° is due to the plane with indices (1,1,1) in the CHA structure.

[0106] 1.1.3. Carbon dioxide permeability and retention In the zeolite membrane composite of the present disclosure, when the permeance of carbon dioxide permeating the zeolite membrane in the carbon dioxide permeation test (1) before the above-mentioned propane contact treatment is P1, and the permeance of carbon dioxide permeating the zeolite membrane in the carbon dioxide permeation test (2) after the above-mentioned propane contact treatment is P2, it is important that P2 / P1 is 0.7 or more. 0.74 or more is more preferable, 0.75 or more is even more preferable, 0.78 or more is even more preferable, and 0.8 or more is particularly preferable. According to the new findings of the present inventors, a zeolite membrane composite that can ensure a maintenance rate of carbon dioxide permeance of 0.7 or more, i.e., 70% or more, after the propane contact treatment compared to before the treatment, has a small decrease in permeance even when applied to the separation or concentration of real gas containing impurities. If it is 0.74 or more, i.e., 74% or more, the effect is more pronounced, if it is 0.75 or more, i.e., 75%, the effect is even more pronounced, if it is 0.78 or more, i.e., 78% or more, the effect is even more pronounced, and if it is 0.8 or more, i.e., 80% or more, the effect is particularly remarkable. For this reason, the method of the present disclosure is suitable, for example, for separating and concentrating high-pressure natural gas into hydrocarbons and carbon dioxide contained in the natural gas.

[0107] The zeolite membrane composite of the present disclosure has a permeance P1 in the above carbon dioxide permeation test (1) of, for example, 1.0 × 10 -8 mol (m 2 s Pa) -1 Above 1.0×10 -4 mol (m 2 s Pa) -1 The lower limit is preferably 1.0×10 or less. -7 mol (m 2s Pa) -1 More preferably, the upper limit is 1.0×10 -5 mol (m 2 s Pa) -1 When the carbon dioxide permeability of the zeolite membrane composite is in such a range, at least carbon dioxide can be more appropriately separated or concentrated from a mixed gas in an actual gas test.

[0108] In the above carbon dioxide permeation tests (1) and (2), the flow rate of carbon dioxide (linear velocity at the zeolite membrane surface) is not particularly limited. This is because, when a single component gas is permeated through a zeolite membrane composite, the gas permeance is constant as long as the "pressure difference between the supply gas and the permeating gas (or the supply gas pressure and the permeating gas pressure, respectively)" and the "temperature" are clear.

[0109] In the above-mentioned propane contact treatment, the propane replacement time is not particularly limited. This is because the supply side pressure and the permeation side pressure are equal to 0.1 MPa during propane replacement, and therefore the deterioration of the zeolite membrane due to propane does not substantially occur (even if it does occur, it is negligible). In the propane contact treatment, the flow rate of propane (linear velocity at the zeolite membrane surface) is not particularly limited. If the two conditions of the differential pressure between the supply gas and the permeation gas (or the supply gas pressure and the permeation gas pressure, respectively) and the temperature are the same, the change in the zeolite membrane composite due to the propane contact treatment will be substantially the same. By carrying out the above-mentioned propane contact treatment, it is possible to confirm the extent to which propane partially or completely penetrates into the zeolite pores and inhibits the permeation of carbon dioxide. The small decrease in carbon dioxide permeance in this test means that the zeolite pores are controlled to a size that does not allow propane to enter, and it is clear that the zeolite membrane composite is capable of maintaining high permeance in actual gas tests in which impurities are present.

[0110] 1.1.4. Methane permeability and sulfur hexafluoride permeability The zeolite membrane composite of the present disclosure has a methane permeance of P under the conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 40° C. CH4 , the permeance of sulfur hexafluoride is P SF6 In this case, P CH4 ≦3.02×P SF6 +8.19×10 -9 It is preferable that P CH4 ≦3.02×P SF6 +7.19×10 -9 , more preferably P CH4 ≦3.02×P SF6 +6.19×10 -9 More specifically, the zeolite membrane composite of the present disclosure is prepared by, for example, supplying a single-component gas of 100% carbon dioxide to the surface of a zeolite membrane under conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 40° C., drying the membrane until the amount of carbon dioxide permeation is stabilized, changing the supply gas to methane, and supplying methane to the surface of the zeolite membrane under conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 40° C., and defining the permeance of methane permeating through the zeolite membrane when the amount of methane permeation is stabilized as P CH4 The supply gas was changed from methane to sulfur hexafluoride, and sulfur hexafluoride was supplied to the surface of the zeolite membrane under the conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 40°C. When the amount of sulfur hexafluoride permeated was stabilized, the permeance of sulfur hexafluoride permeating the zeolite membrane was defined as P SF6 In this case, P CH4 ≦3.02×P SF6 +8.19×10 -9 It is preferable that P CH4 ≦3.02×P SF6 +7.19×10 -9 , more preferably P CH4 ≦3.02×P SF6 +6.19×10 -9Here, 3.02 is the permeance ratio of methane to sulfur hexafluoride in the Knudsen diffusion region. It is known that when the width of the defects in the zeolite membrane is small, the gas molecules that permeate the defects undergo Knudsen diffusion. Since sulfur hexafluoride permeates only the defects in the zeolite membrane, the permeance of methane that permeates the defects is 3.02×P SF6 Here, defects refer to the gaps between zeolite particles, so small defects mean that the gaps between zeolite particles are small, and large defects mean that the gaps between zeolite particles are large. Therefore, P CH4 From 3.02 x P SF6 The value obtained by subtracting , that is, the intercept of the above equation, can be regarded as the permeance of methane passing through the zeolite pores. It is thought that the larger the zeolite pore diameter, the easier it is for methane to pass through the pores, so this value will be larger, and the smaller the zeolite pore diameter, the more difficult it is for methane to pass through the pores, so this value will be smaller. From the above, P CH4 and P SF6 In a zeolite membrane composite that satisfies this relationship, the permeance of methane passing through the zeolite pores is sufficiently small, and the pore size of the zeolite membrane is controlled to a size that does not allow hydrocarbons such as methane to enter, making it easy to maintain high permeance in actual gas tests.

[0111] The present inventors speculate that there are two factors that reduce the permeance in a high-pressure test in which a real gas such as natural gas is to be separated and concentrated: (i) the adsorption of gas (e.g., hydrocarbons, particularly hydrocarbons with 2 or more carbon atoms, such as propane) near the surface of the zeolite membrane, which causes the pores to be blocked; and (ii) the adsorption of gas (e.g., hydrocarbons, particularly hydrocarbons with 2 or more carbon atoms, such as propane) inside the pores of the zeolite membrane, which causes the pores to be blocked. According to the findings of the present inventors, a zeolite membrane composite that can maintain a carbon dioxide permeance of 70% or more before and after contact treatment with propane can avoid the blocking of pores by hydrocarbons near the surface of the zeolite membrane in a high-pressure test in which a real gas such as natural gas is to be separated and concentrated. If the permeance is 74% or more, the effect is more pronounced, if the permeance is 75%, the effect is even more pronounced, if the permeance is 78% or more, the effect is even more pronounced, and if the permeance is 80% or more, the effect is particularly pronounced. Furthermore, it can be said that the zeolite membrane composite having the above-mentioned methane permeability and sulfur hexafluoride permeability has a pore size controlled within the most preferable range, and can more appropriately suppress the intrusion of propane, etc. into the pores of the zeolite membrane.

[0112] 1.1.5. Carbon dioxide adsorption performance The zeolite membrane composite of the present disclosure has a carbon dioxide desorption amount per unit area of ​​the zeolite membrane of 0.085 μmol / cm under specified conditions. 2 As described above, one of the features of the zeolite membrane is that it has a high carbon dioxide adsorption property and also has a high desorption property of the adsorbed carbon dioxide.

[0113] The carbon dioxide adsorption performance of the zeolite membrane is evaluated by heating the membrane composite to desorb the carbon dioxide adsorbed in the zeolite membrane and measuring the amount of carbon dioxide desorbed per membrane area. Specifically, the measurement is performed as follows.

[0114] First, the area of ​​the zeolite membrane of the zeolite membrane composite used for the measurement is calculated. For example, when the zeolite membrane composite is a circular tube and a membrane is formed on the outside of the tube, the membrane area is calculated from the outer diameter and length of the zeolite membrane composite. When the tube is split vertically for measurement, each length can be measured using calipers to calculate the membrane area. In the case of a monolith type, the membrane area is calculated from the inner diameter and length of the hole in which the membrane is formed.

[0115] The zeolite membrane composite to be measured is left in contact with the air at room temperature (20°C) for more than 5 hours, and then the zeolite membrane composite is placed in a chamber and He is flowed from a cylinder at atmospheric pressure and room temperature at 40cc / min. While He is flowing at 40cc / min, the chamber is heated and the temperature is raised from room temperature at a rate of 40°C / min. The components desorbed from the membrane during the temperature rise are measured by MS, and the amount of M / z44 (μmol / g) detected between 100°C and 300°C is calculated. The calculation is performed by introducing a specified amount of CO2 gas into the measurement path in a pulse to create a calibration curve of the gas volume and area after each measurement, and introducing the area of ​​M / z44 obtained in this measurement into this. The MS detection value is output at least once per second.

[0116] Here, the chamber is cylindrical with a diameter of 12 mm, a length of 250 mm or less, and a wall thickness of 1.2 mm or less, and is made of quartz. Heating is performed by infrared heating. The thermometer is connected to the center of the infrared irradiation part of the quartz chamber and measures the temperature outside the sample.

[0117] In the zeolite membrane composite of the present disclosure, the amount of carbon dioxide desorption per unit area of ​​the zeolite membrane obtained as described above is 0.085 μmol / cm 2 or more, preferably 0.10 μmol / cm 2 More preferably, 0.115 μmol / cm 2 More preferably, 0.130 μmol / cm 2 More preferably, 0.145 μmol / cm 2 More preferably, 0.160 μmol / cm 2There is no particular upper limit, but it is preferably 0.3 μmol / cm 2 Less than or equal to 0.2 μmol / cm 2 The following is the result.

[0118] 1.1.6. Carbon dioxide permeability In the zeolite membrane composite of the present disclosure, when a single-component gas of 100% carbon dioxide is used at a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and temperatures of the zeolite membrane and the single-component gas of 30° C., and the permeance of carbon dioxide permeating through the zeolite membrane when the amount of carbon dioxide permeated is stabilized is P1, and then the supply gas is changed to a mixed gas of carbon dioxide and nitrogen in a molar ratio of 50:50, and the mixed gas is supplied at a pressure of 0.4 MPa so that the linear velocity at the zeolite membrane surface is 60 cm / s, the permeation gas pressure is set to 0.1 MPa, and the temperatures of the zeolite membrane and the mixed gas are set to 30° C., and the permeance of carbon dioxide permeating through the zeolite membrane is P2, it is preferable that P2 / P1 is 0.75 or more. Compared to a single-component gas of 100% carbon dioxide, in a mixed gas of carbon dioxide and nitrogen, while the nitrogen also enters the pores, it is thought that the permeance of carbon dioxide decreases because the nitrogen permeates slower than carbon dioxide. The effect of carbon dioxide adsorption is easier to see when a gas that easily enters the pores is used than when a gas that does not easily enter the pores is used, so the strength of carbon dioxide adsorption and desorption can be confirmed more reliably. As described above, the zeolite membrane composite of the present disclosure has improved carbon dioxide adsorption performance, and therefore can maintain high carbon dioxide permeation performance of the zeolite membrane when separating or concentrating a mixed gas containing carbon dioxide.

[0119] In this way, the zeolite separation membrane of the present disclosure has excellent carbon dioxide adsorption and desorption properties, and therefore can achieve both practically sufficient processing capacity and separation performance when separating or concentrating a mixed gas containing carbon dioxide.

[0120] When the zeolite separation membrane of the present disclosure is used for separating or concentrating a mixed gas containing carbon dioxide, carbon dioxide can be efficiently separated or concentrated, and a gas enriched with a desired component can be produced. In this case, the mixture to be separated or concentrated can be, for example, a mixture containing at least one component selected from oxygen, nitrogen, methane, ethane, ethylene, propane, propylene, normal butane, isobutane, 1-butene, 2-butene, isobutene, sulfur hexafluoride, helium, carbon monoxide, nitric oxide, water, etc., and carbon dioxide. In particular, in addition to carbon dioxide, a mixed gas containing methane and helium, a mixed gas containing nitrogen dioxide, etc. can be used for separating or concentrating air, natural gas, combustion gas, coke oven gas, biogas such as landfill gas generated from a garbage landfill, steam reformed gas of methane generated and discharged in the petrochemical industry, etc. The conditions for separating or concentrating these mixed gases may be known conditions according to the target gas species, composition, etc.

[0121] 1.1.7. Surface treatment of zeolite membrane According to the new findings of the present inventors, a zeolite membrane composite capable of maintaining carbon dioxide permeability when separating or concentrating a real gas can be realized by appropriately controlling the pore size of the zeolite membrane. For example, it can be easily obtained by other methods such as a method of imparting metal species to the zeolite membrane surface or a surface treatment such as silylation treatment. That is, the manufacturing method of the zeolite membrane composite of the present disclosure preferably includes a step of forming a zeolite membrane on a porous support and a step of imparting metal species to the surface of the zeolite membrane or performing a surface treatment such as silylation treatment. Furthermore, in the manufacturing method of the zeolite membrane composite of the present disclosure, it is preferable to control the amount of metal species imparted to the zeolite membrane surface so as to satisfy the above-mentioned carbon dioxide permeability and methane permeability. As described above, it is considered that the intrusion of hydrocarbons and the like into the pores can be suppressed by narrowing the pore size of the zeolite membrane by imparting metal species near the zeolite membrane surface, and the blocking of the pores by hydrocarbons can be further suppressed. In addition, since narrowing the pore size of zeolite usually makes it difficult for gas molecules to diffuse through the zeolite pores, it is expected that the permeability of the zeolite membrane will decrease if the above-mentioned treatment is performed over the entire thickness direction of the zeolite membrane. This treatment has the advantage that the pore size at the outermost surface of the zeolite membrane, where the gas to be separated first comes into contact with the zeolite membrane, can be appropriately controlled to suppress the intrusion of hydrocarbons and the like into the pores while maintaining high permeability of the entire zeolite membrane. Here, the outermost surface means about several tens of nm from the outer surface to the inside of the zeolite membrane. The treatment may be performed to a depth of several tens of nm or more, but the permeability tends to decrease.

[0122] The method of applying metal species to the zeolite membrane surface is not particularly limited, but includes a method of applying metal by vapor deposition, a method of applying metal by sputtering, and a method of applying a solution in which a metal salt is dissolved. Methods of applying a solution in which a metal salt is dissolved include a dipping method, a coating method, a spraying method, and the like. From the viewpoint of uniform application at low cost, a method of dipping into an aqueous metal salt solution is preferred. In order to improve separation performance while preventing a decrease in permeation performance, when applying metal species to the zeolite membrane surface, it is preferable to treat only the side of the zeolite membrane that faces the gas to be separated. When the zeolite membrane is formed on a tubular support, for example, the upper and lower ends of the membrane composite are capped to prevent the aqueous solution containing ions from entering the support, and then the dip treatment can be performed to treat only the side that faces the gas to be separated.

[0123] The silylation method is not particularly limited, but may be, as in the case of metal treatment, a method of dipping in a liquid containing silylation, a method of coating, a method of spraying, etc. Also, depending on the boiling point of the silylation agent, silylation can be performed in the gas phase. From the viewpoint of ease of adsorption of carbon dioxide, it is preferable to use a silylation agent having an amino group. For example, aminopropyltriethoxysilane, aminopropyltriethoxysilane, aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, etc. are used.

[0124] The type of metal can be appropriately selected depending on the combination of the pore size and ion size of the zeolite, but when it is desired to change the pore size significantly, a metal with a large size is preferable, and alkali metals and alkaline earth metals in the 6th, 5th, and 4th periods are preferable. When it is desired to slightly adjust the pores, alkali metals, alkaline earth metals, and transition metals in the 2nd and 3rd periods are preferable. For example, Li, Na, K, Rb, Cs, Mg, Ca, Ba, Sr, La, Ti, Zr, Hr, V, Nb, Ta, Cr, Mo, W, Fe, Ni, Pd, Pt, Cu, Ga, etc. are used. The type of metal can be appropriately selected depending on the combination of the pore size and ion size of the zeolite, but when it is desired to change the pore size significantly, a metal with a large size is preferable, and alkali metals and alkaline earth metals in the 6th, 5th, and 4th periods are preferable. When it is desired to slightly adjust the pores, alkali metals, alkaline earth metals, and transition metals in the 2nd and 3rd periods are preferable.

[0125] The metal species to be attached are preferably those that have carbon dioxide adsorption properties in the metal or metal compound itself, those that enter the ion exchange site of the zeolite as ions and exhibit carbon dioxide adsorption properties, and those that act with the silanol of the zeolite and exhibit carbon dioxide adsorption properties. From this viewpoint, Li, Cs, Mg, Ca, Ba, Sr, La, and Cu are preferred. Furthermore, from the viewpoint of exhibiting basicity as an oxide and adding the function of adsorbing carbon dioxide, Mg and Ca are more preferred, and Ca is particularly preferred, in that they are Group 2 elements and have a low CO2 desorption temperature. Two or more of these metals may be used in combination. When two or more types are used in combination, the two or more metal species may be applied to the zeolite membrane simultaneously or sequentially. The location of the metal species and the presence or absence of cross-linking in the zeolite pores vary depending on the type of zeolite and the type of metal species used. CH4 ≦3.02×P SF6 +8.19×10 -9 It is preferable to use these in appropriate combination so as to satisfy the above.

[0126] When a metal salt solution is applied to a zeolite membrane, the type of salt is not particularly limited, and can be nitrates, nitrites, sulfates, sulfites, hydrochlorides, carbonates, acetates, phosphates, carboxylates, etc. The salt can be selected in consideration of the required solubility, and among these, nitrates, sulfates, and hydrochlorides are preferred from the viewpoint of the pH being close to neutral.

[0127] The solvent for dissolving the metal salt is not particularly limited as long as it can dissolve the metal salt, but usually, water, alcohols such as methanol, ethanol, propanol, etc., and ketones such as dimethyl ketone, methyl ethyl ketone, diethyl ketone, etc. can be used. These solvents may be used alone or in combination in any ratio.

[0128] When a metal salt solution is applied, the metal salt concentration of the solution is not particularly limited, but is usually 0.001M or more, preferably 0.005 or more, more preferably 0.01 or more, even more preferably 0.02M or more, particularly preferably 0.03M or more, and particularly preferably 0.05M or more. If the concentration is too low, the amount of metal attached may be insufficient, and carbon dioxide adsorption may not be sufficient. In addition, although there is no particular upper limit, the amount of metal attached may be excessive, resulting in a decrease in permeability or uneven attachment, so that the concentration is usually 20M or less, preferably 15M or less, more preferably 10M or less, and even more preferably 5M or less.

[0129] Usually, after the metal salt solution is applied, a drying process is carried out to evaporate the solution. The drying temperature is not limited, but is usually 20°C or higher, preferably 30°C or higher, and usually 200°C or lower, preferably 150°C or lower. If the temperature is too low, drying takes a long time and may not be sufficient. If the temperature is too high, the adsorption performance may change. The drying time is not particularly limited, but from the viewpoint of sufficiently evaporating the solvent and preventing a change in the adsorption performance, it is preferably from 30 minutes to 5 hours, more preferably 3 hours or less.

[0130] After drying, it can be heated as necessary. Heat treatment can change the state of the metal and the interaction with the zeolite membrane, and can sometimes change the adsorption performance to a favorable state. If the metal species are left without washing, heating can remove the water of crystallization if the metal species has water of crystallization, remove the anion species, and even cause a change to an oxide. If the oxidation reaction is the objective, it is performed with a gas containing oxygen, but air is preferable from the viewpoint of ease of handling. If oxidation is not to occur, the heat treatment can be performed using an inert gas. Examples of inert gas that can be used include N2 and He. Air and an inert gas can be mixed to adjust the rate of the oxidation reaction.

[0131] The temperature in the heat treatment is usually 120°C or higher, preferably 150°C or higher, more preferably 180°C or higher, and usually 900°C or lower, preferably 850°C or lower, more preferably 800°C or lower, and even more preferably 750°C or lower. If the heating temperature is too low, the adsorption performance may not be changed sufficiently, and if the heat treatment temperature is too high, the difference in the thermal expansion coefficient between the support and the zeolite becomes large, which may lead to cracks in the zeolite membrane, and the denseness of the zeolite membrane may be lost, resulting in a decrease in separation performance. In addition, if the heat treatment temperature is too high, the adsorption performance may change in an unintended direction. Since the physical properties, such as the temperature at which the metal becomes an oxide, vary depending on the metal chemical species, an appropriate temperature can be set within the above range depending on the combination of zeolite and metal.

[0132] The heating time may be adjusted appropriately depending on the metal species and the location of the metal, but is usually 30 minutes or more, preferably 1 hour or more, and more preferably 2 hours or more. There is no particular upper limit, but it is usually 72 hours or less, preferably 60 hours or less, and more preferably 48 hours or less. For the purpose of oxidation treatment, contact with oxygen is necessary, but if the effective pore size is small and oxygen permeation is slow, a long heating treatment may be required.

[0133] 1.2. Gas Mixtures In the separation or concentration method of the present disclosure, the mixed gas to be separated or concentrated contains at least carbon dioxide and hydrocarbons. Using the separation or concentration method of the present disclosure, a gas enriched with a desired component can be produced. Examples of components other than carbon dioxide and hydrocarbons include at least one component selected from oxygen, nitrogen, sulfur hexafluoride, helium, carbon monoxide, nitric oxide, water, and the like. Among these gas components, gas components with high permeance permeate the zeolite membrane composite and are separated, and gas components with low permeance are concentrated in the supply gas side.

[0134] Here, permeance (also called "permeability") is the amount of permeating substance divided by the product of the membrane area, time, and the partial pressure difference between the supply side and the permeation side of the permeating substance, and its unit is [mol (m 2 s Pa) -1 ].

[0135] The mixed gas preferably contains at least carbon dioxide, a hydrocarbon having two or more carbon atoms, and methane, and more preferably contains at least carbon dioxide, propane, and methane. Specific examples of the mixed gas include natural gas, air, combustion gas, coke oven gas, biogas such as landfill gas generated from a garbage landfill, and steam reformed methane gas generated and discharged in the petrochemical industry. In particular, it is preferable to use the mixed gas for separation or concentration of natural gas.

[0136] 1.3. An example of separation or concentration of mixed gas using a zeolite membrane composite As described above, in the method for separating or concentrating a mixed gas of the present disclosure, the mixed gas is contacted with the zeolite membrane composite, and a gas component with high permeability is permeated from the mixed gas. For example, a mixed gas containing carbon dioxide or the like is contacted with one side of the support side or the zeolite membrane side of the zeolite membrane composite, and the pressure on the opposite side is set lower than that on the side in contact with the mixed gas, thereby selectively allowing a substance with high permeability (a substance in the mixed gas with relatively high permeability) to permeate the zeolite membrane from the mixed gas, that is, as a main component of the permeating substance. This allows the substance with high permeability to be separated from the mixed gas. As a result, the concentration of a specific component (a substance in the mixed gas with relatively low permeability) in the mixed gas can be increased, and the specific component can be separated, recovered, or concentrated.

[0137] As described above, the zeolite membrane composite of the present disclosure can maintain high permeance even in actual gas tests, i.e., it can adequately exhibit separation and concentration performance even for mixed gases that contain impurities and are under high pressure, such as natural gas.

[0138] The zeolite membrane of the zeolite membrane composite of the present disclosure has high permeability to, for example, carbon dioxide, and therefore it is believed that by contacting a high-pressure mixed gas containing carbon dioxide and the like with the zeolite membrane for separation, the concentration of carbon dioxide in the mixed gas containing carbon dioxide and the like can be reduced and components other than carbon dioxide can be concentrated.

[0139] The conditions for separating and concentrating these mixed gases may be known per se depending on the target gas species, composition, etc.

[0140] The form of the separation membrane module having a zeolite membrane composite used for separating a mixed gas may be a flat membrane type, a spiral type, a hollow fiber type, a cylindrical type, a honeycomb type, etc., and the most suitable form is selected according to the application. Hereinafter, a form in which a cylindrical separation membrane module, which is one of the preferred forms, is used to separate or concentrate a mixed gas, will be described.

[0141] In Fig. 1, a cylindrical zeolite membrane composite 1 is placed in a thermostatic bath (not shown) while being housed in a stainless steel pressure-resistant container 2. The thermostatic bath is equipped with a temperature control device so that the temperature of the sample gas can be adjusted.

[0142] One end of the cylindrical zeolite membrane composite 1 is sealed with a circular end pin 3. The other end is connected to a connection part 4, and the other end of the connection part 4 is connected to a pressure-resistant vessel 2. The inside of the cylindrical zeolite membrane composite 1 is connected to a pipe 10 for discharging a permeation gas 8 via the connection part 4, and the pipe 10 extends to the outside of the pressure-resistant vessel 2. A pressure gauge 5 for measuring the pressure on the gas supply side is connected to any point leading to the pressure-resistant vessel 2. Each connection part is connected airtightly.

[0143] When separating or concentrating a mixed gas, the mixed gas 7 is supplied between the pressure vessel 2 and the zeolite membrane composite 1 at a constant flow rate, and the pressure on the supply side is kept constant by the back pressure valve 6. Some components of the mixed gas 7 permeate the zeolite membrane composite 1 according to the partial pressure difference between the inside and outside of the zeolite membrane composite 1, and are discharged as exhaust gas 8 to the outside of the pressure vessel 2 through a pipe 10. On the other hand, the components of the mixed gas that do not permeate the zeolite membrane composite 1 are recovered as they are to the outside of the pressure vessel 2 as a concentrated mixed gas.

[0144] The temperature for gas separation from a mixed gas is in the range of 0 to 500° C. In view of the separation characteristics of the membrane, a temperature in the range of room temperature to 150° C. is preferable.

[0145] 2. Supplementary Information In the above explanation, the technology of the present disclosure has been described as a "method for separating or concentrating a mixed gas". On the other hand, one feature of the technology of the present disclosure is the constitution and structure of the zeolite membrane composite as an object. That is, the zeolite membrane composite of the present disclosure is characterized in that, when the carbon dioxide permeance in the carbon dioxide permeation test (1) before the above-mentioned propane contact treatment is P1 and the carbon dioxide permeance in the carbon dioxide permeation test (2) after the above-mentioned propane contact treatment is P2, P2 / P1 is 0.7 or more. In addition, the zeolite membrane composite of the present disclosure has a methane permeance under the conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 40°C of P CH4 , the permeance of sulfur hexafluoride is P SF6 In this case, P CH4 ≦3.02×P SF6 +8.19×10 -9 The preferred embodiment of the zeolite membrane composite is as described above, and detailed description thereof will be omitted here. EXAMPLES

[0146] The method for separating or concentrating a mixed gas using a zeolite membrane composite and the zeolite membrane composite will be described in more detail below with reference to examples, but the method of the present disclosure is not limited to the following examples as long as it does not deviate from the gist of the method. Note that the values ​​of various production conditions and evaluation results in the following examples can be said to have the meaning of preferred upper or lower limit values ​​in the embodiment of the method of the present disclosure, and the preferred range may be a range defined by a combination of the above upper or lower limit values ​​and the values ​​of the following examples or values ​​between the examples.

[0147] 1. Preparation of Zeolite Membrane Composite [Example 1] Aluminum hydroxide (containing 53.5% by mass of Al2O3, manufactured by Aldrich) was added to 1 mol / L-NaOH aqueous solution and 1 mol / L-KOH aqueous solution, and stirred to dissolve, and then demineralized water was added and stirred to obtain a transparent solution. An aqueous solution of N,N,N-trimethyl-1-adamantanammonium hydroxide (hereinafter referred to as "TMADAOH") (containing 25% by mass of TMADAOH, manufactured by Seichem Co., Ltd.) was added as an organic template, and colloidal silica (Snowtech-40, manufactured by Nissan Chemical Co., Ltd.) was added and stirred for 30 minutes or more to obtain an aqueous reaction mixture.

[0148] The composition (molar ratio) of this aqueous reaction mixture is SiO2 / Al2O3 / NaOH / KOH / H2O / TMADAOH=1 / 0.014 / 0.02 / 0.08 / 100 / 0.04, and SiO2 / Al2O3=70.

[0149] As the inorganic porous support, a porous alumina tube (outer diameter 12 mm, inner diameter 8 mm) was used which had been washed with desalted water and then dried.

[0150] The seed crystals used were CHA-type zeolite crystallized by hydrothermal synthesis for 2 days at 160° C. in a gel composition (molar ratio) of SiO2 / Al2O3 / NaOH / KOH / H2O / TMADAOH=1 / 0.033 / 0.1 / 0.06 / 20 / 0.07. The seed crystals were dispersed in water at 1% by mass, and the support was immersed for a predetermined time in the dispersion to attach the seed crystals by a dipping method, and the support surface was rubbed.

[0151] The support with the seed crystals attached was immersed vertically in a reaction vessel containing the aqueous reaction mixture, the reaction vessel was sealed, and the mixture was heated at 180°C for 15 hours under autogenous pressure in a stationary state. At that time, the ratio of the aqueous reaction mixture to the support was about 600 g of the aqueous reaction mixture per 1 m of the support, and the entire support was in contact with the aqueous reaction mixture. After a predetermined time had passed, the zeolite membrane composite was taken out of the aqueous reaction mixture after being left to cool, washed, and dried at 120°C for 1 hour or more.

[0152] The obtained CHA-type zeolite membrane composite was treated to attach Ca to the membrane surface. Calcium nitrate tetrahydrate was dissolved in demineralized water to prepare a 0.1M calcium nitrate aqueous solution. The zeolite membrane composite was placed in the prepared 0.1M calcium nitrate aqueous solution with plugs at the top and bottom of the membrane to prevent the calcium nitrate aqueous solution from entering the inside of the support, immersed for 1 minute, and then removed. It was then air-dried and dried at 100°C for 1 hour. It was then heated in air at 400°C for 2 hours.

[0153] [Example 2] A zeolite membrane composite was produced in the same manner as in Example 1, except that, when performing the treatment of adhering Ca to the membrane surface of the CHA-type zeolite membrane composite, the concentration of the calcium nitrate aqueous solution was set to 1 M and heating was performed in air at 250°C for 48 hours.

[0154] [Example 3] A zeolite membrane composite was produced in the same manner as in Example 1, except that heating in air was performed at 250°C for 48 hours when performing the treatment for adhering Ca to the membrane surface of the CHA-type zeolite membrane composite.

[0155] [Example 4] A zeolite membrane composite was produced in the same manner as in Example 1, except that the composition of the aqueous reaction mixture into which the support with the attached seed crystals was immersed was SiO2 / Al2O3 / NaOH / KOH / H2O / TMADAOH=1 / 0.025 / 0.024 / 0.097 / 100 / 0.04, SiO2 / Al2O3=40, and that the treatment of attaching Ca to the membrane surface of the obtained CHA-type zeolite membrane composite was not performed.

[0156] [Example 5] A treatment for attaching Na to the membrane surface of the CHA-type zeolite membrane composite obtained in the same manner as in Example 1 was performed. A zeolite membrane composite was produced in the same manner as in Example 1, except that sodium nitrate was used instead of calcium nitrate and the concentration of the aqueous sodium nitrate solution was set to 1M.

[0157] [Example 6] A zeolite composite membrane was produced in the same manner as in Example 1, except that calcium acetate was used instead of calcium nitrate and the concentration of the aqueous calcium acetate solution was 1M.

[0158] [Example 7] Instead of carrying out a treatment to attach Ca to the membrane surface of the CHA-type zeolite membrane composite obtained in the same manner as in Example 1, K ion exchange was carried out on the zeolite membrane of the CHA-type zeolite membrane composite. A zeolite membrane composite was produced in the same manner as in Example 1, except that K nitrate was used instead of Ca nitrate, the concentration of the K nitrate aqueous solution was 0.1 M, the zeolite membrane composite was not plugged during the immersion operation, the entire composite was immersed in the entire K nitrate aqueous solution at 90°C for 1 hour, and the immersed composite was washed with running water before air drying.

[0159] [Example 8] The membrane surface of the CHA-type zeolite membrane composite obtained in the same manner as in Example 1 was modified with N-(2-aminoethyl)-3-aminopropyltrimethoxysilane instead of performing a treatment to attach Ca to the membrane surface of the CHA-type zeolite membrane composite. N-(2-aminoethyl)-3-aminopropyltrimethoxysilane was dissolved in ethanol to prepare a 0.1 wt% N-(2-aminoethyl)-3-aminopropyltrimethoxysilane ethanol solution. The prepared solution was applied to the membrane surface of the zeolite membrane composite, air-dried, and then dried at 100°C for 1 hour. It was further heated in air at 360°C for 1 hour and 15 minutes.

[0160] [Comparative Example 1] A zeolite membrane composite was produced in the same manner as in Example 1, except that the treatment for adhering Ca to the membrane surface of the CHA-type zeolite membrane composite was not performed.

[0161] [Comparative Example 2] By adding the CHA-type zeolite used as the seed crystals in Example 1 to an aqueous reaction mixture under the conditions for synthesizing the seed crystals in Example 1, seed crystals of CHA-type zeolite having about twice the particle size of the seed crystals used in Example 1 were obtained. A zeolite membrane composite was produced in the same manner as in Example 1, except that a CHA-type zeolite membrane composite was obtained using this as the seed crystals and no treatment for adhering Ca was performed.

[0162] 2. Performance evaluation of zeolite membrane composite 1, various gas permeation tests were carried out on the CHA-type zeolite membrane composites according to Examples 1 to 8 and Comparative Examples 1 and 2. The sample gases used were CO2 (liquefied carbon dioxide gas, manufactured by Toho Oxygen Industries Co., Ltd.), C3H8 (liquefied propane gas, manufactured by Sumitomo Seika Chemicals Co., Ltd.), CH4 (compressed pure methane gas G1 grade, manufactured by Japan Fine Products Co., Ltd.), and SF6 (liquefied sulfur hexafluoride gas, manufactured by Kanto Denka Kogyo Co., Ltd.).

[0163] In the apparatus of FIG. 1, a cylindrical zeolite membrane composite 1 is placed in a thermostatic chamber (not shown) while being housed in a stainless steel pressure vessel 2. The thermostatic chamber is equipped with a temperature control device so that the temperature of the sample gas can be adjusted. One end of the cylindrical zeolite membrane composite 1 is sealed with a circular end pin 3. The other end is connected to a connection part 4, and the other end of the connection part 4 is connected to the pressure vessel 2. The inside of the cylindrical zeolite membrane composite 1 is connected to a pipe 10 for discharging the permeated gas via the connection part 4, and the pipe 10 extends to the outside of the pressure vessel 2. In addition, a pressure gauge 5 for measuring the pressure on the supply side of the mixed gas and a back pressure valve 6 for adjusting the pressure on the supply side are connected to any point leading to the pressure vessel 2. Each connection part is airtightly connected. When separating or concentrating a mixed gas, the mixed gas 7 is supplied between the pressure vessel 2 and the zeolite membrane composite 1 at a constant pressure, and the permeated gas 8 that has permeated the zeolite membrane composite 1 is measured by a flow meter (not shown) connected to a pipe. In order to remove components such as moisture and air, the mixture is dried at a temperature equal to or higher than the measurement temperature, and purged by exhaust or with the supply gas to be used. The sample temperature and the differential pressure between the supply gas 7 side and the permeated gas 8 side of the zeolite membrane composite 1 are kept constant, and after the permeated gas flow rate has stabilized, the flow rate of the sample gas (permeated gas 8) that has permeated the zeolite membrane composite 1 is measured, whereby the gas permeance [mol·(m 2 s Pa) -1 The pressure difference between the supply side and the permeation side of the supply gas (differential pressure) is used when calculating the permeance.

[0164] 2.1. CH4 permeation test and SF6 permeation test In the following test, gas species with molecular diameters smaller and larger than the zeolite pores were used to determine the permeance of gas that only penetrated the zeolite pores. Since gas species with molecular diameters smaller than the zeolite pores penetrate the zeolite pores and the gaps between zeolite particles, the gas permeance obtained by measurement is the sum of the permeance of gas that penetrates the zeolite pores and the permeance of gas that penetrates the gaps between zeolite particles. On the other hand, gas species with molecular diameters larger than the zeolite pores have a gas amount that penetrates the zeolite pores of 0, so the gas permeation amount obtained by measurement can be regarded as the permeation amount of only gas that penetrated the gaps between zeolite particles. Here, the permeance of SF6, which has a molecular diameter larger than the zeolite pores, is used to calculate the gas permeance of CH4, which has a molecular diameter smaller than the zeolite pores, that penetrated the zeolite pores.

[0165] Prior to the calculation, the ratio of the permeance of carbon dioxide (CO2) to that of methane (CH4) (CO2 / CH4 permeance ratio) is measured to confirm whether the gaps between zeolite particles are sufficiently small. Both CO2 and CH4 are gas species with molecular diameters smaller than the zeolite pores, and if the zeolite membrane is sufficiently dense, separation occurs through the pores of the zeolite membrane, and CO2 shows a permeance two orders of magnitude higher than CH4 due to its molecular sieving ability. The CO2 / CH4 permeance ratio in the Knudsen diffusion region of CO2 and CH4 is 0.36, with CH4 having a smaller molecular weight showing a higher permeance. If the permeance ratio by membrane separation is greater than 0.36, it can be considered that separation occurs through the zeolite pores.

[0166] On the other hand, when the gaps between the particles of the zeolite membrane are large, it is in the region of normal molecular diffusion, and the permeance ratio is considered to be the ratio of the diffusion coefficients. The diffusion coefficients at 20°C and 1 atm are 1.6 for CO2 and 1.06 for CH4, respectively, so it is 1.5. Since the diffusion coefficient of an ideal gas is proportional to the 3 / 2 power of temperature and the -1 power of pressure, it is estimated that the ratio of the diffusion coefficients of CO2 and CH4 will be about 1.5 under the same temperature and pressure conditions. Therefore, when a zeolite membrane composite shows a CO2 / CH4 permeance ratio of more than 1.5, it is considered that separation occurs through the zeolite pores, and since the gaps between the zeolite particles can be assumed to be sufficiently small, it can be assumed that the permeation mechanism of each gas molecule through these gaps is dominated by Knudsen diffusion.

[0167] In this case, SF6, which has a molecular diameter larger than the zeolite pores, will only pass through the particle interfaces and will be dominated by Knudsen diffusion, while CH4 may pass through the zeolite pores as well as the particle interfaces, so will diffuse by both Knudsen diffusion and diffusion within the zeolite pores. If the zeolite pores are larger than 5.5 Å, the molecular diameter of SF6, then both CH4 and SF6 will pass through the pores and gaps between particles, but in that case, the CH4 / SF6 permeance ratio within the pores is thought to be greater than that dominated by Knudsen diffusion, so CH4 permeance is 3.02×P SF6 +8.19×10 -9 and is expected to be outside the preferred range.

[0168] The diffusion coefficient of gas molecules in the Knudsen diffusion region is generally d / 3×(8RT / πMW) 1 / 2Here, d is the diameter of the permeation path, R is the gas constant, T is the absolute temperature, π is the circular constant, and MW is the molecular weight of the diffusing gas molecule. If the ratio of the diffusion coefficients for two types of gas molecules is calculated and rearranged, the value becomes the reciprocal of the square root of the molecular weight of the two types of gas molecules. Therefore, the permeation rate ratio of CH4 molecules to SF6 molecules is calculated from the following formula (1). Since the permeation rate is the reciprocal of the square root of the molecular weight under Knudsen diffusion control, the following formula (1) indicates that the SF6 permeance in the gaps between particles is 3.02 times the permeance of CH4. MW SF6 1 / 2 / MW CH4 1 / 2 =3.02 (1) Here, MW in equation (1) SF6 and M.W. CH4 are the molecular weights of SF6 and CH4, respectively. Using the permeation rate ratio obtained from equation (1), the permeance of methane permeating the gaps between zeolite particles by Knudsen diffusion is 3.02P SF6 Therefore, the permeance P of CH4 that penetrated the zeolite pores is P can be calculated using the following formula (2). P P =P CH4 -3.02P SF6 (2) Here, P in formula (2) CH4 and P SF6 indicate the permeance of CH4 and SF6 calculated from the results of the single gas permeation tests described above, respectively.

[0169] Taking the above into consideration, a single component gas of 100% carbon dioxide was supplied to the surface of the zeolite membrane under the conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 40°C, and the amount of carbon dioxide permeated became stable (at this time, the permeance of carbon dioxide (P CO2After drying until the membrane was completely dried, the feed gas was changed to methane, and methane was fed to the surface of the zeolite membrane under the conditions of a feed gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 40°C. The permeance (P CH4 After that, the supply gas was changed from methane to sulfur hexafluoride, and sulfur hexafluoride was supplied to the surface of the zeolite membrane under the conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 40°C. When the amount of sulfur hexafluoride permeated was stabilized, the permeance (P SF6 ) was calculated. In addition, P CH4 and P SF6 From the calculation results, the permeance P of methane that permeated the pores of the zeolite membrane was P The results are shown in Table 1.

[0170] [Table 1]

[0171] As shown in Table 1, the zeolite membrane composites of Examples 1, 2, 5, and 6 had smaller permeance of methane permeating through the zeolite pores than the zeolite membrane composites of Comparative Examples 1 and 2. From Table 1 above, it can be seen that Examples 1, 2, and 5 had lower permeance of methane permeating through the zeolite pores. CH4 ≦3.02×P SF6 +6.19×10 -9 In Example 6, P CH4 ≦3.02×P SF6 +7.19×10 -9 The comparative example does not satisfy this relationship, and CH4 ≦3.02×P SF6 +8.19×10 -9 This is presumably because the zeolite pores are narrowed by the surface treatment of the metal species.

[0172] As shown in Table 1, the zeolite membrane composites of Examples 4 and 7 had smaller permeance of methane that permeated through the zeolite pores than the zeolite membrane composites of Comparative Examples 1 and 2. From Table 1 above, Example 7 had a lower permeance of methane than the zeolite membrane composites of Comparative Examples 1 and 2. CH4 ≦3.02×P SF6 +6.19×10 -9 In Example 4, P CH4 ≦3.02×P SF6 +8.19×10 -9 It can be seen that the above relationship is satisfied in the comparative example, but not in the comparative example. This is presumably due to the fact that the zeolite pore size is narrowed by the appropriate adjustment of the composition of the aqueous reaction mixture during the production of the zeolite membrane and by the metal cations introduced into the zeolite pores by the ion exchange treatment.

[0173] As shown in Table 1, the zeolite membrane composite of Example 8 had a smaller permeance of methane that permeated through the zeolite pores than the zeolite membrane composites of Comparative Examples 1 and 2. From Table 1 above, it can be seen that Example 8 had a smaller permeance of methane that permeated through the zeolite pores than the zeolite membrane composites of Comparative Examples 1 and 2. CH4 ≦3.02×P SF6 +6.19×10 -9 It can be seen that the relationship is satisfied in the comparative example, but not in the comparative example. This is presumably because the zeolite pores are narrowed by subjecting the surface of the zeolite membrane to a silylation treatment.

[0174] 2.2. Carbon dioxide permeation test before and after propane contact treatment 2.2.1. Carbon dioxide permeation test (1) As a pretreatment, the zeolite membrane composite was dried at 90°C by introducing carbon dioxide as a supply gas 7 between the cylinder of the pressure vessel 2 and the zeolite membrane composite 1, keeping the pressure at about 0.2 MPa, and setting the inside of the cylinder of the zeolite membrane composite 1 at 0.1 MPa until the amount of carbon dioxide permeation stabilized. From the amount of carbon dioxide permeating the zeolite membrane at this time, the carbon dioxide permeance (P1) was measured. The results are shown in Table 2 below.

[0175] 2.2.2. Propane contact treatment After the single component gas permeation test (1), the supply gas was changed from carbon dioxide to propane, and the atmosphere on the supply side and permeation side was replaced with propane by supplying propane to the inner and outer surfaces of the zeolite membrane under conditions of a supply gas pressure of 0.1 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C. Subsequently, propane was supplied to the inner and outer surfaces of the zeolite membrane for 30 minutes under conditions of a supply gas pressure of 0.4 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C.

[0176] 2.2.3. Carbon dioxide permeation test (2) After the propane contact treatment, the feed gas was changed from propane to a single-component gas of 100% carbon dioxide, and carbon dioxide was supplied to the inner and outer surfaces of the zeolite membrane for 5 minutes under conditions of a feed gas pressure of 0.1 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C, replacing the atmosphere on the feed side and permeation side with carbon dioxide. Carbon dioxide was then supplied to the surface of the zeolite membrane under conditions of a feed gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90°C, and the permeance (P2) of carbon dioxide permeating the zeolite membrane was measured. The results are shown in Table 2 below.

[0177] [Table 2]

[0178] As shown in Table 2, in the zeolite membrane composites of Comparative Examples 1 and 2, the carbon dioxide permeance after the propane contact treatment was reduced to less than 80% of that before the propane contact treatment. CH4 ≦3.02×P SF6 +6.19×10 -9 In the zeolite membrane composites of Examples 1 and 2, which satisfied the above relationship, the carbon dioxide permeance was maintained at 80% or more of that before the propane contact treatment even after the propane contact treatment. CH4 ≦3.02×P SF6 +7.19×10 -9The zeolite membrane composite of Example 4, which satisfied the above relationship, also had a carbon dioxide permeance after the propane contact treatment of 70% or more of that before the propane contact treatment. Also, it showed a higher maintenance rate than Comparative Examples 1 and 2. From this, it was confirmed that the effect was weaker than Examples 1 and 2, but that it was easy to maintain a high permeance.

[0179] In addition, the zeolite membrane composite of Example 3 also showed a carbon dioxide permeance after the propane contact treatment of 75% or more of that before the propane contact treatment, and showed a higher maintenance rate than those of Comparative Examples 1 and 2. From this, it was confirmed that, although the effect was weaker than that of Examples 1 and 2, there was a similar tendency for the permeance to be easily maintained.

[0180] 2.3. Mixed gas separation test In the surface treatment of zeolite membranes, the main purpose is to control the zeolite pore size, but depending on the selection of the substance and treatment method used in the surface treatment, it is possible to favorably impart carbon dioxide adsorption / desorption properties to the zeolite membrane surface and improve the carbon dioxide permeability. The following tests were conducted to confirm the imparting of carbon dioxide adsorption / desorption properties and the resulting improvement in carbon dioxide permeability. Mixed gas separation tests were conducted as follows using the device shown diagrammatically in Figure 1. The sample gases used were two types of gases mixed using a flow regulator at molar ratios of CO2 / N2 = 35 / 65 and CO2 / N2 = 50 / 50.

[0181] 1, a sample gas (supply gas 7) is supplied between a pressure vessel 2 and a zeolite membrane composite 1, the pressure of the sample gas is adjusted using a back pressure valve 6, and the flow rate of a permeated gas 8 that has permeated the zeolite membrane composite is measured using a flow meter (not shown) connected to a pipe 10. Furthermore, a portion of the permeated gas 8 is sampled and analyzed by gas chromatography to determine the gas composition.

[0182] More specifically, in order to remove components such as moisture and air, the sample is dried at a temperature equal to or higher than the measurement temperature, and then purged with exhaust or the supply gas to be used. After the sample temperature and the pressure difference between the supply gas 7 side and the permeation gas 8 side of the zeolite membrane composite 1 are kept constant, the permeation gas flow rate is stabilized, and the flow rate and gas composition of the sample gas (permeation gas 8) that has permeated the zeolite membrane composite 1 are measured, and the gas permeance [mol (m 2 s Pa) -1 The pressure of each gas used in calculating the permeance is the difference between the average partial pressure of the supply gas 7 and non-permeating gas 9 and the partial pressure of the permeating gas 8.

[0183] The ratio of the permeance of each gas, CO2 and N2, calculated based on the above measurement results can be calculated to obtain the permeance ratio.

[0184] [Example 9] The above single-component gas permeation test was carried out using the CHA-type zeolite membrane composite prepared under the same conditions as in Example 3. Specifically, as a pretreatment, the zeolite membrane composite was dried at 40°C by introducing carbon dioxide as the supply gas 7 between the cylinder of the pressure vessel 2 and the zeolite membrane composite 1, keeping the pressure at about 0.2 MPa, and setting the inside of the cylinder of the zeolite membrane composite 1 to 0.1 MPa (atmospheric pressure) until the carbon dioxide permeation amount was stabilized. Thereafter, the temperature of the thermostatic chamber was set to 30°C, and the permeation amount was measured and the permeance (P3) was calculated in a state where the carbon dioxide permeation amount was stabilized. The results are shown in Table 3 below.

[0185] Thereafter, the above mixed gas separation test was carried out while maintaining the temperature at 30°C. Specifically, after the single component gas permeation test, the supply gas was changed to a CO2 / N2 mixed gas, and introduced between the cylinders of the pressure vessel 2 and the zeolite membrane composite 1. The supply side pressure was kept at 0.4 MPa, and the supply gas amount was set to 5.2 NL / min so that the average linear velocity of the gas between the cylinders of the pressure vessel 2 and the zeolite membrane composite 1 at the measurement temperature and pressure was 60 cm / s. The amount and composition of the permeating gas were measured, and the permeance (P4) was calculated. The results are shown in Table 3 below.

[0186] Carbon dioxide adsorption performance The carbon dioxide adsorption performance of the zeolite membrane composite is measured as follows. That is, after leaving the zeolite membrane composite in contact with the air at room temperature (20°C) for 5 hours or more, the zeolite membrane composite is placed in a chamber, and He is flowed from a cylinder at atmospheric pressure and room temperature at 40cc / min. While He is flowing at 40cc / min, the chamber is heated and the temperature is raised from room temperature at a rate of 40°C / min. The components desorbed from the membrane during the temperature rise are measured by MS, and the amount of M / z44 detected between 100°C and 300°C is calculated. The calculation is performed by introducing a predetermined amount of CO2 gas into the measurement path in a pulse to create a calibration curve of the gas volume and area after each measurement, and introducing the area of ​​M / z44 obtained in this measurement into this. The MS detection value is output at least once per second. The M / z 44 derived from the zeolite membrane composite is a value calculated by subtracting the amount of M / z 44 obtained by a blank measurement in the same manner as above, but without placing a zeolite membrane composite in the chamber.

[0187] Here, the chamber is cylindrical with a diameter of 12 mm, a length of 250 mm or less, and a wall thickness of 1.2 mm or less, and is made of quartz. Heating is performed by infrared heating. The thermometer is connected to the center of the infrared irradiation part of the quartz chamber and measures the temperature outside the sample. After the above single component gas permeation test and mixed gas separation test, the zeolite membrane composite was heated to remove the adsorbed components, and then the above carbon dioxide adsorption performance was evaluated. The results are shown in Table 3 below.

[0188] [Comparative Example 3] The zeolite membrane composite prepared under the same conditions as in Comparative Example 1, except that no treatment for adhering Ca to the CHA-type zeolite membrane composite was performed, and the single component gas permeation test, mixed gas separation test, and carbon dioxide adsorption performance evaluation were performed in the same manner as described above. The results are shown in Table 3 below.

[0189] [Table 3]

[0190] As is clear from the results shown in Table 3, when the zeolite membrane composite of Comparative Example 3 is used to separate or concentrate a mixed gas containing carbon dioxide, carbon dioxide is less likely to be adsorbed by the zeolite membrane and both carbon dioxide and nitrogen are more likely to enter the zeolite pores than in the zeolite membrane composite of Example 9, and therefore the gas separation performance and gas permeation performance of the zeolite membrane are reduced due to the influence of nitrogen. In contrast, the zeolite membrane composite of Example 9 has high carbon dioxide adsorption performance, and therefore can maintain the gas separation performance and gas permeation performance of the zeolite membrane when separating or concentrating a mixed gas containing carbon dioxide.

[0191] In the above examples, the zeolite membrane composite of the present disclosure is not limited to the embodiment in which Ca is attached to the surface of the zeolite membrane as a specific means for improving the carbon dioxide absorption performance of the zeolite membrane. It is considered that the desired effect can be achieved even in the embodiment other than the embodiment in which Ca is attached, as long as the carbon dioxide absorption performance of the zeolite membrane can be improved.

[0192] 3. Actual gas testing For the CHA-type zeolite membrane composites according to Examples 1 and 2 and Comparative Examples 1 and 2, a permeation test and a separation test of a high-pressure gas containing carbon dioxide and a hydrocarbon were carried out.

[0193] The sample gases were CO2 (liquefied carbon dioxide, produced by Nippon Ekitan Co., Ltd.) and LNG (liquefied natural gas, produced by Kitakyushu LNG Co., Ltd., molar composition example: CH4 / C2H6 / C3H8 / C4H 10 = 91.2 / 5.2 / 2.6 / 1.0) was used. CO2 and LNG were mixed in an arbitrary ratio.

[0194] The zeolite membrane composite was stored in the same pressure-resistant container as in the low pressure test, and the sample gas was supplied between the pressure-resistant container and the zeolite membrane composite. At a temperature of 40°C, a supply gas pressure of 4.0 MPa, and a permeation side pressure of 0.1 MPa, the permeance when CO2 single gas was supplied was defined as P5, and the CO2 permeance when CO2 / LNG=20 / 80 mixed gas was supplied was defined as P6. The change over time in the CO2 permeance maintenance rate P6 / P5 when the mixed gas was supplied was recorded. The permeance maintenance rate was evaluated from the value of P6 / P5 after a predetermined time from the start of the supply of the CO2 / LNG mixed gas. The permeance maintenance rate P6 / P5 [%] of Comparative Example 1 was used as the standard, and samples with a difference in this maintenance rate higher than Comparative Example 1 by 5 [percentage points] were marked as "◯", samples with a difference in maintenance rate higher than Comparative Example 1 but 5 [percentage points] or less were marked as "△", and samples with the same or lower than Comparative Example were marked as "X". The results are shown in Table 4 below.

[0195] [Table 4]

[0196] In addition, the following test was also conducted, which allows the effects of real gas to be confirmed more easily. After supplying a CO2 / LNG mixed gas for a specified period of time under similar conditions, a CO2 permeation test was conducted under the same conditions as the CH4 permeation test and the SF6 permeation test, and the carbon dioxide permeance P7 in the low-pressure evaluation after the real gas test was measured. At this time, the maintenance rate P7 / P CO2 The value of the permeance maintenance rate P7 / P CO2 Using [%] as the standard, samples with a difference in retention rate that is 10 percentage points higher than Comparative Example 1 are marked as "O", samples with a retention rate that is higher than Comparative Example 1 but the difference is 10 percentage points or less are marked as "△", and samples with a retention rate that is equal to or lower than the Comparative Example are marked as "X". The results are shown in Table 5 below.

[0197] [Table 5]

[0198] It is also expected that the performance retention rate of the zeolite membrane composite in real gas will differ depending on the composition of carbon dioxide and hydrocarbons contained in the real gas. For this reason, real gas tests were also conducted under conditions with a higher hydrocarbon composition, which makes it easier for performance to decrease. In this case, evaluation was conducted using the following method, which makes it easier to confirm the effects of real gas. The same procedure was used to evaluate the carbon dioxide permeance retention rate in the low pressure evaluation before and after the real gas test, P8 / P, except that the supply gas pressure was 3.5 MPa, the composition of the supplied mixed gas was CO2 / LNG = 10 / 90, and the carbon dioxide permeance in the low pressure evaluation after the real gas test was P8. CO2 The value of P8 / P was calculated. CO2 Using [%] as the standard, samples with a difference in retention rate that is 10 percentage points higher than Comparative Example 1 are marked as "O", samples with a higher retention rate than Comparative Example 1 but with a difference of 10 percentage points or less are marked as "△", and samples with a retention rate equal to or lower than the Comparative Example are marked as "X". The results are shown in Table 6 below.

[0199] [Table 6]

[0200] As shown in Tables 4 to 6, the zeolite membrane composites of Examples 1 to 4 were able to maintain high permeance even in the actual gas test. In addition, it was found that the zeolite membrane composites of Examples 1 and 2 had a higher permeance maintenance rate than Examples 3 and 4. As described above, the permeance of methane passing through the pores was low, and the P CH4 ≦3.02×P SF6 +8.19×10 -9Zeolite membrane composites that satisfy the above relationship and zeolite membrane composites that have a carbon dioxide permeance of 70% or more after propane is supplied to the zeolite membrane surface when propane is supplied under specified conditions compared to the carbon dioxide permeance before propane is supplied have been found to have a high carbon dioxide permeance maintenance rate in actual gas tests. If the permeance is 80% or more, the effect is even higher. This is presumably because the pore size is controlled to be approximately the same as the dynamic molecular diameter of methane molecules, the smallest hydrocarbon. [Explanation of symbols]

[0201] 1 Zeolite membrane composite 2. Pressure vessel 3 Endpin 4 Connection 5. Pressure gauge 6 Backpressure valve 7 Supply gas (mixture of gases) 8. Gas permeation 9. Exhaust Gas 10 Piping

Claims

1. A method for separating or concentrating a mixed gas, comprising contacting a mixed gas containing at least carbon dioxide and a hydrocarbon and having a pressure of 1 MPa or more at a normal temperature or at 35° C. with a zeolite membrane composite having a zeolite membrane formed on a porous support, the zeolite membrane having a surface to which a metal species has been added or which has been subjected to a silylation treatment, and allowing a gas component with high permeability to permeate from the mixed gas, comprising the steps of: The zeolite membrane composite is The carbon dioxide permeance in the carbon dioxide permeation test (1) before the propane contact treatment described below is P 1 The carbon dioxide permeance in the carbon dioxide permeation test (2) after the following propane contact treatment was P 2 In this case, P 2 / P 1 is 0.70 or more, A method for separating or concentrating a gas mixture. Carbon dioxide permeation test (1): When a single component gas of 100% carbon dioxide is supplied to the surface of the zeolite membrane under the conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90° C., the permeance of carbon dioxide permeating the zeolite membrane is P 1 Let us assume that. Propane contact treatment: After the carbon dioxide permeation test (1), the supply gas was changed from a single component gas of 100% carbon dioxide to propane, and propane was supplied to the surface of the zeolite membrane under conditions of a supply gas pressure of 0.1 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90° C. to replace the carbon dioxide with the propane, and then propane was supplied to the surface of the zeolite membrane for 30 minutes under conditions of a supply gas pressure of 0.4 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90° C. Carbon dioxide permeation test (2): After the propane contact treatment, the supply gas was changed from propane to a single-component gas of 100% carbon dioxide. When a single-component gas of 100% carbon dioxide was supplied to the surface of the zeolite membrane under the conditions of a supply gas pressure of 0.2 MPa, a permeation gas pressure of 0.1 MPa, and a temperature of 90° C., the permeance of carbon dioxide permeating the zeolite membrane was measured as P 2 Let us assume that.

2. The zeolite membrane composite is Methane under conditions of supply gas pressure 0.2 MPa, permeation gas pressure 0.1 MPa, and temperature 40°C The permeance of P CH4 , the permeance of sulfur hexafluoride is P SF6 In this case, P CH4 ≦3.02×P SF6 +8.19 x 10 -9 Fulfilling The method for separating or concentrating a mixed gas according to claim 1.

3. The zeolite constituting the zeolite membrane has a pore structure with an oxygen ring of 8 or less members.

3. A method for separating or concentrating a mixed gas according to claim 1 or 2.

4. The zeolite constituting the zeolite membrane is a CHA-type zeolite.

3. A method for separating or concentrating a mixed gas according to claim 1 or 2.

Citation Information

Patent Citations

  • Mixed matrix membrane incorporating chabazite-type molecular sieves

    JP2005503260A

  • Carbon dioxide separation method

    JP2018202416A

  • Zeolite membrane complex

    WO2013125660A1

  • Zeolite membrane, production method therefor, and separation method using same

    WO2016006564A1

  • Method for separating carbon dioxide and apparatus for separating carbon dioxide

    WO2017150737A1