Capacitor and manufacturing method thereof

The capacitor design with a laminated cathode foil structure and carbon layer addresses the load and vibration issues of long capacitors, enhancing rigidity and durability for improved performance.

JP2024170017APending Publication Date: 2024-12-06NIPPON CHEMI CON CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023086927
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Long capacitors exceeding 60 mm in length face challenges with increased load on the tab due to the weight of the capacitor element, leading to potential damage and reduced vibration resistance, which is not addressed by existing technologies.

Method used

A capacitor design with a laminated structure where the cathode foil protrudes from the anode foil, increasing the rigidity of the capacitor element and reducing the load on the tab, combined with a carbon layer on the cathode foil for enhanced strength and a specific margin distance configuration to prevent short circuits.

Benefits of technology

The laminated structure enhances the rigidity and vibration resistance of the capacitor, reducing tab damage and improving durability, allowing for expanded applications of long capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024170017000001_ABST
    Figure 2024170017000001_ABST
Patent Text Reader

Abstract

To reduce the load applied on a tab of a long capacitor, for example, with a length exceeding 60 mm.SOLUTION: A capacitor (2) includes: an exterior case (4) having a length exceeding 60 mm; and a capacitor element (8) that includes an anode foil (44), a cathode foil (42) and a separator (46) which are stacked, and that is brought into contact with the bottom (16) of the exterior case in a pressurized state while being stored in the exterior case. The cathode foil protrudes from a side end (44-1) of the anode foil, on a side of the bottom of the exterior case.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a capacitor and a method for manufacturing the same. [Background technology]

[0002] A capacitor such as an electrolytic capacitor includes, for example, a capacitor element housed in an exterior case and a sealing plate that seals the opening of the exterior case. An external terminal attached to the sealing plate is connected to a lead (tab) drawn out from the capacitor element (for example, Patent Document 1). The connection between the external terminal and the lead makes it possible to store electricity in the capacitor element and to extract electricity from the capacitor element. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-44068 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in recent years, there has been a demand for a capacitor with a higher capacity. In addition, the performance, size, and weight of electric and electronic devices and information and communication devices in which capacitors are used are being actively promoted, and it is desired to make the power supply devices used in these devices and devices smaller and more efficient. Therefore, not only is there a demand for a capacitor with a higher capacity, but there is also a tendency for the mounting area of ​​the capacitor on the board to become smaller, and the space for arranging the capacitor tends to be limited due to the arrangement of other electronic components on the board. In order to meet such demands, for example, the capacitor has been made elongated. By placing a capacitor having an elongated external shape upright so that the bottom surface of the outer case is separated from the board, it is possible to reduce the diameter of the mounting area. In addition, by placing the capacitor lying down so that the side of the outer case is parallel to the board, the capacitor can be mounted in the elongated space of the board. However, if an attempt is made to realize a high capacity of a capacitor in an elongated capacitor, the capacitor element also becomes longer and the weight of the capacitor element also becomes larger. If the capacitor element moves inside the outer case, a load is applied to the lead. The load on the lead (tab) increases with the weight of the capacitor element, etc. Therefore, for long capacitors, for example those with a length exceeding 60 millimeters (hereafter referred to as "mm"), measures to reduce the load on the lead (tab) are required that differ from those for short, normal capacitors.

[0005] Patent Document 1 does not disclose or suggest such a problem, and the configuration disclosed in Patent Document 1 cannot solve such a problem.

[0006] Therefore, a first object of the present disclosure is to suppress the load on the tabs of a long-dimension capacitor having a length exceeding, for example, 60 mm.

[0007] A second object of the present disclosure is to suppress damage to the tabs of, for example, long-dimension capacitors.

[0008] A third object of the present disclosure is to provide a vibration-resistant structure that can withstand an increase in element weight of a long capacitor, for example, and to improve the vibration resistance or durability of the long capacitor.

[0009] A fourth object of the present disclosure is to expand the applications of long-dimension capacitors, for example. [Means for solving the problem]

[0010] In order to achieve the above object, according to a first aspect of the present disclosure, a capacitor includes an exterior case having a length of more than 60 mm, and a capacitor element including a stacked anode foil, a cathode foil, and a separator, the capacitor element being housed in the exterior case and in contact with a bottom of the exterior case under pressure, and the cathode foil protrudes from a side end of the anode foil on the bottom side of the exterior case.

[0011] The capacitor element may have a laminated structure of the protruding portion of the cathode foil and the separator on the outer side of the side end portion of the anode foil.

[0012] On the bottom side of the exterior case, a side end of the cathode foil may be disposed in a region between the side end of the anode foil and a side end of the separator.

[0013] At the bottom side of the exterior case, a cathode margin distance between a side end of the cathode foil and a side end of the separator may be equal to or less than half an anode margin distance between the side end of the anode foil and the side end of the separator. The cathode margin distance may be equal to or less than one-fifth of the anode margin distance.

[0014] In the above capacitor, the cathode foil may include a carbon layer.

[0015] In order to achieve the above-mentioned object, according to a second aspect of the present disclosure, a method for manufacturing a capacitor includes: a step of making or preparing a capacitor element including a stacked anode foil, a cathode foil, and a separator, where the cathode foil protrudes from a side end of the anode foil at one end; and a step of inserting the capacitor element into a bottomed cylindrical exterior case and bringing the one end of the capacitor element into contact with a bottom of the exterior case under pressure, wherein the exterior case has a length exceeding 60 mm. Effect of the Invention

[0016] According to the present disclosure, the following effects can be obtained.

[0017] (1) Since the cathode foil protrudes from the side end of the anode foil, the rigidity of the capacitor element is increased at the bottom side of the exterior case. Therefore, the pressure absorption of the capacitor element in a pressurized state is suppressed, and the pressing force of the capacitor element against the sealing plate, etc. is increased.

[0018] (2) Movement of the capacitor element and the load on the tab are suppressed, thereby preventing damage to the tab.

[0019] (3) The vibration resistance or durability of a long capacitor can be improved.

[0020] (4) The improved vibration resistance and durability can expand the applications of long capacitors. [Brief description of the drawings]

[0021] [Figure 1] FIG. 2 is a diagram illustrating an example of a capacitor according to an embodiment. [Diagram 2] 1A and 1B are diagrams illustrating an example of the structure of a capacitor element. [Diagram 3] 13A and 13B are diagrams illustrating an example of the structure of another capacitor element. [Figure 4] 13 is a graph showing an example of confirmation results of compressive stress of a capacitor element. [Diagram 5]FIG. 13 is a diagram showing an example of an experimental result of a capacitor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Fig. 1 shows an example of a capacitor according to an embodiment. In Fig. 1, an outer case 4 and a sealing plate 6 are shown in cross section at the center. Fig. 2 shows an example of the structure of a capacitor element. The configurations shown in Figs. 1 and 2 are merely examples, and the technology of the present disclosure is not limited to the configurations shown in Figs. 1 and 2.

[0023] The capacitor 2 is, for example, an electrolytic capacitor. The capacitor 2 includes, for example, an exterior case 4, a sealing plate 6, and a capacitor element 8 having a tab 32. The capacitor element 8 is housed inside the exterior case 4, and the sealing plate 6 is disposed and fixed in the opening 10 of the exterior case 4. In addition, the tab 32 pressed against at least the external terminal 22 of the sealing plate 6 is pressed into the capacitor element 8. Therefore, the element end surface 8-1 and the element end surface 8-2 of the capacitor element 8 are in contact with the sealing plate 6 under pressure via the bottom 16 of the exterior case 4, the tab 32, and the external terminal 22, respectively, and the capacitor element 8 is fixed by the bottom 16 of the exterior case 4 and the sealing plate 6. The capacitor 2 has a length L that exceeds, for example, 60 mm. The length L of the capacitor 2 is equal to the length from the bottom 16 of the exterior case 4 to the apex of the end crimping portion 14 after the end crimping.

[0024] The outer case 4 is, for example, a metal case such as an aluminum case, and is a cylindrical container with a bottom. The outer case 4 has a side crimping portion 12 on the side facing the opening 10, and an end crimping portion 14 on the end facing the opening 10. The side crimping portion 12 determines the position of the sealing plate 6, and the end crimping portion 14 presses the sealing plate 6 against the side crimping portion 12. The outer case 4 may have a fragile portion 18 on a bottom 16 of the outer case 4. The fragile portion 18 breaks when the internal pressure of the outer case 4 rises above a set value, thereby reducing the internal pressure of the outer case 4. The fragile portion 18 prevents the capacitor 2 from bursting.

[0025] The sealing plate 6 is disposed inside the opening 10 of the outer case 4, between the side crimping portion 12 and the end crimping portion 14. The sealing plate 6 is pressed against the side crimping portion 12 by the end crimping portion 14, and is thereby fixed to the opening 10 of the outer case 4. The sealing plate 6 seals the opening 10 of the outer case 4. The sealing plate 6 has a shape corresponding to the shape of the opening 10 of the outer case 4, and for example, has a disk shape with a diameter equal to or close to that of the circular opening 10. The sealing plate 6 may have a shape and size corresponding to the polygonal opening 10. The sealing plate 6 includes, for example, a laminate 20 in which a plurality of members with different functions are laminated, and, for example, two external terminals 22. The laminate 20 includes, for example, a rubber layer 24 and a resin layer 26. The rubber layer 24 has a function of allowing gas to pass through but blocking liquid. The rubber layer 24 is made of a rubber material such as ethylene propylene rubber, butyl rubber, or silicone rubber. The resin layer 26 has a higher rigidity than the rubber layer 24, and is, for example, a paper phenolic resin. The paper phenolic resin is a synthetic material in which a paper base material is impregnated with a phenolic resin. The resin layer 26 may be a single structure made of paper phenolic resin, or may be a laminate structure in which other materials (not shown) are superimposed. The rubber layer 24 is disposed on the outer side of the sealing plate 6 (i.e., on the side of the end crimping portion 14 of the exterior case 4) and forms the outer surface of the sealing plate 6. The resin layer 26 is disposed on the inner side of the sealing plate 6 (i.e., on the side of the capacitor element 8) and forms the inner surface of the sealing plate 6. The laminate 20 has a through hole 27 through which the rivet 30 of the external terminal 22 passes.

[0026] The external terminal 22 includes an electrode terminal 28 and a rivet 30. The electrode terminal 28 is disposed on the outer surface of the sealing plate 6, and functions as an anode terminal or a cathode terminal of the capacitor 2. The electrode terminal 28 has, for example, an L-shape, and has an upright portion that stands upright on the laminate 20 and is for connecting to an external component, and a flat portion that is disposed parallel to the surface of the laminate 20. The flat portion has a through hole through which the rivet 30 passes.

[0027] The rivet 30 penetrates the laminate 20 and protrudes from the outer surface and the inner surface of the laminate 20. The rivet 30 has flanges 34-1, 34-2, 34-3 and a cylindrical portion 36. The flange 34-1 is disposed on the outer surface side of the sealing plate 6, and the flanges 34-2, 34-3 are disposed on the inner surface side of the sealing plate 6. The cylindrical portion 36 is disposed between the flanges 34-1, 34-2 and between the flanges 34-2, 34-3, and is integrated with the flanges 34-1, 34-2, 34-3. The cylindrical portion 36 penetrates the flat portion of the electrode terminal 28 and the laminate 20, and the flanges 34-1, 34-2 sandwich the flat portion of the electrode terminal 28 and the laminate 20. Therefore, the electrode terminal 28 is fixed to the laminate 20. The cylindrical portion 36 passes through the through-hole of the tab 32, and the flange portions 34-2, 34-3 sandwich the tab 32. As a result, the tab 32 is fixed to the external terminal 22. That is, the rivet 30 is connected to the tab 32 of the capacitor element 8, for example, by pressure welding or sandwiching. A connection portion of the tab 32 to the rivet 30 is integrated with the rivet 30 to form the external terminal 22. The rivet 30 is made of a conductive metal material or has a metal-plated surface, and is electrically connected to the electrode terminal 28 and the tab 32.

[0028] A part of the external terminal 22 is pressed into the element end face 8-2 of the capacitor element 8. The capacitor element 8 is fixed to the bottom 16 of the exterior case 4 and the sealing plate 6 by the pressing of the external terminal 22. The pressing of the external terminal 22 generates a pressure P1 from the sealing plate 6 to the capacitor element 8 and a pressure P2 from the bottom 16 of the exterior case 4 to the capacitor element 8, as shown in FIG. 1. The pressure P2 is a repulsive force of the pressure P1. When the pressing amount of the external terminal 22 is smaller than the protruding distance of the external terminal 22, the element end face 8-2 is separated from the sealing plate 6 in the portion other than the external terminal 22, as shown in FIG. 1. However, the pressing amount of the external terminal 22 may be larger than the protruding distance of the external terminal 22, and the element end face 8-2 may contact the sealing plate 6 in the portion other than the external terminal 22.

[0029] 2, includes a cathode foil 42, an anode foil 44, and a separator 46. The cathode foil 42, the anode foil 44, and the separator 46 are stacked and wound to form a wound element such that the separator 46 is disposed between the cathode foil 42 and the anode foil 44. The wound element forms the capacitor element 8.

[0030] The width x of the anode foil 44 and the width y of the cathode foil 42 are both shorter than the width z of the separator 46, and the width x of the anode foil 44 is shorter than the width y of the cathode foil 42, for example. At one end 8-3 of the capacitor element 8, the cathode foil 42 protrudes from the side end 44-1 of the anode foil 44. Therefore, in the region between the side end 44-1 of the anode foil 44 and the side end 46-1 of the separator 46 (hereinafter referred to as the "outside region of the side end 44-1"), the capacitor element 8 has a laminated structure 58 of the protruding portion 42-3 of the cathode foil 42 and the separator 46. The one end 8-3 of the capacitor element 8 includes the element end surface 8-1 and its vicinity, and is disposed on the bottom 16 side of the exterior case 4. The laminated structure 58 of the capacitor element 8 increases the rigidity of the capacitor element 8 in the outside region of the side end 44-1. That is, the capacitor element 8 has a higher rigidity as a whole than a capacitor element 8 without the laminated structure 58.

[0031] At one end 8-3 of the capacitor element 8, the side end 42-1 of the cathode foil 42 overlaps, for example, the side end 46-1 of the separator 46. The side end 42-1 of the cathode foil 42 may be disposed in the outer region of the side end 44-1 as in the capacitor element 108 shown in FIG. 3, or may be disposed in the vicinity of the side end 46-1 of the separator 46. The vicinity of the side end 46-1 is a location where the cathode margin distance w1 (A in FIG. 3) is, for example, less than half or less than one fifth of the anode margin distance v1. The cathode margin distance w1 is the distance between the side end 42-1 of the cathode foil 42 and the side end 46-1 of the separator 46, and is 0 when the side end 42-1 overlaps the side end 46-1. Anode margin distance v1 is the distance between side end 44-1 of anode foil 44 and side end 46-1 of separator 46. Anode margin distance v1 is equal to or greater than the distance necessary to prevent anode foil 44, whose potential increases due to charge storage, from contacting exterior case 4, and is, for example, 2 mm.

[0032] 2A and 2B, at the other end 8-4 of the capacitor element 8, the side end 42-2 of the cathode foil 42 overlaps, for example, the side end 44-2 of the anode foil 44. The cathode margin distance w2 is the distance between the side end 42-2 of the cathode foil 42 and the side end 46-2 of the separator 46, and the anode margin distance v2 is the distance between the side end 44-2 and the side end 46-2 of the anode foil 44. The cathode margin distance w2 and the anode margin distance v2 are equal to or greater than the distance required to prevent the cathode foil 42 and the anode foil 44 from being short-circuited to the external terminal 22, and are, for example, 3 mm.

[0033] The capacitor element 8 has two tabs 32 protruding from an element end surface 8-2. The tabs 32 are connected to the anode foil 44 or the cathode foil 42, and the protruding portions of the tabs 32 are connected to the external terminals 22.

[0034] Cathode foil 42 is an example of an electrode foil, and constitutes the cathode of capacitor 2. Cathode foil 42 is, for example, a strip-shaped foil, and has a base foil and a carbon layer.

[0035] The base foil is the base metal of the cathode foil 42, and is, for example, a valve metal foil such as aluminum foil, tantalum foil, niobium foil, titanium foil, hafnium foil, zirconium foil, zinc foil, tungsten foil, bismuth foil, or antimony foil. The surface of the base foil has irregularities formed, for example, by etching, and the surface area of ​​the base foil is enlarged. The surface of the base foil may include, for example, tunnel-shaped or spongy etching pits, and the tunnel-shaped or spongy etching pits may form the irregularities.

[0036] The carbon layer is disposed, for example, on both sides or one side of the base foil. The carbon layer partially penetrates into the interior of the unevenness, and therefore adheres closely to and engages with the unevenness of the base foil, thereby increasing the strength of the cathode foil 42. The carbon layer contains, for example, a carbon material as a main material, and a binder and a dispersant as additives.

[0037] Carbon materials include activated carbon, carbon black, carbon nanohorns, amorphous carbon, natural graphite, artificial graphite, graphitized Ketjen black, mesoporous carbon, and fibrous carbon. Activated carbon is produced from, for example, natural plant tissue such as coconut shells, synthetic resins such as phenol, and fossil fuels such as coal, coke, and pitch. Carbon black includes Ketjen black, acetylene black, channel black, and thermal black. Fibrous carbon includes carbon nanotubes and carbon nanofibers. Carbon nanotubes may be single-walled carbon nanotubes, which have one graphene sheet, or multi-walled carbon nanotubes (MWCNTs), which have two or more graphene sheets rolled coaxially to form multiple tube walls.

[0038] The binder is a resin-based binder such as styrene butadiene rubber, polyvinylidene fluoride, or polytetrafluoroethylene, which binds the carbon material together. The dispersant is, for example, sodium carboxymethylcellulose.

[0039] The anode foil 44 is an example of an electrode foil and constitutes the anode of the capacitor 2. The anode foil 44 is, for example, the valve metal foil described above, and is a strip-shaped foil. An expanded surface portion having a porous structure is formed on the surface of the anode foil 44. The porous structure is formed, for example, by tunnel-like pits, spongy pits, or voids between densely packed powder particles formed by etching. The surface of the expanded surface portion includes a dielectric oxide film formed by chemical conversion treatment.

[0040] Separator 46 is disposed between anode foil 44 and cathode foil 42 to prevent short circuit between anode foil 44 and cathode foil 42. Separator 46 is an insulating material and includes kraft as a separator material, and may include other separator materials such as manila, esparto, hemp, rayon, cellulose, mixtures thereof, and the like.

[0041] The electrolyte is an electrolytic solution, a gel electrolyte, a solid electrolyte containing a conductive polymer, etc. The electrolyte may include an electrolytic solution or a gel electrolyte, and a solid electrolyte containing a conductive polymer to form a so-called hybrid electrolytic capacitor.

[0042] The capacitor 2 can be fabricated, for example, by the following manufacturing process. The configurations shown in the following manufacturing processes are merely examples, and the technology of the present disclosure is not limited to the configurations shown in the following manufacturing processes.

[0043] The manufacturing process of capacitor 2 is an example of a manufacturing method of capacitor 2 of the present disclosure, and includes, for example, a process of making outer case 4, a process of making sealing plate 6, a process of making capacitor element 8, a process of connecting sealing plate 6 and tab 32 of capacitor element 8, a process of encapsulating capacitor element 8, and a crimping process.

[0044] In the process of manufacturing the outer case 4, a metal material such as aluminum is, for example, formed into a bottomed cylindrical shape to manufacture the outer case 4 before forming the side crimped portions 12 and the end crimped portions 14. In the process of manufacturing the outer case 4, the outer case 4 before forming the side crimped portions 12 and the end crimped portions 14 may be prepared, for example, by purchase.

[0045] The process of producing the sealing plate 6 includes a step of producing the laminate 20 and a step of attaching the external terminals 22 to the laminate 20.

[0046] In the process of producing the laminate 20, the above-mentioned rubber material for forming the rubber layer 24 is layered on, for example, a paper phenolic resin for forming the resin layer 26, and the rubber material and the paper phenolic resin are heated and pressed to produce a laminate. The produced laminate is punched into the shape and dimensions of the sealing plate 6 by, for example, a press process to produce the laminate 20. In the press process, the laminate is cut by, for example, a shear blade of a press machine. Through holes 27 for passing the external terminals 22 are formed in the laminate 20 by a hole-making device such as a drill or a punching device.

[0047] In the process of attaching the external terminal 22 to the laminate 20, the columnar portion 36 of the rivet 30, which has a columnar portion 36 and a flange portion 34-2 before being crushed, is inserted into the through-hole 27 of the laminate 20 from the resin layer 26 side, and is also inserted into the through-hole in the flat portion of the electrode terminal 28. With the flange portion 34-2 in contact with the resin layer 26, the columnar portion 36 protruding from the flat portion of the electrode terminal 28 is crushed to form the flange portion 34-1. The electrode terminal 28, the rivet 30, and the laminate 20 are integrated by sandwiching the flange portions 34-1 and 34-2. In the state in which the external terminal 22 is attached to the laminate 20, the rivet 30 is made to protrude from the surface of the resin layer 26 so that the tab 32 of the capacitor element 8 can be attached. In the process of producing the sealing plate 6, the sealing plate 6, the laminate 20, the external terminal 22, the rubber layer 24, the resin layer 26, the electrode terminal 28, or the rivet 30 may be prepared, for example, by purchase.

[0048] The process of producing capacitor element 8 includes a step of producing anode foil 44, a step of producing cathode foil 42, a step of producing separator 46, and a lamination step.

[0049] In the process of producing the anode foil 44, for example, an enlarged surface portion having a porous structure is formed on the surface of the valve metal foil described above, and a dielectric oxide film is formed on the surface of the valve metal foil on which the enlarged surface portion is formed by chemical conversion treatment. The enlarged surface portion is formed by direct current etching, alternating current etching, or by vapor deposition or sintering of metal particles on the valve metal foil. In direct current etching or alternating current etching, a direct current or alternating current is typically applied to the valve metal foil immersed in an acidic aqueous solution containing halogen ions such as hydrochloric acid. The valve metal foil on which the dielectric oxide film is formed is cut to produce the anode foil 44.

[0050] In the process of producing the cathode foil 42, a base foil is produced by, for example, forming irregularities on the surface of the valve action metal foil described above by etching. The etching of the cathode foil 42 may be the same as or different from the etching of the anode foil 44. The cathode foil 42 is produced by forming a carbon layer on the base foil, and cutting the base foil and the carbon layer into strips.

[0051] The carbon layer is formed, for example, as follows: The carbon material, binder, and dispersant described above are added to a diluent, and mixed by a dispersion process such as a mixer, jet mixing (jet collision), ultracentrifugation, or ultrasonic treatment to form a slurry. The diluent is, for example, alcohol, a hydrocarbon solvent, an aromatic solvent, an amide solvent, water, or a mixture thereof. The alcohol is, for example, methanol, ethanol, or 2-propanol. The amide solvent is, for example, N-methyl-2-pyrrolidone (NMP) or N,N-dimethylformamide (DMF).

[0052] The slurry is applied to the base foil, the solvent is evaporated to form a carbon layer, and the carbon layer is pressed. The pressing can, for example, force the carbon material into the pores of the unevenness, or, if the carbon material is larger than the pores of the unevenness, can deform the carbon material along the uneven surface of the unevenness. For example, the adhesion and fixation between the carbon layer and the base foil can be improved by forcing the carbon material into the pores of the unevenness or by deforming the carbon material along the uneven surface of the unevenness.

[0053] In the process of producing the separator 46, the separator member described above is cut to produce the separator 46.

[0054] In the lamination process, the anode foil 44, the cathode foil 42, and the separator 46 are laminated so that the separator 46 is disposed between the anode foil 44 and the cathode foil 42, and the anode foil 44, the cathode foil 42, and the separator 46 are wound to produce the capacitor element 8. Before or during winding, the anode foil 44 and the cathode foil 42 are each connected to a tab 32, and the tab 32 is made to protrude from the element end surface 8-2. When the anode foil 44 and the cathode foil 42 are laminated on the element end surface 8-1 side so that the cathode foil 42 protrudes from the side end 44-1 of the anode foil 44, the laminated structure 58 described above can be formed at one end 8-3. In the process of producing the capacitor element 8, the cathode foil 42, the anode foil 44, the separator 46, or the capacitor element 8 may be prepared, for example, by purchase.

[0055] In the process of connecting the sealing plate 6 and the tab 32 of the capacitor element 8, the columnar portion 36 protruding from the inner surface of the sealing plate 6 is inserted into the through hole of the tab 32. With the flange portion 34-2 in contact with the tab 32, the columnar portion 36 protruding from the tab 32 is crushed to form the flange portion 34-3. The tab 32 and the external terminal 22 are integrated by being sandwiched between the flange portions 34-2 and 34-3.

[0056] In the process of encapsulating capacitor element 8, capacitor element 8 impregnated with an electrolyte such as an electrolytic solution is inserted into exterior case 4, and sealing plate 6 is placed at opening 10 of exterior case 4. At this time, tab 32 may be folded into the gap between sealing plate 6 and capacitor element 8 for storage.

[0057] In the crimping process, the attachment position of sealing plate 6 and the formation position of side crimp portion 12 are determined so that external terminal 22, or tab 32 that overlaps with external terminal 22 to form external terminal 22, is pressed into capacitor element 8. The attachment position and formation position may be determined by calculation processing, or may be determined from the relationship between the attachment position and formation position of previously manufactured capacitor 2 and the presence or absence of pressing in of capacitor element 8 or the amount of compression.

[0058] In the crimping process, side crimp portion 12 is formed at the determined formation position by crimping. Also, the end of opening 10 of exterior case 4 is bent to form end crimp portion 14. By forming end crimp portion 14, sealing plate 6 is pressed against side crimp portion 12 and fixed, and external terminals 22 are pressed into capacitor element 8, so that capacitor element 8 is fixed between bottom 16 of exterior case 4 and sealing plate 6.

[0059] Fig. 4 shows the results of confirming the compressive stress of the capacitor element. In the graph shown in Fig. 4, the horizontal axis represents the indentation depth, and the vertical axis represents the compressive stress. The results shown in Fig. 4 are merely an example, and the technology of the present disclosure is not limited to such results.

[0060] In order to confirm the action and effect of the protrusion of cathode foil 42, capacitor element 8 already described, capacitor element 108 shown in FIG. 3, and a capacitor element for comparison (hereinafter referred to as a "comparative element") were fabricated.

[0061] As shown in Figures 2A and 2B, in the produced capacitor element 8, a laminate structure 58 was formed in the entire or nearly the entire outer region of the side end 44-1. As shown in Figures 3A and 3B, in the produced capacitor element 108, a laminate structure 58 was formed in a portion of the outer region of the side end 44-1. In the comparative element, the side end 42-1 of the cathode foil 42 was overlapped with the side end 44-1 of the anode foil 44 so that the comparative element did not have the laminate structure 58.

[0062] Capacitor elements 8, 108 and the comparative element have the element length, element diameter, anode foil width x, cathode foil width y, separator width z, and cathode margin distance w1 shown in Table 1. The element length is the length of the capacitor element and corresponds to the separator width z. The element diameter is the diameter of the capacitor element. [Table 1]

[0063] The anode foil 44 has the tunnel-shaped pits described above, and the separator 46 has a density of 0.95 g / cm 3 , thickness 25μm kraft and density 0.85g / cm 3 The capacitor elements 8 and 108 and the comparative element were impregnated with an electrolyte. The electrolyte contained ethylene glycol as a solvent, diethylamine azelate as a solute, and polyoxyethylene glycerin as a pressure resistance improver.

[0064] To evaluate the repulsive force, the element end surface 8-2 of the capacitor element 8, capacitor element 108, or comparison element impregnated with the electrolyte was pressed toward the element end surface 8-1 with a force gauge at a pressing depth of 0 to 3 mm, and the compressive stress was measured and confirmed three times. The force gauge used for the measurements was a digital force gauge (ZTA-5000N) manufactured by Imada Co., Ltd.

[0065] As shown in Fig. 4A, the compressive stress of capacitor element 8 having laminate structure 58 was greater than the compressive stress of a comparative element not having laminate structure 58. Also, as shown in Fig. 4B, the compressive stress of capacitor element 8 in which laminate structure 58 is formed over the entire or almost entire outer region of end portion 44-1 was greater than the compressive stress of capacitor element 108 in which laminate structure 58 is formed only in a portion of the outer region of end portion 44-1. From these results, it was found that laminate structure 58 increases the compressive stress, and that the compressive stress, i.e., the repulsive force, increases as the region in which only separator 46 is laminated becomes narrower.

[0066] Fig. 5 shows the experimental results of the capacitor. The experimental results shown in Fig. 5 are merely an example, and the technology of the present disclosure is not limited to such experimental results.

[0067] In order to confirm the action or effect of the protrusion of cathode foil 42, capacitors 2 according to Experiment Nos. 1 and 2 were fabricated as an example, and capacitors according to Experiment Nos. 3 and 4 were fabricated as comparative examples.

[0068] The basic structure of the capacitor 2 according to the experiment numbers 1 and 2 is the same as that of the capacitor 2 including the capacitor element 8 already described. The basic structure of the capacitor according to the experiment numbers 3 and 4 is the same as that of the capacitor 2 already described, except that the capacitor according to the experiment numbers 3 and 4 does not have the laminated structure 58. The capacitor 2 according to the experiment numbers 1 and 2 and the capacitor according to the experiment numbers 3 and 4 have a product diameter of 35 mm and an element diameter of 33.5 mm, and have the product height, element length, anode foil width x, cathode foil width y, separator width z, cathode margin distance w1, and compression amount shown in FIG. 5. The product diameter is the diameter of the capacitor, and the element diameter is the diameter of the capacitor element. The product height is the length L already described, and the element length is the length of the capacitor element before the external terminal 22 is pushed in. The compression amount is the difference between the length of the capacitor element before the external terminal 22 is pushed in and the length of the capacitor element at the portion where the external terminal 22 is pushed in.

[0069] The anode foil 44 has the tunnel-shaped pits described above, and the separator 46 has a density of 0.70 g / cm 3 The electrolyte contains ethylene glycol as a solvent.

[0070] Capacitor 2 from experiment numbers 1 and 2 and capacitors from experiment numbers 3 and 4 were evaluated by a vibration test (modified vibration test). The modified vibration test is a vibration test that partially modifies the standard vibration test in accordance with "4.8 Vibration" of Japanese Industrial Standards (JIS) C5101-4:2019 "Fixed capacitors for electronic equipment - Part 4: General rules by type - Fixed aluminum solid (MnO2) and non-solid electrolytic capacitors" and "4.17 Vibration" of JIS C5101-1:2019 "Fixed capacitors for electronic equipment - Part 1: General rules by type". The conditions for the standard vibration test are as follows. The X, Y, and Z directions are as shown in Figure 1. Frequency: 10~55Hz Amplitude or acceleration: Single amplitude 0.75mm or 100m / s 2 (Whichever is looser) Sweep rate: 10Hz-55Hz-10Hz (approximately 1 minute) Sweep direction and test time: (sweep direction) first X direction, then Y direction, and finally Z direction (Test time) 2 hours for each direction (total 6 hours)

[0071] In the modified vibration test, an amplitude is used that is 2.0 times (i.e., a single amplitude of 1.50 mm) larger than the amplitude used in the standard vibration test (i.e., a single amplitude of 0.75 mm). The larger the amplitude, the larger the vibration energy applied to the capacitor 2. In other words, the modified vibration test is a stricter test than the standard vibration test.

[0072] 5 is an evaluation item for the capacitor 2. The evaluation result of "tab damage" indicates the presence or absence of damage to the tab 32 after the vibration test, with the evaluation result "OK" indicating that the tab 32 was not damaged and the evaluation result "NG" indicating that the tab 32 was damaged. It was found that the capacitor 2 according to the experiment numbers 1 and 2 as the embodiment obtained an evaluation result of "OK", and the capacitor according to the experiment numbers 3 and 4 as the comparative example obtained an evaluation result of "NG". In other words, it was found that the capacitor 2 according to the embodiment was less susceptible to tab damage than the capacitor according to the comparative example.

[0073] According to the embodiment, for example, the following effects can be obtained.

[0074] (1) The laminate structure 58 increases the rigidity of the capacitor element 8 in the outer region of the side end 44-1. The laminate structure 58 increases the compressive stress (repulsive force) of the capacitor element 8, making it easier to fix the capacitor element 8. The load on the tab 32 due to vibration of the capacitor element 8 is suppressed, and damage to the tab 32 (e.g., breakage of the tab 32) can be suppressed.

[0075] (2) As capacitor element 8 becomes larger, the load on tab 32 increases, for example, when capacitor element 8 vibrates. Multilayer structure 58 can improve the vibration resistance or durability of long capacitor 2 having a length exceeding 60 mm, and can resolve issues specific to long capacitors.

[0076] (3) By generating a compressive stress in the capacitor element 8, the vibration state of the tab 32 and the vibration state of the capacitor element 8 can be made as close as possible. Damage to the tab 32 occurs when stress is applied to the tab 32. The application of stress to the tab 32 may be caused by the tab 32 and the capacitor element 8 vibrating separately. The vibration of the capacitor 2 may cause the tab 32 and the capacitor element 8 to vibrate separately or cause vibration resonance. When the tab 32 is exposed to such swinging or vibration resonance, excessive vibration stress is concentrated on the tab 32. As a result, there is a risk of damaging the tab 32. However, by integrating the tab 32 and the capacitor element 8 by generating a compressive stress, it is possible to suppress vibration resonance and reduce the stress on the tab 32.

[0077] (4) The improved vibration resistance and durability of the long capacitor 2 can expand the range of uses.

[0078] (5) When cathode foil 42 includes a carbon layer, the strength of cathode foil 42 and capacitor element 8 is improved. Therefore, the pressure resistance of capacitor element 8 against pressures P1 and P2 is improved.

[0079] (6) When the cathode margin distance w2 and the anode margin distance v2 are wider than the cathode margin distance w1 and the anode margin distance v1, the product height is reduced and short circuits between the pressed-in external terminal 22 and the electrode foil are reduced.

[0080] Regarding the embodiment described above, the following features and modifications will be listed below.

[0081] (1) The outer case 4, the sealing plate 6, the capacitor element 8, the electrolyte, etc. are not limited to those described in the embodiment. These materials may be other materials used in aluminum electrolytic capacitors or similar capacitors. The capacitor element 8 may be, for example, a laminated element in which a plurality of flat cathode foils 42, anode foils 44, and separators 46 are laminated. The material of the carbon layer is not limited to those described in the embodiment. The material forming the carbon layer may be any conductive material containing carbon. The state of adhesion or engagement of the carbon layer with the base foil is not limited to those described in the embodiment. The cathode foil 42 may not include a carbon layer, and may be made, for example, only of the valve action metal foil already described.

[0082] (2) Unlike the anode foil 44, the cathode foil 42 is basically unrelated to the rise in potential. Therefore, the cathode foil 42 may be in contact with the bottom 16 of the exterior case 4, or may protrude from the side end 46-1 of the separator 46.

[0083] (3) The other end 8-4 of the cathode foil 42 may protrude from the side end 44-2 of the anode foil 44 without contacting the external terminal 22. In other words, the capacitor element 8, 108 may have the laminated structure 58 at both the one end 8-3 and the other end 8-4.

[0084] (4) In the embodiment, the electrode terminal 28, the rivet 30, and the laminate 20 are integrated by sandwiching the flange portions 34-1 and 34-2, and the tab 32 and the external terminal 22 are integrated by sandwiching the flange portions 34-2 and 34-3. However, the electrode terminal 28 and the tab 32 may be attached to the rivet 30 by, for example, cold welding.

[0085] (5) The laminate structure 58 may be applied to short conventional capacitors.

[0086] (6) In the embodiment, bottom 16 of outer case 4 is flat as shown in Fig. 1. However, a protrusion may be formed on bottom 16 of outer case 4, and the protrusion of bottom 16 may press into element end face 8-1 of capacitor element 8. The protrusion of bottom 16 can reduce the pressing load caused by external terminal 22.

[0087] (7) Exterior case 4 may have ribs on the inner surface of exterior case 4. The ribs reduce the distance between the inner surface of exterior case 4 and the side of capacitor element 8. As a result, the ribs can suppress movement of capacitor element 8 in the X and Y directions, and improve the vibration resistance of capacitor 2.

[0088] As described above, the most preferred embodiment of the present disclosure has been described. The technology of the present disclosure is not limited to the above description. Based on the gist of the invention described in the claims or disclosed in the specification, those skilled in the art can make various modifications and changes. It goes without saying that such modifications and changes are included in the scope of the present disclosure. [Industrial Applicability]

[0089] INDUSTRIAL APPLICABILITY The technology of the present disclosure is useful in that it can provide a capacitor having vibration resistance or durability. [Explanation of symbols]

[0090] 2. Capacitor 4 Outer case 6 Sealing plate 8, 108 Capacitor element 8-1, 8-2 Element end face 8-3 One end 8-4 Other end 10 Opening 12 Side crimping part 14 End crimping part 16 Bottom 18 Weakened Part 20 Laminate 22 External terminal 24 Rubber layer 26 Resin layer 27 Through hole 28 Electrode terminal 30 Rivet 32 Tabs 34-1, 34-2, 34-3 Flange 36 Cylinder section 42 Cathode foil 44 Anode foil 46 Separator 42-1, 42-2, 44-1, 44-2, 46-1, 46-2 side end 42-3 Protrusion 58 Laminated structure

Claims

1. An outer case having a length exceeding 60 mm; a capacitor element including anode foil, cathode foil, and a separator stacked together, the capacitor element being housed in the exterior case and in contact with a bottom of the exterior case under pressure; Equipped with A capacitor, characterized in that the cathode foil protrudes from a side end of the anode foil on the bottom side of the exterior case.

2. 2. The capacitor according to claim 1, wherein the capacitor element has a laminated structure of the protruding portion of the cathode foil and the separator on the outer side of the side end portion of the anode foil.

3. 2. The capacitor according to claim 1, wherein a side end of the cathode foil is disposed in a region between the side end of the anode foil and a side end of the separator on the bottom side of the exterior case.

4. 2. The capacitor according to claim 1, wherein, at the bottom side of the exterior case, a cathode margin distance between a side end of the cathode foil and a side end of the separator is equal to or less than half of an anode margin distance between the side end of the anode foil and the side end of the separator.

5. 5. The capacitor of claim 4, wherein said cathode margin distance is less than or equal to one-fifth of said anode margin distance.

6. 6. The capacitor of claim 1, wherein the cathode foil includes a carbon layer.

7. making or providing a capacitor element comprising a stacked anode foil, a cathode foil and a separator, with the cathode foil protruding at one end beyond a side edge of the anode foil; a step of inserting the capacitor element into a cylindrical exterior case having a bottom and bringing the one end of the capacitor element into contact with a bottom of the exterior case under pressure; Equipped with The method for manufacturing a capacitor, wherein the outer case has a length exceeding 60 mm.

Citation Information

Patent Citations

  • Electrolytic capacitor

    JP2012044068A