Easily openable packaging material and packaging bag
A laminated packaging material with a paper base, anchor coat, and gas barrier layers addresses tearability issues and reduces plastic use, ensuring easy opening and manufacturing suitability while maintaining gas barrier properties.
Patent Information
- Application Number
- JP2023086943
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Packaging materials with paper bases often suffer from poor tearability when not having a notch, leading to breakage during manufacturing and transportation, and there is a need to reduce plastic usage while maintaining gas barrier properties.
A laminated packaging material structure comprising a paper base material with an anchor coat layer, a gas barrier layer, and a sealant layer, where the paper base material constitutes at least 50% of the total weight, and specific resin compositions enhance tearability and adhesion, allowing for easy opening without notches.
The packaging material achieves excellent MD tearability, reduced plastic usage, and maintains high gas barrier properties, ensuring easy opening and suitable processing during manufacturing.
Smart Images

Figure 2024170028000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an easy-open packaging material and a packaging bag. [Background technology]
[0002] In recent years, the trend towards a plastic-free society has been growing due to growing environmental awareness sparked by the problem of marine plastic waste. In the field of packaging materials, there is also a growing demand to replace plastic with paper packaging materials. Packaging materials with gas barrier properties are being used to prevent the permeation of water vapor, which deteriorates the quality of the contents.
[0003] Patent Document 1 discloses a packaging material in which a paper base material, an adhesive layer containing a specific material, a metal layer in contact with the adhesive layer, and a sealant layer are laminated in this order, and the thickness of the adhesive layer is within a specific range. Patent Document 2 discloses a packaging material in which a paper base material, an adhesive layer in contact with the paper base material, and a sealant layer are laminated in this order, and the arithmetic mean roughness of the paper base material and the tensile strength of the packaging material satisfy specific conditional expressions. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-116880 A [Patent Document 2] JP 2020-49913 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the inventors have found through their investigations that the packaging materials disclosed in the above Patent Documents 1 and 2 have poor tearability when the packaging material does not have a notch.
[0006] Incidentally, for example, when a roll-shaped packaging material is conveyed to a packaging machine to manufacture a package, tension is applied to the packaging material in the longitudinal direction. The inventors have found through their studies that this tension causes the packaging material to break when the packaging material is made of paper. The package is composed of a packaging bag obtained from the packaging material and the contents contained in the packaging bag. Hereinafter, the machine direction of the packaging material is referred to as MD, and the cross direction perpendicular to the machine direction is referred to as CD.
[0007] Furthermore, from the perspective of the Law for Promoting Effective Utilization of Resources, there is a demand to reduce the amount of plastic used in packaging materials as well.
[0008] The present disclosure provides an easy-open packaging material having a paper base material, which has excellent MD tearability even when it does not have a notch, and has excellent processability during production of a package, and a packaging bag formed from the same. [Means for solving the problem]
[0009] The gist of the present disclosure lies in the following [1] to
[10] . [1] A paper base material; An anchor coat layer; A gas barrier layer; A sealant layer; A packaging material having a laminated structure comprising, in this order, The weight of the paper base material is 50% or more by mass based on the entire packaging material, The thickness of the sealant layer is 2 to 40 μm, the sealant layer comprises a first polyolefin-based resin; The tensile breaking strength of CD is 30 to 70 N / 15 mm. An easy-open packaging material with MD tensile breaking strength of greater than 70N / 15mm. [2] The easy-open packaging material according to [1], wherein the first polyolefin resin has at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group. [3] The easy-open packaging material according to [1] or [2], wherein the sealant layer has a thickness of 2 to 20 μm. [4] The easy-open packaging material according to any one of [1] to [3], further comprising an adhesive layer between the gas barrier layer and the sealant layer. [5] An overcoat layer is further provided between the gas barrier layer and the adhesive layer, The easy-open packaging material according to [4], wherein the overcoat layer contains a second polyolefin resin having at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group. [6] The easy-open packaging material according to any one of [1] to [5], wherein the anchor coat layer contains a third polyolefin resin having at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group. [7] The easy-open packaging material according to any one of [1] to [5], wherein the anchor coat layer contains a polyvinyl alcohol-based resin. [8] The easy-open packaging material according to any one of [1] to [5], wherein the anchor coat layer contains a polyurethane-based resin. [9] A packaging bag comprising the easy-open packaging material according to any one of [1] to [8].
[10] The packaging bag described in [9], having a folded portion. Effect of the Invention
[0010] According to the present disclosure, there is provided an easy-open packaging material having a paper base material, which has excellent MD tearability even when it does not have a notch, and has excellent processability during manufacturing of the package, and a packaging bag formed therefrom.
[0011] In addition, the packaging material and packaging bag according to one aspect of the present disclosure have excellent water vapor barrier properties. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic cross-sectional view showing an easy-open packaging material according to an embodiment of the present disclosure. [Diagram 2]FIG. 2 is a schematic cross-sectional view showing an easy-open packaging material according to another embodiment of the present disclosure. [Diagram 3] FIG. 1 is a perspective view showing a packaging bag according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings where necessary. However, the present disclosure is not limited to the following embodiments.
[0014] <Easy-to-open packaging material> {First embodiment} The easy-open packaging material according to the first embodiment will be described below. Fig. 1 is a schematic cross-sectional view showing the packaging material according to the first embodiment. The packaging material 10 according to one embodiment has a laminated structure including a paper base material 1, an anchor coat layer 2, a gas barrier layer 3, and a sealant layer 4 in this order.
[0015] [Paper base material] The paper base material 1 is not particularly limited, and may be appropriately selected depending on the application of the packaging bag to which the packaging material 10 is applied. There are no particular limitations on the paper base material 1 as long as it is made mainly of plant-derived pulp, and specific examples of the paper base material 1 include fine paper, special fine paper, coated paper, art paper, cast-coated paper, imitation paper, kraft paper, and glassine paper. The basis weight of the paper base material 1 is, for example, 20 g / m2, which provides better tearability. 2 More than 30g / m 2 More than 35g / m 2 or more than 40g / m 2 or more, and 2 Below 300g / m 2 or less than 100g / m 2 It may be the following:
[0016] The paper base material 1 may have a coating layer at least on the side in contact with the anchor coat layer 2 described below. By providing the coating layer, it is possible to prevent the anchor coat layer from penetrating into the paper, and it also plays a role of filling the unevenness of the paper, and the anchor coat layer can be formed uniformly without defects. For example, the coating layer may contain various copolymers such as styrene-butadiene, styrene-acrylic, and ethylene-vinyl acetate copolymers, polyvinyl alcohol resin, cellulose resin, and paraffin (WAX) as binder resins, and may contain clay, kaolin, calcium carbonate, talc, mica, and the like as fillers.
[0017] The thickness of the coating layer is not particularly limited, but may be, for example, 1 to 10 μm, or 3 to 8 μm.
[0018] When the weight of the paper base material 1 is 50% by mass or more based on the entire packaging material, the packaging material 10 has excellent tearability even if it does not have a notch. Furthermore, when the weight of the paper base material 1 is 50% by mass or more based on the entire packaging material, the amount of plastic material used can be sufficiently reduced, the entire packaging material can be said to be made of paper, and it has excellent recyclability. From the same viewpoint, the weight of the paper base material is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more.
[0019] It is preferable that the paper base material 1 has paper fibers oriented along the MD, i.e., anisotropic, because this provides the packaging material with better MD tearability and better processability during the production of the package.
[0020] The tensile breaking strength (T1) of the paper base 1 in the MD may be 70 to 200 N / 15 mm. The tensile breaking strength (T2) of the paper base 1 in the CD may be 10 to 70 N / 15 mm. The ratio (T1 / T2) of the tensile breaking strength (T1) in the MD to the tensile breaking strength (T2) in the CD of the paper base 1 is preferably 1.1 or more, more preferably 1.5 or more, and even more preferably 2.0 or more, so that the packaging material has better MD tearability and better processability during the manufacture of the package. The ratio (T1 / T2) may be 5.0 or less.
[0021] The difference (T1-T2) between the tensile breaking strength in the MD and the tensile breaking strength in the CD of the paper base material 1 is preferably 5N / 15mm or more, more preferably 20N / 15mm or more, and even more preferably 30N / 15mm or more, in order to provide a packaging material with better MD tearability and better processability during the manufacture of packaging bodies. The difference (T1-T2) may be 60N / 15mm or less.
[0022] The tensile breaking strength is measured by pulling a test piece (longitudinal length: 100 mm, transverse length: 15 mm) cut from the paper base material 1 in the longitudinal direction using a tensile tester (test length: 50 mm, pulling speed: 200 mm / min).
[0023] [Anchor coat layer] The anchor coat layer 2 is provided on the surface of the paper base material 1 to improve adhesion between the paper base material 1 and the gas barrier layer 3 described below, and to improve the gas barrier properties of the packaging material. The material of the anchor coat layer 2 is not particularly limited, but examples thereof include polyurethane resins, polyvinyl alcohol resins, and a third polyolefin resin having a polar group.
[0024] By including a polyurethane resin in the anchor coat layer 2, the wettability is good, resulting in excellent coating stability and good adhesion between the paper base material 1 and the gas barrier layer 3. Furthermore, by improving the surface smoothness of the anchor coat layer 2, the gas barrier layer 3 is easily formed densely, resulting in even better gas barrier properties. By using a polyurethane resin with gas barrier properties, further improvements in gas barrier properties can be expected.
[0025] From the viewpoint of barrier properties, the polyurethane resin preferably contains at least one of a metaxylylene diisocyanate-derived structural unit and a hydrogenated metaxylylene diisocyanate-derived structural unit. When the polyurethane resin contains such a structural unit, it exhibits high cohesive strength due to hydrogen bonds and stacking effect between xylylene groups, and therefore tends to have better gas barrier properties. From the viewpoint of coatability, the coating liquid used when forming an anchor coat layer containing a polyurethane resin is preferably a coating liquid dispersed in water, such as a dispersion or emulsion. An example of such a coating liquid is Takelac WPB manufactured by Mitsui Chemicals.
[0026] The anchor coat layer 2 contains the third polyolefin resin, which allows the formation of a dense film due to the crystallinity of the polyolefin, and exhibits water vapor barrier properties. The crystallinity of the polyolefin exhibits water vapor barrier properties, and the inclusion of polar groups exhibits adhesion to the gas barrier layer 3.
[0027] The third polyolefin resin may have at least one selected from a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic ester.
[0028] As the third polyolefin-based resin, copolymers of ethylene or propylene with unsaturated carboxylic acids (unsaturated compounds having a carboxyl group, such as acrylic acid, methacrylic acid, and maleic anhydride), unsaturated carboxylic acid esters, and salts of carboxylic acids neutralized with basic compounds may be used, as well as copolymers of vinyl acetate, epoxy compounds, chlorine compounds, urethane compounds, polyamide compounds, and the like.
[0029] Specific examples of the third polyolefin resin include a copolymer of an acrylic acid ester and maleic anhydride, an ethylene-vinyl acetate copolymer, and an ethylene glycidyl methacrylate copolymer.
[0030] The polyvinyl alcohol resin is, for example, a fully saponified polyvinyl alcohol resin, a partially saponified polyvinyl alcohol resin, a modified polyvinyl alcohol resin, an ethylene-vinyl alcohol copolymer resin, etc. The degree of polymerization of the polyvinyl alcohol resin is preferably 300 or more and 1700 or less. If the degree of polymerization is 300 or more, the gas barrier property and bending resistance of the packaging material become good, and if the degree of polymerization is 1700 or less, the viscosity of the coating liquid of the polyvinyl alcohol resin described below becomes low, and the coating property becomes good.
[0031] When the anchor coat layer 2 contains a polyvinyl alcohol-based resin, it has excellent flexibility, and can suppress cracking of the gas barrier layer 3 after bending (folding), thereby suppressing deterioration of the gas barrier properties, and can improve adhesion between the gas barrier layer 3 and the anchor coat layer 2.
[0032] The anchor coat layer 2 may contain other components in addition to the polyurethane resin, the third polyolefin resin, and the polyvinyl alcohol resin. Examples of the other components include polyolefin resins other than the third polyolefin resin, silane coupling agents, organic titanates, polyacrylics, polyesters, polyurethanes, polycarbonates, polyureas, polyamides, polyimides, melamines, and phenols.
[0033] The content of the polyurethane resin in the anchor coat layer 2 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.
[0034] The content of the third polyolefin resin in the anchor coat layer 2 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.
[0035] The content of the polyvinyl alcohol-based resin in the anchor coat layer 2 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.
[0036] The thickness of the anchor coat layer 2 may be, for example, 1 μm or more, 2 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. If the thickness of the anchor coat layer 2 is 1 μm or more, the unevenness of the paper base material 1 can be efficiently filled, and the gas barrier layer 3 can be laminated uniformly. Also, if the thickness of the anchor coat layer 2 is 20 μm or less, the gas barrier layer 3 can be laminated uniformly while suppressing costs.
[0037] The method of providing the anchor coat layer 2 includes a method of applying a coating liquid containing at least a material for forming the anchor coat layer and a solvent on a paper substrate, and drying the coating liquid. When the anchor coat layer 2 contains a third polyolefin resin, the third polyolefin resin in the coating liquid should have a small particle size. The particle size is not particularly limited, but is preferably 0.1 to 0.7 μm. When the particle size is small, the anchor coat layer 2 has excellent smoothness, and the formed gas barrier layer 3 tends to have a uniform thickness with little variation. As a result, the gas barrier property of the packaging material 10 tends to be further improved.
[0038] Examples of the solvent contained in the coating liquid of the anchor coat layer 2 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Also, from the viewpoint of environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.
[0039] [Gas barrier layer] The gas barrier layer has gas barrier properties. The gas barrier layer 3 may be a vapor-deposited layer obtained by vapor-depositing an inorganic oxide, a metal, or a metal oxide. The vapor-deposited layer may be one obtained by vapor-depositing silica or aluminum, and may be one obtained by vapor-depositing aluminum oxide (AlO x ) etc.
[0040] The thickness of the gas barrier layer 3 may be appropriately set depending on the intended use, but may be preferably 10 nm or more, 30 nm or more, 50 nm or more, and 300 nm or less, 100 nm or less, 80 nm or less. By setting the thickness of the gas barrier layer 3 to 10 nm or more, it is easy to ensure sufficient continuity of the gas barrier layer 3, and by setting the thickness to 300 nm or less, it is easy to sufficiently suppress the occurrence of curling and cracking, and it is easy to achieve sufficient gas barrier performance and flexibility.
[0041] The gas barrier layer 3 is preferably formed by a vacuum deposition method from the viewpoint of oxygen gas barrier performance and film uniformity. There are known deposition methods such as vacuum deposition, sputtering, and chemical vapor deposition (CVD), but vacuum deposition is preferred because of its high deposition rate and high productivity. Among the vacuum deposition methods, deposition by electron beam heating is particularly effective because the deposition rate can be easily controlled by the irradiation area and electron beam current, and the temperature of the deposition material can be raised and lowered in a short time.
[0042] [Sealant layer] The sealant layer 4 is provided on the surface of the gas barrier layer 3 so as to be in contact with the gas barrier layer 3. The sealant layer 4 has a thickness of 2 to 40 μm. The sealant layer 4 contains a first polyolefin resin. The first polyolefin resin has a polar group.
[0043] The sealant layer 4 contains the first polyolefin resin, which allows the formation of a dense film due to the crystallinity of the polyolefin, and exhibits water vapor barrier properties. Furthermore, the polyolefin resin has a polar group, which allows for adhesion to the gas barrier layer 3, eliminating the need for a separate adhesive layer. This increases the ratio of paper in the packaging material, further improving tearability.
[0044] Examples of the polar group include a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic ester.
[0045] The first polyolefin resin may be a copolymer of ethylene or propylene with an unsaturated carboxylic acid (an unsaturated compound having a carboxyl group, such as acrylic acid, methacrylic acid, or maleic anhydride), an unsaturated carboxylic acid ester, or a salt of a carboxylic acid neutralized with a basic compound. In addition, copolymers of ethylene or propylene with vinyl acetate, epoxy compounds, chlorine compounds, urethane compounds, polyamide compounds, or the like may also be used.
[0046] Specific examples of the first polyolefin resin include a copolymer of an acrylic acid ester and maleic anhydride, an ethylene-vinyl acetate copolymer, and an ethylene glycidyl methacrylate copolymer.
[0047] The sealant layer 4 may contain other components in addition to the first polyolefin resin, such as a silane coupling agent, an organic titanate, polyacrylic, polyester, polyurethane, polycarbonate, polyurea, polyamide, a polyolefin emulsion, polyimide, melamine, and phenol.
[0048] The content of the first polyolefin resin in the sealant layer 4 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.
[0049] The thickness of the sealant layer 4 is 2 to 40 μm. When the thickness of the sealant layer 4 is 2 μm or more, sufficient seal strength for protecting the contents can be obtained. When the thickness of the sealant layer 4 is 40 μm or less, the packaging material 10 has excellent tearability regardless of the tearing direction even if it does not have a notch, and the amount of plastic material used can be sufficiently reduced. From the same viewpoint, the thickness of the sealant layer 4 may be 10 μm or less, or may be 5 μm or less. The packaging material 10 having a sealant layer 4 of such a thickness can be suitably used as a packaging material for packaging light-weight contents.
[0050] The sealant layer 4 may be a single layer, or may be a multilayer consisting of two or more layers.
[0051] The sealant layer 4 can be provided by applying a coating liquid containing the first polyolefin resin and a solvent onto the gas barrier layer 3, and drying the coating liquid.
[0052] Examples of the solvent contained in the coating liquid of the sealant layer 4 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Furthermore, from the viewpoint of the environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.
[0053] The melting point of the first polyolefin resin in the coating liquid is preferably 70 to 160°C, more preferably 80 to 120°C. A low melting point has the advantage of lowering the start-up temperature during heat sealing. A high melting point of the first polyolefin resin increases the risk of blocking in a high-temperature environment. In order to prevent blocking, the particle size is preferably large so that the contact area is small. Although not particularly limited, the particle size may be specifically 1 nm or more, 0.1 μm or more, 1 μm or less, 0.7 μm or less, or 0.5 μm or less.
[0054] The tensile breaking strength of the packaging material 10 is 30 to 70 N / 15 mm in the CD and more than 70 N / 15 mm in the MD. Since the tensile breaking strengths of the packaging material 10 in the CD and MD are within the above ranges, the packaging material 10 has excellent tearability in the MD even when it does not have a notch, and has excellent processability during the production of the package. The tensile breaking strength of the packaging material 10 in the CD is preferably 60 N / 15 mm or less because the packaging material 10 has even better tearability. The tensile breaking strength of the packaging material 10 in the MD is preferably 90 N / 15 mm or less because the packaging material 10 has even better tearability. The tensile breaking strength is measured by pulling a test piece (longitudinal length: 100 mm, transverse length: 15 mm) cut out from the packaging material 10 in the longitudinal direction using a tensile tester (test length: 50 mm, pulling speed: 200 mm / min).
[0055] {Second embodiment} The easy-open packaging material according to the second embodiment will be described below. Any points not described below are the same as those of the easy-open packaging material according to the first embodiment unless inconsistencies arise. Fig. 2 is a schematic cross-sectional view showing a packaging material according to the second embodiment. The packaging material 15 according to one embodiment has a laminated structure including a paper base material 1, an anchor coat layer 2, a gas barrier layer 3, an overcoat layer 11, an adhesive layer 12, and a sealant layer 4 in this order.
[0056] [Sealant layer] The sealant layer 4 is provided on the surface of the adhesive layer 12 so as to be in contact with the adhesive layer 12. The sealant layer 4 contains a first polyolefin resin. Examples of the first polyolefin resin include low-density polyethylene resin (LDPE), medium-density polyethylene resin (MDPE), high-density polyethylene resin (HDPE), linear low-density polyethylene resin (LLDPE), ethylene-vinyl acetate copolymer (EVA), propylene homopolymer, ethylene-propylene block copolymer, and ethylene-propylene random copolymer. These may be used alone or in combination of two or more.
[0057] The thickness of the sealant layer 4 is 2 to 40 μm. The thickness of the sealant layer 4 may be 10 μm or more since this tends to improve the strength of the packaging material 15, or may be 20 μm or less since this provides better tearability and allows for a further reduction in the amount of plastic material used. The packaging material 15 having a sealant layer 4 of such a thickness can be suitably used as a packaging material for packaging heavy contents.
[0058] Methods for forming the sealant layer 4 include, for example, extrusion lamination and dry lamination, and from the viewpoint of protecting the gas barrier layer 3, the dry lamination is preferred.
[0059] [Overcoat layer] The overcoat layer 11 is provided on the surface of the gas barrier layer 3 so as to be in contact with the gas barrier layer 3, and contains a second polyolefin resin having a polar group. By providing the overcoat layer 11, the gas barrier property of the packaging material 15 is further improved. In addition, the adhesion between the overcoat layer 11 and the gas barrier layer 3 and the adhesion between the overcoat layer 11 and the adhesive layer 12 are superior to the adhesion between the gas barrier layer 3 and the adhesive layer 12, so that the packaging material 15 including the overcoat layer 11 has excellent adhesion. The packaging material 15 does not need to include the overcoat layer 11.
[0060] The second polyolefin resin may have at least one selected from a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic ester.
[0061] The second polyolefin resin may be a copolymer of ethylene or propylene with an unsaturated carboxylic acid (an unsaturated compound having a carboxyl group, such as acrylic acid or methacrylic acid), an unsaturated carboxylic acid ester, or a salt of a carboxylic acid neutralized with a basic compound. In addition, copolymers of ethylene or propylene with vinyl acetate, epoxy compounds, chlorine compounds, urethane compounds, polyamide compounds, or the like may also be used.
[0062] Specific examples of the second polyolefin resin include a copolymer of an acrylic acid ester and maleic anhydride, an ethylene-vinyl acetate copolymer, and an ethylene glycidyl methacrylate copolymer.
[0063] Such an overcoat layer 11 has excellent flexibility, can suppress cracking of the gas barrier layer 3 after bending (folding), and has excellent adhesion to the gas barrier layer 3. Furthermore, by including the second polyolefin resin, a dense film can be formed due to the crystallinity of the polyolefin, and water vapor barrier properties are exhibited. Furthermore, by having a polar group, adhesion to the gas barrier layer 3 is exhibited.
[0064] The overcoat layer 11 may contain other components in addition to the second polyolefin resin, such as a silane coupling agent, an organic titanate, polyacrylic, polyester, polyurethane, polycarbonate, polyurea, polyamide, a polyolefin emulsion, polyimide, melamine, and phenol.
[0065] The content of the second polyolefin resin in the overcoat layer 11 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.
[0066] The thickness of the overcoat layer 11 may be, for example, 0.05 μm or more, 0.5 μm or more, 1 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. If the thickness of the overcoat layer 11 is 20 μm or less, the adhesion to the gas barrier layer and the gas barrier properties can be sufficiently exhibited while suppressing costs.
[0067] The overcoat layer 11 can be provided by applying a coating liquid containing the second polyolefin resin and a solvent onto the gas barrier layer 3, and drying the coating liquid.
[0068] Examples of the solvent contained in the coating liquid for the overcoat layer 11 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Furthermore, from the viewpoint of the environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.
[0069] The melting point of the second polyolefin resin in the coating liquid is preferably 70 to 160°C, more preferably 80 to 120°C. If the melting point of the second polyolefin resin is high, there is a high possibility of blocking in a high temperature environment. From the viewpoint of preventing blocking, it is better that the particle size is large so that the contact area is small. Although not particularly limited, the particle size may specifically be 1 nm or more, 0.1 μm or more, 1 μm or less, 0.7 μm or less, or 0.5 μm or less.
[0070] [Adhesive layer] The adhesive layer 12 is provided on the surface of the overcoat layer 11. As the adhesive layer 12, various materials can be used as long as they can bond the overcoat layer 11 and the sealant layer 4 to each other, and an example of the adhesive layer 12 is a cured product of a urethane adhesive.
[0071] The urethane adhesive is a resin composition containing a polyol having two or more hydroxyl groups in one molecule and an isocyanate compound having two or more isocyanate groups in one molecule. The urethane adhesive is cured to generate a urethane bond. The urethane adhesive is preferably a two-liquid curing type. The urethane adhesive may have gas barrier properties.
[0072] The thickness of the adhesive layer 12 is preferably 0.1 μm or more from the viewpoint of improving the adhesiveness of the adhesive layer 12, and is preferably 5 μm or less from the viewpoint of further reducing the amount of plastic material used.
[0073] <Packaging bag> 3 is a perspective view showing a gusset bag 20 made of packaging material 10. A packaging bag is manufactured by sealing the opening at the top of the gusset bag 20. The gusset bag 20 has portions where the packaging material 10 is folded (folded portions B1, B2). Folded portion B1 is a portion where the packaging material 10 is folded in a valley direction when viewed from the innermost layer side, while folded portion B2 is a portion where the packaging material 10 is folded in a mountain direction when viewed from the innermost layer side.
[0074] The packaging bag may be formed by folding one sheet of packaging material in half so that the sealant layers 4 face each other, and then folding and heat sealing the sheet into the desired shape, or may be formed by stacking two sheets of packaging material together so that the sealant layers 4 face each other, and then heat sealing the sheet into the bag shape.
[0075] In the packaging bag according to the present embodiment, the heat seal strength is not particularly limited. The heat seal strength can be appropriately changed by changing the thickness of the sealant layer 4. For example, when a light-weight content is to be stored, the heat seal strength may be 2N or more and 10N or less. When a heavy-weight content is to be stored, the heat seal strength is preferably 10N or more.
[0076] The packaging bag can contain food, medicine, and the like. It is particularly suitable for containing food, such as sweets. The packaging bag according to the present embodiment can maintain high gas barrier properties even in a shape having a folded portion.
[0077] In the present embodiment, a gusset bag is given as an example of a packaging bag, but the packaging material according to the above embodiment may be used to produce, for example, a pillow bag, a three-side sealed bag, or a standing pouch. The packaging bag may be made of packaging material 15. EXAMPLES
[0078] Hereinafter, the present disclosure will be described more specifically based on examples and comparative examples, but the present disclosure is not limited to the following examples.
[0079] <Production of packaging materials> Example 1 Paper (clay coated paper, basis weight: 60 g / m) with MD tensile strength of 68 N / 15 mm and CD tensile strength of 33 N / 15 mm. 2 A water-dispersible polyurethane resin was applied to the surface of the paper (paper thickness: 55 μm, clay coat thickness: 5 μm) using a bar coater, and dried in an oven to form an anchor coat layer (thickness: 3 μm). Subsequently, AL deposition was performed on the anchor coat layer to form an AL deposition layer (thickness: 50 nm). A coating liquid containing a polyolefin resin having a carboxyl group and a salt of a carboxyl group (product name: Chemipearl S500, ionomer type, particle size: <0.5 μm, solvent: water and IPA, manufactured by Mitsui Chemicals, Inc.) was applied to the surface of the deposition layer using a bar coater, and dried in an oven to form a sealant layer (thickness: 3 μm) to obtain a packaging material. The weight of the paper in the packaging material is shown in Table 1. The tensile breaking strength of the paper substrate was measured by the method described below.
[0080] Example 2 Except for forming the anchor coat layer using a polyvinyl alcohol-based resin (saponification degree: 98%, polymerization degree: 500), a packaging material was obtained in the same manner as in Example 1. The weight of the paper in the packaging material is shown in Table 1.
[0081] Example 3 A packaging material was obtained in the same manner as in Example 1, except that a linear low-density polyethylene resin (LLDPE) film (thickness: 20 μm) was dry-laminated on the deposition layer using an adhesive (product name: Takelac A525 / Takenate A52, urethane-based two-liquid type, manufactured by Mitsui Chemicals, Inc.). The thickness of the adhesive layer was 2 μm. The weight of the paper in the packaging material is shown in Table 1.
[0082] Example 4 A packaging material was obtained in the same manner as in Example 1, except that a linear low-density polyethylene resin (LLDPE) film (thickness: 40 μm) was dry-laminated on the deposition layer using an adhesive (product name: Takelac A525 / Takenate A52, urethane-based two-liquid type, manufactured by Mitsui Chemicals, Inc.). The thickness of the adhesive layer was 2 μm. The weight of the paper in the packaging material is shown in Table 1.
[0083] Example 5 A packaging material was obtained in the same manner as in Example 1, except that an anchor coat layer was formed using a coating liquid containing a polyolefin resin (product name: Chemipearl S500, ionomer type, particle size: <0.5 μm, solvent: water and IPA, manufactured by Mitsui Chemicals, Inc.). The weight of the paper in the packaging material is shown in Table 1.
[0084] Comparative Example 1 A packaging material was obtained in the same manner as in Example 1, except that a non-oriented polypropylene resin (CPP) film (thickness: 60 μm) was dry laminated on the deposition layer using an adhesive (product name: Takelac A525 / Takenate A52, urethane-based two-liquid type, manufactured by Mitsui Chemicals, Inc.). The thickness of the adhesive layer was 2 μm. The weight of the paper in the packaging material is shown in Table 2.
[0085] Comparative Example 2 Paper (clay-coated paper, basis weight: 60 g / m) with a tensile breaking strength of 46 N / 15 mm in MD and 45 N / 15 mm in CD. 2 A packaging material was obtained in the same manner as in Example 1, except that the following materials were used: paper thickness: 55 μm, clay coat thickness: 5 μm. The weight of the paper in the packaging material is shown in Table 2.
[0086] Comparative Example 3 Paper (clay-coated paper, basis weight: 60 g / m) with a tensile breaking strength of 46 N / 15 mm in MD and 45 N / 15 mm in CD. 2 A packaging material was obtained in the same manner as in Example 1, except that a linear low-density polyethylene resin (LLDPE) film (thickness: 40 μm) was dry laminated on the deposition layer using an adhesive (product name: Takelac A525 / Takenate A52, urethane-based two-component type, manufactured by Mitsui Chemicals, Inc.) and a paper thickness of 55 μm and a clay coat thickness of 5 μm. The thickness of the adhesive layer was 2 μm. The weight of the paper in the packaging material is shown in Table 2.
[0087] Comparative Example 4 Paper (clay-coated paper, basis weight: 60 g / m) with a tensile breaking strength of 46 N / 15 mm in MD and 45 N / 15 mm in CD. 2 A packaging material was obtained in the same manner as in Example 1, except that an anchor coat layer was formed on the surface of the paper (paper thickness: 55 μm, clay coat thickness: 5 μm) using a coating liquid containing a polyolefin resin (product name: Chemipearl S500, ionomer type, particle size: <0.5 μm, solvent: water and IPA, manufactured by Mitsui Chemicals, Inc.). The weight of the paper in the packaging material is shown in Table 2.
[0088] <Evaluation of tearability> The packaging materials according to the examples and the comparative examples were bonded together with the sealant layers facing each other to prepare a three-sided pouch (size: 10 cm square, seal width: 5 mm). Five evaluators were randomly selected from 10 men and 10 women, and the selected evaluators tore the three-sided pouch and evaluated the ease of tearing according to the following criteria. The three-sided pouch was torn so that a tear occurred along the MD of the packaging material constituting the three-sided pouch and the two ends generated on the sides of the three-sided pouch by the tear were separated along a direction perpendicular to the main surface of the three-sided pouch. The worst evaluation result among the evaluation results of the selected evaluators was determined to be the evaluation result of that packaging material. The results are shown in Tables 1 and 2.
[0089] (Evaluation Criteria) A: Easily torn and no stretching of the sealant layer observed B: The sealant layer is stretched even though it can be torn. C: Non-tearable
[0090] <Measurement of tensile breaking strength of paper substrate> Test pieces were cut out from the paper substrates according to the examples and comparative examples. The size of the test piece was 100 mm in MD and 15 mm in CD. The obtained test piece was stored in a high-temperature and high-humidity chamber at standard temperature and humidity (23°C, 50%) for 24 hours, and then the test piece was pulled in the longitudinal direction (MD) with a tensile tester under conditions that satisfy at least one of the following: the test piece was taken out and then measured within 5 minutes, or the temperature and humidity of the test environment was kept at 23°C, 50%. The test piece was pulled in the longitudinal direction (MD) with a tensile tester, and the tensile breaking strength in MD was measured. The test length was 50 mm, and the pulling speed was 200 mm / min. The measurement was performed on five test pieces. The average value of the measured values obtained from the five test pieces was taken as the tensile breaking strength in MD of the paper substrate. In addition, the tensile breaking strength of a test piece with a CD length of 100 mm and a MD length of 15 mm was measured in the same manner as the tensile breaking strength in MD, and the CD tensile breaking strength was taken as the tensile breaking strength.
[0091] <Measurement of tensile breaking strength of packaging materials> Test pieces were cut out from the packaging materials according to the examples and comparative examples. The size of the test piece was 100 mm in MD and 15 mm in CD. The obtained test piece was stored in a high-temperature, high-humidity chamber at standard temperature and humidity (23°C, 50%) for 24 hours, and then the test piece was pulled in the longitudinal direction (MD) with a tensile tester under conditions that satisfy at least one of the following: the test piece was taken out and then measured within 5 minutes, or the temperature and humidity of the test environment was kept at 23°C, 50%. The test piece was pulled in the longitudinal direction (MD) with a tensile tester, and the tensile breaking strength in MD was measured. The test length was 50 mm, and the pulling speed was 200 mm / min. The measurement was performed on five test pieces. The average value of the measured values obtained from the five test pieces was taken as the tensile breaking strength in MD of the packaging material. In addition, the tensile breaking strength of a test piece with a CD length of 100 mm and a MD length of 15 mm was measured in the same manner as the tensile breaking strength in MD, and was taken as the tensile breaking strength in CD. The results are shown in Tables 1 and 2.
[0092] <Measurement of water vapor permeability> The water vapor permeability of the packaging materials according to the examples and comparative examples was measured by the MOCON method. The measurement conditions were a temperature of 40°C and a relative humidity of 90%. The measurement device used was a PERMATRAN (product name, manufactured by MOCON). The results are shown in Tables 1 and 2 in units of [g / m 2 ·day].
[0093] <Evaluation of processing suitability> Bags were made and the contents were filled using the packaging materials according to the examples and comparative examples, and the processing suitability of the packaging materials was evaluated. That is, a raw roll of the packaging material (width: 220 mm) was set in the unwinding section of a vertical pillow filling packaging machine. The packaging material was unwound while tension was applied in the longitudinal direction of the packaging material, and the packaging material was folded so that the sealant layers of the packaging material faced each other to form a cylindrical shape. The cylindrical packaging material was heat-sealed along the width direction and cut along the width direction. 5 g of rice resin was filled into the opening of the packaging material, and the opening was heat-sealed to obtain a package. The bag making conditions were as shown below. During bag making and filling, tension is applied to the packaging material in the longitudinal direction. This tension may cause breaks or cracks in the packaging material. 100 packages were made, and breaks and cracks were visually observed and evaluated according to the following evaluation criteria.
[0094] (Evaluation Criteria) A: No cracks were found in any of the packaging materials out of 100 packaging bags. B: Of 100 packaging bags, none of the packaging bags had a complete break in the packaging material or paper tears, but one or more packaging bags had a crack in part of the packaging material and were completely broken. C: Of 100 packaging bags, one or more packaging bags had completely broken packaging material and paper breaks (Bag making conditions) Bag making speed: 90m / min Packaging bag size: width 100mm x height 150mm Seal width: 10mm
[0095] [Table 1]
[0096] [Table 2] [Explanation of symbols]
[0097] Reference Signs List 1: paper base material, 2: anchor coat layer, 3: gas barrier layer, 4: sealant layer, 10, 15: packaging material, 11: overcoat layer, 12: adhesive layer, 20: gusset bag, B1, B2: folded portion.
Claims
1. A paper substrate; An anchor coat layer; A gas barrier layer; A sealant layer; A packaging material having a laminated structure comprising, in this order, The weight of the paper base material is 50% by mass or more based on the entire packaging material, The thickness of the sealant layer is 2 to 40 μm, the sealant layer comprises a first polyolefin-based resin, The tensile breaking strength of CD is 30 to 70 N / 15 mm; An easy-open packaging material having a tensile breaking strength in the MD of greater than 70 N / 15 mm.
2. The easy-open packaging material according to claim 1 , wherein the first polyolefin resin has at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group.
3. 2. The easy-open packaging material according to claim 1, wherein the sealant layer has a thickness of 2 to 20 μm.
4. The easy-open packaging material according to claim 1 , further comprising an adhesive layer between the gas barrier layer and the sealant layer.
5. an overcoat layer is further provided between the gas barrier layer and the adhesive layer, The easy-open packaging material according to claim 4 , wherein the overcoat layer comprises a second polyolefin resin having at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group.
6. The easy-open packaging material according to claim 1 , wherein the anchor coat layer comprises a third polyolefin resin having at least one selected from the group consisting of a carboxyl group and a salt of a carboxyl group.
7. The easy-open packaging material according to claim 1 , wherein the anchor coat layer contains a polyvinyl alcohol-based resin.
8. The easy-open packaging material according to claim 1 , wherein the anchor coat layer comprises a polyurethane-based resin.
9. A packaging bag comprising the easy-open packaging material according to any one of claims 1 to 7.
10. The packaging bag according to claim 9, having a folded portion.
Citation Information
Patent Citations
Packaging material and packaging bag using package material, and manufacturing method of packaging material
JP2020049913A
Packaging material, and packaging bag including the packaging material, and method for producing the packaging material
JP2020116880A