Cathode active materials, methods of making and using same
Patent Information
- Application Number
- JP2023552383
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-11-13
- Filing Date
- 2021-11-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-11-05
AI Technical Summary
Existing lithium ion batteries face issues with cycling stability and capacity due to interlaminar shrinkage during high voltage charging, leading to cathode instability and reduced cycle life in Ni-rich materials.
A method for producing a composite oxide with a specific formula, x Li2Ni1-y1-y2Mn1y1M1y2O3·(1-x)·LiNi1-zM2zO2, involving controlled heat treatment and lithium source addition in an oxygen-containing atmosphere, to minimize interlaminar shrinkage and enhance cycling stability.
The method results in an electrode active material with minimal interlaminar shrinkage (<1%) and improved cycling stability, retaining higher capacity retention rates compared to conventional methods.
Smart Images

Figure 00000016_0000 
Figure 00000016_0001 
Figure 00000016_0002
Abstract
Description
[Technical field]
[0001] The present invention relates to a compound having the formula x Li2Ni 1-y1-y2 Mn y1 M 1 y2 O3 (1-x) LiNi 1-z M 2 z O2 (wherein x is in the range of 0.01 to 0.5, and z is in the range of 0 to 0.5, preferably 0.01 to 0.4, and more preferably 0.01 to 0.1); M 1 is selected from Ti, Zr, Sn, Ge, Ta, Nb, Sb, W, Mo, and a combination of at least two of the above; M 2 is selected from Na, K, Co, Al, Mg, Fe, Mn, and a combination of at least two of the above, with Co, Al, Mg, Fe, Mn, and a combination of at least two of the above being preferred; 0.1≦y1≦0.75, 0≦y2≦0.05) The present invention relates to a method for producing a composite oxide by The method comprises the steps of: (a) General formula x Ni 1-y1-y2 Mn y1 M 1 y2 (1-x)M 2 Particulate hydroxides, oxides or oxyhydroxides of TM having Mn, M 1 and / or M 2 providing a corresponding species that does not contain (b) a lithium source, and optionally M 1 and / or M 2 The source of Li:(Ni+Mn+M 1 +M 2 ) in a molar ratio of (c) heating the mixture obtained from step (b) to 680-800° C. in an oxygen-containing atmosphere; (d) adding a lithium source; (e) heating the mixture obtained from step (d) to 450-580° C. in an atmosphere containing at least 90% by volume of oxygen; Includes.
[0002] The present invention further relates to electrode active materials and methods of using same. [Background technology]
[0003] Lithiated transition metal oxides are currently used as electrode active materials in lithium-ion batteries. Extensive research and development has been carried out over the past few years to improve properties such as charge density, specific energy, and other properties such as cycle life degradation and capacity loss that adversely affect the life or applicability of lithium-ion batteries. Further efforts are being made to improve the manufacturing methods.
[0004] In a typical process for the preparation of cathode materials for lithium-ion batteries, a so-called precursor is first formed by co-precipitation of a transition metal as a carbonate, oxide, or preferably as a hydroxide, e.g., oxyhydroxide, which may or may not be basic. This precursor is then mixed with a lithium source, e.g., a lithium compound, such as, but not limited to, LiOH, Li2O, or Li2CO3. The lithium compound(s) can be used as hydrate(s) or in dehydrated form. Calcination or calcination, also commonly referred to as thermal or heat treatment of the precursor, is usually carried out at temperatures in the range of 600-1000°C. During the heat treatment, a solid-state reaction takes place to form the electrode active material. The heat treatment is carried out in a heated zone of an oven or kiln.
[0005] A typical type of cathode active material that achieves high energy density is Ni-rich, e.g., at least 80 mol % Ni relative to the non-lithium metal content, but in this case the cycle life is limited due to the problem of cathode instability under charging conditions.
[0006] Existing lithium-ion batteries still have room for improvement, especially in terms of cycling stability and capacity. Numerous theories have been developed regarding cycling stability. Particle aggregate cracking is believed to be one of the main degradation mechanisms of cation-layered Ni-rich materials with cycling. In particular, minimizing the large contraction of interlayer spacing (typically more than 4%) during high-voltage charging is critical to improving the cycling stability of such materials. Summary of the Invention [Problem to be solved by the invention]
[0007] It was therefore an object of the present invention to provide an electrode active material that experiences minimal interlayer shrinkage (≦1% at high voltages) and to provide a method for producing such an electrode active material. [Means for solving the problem]
[0008] Thus, the method and material defined at the outset have been found. The method is also called "method of the invention" or "method according to the invention" below. The method of the invention comprises three steps (a), (b), (c), which are also called step (a), step (b) and step (c) respectively in the context of the present invention. Steps (a), (b) and (c) are carried out sequentially. The method of the invention is described in more detail below. [Brief description of the drawings]
[0009] [Figure 1]Figure 1 shows plots of the XRD patterns of CAM.1 and C-CAM.2. Both CAM.1 and C-CAM.2 have a typical O3 layered structure (space group: R-3m with Bragg peaks). In Figure 1(b), CAM.1 has a superstructure reflection observed around 2θ = 10-15°, which corresponds to the ordering of transition metal ions and Li ions in the transition metal layers of the layered lattice. Since the excess Li does not significantly change the major reflections except the superstructure reflections, CAM.1 maintains the O3 layered structure with excess Li in the transition metal layers in the bulk structure. The superstructure reflections show a honeycomb ordering of Li with respect to Ni / Mn in the Li2Ni0.55Mn0.45O3 domains. [Diagram 2] Figure 2 is a series of plots showing the first charge / discharge voltage curves and dQ / dV curves of C-CAM.2 and CAM.1 at 10 mA / g rate in the 4.3-2.5 V voltage window. In this voltage window, sample C-CAM.2 shows a reversible capacity of ~215 mAh / g in the first cycle, while CAM.1 shows a smaller reversible capacity of ~185 mAh / g in the first cycle. Sample CAM.2 shows a strong plateau around 4.2 V in the charge profile, which can be mainly attributed to the H2-H3 phase transition. The H2-H3 phase transition around 4.2 V is accompanied by a strong discontinuous contraction of the c lattice constant with volume change, which ultimately leads to fatigue and mechanical degradation. Compared to this 4.2 V plateau of sample CAM.2, CAM.1 shows a weaker plateau. [Diagram 3]Figure 3 is a series of plots showing the first charge / discharge voltage curves and dQ / dV curves of C-CAM.2 and CAM.1 at 10 mA / g rate in the voltage window from 4.8 to 2.5 V. Sample CAM.2 shows a reversible capacity of ~250 mAh / g in the first cycle, which is similar to the theoretical capacity (~275 mAh / g) due to Ni redox. Also, the voltage profile of C-CAM.2 is almost similar to the voltage profile from 4.3 to 2.5 V without any additional plateaus. However, CAM.1 shows a plateau near 4.5 V in the first charge profile, which is mainly due to a combination of reversible oxygen oxidation and irreversible oxygen loss from the layered lattice, both made possible by / indicating the presence of Li2Ni0.55Mn0.45O3 domains. Also, as shown in Figure 4(c), the Li-rich sample exhibits a higher reversible capacity of ~230 mAh / g in the first cycle than the theoretical capacity (~200 mAh / g) due to Ni redox reaction, which is attributed to the reversible oxygen redox reaction. Without being bound by any theory, the difference between the charge and discharge capacities is attributed to an irreversible oxidation reaction, possibly involving oxygen gas release from the material. Thus, CAM.1 can be cycled at a lower voltage window to achieve a lower capacity but no oxygen gas release occurs; or, by cycling to a higher voltage (>4.3 V), a higher capacity can be achieved but potentially oxygen gas release occurs. In both cases, the H2-H3 phase transition and interlayer shrinkage are mitigated. [Figure 4] FIG. 4 shows the cycling performance of CAM.1 and C-CAM.2 at 10 mA / g between 4.8 and 2.5 V for 20 cycles. C-CAM.2 shows 88.1% capacity retention at 20 cycles. In contrast, CAM.1 shows improved capacity retention (93.5%) over the first 20 cycles. Without wishing to be bound by any theory, it is believed that the superior cycling performance of CAM.1 is due to the suppression of the H2-H3 phase transition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The method of the present invention is directed to a compound of the formula x LiNi1-y1-y2 Mn y1 M 1 y2 O3 (1-x) LiNi 1-z M 2 z O2 (In the formula, x is in the range of 0.01 to 0.5, preferably 0.1 to 0.3, z is in the range of 0 to 0.5, preferably 0.01 to 0.4, and more preferably 0.01 to 0.1; M 1 is selected from Ti, Zr, Sn, Ge, Ta, Nb, Sb, W, Mo, and a combination of at least two of the above, with Ti, Zr, Sn, W, Mo, and a combination of at least two of the above being preferred; M 2 is one of Co, Al, Mg, Mn, or Fe, and combinations of at least two of the above, with Co, Al, Mn, and combinations of at least two of the above being preferred; 0.1≦y1≦0.75, 0≦y2≦0.05) This is a method for producing a composite oxide by the above process.
[0011] Preferably, 0.15≦(y1+y2)≦0.6, and more preferably, 0.3≦(y1+y2)≦0.55.
[0012] From the above formula, Ni, Mn, M 1 and M 2 We can conclude that the average oxidation state of is equal to 4x+3(1-x).
[0013] In a preferred embodiment, z≦0.1 and M 2 contains at least one of Co, Mn and Al. Even more preferably, M 2 does not contain Co.
[0014] Some elements are ubiquitous. In the context of the present invention, trace amounts of ubiquitous metals such as sodium, calcium or zinc as impurities are not taken into account in the present specification. In this case of precursors, trace amounts in this context mean amounts of 0.02 mol % or less relative to the total metal content of the starting material.
[0015] The method of the present invention comprises the steps of: (a) Compounds of general formula x Ni, hereafter referred to as precursors 1-y1-y2 Mn y1 M 1 y2 (1-x)M 2 Particulate hydroxides, oxides or oxyhydroxides of TM having Mn, M 1 and / or M 2 providing a corresponding species that does not contain
[0016] In one embodiment of the present invention, the precursor provided in step (a) is composed of secondary particles that are agglomerates of primary particles.Preferably, the precursor provided in step (a) is composed of spherical secondary particles that are agglomerates of primary particles.Even more preferably, the precursor provided in step (a) is composed of spherical secondary particles that are agglomerates of spherical primary particles or platelets.
[0017] In one embodiment of the present invention, the precursor provided in step (a) has an average particle size (D50) in the range of 3 to 20 μm, preferably 5 to 16 μm. The average particle size can be determined, for example, by light scattering or laser diffraction or electroacoustic spectroscopy. The particles are usually composed of aggregates from primary particles, and the above particle size refers to the particle size of the secondary particles.
[0018] In one embodiment of the invention, the specific surface area (BET) of the precursor is between 2 and 15 m, determined by nitrogen adsorption, for example according to DIN-ISO 9277:2003-05. 2 / g range.
[0019] In one embodiment of the invention, the precursor may have a particle size distribution span in the range of 0.5 to 0.9, the span being defined as [(D90)-(D10)] divided by (D50), all determined by LASER analysis. In another embodiment of the invention, the precursor may have a particle size distribution span in the range of 1.1 to 1.8.
[0020] The precursors are Ni, Mn, and, where applicable, M 1 and M 2 and then drying in air.
[0021] In step (b), a lithium source and, optionally, M 1 and / or M 2 The source of Li:(Ni+Mn+M 1 +M 2 ) to the precursor.
[0022] Examples of lithium sources include Li2O, LiNO3, LiOH, Li2O2, Li2CO3, each anhydrous or hydrated where applicable, e.g. LiOH·H2O. LiOH, Li2O and Li2O2 are preferred. A more preferred lithium source is lithium hydroxide.
[0023] Examples of suitable equipment for carrying out step (b) include tumbler mixers, high shear mixers, plowshare mixers and free-fall mixers. At laboratory scale, mortars with pestles and ball mills can be used as well.
[0024] In one embodiment of the invention, step (b) is carried out for a period of from 1 minute to 10 hours, preferably from 5 minutes to 1 hour.
[0025] In one embodiment of the invention, the mixing in step (b) is carried out without external heating.
[0026] In one embodiment of the invention, no dopant is added in step (b).
[0027] In a particular embodiment of the invention, in step (b) oxides, hydroxides or oxyhydroxides of Mg, Al, Sn, Ge, Ti, Zr, Co, Mn and Al, preferably of Al, Ti, Zr or Ge, hereinafter also referred to as dopants, are added, or a combination of at least two of the above.
[0028] Such dopants are selected from the oxides, hydroxides and oxyhydroxides of Mg, Ti, Zr, Mo, W, Co, Mn, Nb and Ta, and especially Al. Lithium titanate can also be used as a source of titanium. Examples of dopants include TiO2 selected from rutile and anatase (preferably anatase), further basic titania such as TiO2·aq, TiO(OH)2, further Li4Ti5O 12 , ZrO2, Zr(OH)4, ZrO2·aq, Li2ZrO3, ZrO(OH)2, as well as MnO, Mn2O3, Mn3O4, MnO2, Mn(OH)2, MoO2, MoO3, Fe(OH)2, Fe(OH)3, Fe2O3, Fe3O4, SnO2, GeO2, Ta2O5, Sb2O3, Sb2O5, "NbO2" (Nb2O4), Nb2O5, WO2, WO3, MgO, Mg(OH)2, Mg(NO3)2, Nb2O5, as well as Al(OH)3, Al2O3, Al2O3·aq and AlOOH. Al compounds, such as Al(OH)3, α-Al2O3, γ-Al2O3, Al2O3·aq and AlOOH, are preferred. Even more preferred dopants are Al2O3 selected from α-Al2O3, γ-Al2O3, with γ-Al2O3 being most preferred.
[0029] In one embodiment of the present invention, such dopants are 1 to 200 m 2 / g, preferably 50 to 150m 2 / g。 The specific surface area (BET) can be determined by nitrogen adsorption, for example according to DIN-ISO 9277: 2003-05.
[0030] In one embodiment of the present invention, such dopants are nanocrystalline. Preferably, the average crystallite size of the dopant is at most 100 nm, preferably at most 50 nm, even more preferably at most 15 nm. The smallest diameter may be 4 nm.
[0031] In one embodiment of the present invention, such dopant(s) are particulate material(s) having an average diameter (D50) in the range of 1 to 10 μm, preferably 2 to 4 μm. The dopant(s) are usually in the form of aggregates. The particle size refers to the diameter of said aggregates.
[0032] In a preferred embodiment, the dopant(s) is applied in an amount up to 1.5 mol %, preferably between 0.1 and 0.5 mol % (relative to the total metal content of the respective precursor).
[0033] Although it is possible in step (b) to add an organic solvent, such as glycerol or glycol, or water and mix in a ball mill, it is preferred that step (b) is carried out dry, i.e. without the addition of water or organic solvent.
[0034] From step (b) a mixture is obtained, which is then heat treated in an oxygen-containing atmosphere as follows: (c) heating the mixture obtained from step (b) to 680-800° C., preferably 700-750° C., in an oxygen-containing atmosphere; (d) adding a lithium source; and (e) heating the mixture from step (d) to 450-580°C, preferably 500-580°C, more preferably 525-575°C in an atmosphere containing at least 90% by volume of oxygen.
[0035] Step (c) may be carried out once or twice.
[0036] The atmosphere in step (c) is oxidizing, for example air or a mixture of air and a non-oxidizing gas such as nitrogen or argon, or pure oxygen. The atmosphere in step (c) is preferably air or so-called synthetic air, a mixture of 21% by volume of oxygen and 79% by volume of nitrogen, determined under normal conditions. Even more preferred is pure oxygen.
[0037] The oxygen atmosphere in step (e) contains at least 90% by volume of oxygen. Thus, the oxygen atmosphere in step (e) may be pure oxygen or oxygen diluted with a small amount of a non-oxidizing gas, such as, for example, oxygen diluted with less than 10% by volume of nitrogen or argon, determined under normal conditions. Even more preferably, the atmosphere in step (e) is pure oxygen.
[0038] Steps (c) and (e) may be carried out in the same vessel or in different vessels.
[0039] In one embodiment of the present invention, steps (c) and (e) are carried out in a roller hearth kiln, a pusher kiln or a rotary kiln, or a combination of at least two of them. A rotary kiln has the advantage that the homogenization of the material produced therein is very good. In roller hearth kilns and pusher kilns, different reaction conditions for different steps can be set very easily. In laboratory scale experiments, box furnaces, tube furnaces and split tube furnaces can also be used.
[0040] In one embodiment of the present invention, steps (c) and (e) of the present invention are carried out under a forced flow of gas, such as air, oxygen and oxygen-enriched air. Such a gas flow may be called a forced gas flow. Such a gas flow may be in the range of 0.5 to 15 m 3 The specific flow rate may be in the range of 1 / (h·kg) / (h·kg), and the particulate complex oxide of the present invention may be obtained. The volume is determined under normal conditions (298 Kelvin and 1 atm). The forced gas flow is useful for removing gaseous cleavage products such as water.
[0041] In one embodiment of the present invention, steps (c) and (e) have a duration ranging from 2 to 30 hours, preferably from 10 to 24 hours, more preferably from 5 to 20 hours. In this context, the cooling time is ignored.
[0042] The method of the present invention includes a step (d) of adding a lithium source between steps (c) and (e). It is preferable to cool the intermediate from step (c) to a maximum of 100° C., for example 20 to 50° C., before adding the lithium source. The Li:(Ni+Mn+M 1 +M 2 The molar amount of ) is in the range of 0.01 to 0.6, preferably 0.1 to 0.4, and further more preferably 0.1 to 0.2.
[0043] The lithium source added in step (d) is selected from the same compounds as in step (b) and may be different or the same as in step (b). Preferred lithium sources in step (d) are Li2O2, LiOH and LiNO3, respectively, either free of water or as a hydrate.
[0044] The mixing in step (d) can be carried out similarly to step (d), mutatis mutandis.
[0045] After the heat treatment according to step (e), the electrode active material thus obtained is cooled before being further processed. Additional (optional) steps before the electrode active material obtained is further processed are sieving and deagglomeration steps.
[0046] After carrying out steps (a) to (e) of the method of the invention, an electrode active material is obtained which fulfills the objectives as explained at the beginning.
[0047] In one embodiment of the present invention, after step (b) and before step (c), a pre-baking step is performed, for example at a temperature in the range of 150-300° C. Said pre-baking step may have a duration in the range of 1-5 hours.
[0048] In one embodiment of the present invention, the pre-baking step is carried out in an atmosphere containing, for example, 20 to 100% by volume, preferably 60 to 95% by volume of oxygen, determined at room temperature.
[0049] In one embodiment of the invention, the process of the invention comprises an additional step (f) subsequent to step (e), said step (f) being selected from a coating step and a wet processing step.
[0050] Another aspect of the present invention relates to an electrode active material, hereinafter also referred to as the inventive electrode active material or the inventive cathode active material.
[0051] The electrode active material of the present invention has the formula x·Li2Ni 1-y1-y2 Mn y1 M 1 y2 O3 (1-x) LiNi 1-z M 2 z It is a complex oxide of O2, where the variables are defined as follows: x is in the range of 0.01 to 0.5, preferably 0.1 to 0.3; z is in the range of 0 to 0.5, preferably 0.01 to 0.4, and more preferably 0.01 to 0.1; M 1 is selected from Ti, Zr, Sn, Ge, Ta, Nb, Sb, W, Mo, and a combination of at least two of the above, with Ti, Zr, Sn, W, Mo, and a combination of at least two of the above being preferred; M 2 is one of Na, K, Co, Al, Mg, Fe, or Mn, and a combination of at least two of the above, with Co, Al, Mg, Fe, or Mn, and a combination of at least two of the above being preferred, and Co, Al, Mn, and a combination of at least two of the above being more preferred; 0.1≦y1≦0.75, 0≦y2≦0.05.
[0052] Preferably, 0.15≦(y1+y2)≦0.6, and more preferably, 0.3≦(y1+y2)≦0.55.
[0053] From the above formula, M 1 The average oxidation state of M is +4. 2 It can be concluded that the average oxidation state of is +3.
[0054] In a preferred embodiment, z≦0.1 and M 2 contains at least one of Co, Mn and Al. Even more preferably, M 2 In the context of the present invention, "Co-free" means that M 2 This means that the Co content is 0.5 mol % or less.
[0055] In one embodiment of the electrode active material of the present invention, domains are observed, for example, by transmission electron microscopy ("TEM") or high-resolution transmission electron microscopy. In such domains, preferably Li2Ni 1-y1-y2 Mn y1 M 1 y2 O3 domain and LiNi 1-z M 2 z Both cations in the O2 domain show a substantially layered order, where Li2Ni 1-y1-y2 Mn y1 M 1 y2 The O3 domain is Li and Li 1 / 3 [Ni 1-y1-y2 Mn y1 M 1 y2 ] 2 / 3 The cation layers are alternating, LiNi 1-z M 2 z The O2 domain is Ni / M 2 and Li cation layers alternate. 1-y1-y2 Mn y1 M 1 y2 Li in the O3 domain 1 / 3 [Ni 1-y1-y2 Mny1 M 1 y2 ] 2 / 3 The cation layers exhibit a substantially honeycomb-type cation order, as determined by the presence of in-plane superstructure peaks in the X-ray diffraction diagram, where each Li cation has no further Li cations as nearest neighbors within the same cation layer.
[0056] Some elements are ubiquitous. In the context of the present invention, trace amounts of ubiquitous metals such as sodium, calcium or zinc as impurities are not taken into account in the present specification. In this case of precursors, trace amounts in this context mean amounts of 0.02 mol % or less relative to the total metal content of the starting material.
[0057] The electrode active material of the present invention is particulate. In one embodiment of the present invention, the average particle size (D50) of the electrode active material of the present invention is in the range of 2 to 15 μm, preferably 5 to 10 μm. The average particle size (D50) in the context of the present invention refers to the average value of the particle size based on the volume, which can be determined, for example, by light scattering, and refers to the particle size of secondary particles.
[0058] In one embodiment of the present invention, the specific surface area (BET) of the electrode active material of the present invention is between 0.1 and 1.5 m, determined by nitrogen adsorption, for example according to DIN-ISO 9277:2003-05. 2 / g range.
[0059] In one embodiment of the present invention, the electrode active material of the present invention may have a particle size distribution span in the range of 0.5 to 0.9, the span being defined as [(D90)-(D10)] divided by (D50), all determined by LASER analysis. In another embodiment of the present invention, the electrode active material of the present invention may have a particle size distribution span in the range of 1.1 to 1.8.
[0060] In one embodiment of the present invention, the electrode active material of the present invention has a capacitance of, for example, 2.9 to 3.7 g / cm 3 It has a high compressed density, which can be obtained at a pressure of 250 MPa.
[0061] In one embodiment of the invention, the electrode active material of the invention contains a measurable amount of Ni in the lithiated state as determined by the presence of an absorption peak at 855 eV at the Ni L3 edge. 4+ Contains a cation.
[0062] A further aspect of the present invention relates to electrodes comprising at least one electrode active material according to the present invention. These are particularly useful for lithium-ion batteries. Lithium-ion batteries comprising at least one electrode according to the present invention show very good discharge behavior. Electrodes comprising at least one electrode active material according to the present invention are also referred to as cathodes of the present invention or cathodes of the present invention below.
[0063] In particular, the cathode of the present invention comprises (A) at least one electrode active material of the present invention; (B) carbon in a conductive state, and (C) a binder material, also called binder (C), and preferably (D) Current collector Contains:
[0064] In a preferred embodiment, the cathode of the present invention comprises, based on the sum of (A), (B) and (C), (A) 80 to 98 mass % of the electrode active material of the present invention, (B) 1 to 17 mass% carbon, (C) 1 to 15 mass % of a binder material Contains:
[0065] The cathodes according to the present invention may include additional components. They may include a current collector, such as, but not limited to, aluminum foil. They may further include conductive carbon and a binder.
[0066] The cathode according to the present invention contains a conductively modified carbon, also called carbon (B) for short, which can be selected from soot, activated carbon, carbon nanotubes, graphene, and graphite, and combinations of at least two of the above.
[0067] Suitable binders (C) are preferably selected from organic (co)polymers. Suitable (co)polymers, i.e. homopolymers or copolymers, can be selected, for example, from (co)polymers obtainable by anionic, catalytic or free radical (co)polymerization, in particular from polyethylene, polyacrylonitrile, polybutadiene, polystyrene and copolymers of at least two comonomers selected from ethylene, propylene, styrene, (meth)acrylonitrile and 1,3-butadiene. Polypropylene is also suitable. Polyisoprene and polyacrylates are furthermore suitable. Polyacrylonitrile is particularly preferred.
[0068] In the context of the present invention, polyacrylonitrile is understood to mean not only polyacrylonitrile homopolymers but also copolymers of acrylonitrile with 1,3-butadiene or with styrene. Polyacrylonitrile homopolymers are preferred.
[0069] In the context of the present invention, polyethylene refers not only to homopolyethylenes, but also to copolymerized ethylene with at least 50 mol % and up to 50 mol % of at least one further comonomer, such as α-olefins, such as propylene, butylene (1-butene), 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-pentene, and also isobutene, vinyl aromatics, such as styrene, and also (meth)acrylic acid, vinyl acetate, vinyl propionate, C1-C2 copolymers of (meth)acrylic acid. 10-alkyl esters, in particular methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, 2-ethylhexyl acrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, and also copolymers of ethylene with maleic acid, maleic anhydride and itaconic anhydride. The polyethylene may be HDPE or LDPE.
[0070] In the context of the present invention, polypropylene is understood to mean not only homopolypropylene but also copolymers of propylene with at least 50 mol % copolymerized propylene and up to 50 mol % of at least one further comonomer, such as ethylene, and α-olefins, such as butylene, 1-hexene, 1-octene, 1-decene, 1-dodecene and 1-pentene. The polypropylene is preferably isotactic polypropylene or essentially isotactic polypropylene.
[0071] In the context of the present invention, polystyrene refers not only to homopolymers of styrene, but also to C1-C4 copolymers of acrylonitrile, 1,3-butadiene, (meth)acrylic acid, and (meth)acrylic acid. 10 -alkyl esters, divinylbenzene, in particular 1,3-divinylbenzene, 1,2-diphenylethylene and α-methylstyrene copolymers are also understood to mean.
[0072] Another preferred binder (C) is polybutadiene.
[0073] Other suitable binders (C) are selected from polyethylene oxide (PEO), cellulose, carboxymethyl cellulose, polyimides and polyvinyl alcohol.
[0074] In one embodiment of the invention, the binder (C) has an average molecular weight M ranging from 50,000 g / mol to 1,000,000 g / mol, preferably up to 500,000 g / mol. W The (co)polymers are selected from those having the formula:
[0075] The binder (C) may be a crosslinked or non-crosslinked (co)polymer.
[0076] In a particularly preferred embodiment of the present invention, the binder (C) is selected from halogenated (co)polymers, in particular fluorinated (co)polymers.Halogenated or fluorinated (co)polymers are understood to mean (co)polymers that contain at least one (co)polymerized (co)monomer with at least one halogen atom or at least one fluorine atom per molecule, more preferably at least two halogen atoms or at least two fluorine atoms per molecule.Examples include polyvinyl chloride, polyvinylidene chloride, polytetrafluoroethylene, polyvinylidene fluoride (PVdF), tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), vinylidene fluoride-tetrafluoroethylene copolymer, perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, and ethylene-chlorofluoroethylene copolymer.
[0077] Suitable binders (C) are especially polyvinyl alcohol and halogenated (co)polymers such as polyvinyl chloride or polyvinylidene chloride, especially fluorinated (co)polymers such as polyvinyl fluoride and especially polyvinylidene fluoride and polytetrafluoroethylene.
[0078] The cathode of the present invention may comprise 1 to 15% by weight of binder(s) relative to the electrode active material of the present invention. In other embodiments, the cathode of the present invention may comprise 0.1 to less than 1% by weight of binder(s).
[0079] A further aspect of the invention is a battery containing at least one cathode comprising the electrode active material of the invention, carbon and a binder, at least one anode, and at least one electrolyte.
[0080] The cathode embodiments of the present invention have already been described in detail above.
[0081] The anode may contain at least one anode active material, such as carbon (graphite), TiO2, lithium titanium oxide, silicon, or tin. The anode may further contain a current collector, such as a metal foil, such as copper foil.
[0082] The electrolyte may include at least one non-aqueous solvent, at least one electrolyte salt, and optionally, additives.
[0083] The non-aqueous solvent for the electrolyte may be liquid or solid at room temperature and is preferably selected from polymers, cyclic or acyclic ethers, cyclic and acyclic acetals, and cyclic or acyclic organic carbonates.
[0084] Examples of suitable polymers are in particular polyalkylene glycols, preferably poly-C1-C4-alkylene glycols and in particular polyethylene glycols, where the polyethylene glycols may contain up to 20 mol % of one or more C1-C4-alkylene glycols. The polyalkylene glycols are preferably polyalkylene glycols with two methyl or ethyl end caps.
[0085] The molecular weight M of suitable polyalkylene glycols, particularly suitable polyethylene glycols, W may be at least 400 g / mol.
[0086] The molecular weight M of suitable polyalkylene glycols, particularly suitable polyethylene glycols, W can be up to 5,000,000 g / mol, preferably up to 2,000,000 g / mol.
[0087] Examples of suitable acyclic ethers are, for example, diisopropyl ether, di-n-butyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, with 1,2-dimethoxyethane being preferred.
[0088] Examples of suitable cyclic ethers are tetrahydrofuran and 1,4-dioxane.
[0089] Examples of suitable acyclic acetals are, for example, dimethoxymethane, diethoxymethane, 1,1-dimethoxyethane and 1,1-diethoxyethane.
[0090] An example of a suitable cyclic acetal is 1,3-dioxane, and especially 1,3-dioxolane.
[0091] Examples of suitable acyclic organic carbonates are dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate.
[0092] Examples of suitable cyclic organic carbonates are compounds according to general formulae (II) and (III) [ka] (In the formula, R 1 , R 2 and R 3 can be the same or different and are selected from hydrogen and C1-C4-alkyl, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl, preferably R 2 and R 3 (Both cannot be tert-butyl).
[0093] In a particularly preferred embodiment, R 1 is methyl, R 2 and R 3 are each hydrogen or R 1 , R 2 and R 3are hydrogen.
[0094] Another preferred cyclic organic carbonate is vinylene carbonate of formula (IV).
[0095] [ka]
[0096] Preferably, the solvent or solvents are used in an aqueous state, ie with a water content in the range of 1 ppm to 0.1% by weight, which can be determined, for example, by Karl Fischer titration.
[0097] The electrolyte (C) further comprises at least one electrolyte salt. Suitable electrolyte salts are in particular lithium salts. Examples of suitable lithium salts are LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC(C n F 2n+1 SO2)3, lithium imide, e.g. LiN(C n F 2n+1 SO2)2 (wherein n is an integer ranging from 1 to 20), LiN(SO2F)2, Li2SiF6, LiSbF6, LiAlCl4, and compounds of the general formula (C n F 2n+1 SO2) t It is the salt of YLi. where t=1 when Y is selected from oxygen and sulfur; when Y is selected from nitrogen and phosphorus, t=2; When Y is selected from carbon and silicon, t=3).
[0098] Preferred electrolyte salts are selected from LiC(CF3SO2)3, LiN(CF3SO2)2, LiPF6, LiBF4, LiClO4, with LiPF6 and LiN(CF3SO2)2 being particularly preferred.
[0099] In an embodiment of the invention, the battery according to the invention comprises one or more separators by which the electrodes are mechanically separated. Suitable separators are polymer films, especially porous polymer films, which are unreactive towards metallic lithium. Particularly suitable materials for the separators are polyolefins, especially film-forming porous polyethylene and film-forming porous polypropylene.
[0100] A separator made of polyolefin, particularly polyethylene or polypropylene, may have a porosity in the range of 35 to 45%. A suitable pore size is, for example, in the range of 30 to 500 nm.
[0101] In another embodiment of the present invention, the separator can be selected from PET nonwoven fabrics filled with inorganic particles. Such separators can have a porosity in the range of 40-55%. Suitable pore sizes are, for example, in the range of 80-750 nm.
[0102] The battery according to the invention further comprises a housing which may have any shape, for example a cube, or the shape of a cylindrical disk or can. In one variant, a metal foil configured as a pouch is used as the housing.
[0103] The battery according to the invention exhibits good discharge behaviour, for example very good discharge and cycling behaviour at low temperatures (below 0° C., for example even up to below −10° C.).
[0104] The battery according to the present invention may comprise two or more electrochemical cells that are combined with each other, for example, connected in series or connected in parallel. A series connection is preferred. In the battery according to the present invention, at least one electrochemical cell contains at least one cathode according to the present invention. Preferably, in the electrochemical cell according to the present invention, the majority of the electrochemical cells contain the cathode according to the present invention. Even more preferably, in the battery according to the present invention, all the electrochemical cells contain the cathode according to the present invention.
[0105] The present invention further provides a method for using the battery according to the present invention in equipment, especially mobile equipment.Examples of mobile equipment are vehicles, such as automobiles, bicycles, aircraft, or water vehicles, such as boats or ships.Other examples of mobile equipment are manually operated, such as computers, especially laptops, phones, or powered hand tools, for example in the construction sector, especially drills, battery-powered drivers, or battery-powered staplers.
[0106] The present invention is further illustrated by the following examples. EXAMPLES
[0107] General: Li2O2 (90% purity) and LiOH·H2O were purchased from Sigma Aldrich. rpm: Revolutions per minute.
[0108] Example 1: Preparation of CAM.1 of the invention Example 1 is Li-excess x·Li2Ni 1-y1-y2 Mn y1 M 1 y2 O3 (1-x) LiNi 1-z M 2 z O2 (where x = 0.22, y1 = 0.45, y2 = z = 0) (i.e., 0.22 Li2Ni 0.55 Mn 0.45 O3 0.78 LiNiO2, Li 1.1 [Ni 0.9 Mn 0.1 ] 0.9 O2 or Li 1.1 Ni 0.81 Mn 0.09 The synthesis of O2, CAM.1) is described below.
[0109] Step (a.1): Spherical Ni was prepared by combining an aqueous solution of nickel and manganese sulfate (1.65 mol / kg solution) with a 25% by weight aqueous solution of NaOH using ammonia as a complexing agent. 0.9 Mn 0.1(OH)2 precursor was obtained. The pH value was set to 12.6. The freshly precipitated Ni(OH)2 was washed with water, sieved and dried at 120 °C for 12 h. P-CAM.1 was obtained. Average particle size (D50): 10 μm.
[0110] Step (b.1): 5.0 g of P-CAM.1 and 2.383 g of LiOH·H2O (with a molar ratio of transition metal to lithium of 1:1) were mixed and milled in a planetary ball mill at 300 rpm for 1 h without the use of a solvent. A mixture was obtained.
[0111] Step (c.1): The mixture obtained from step (b.1) was heated in a tube furnace in an atmosphere of 100% oxygen to 200°C at a heating rate of 3°C / min for 2 hours and then cooled to room temperature. After re-grinding, the mixture was calcined in an atmosphere of 100% O2 at 700°C for 24 hours and then allowed to cool naturally to room temperature.
[0112] Step (d.1): The material produced in step (c.1) was mixed with Li2O2 by mixing 0.25 g of the intermediate from step (c.1) and 0.0145 g of Li2O2 using a mortar and pestle.
[0113] Step (e.1): The resulting mixture was then heated in a tube furnace in an atmosphere of 100% O2 at a heating rate of 3°C / min to 550°C for 20 hours, and then allowed to cool naturally to room temperature. CAM.1 was obtained.
[0114] Comparative Example 2: Production of C-CAM.2 The same procedure as in Example 1 was carried out, except that steps (d.1) and (e.1) were omitted, to obtain Li 1.0 Ni0 .9 Mn 0.1 A stoichiometric layered material, C-CAM.2, was fabricated with a composition of O2.
[0115] Example 3: Preparation of cathode active material CAM.3 of the present invention Step (b.3): 3.0 g of P-CAM.1 and 1.752 g of LiOH·H2O (the molar ratio of transition metal to lithium is 1:1) were mixed and milled in a tube mill at 8000 rpm for 5 min without using a solvent. A mixture was obtained.
[0116] Step (c.3): The mixture obtained from step (b.3) was heated in a tubular furnace in 100% oxygen atmosphere to 200° C. at a heating rate of 3° C. / min for 2 hours, then heated to 750° C. in 100% oxygen atmosphere for 15 hours, and then allowed to cool naturally to room temperature.
[0117] Step (d.3): The material produced in step (c.3) was mixed with Li2O2 by mixing 0.5 g of the intermediate from step (c.3) and 0.0239 g of Li2O2 using a mortar and pestle. The overall molar ratio of Li to transition metals was 1.1:0.9.
[0118] Step (e.3): The resulting mixture was then heated in a tube furnace in an atmosphere of 100% O2 at a heating rate of 3°C / min to 570°C for 15 hours, and then allowed to cool naturally to room temperature. CAM.3 was obtained.
[0119] Cathode Active Material Evaluation: - Characterization of the cathode active materials: XRD patterns of CAM.1 and C-CAM.2 were recorded with Mo Kα radiation from 5° to 45°. - Battery characteristics: Electrochemical performance was evaluated using CR2032 at 2.5-4.8V and 2.5-4.3V. The cathode was prepared by mixing 80% by weight of active material with 10% by weight of carbon black and 0% by weight of PVDF binder and casting the mixture into a thin sheet of about 150 μm on Al foil using a doctor blade. Coin cells were assembled using the thus-prepared cathode, lithium foil anode, 1M LiPF6 in ethylene carbonate / diethyl carbonate (EC / DEC) electrolyte, and Celgard polypropylene separator.
Claims
1. Formula x Li 2 Ni 1-y Mn y O 3 ・(1-x)・LiNiO 2 (wherein x ranges from 0.1 to 0.5; 0.1≦y≦0.75) A method for producing a cobalt-free composite oxide according to the present invention, The method comprises the steps of: (a) General formula x・Ni 1-y Mn y Providing a particulate hydroxide, oxide or oxyhydroxide of TM having (1-x)Ni; (b) adding a source of lithium, and optionally at least one oxide, hydroxide or oxyhydroxide of Mn, in a molar ratio of Li:(Ni+Mn) of 0.9:1 to 1.1:1; (c) heating the mixture resulting from step (b) to 680-800° C. in an oxygen-containing atmosphere; (d) adding a lithium source; (e) heating the mixture resulting from step (d) to 450-580° C. in an atmosphere containing at least 90% by volume of oxygen; A method comprising:
2. 2. The method of claim 1 , wherein 0.15≦y≦0.
6.
3. 3. The method of claim 1 or 2, wherein steps (c) and (e) are carried out under a forced flow of gas.
4. 4. The method of claim 1, wherein the lithium source is selected from lithium hydroxide, lithium carbonate, lithium nitrate, and lithium oxide.
5. 5. The method of claim 1, wherein x is in the range of 0.1 to 0.
3.
6. 6. The method according to any one of claims 1 to 5, wherein the method comprises an additional step (f) following step (e), said step (f) being selected from a coating step and a wet processing step.
7. Composition x・Li 2 Ni 1-y Mny O 3 ・(1-x)・LiNiO 2 (wherein x ranges from 0.1 to 0.5; 0.1≦y≦0.75) A particulate composite oxide not containing cobalt.
8. 8. The composite oxide particulate according to claim 7, wherein 0.15≦y≦0.
6.
9. The particulate composite oxide according to claim 7 or 8, wherein x is in the range of 0.1 to 0.
3.
10. Li 2 Ni 1-y Mn y O 3 Domain and LiNiO 2 Both cations in the domain exhibit a substantially layered order, Li 2 Ni 1-y Mn y O 3 The domain is a Li cation layer and a Li 1/3 [Ni 1-y Mn y ] 2/3 The cation layers are alternated, LiNiO 2 The domains exhibit alternating Ni and Li cation layers, and Li 2 Ni 1-y Mn y O 3 Li in the domain 1/3 [Ni 1-y Mn y ] 2/3 10. The particulate complex oxide according to claim 7, wherein the cation layers exhibit a substantially honeycomb-type cation order, and no Li cation has another Li cation as a nearest neighbor cation within the same cation layer.
11. (A) at least one particulate composite oxide according to any one of claims 7 to 10; (B) carbon in a conductive state; (C) at least one binder a cathode.
12. 12. An electrochemical cell comprising the cathode of claim 11.