Battery cell, preparation method thereof and lithium ion battery

By introducing a safety coating into the positive electrode of the lithium battery, the problem of difficult to take into account both the mechanical safety performance of the battery cell and the safety performance of the thermal abuse are improved, and the mechanical safety and heat box performance of the battery are improved without changing the original process. Low temperature and rate discharge performance.

CN118970147AActive Publication Date: 2024-11-15ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411453779.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-17
Publication Date
2024-11-15
Estimated Expiration
2044-10-17

AI Technical Summary

Technical Problem

The prior art cannot effectively improve the mechanical safety performance and thermal abuse safety performance of lithium battery cells at the same time, and conventional methods have problems of long development cycles and high costs.

Method used

The safety coating is introduced into the positive electrode sheet of the lithium battery, including the first active substance and the dispersant. By defining the capacity of the first active substance in the safety coating and the use of the dispersant, the mechanical safety performance of the battery cell and the heat box performance are ensured. and cycle performance, while improving low-temperature discharge performance and magnification discharge performance.

Benefits of technology

Without changing the original process, the mechanical safety performance, heat box performance and cycling performance of the battery cell are taken into account, which improves the safety and energy density of the battery, reduces the internal resistance of the battery, and improves the low-temperature and magnification discharge performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970147A_ABST
    Figure CN118970147A_ABST
Patent Text Reader

Abstract

The invention discloses a battery cell, a preparation method thereof and a lithium ion battery, and relates to the technical field of secondary battery materials. According to the battery cell provided by the invention, the safety coating is introduced into the positive plate, and the capacity exerted by the first active substance in the safety coating is limited. The first active substance not only reduces the possibility of contact between the positive electrode and the negative electrode, improves the mechanical safety performance of the battery cell, but also can exert certain capacity, thereby reducing the N / P ratio (the ratio of the negative electrode capacity to the positive electrode capacity) of the battery cell, reducing the potential of the positive electrode in a full charge state, and improving the thermal abuse performance and the cycle performance of the battery. Finally, by limiting related parameters, the invention provides the battery cell which can consider the mechanical safety performance, the hot box performance and the cycle performance of the battery cell and improve the low-temperature discharge performance and the rate discharge performance under the condition that the original process does not need to be changed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary battery materials, and in particular to a battery cell and a preparation method thereof, and a lithium ion battery. Background Art

[0002] Lithium-ion batteries are widely used in products such as 3C, electric vehicles and power tools due to their advantages such as high energy density, no memory effect, long cycle life, environmental friendliness and ability to adapt to various environments.

[0003] In practical applications, the requirements for mechanical safety tests such as lithium battery puncture and thermal abuse safety tests such as hot boxes are becoming increasingly higher. In order to improve the mechanical safety performance of the battery cell, the industry mostly adopts the measure of coating a safety coating on the positive electrode current collector. The safety coating usually contains a certain proportion of inorganic fillers, conductive agents and binders, but conventional safety coatings have poor effects on improving the thermal abuse safety performance of the battery cell. In order to improve the thermal abuse safety performance of the battery cell, most of them adopt methods such as doping and coating the positive and negative active materials, or developing electrolytes with high thermal stability. However, such methods have shortcomings such as long development cycle and high development cost.

[0004] Therefore, it is of great significance to solve the problem that the current conventional improvement measures cannot effectively improve the mechanical safety performance and thermal abuse safety performance of the battery cell at the same time, and to provide a battery cell that can take into account the mechanical safety performance, hot box performance and cycle performance without changing the original process, and improve the low-temperature discharge performance and rate discharge performance. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a battery cell and a preparation method thereof, and a lithium-ion battery, aiming to solve the problem that conventional improvement measures cannot effectively improve the mechanical safety performance and thermal abuse safety performance of the battery cell at the same time.

[0006] In a first aspect of the present invention, a battery cell is provided, comprising: a positive electrode sheet and a negative electrode sheet; the positive electrode sheet comprises a safety coating and a positive electrode active material layer, the safety coating comprises a first active material and a dispersant, and the positive electrode active material layer comprises a positive electrode active material; the negative electrode sheet comprises a negative electrode active material layer, and the negative electrode active material layer comprises a negative electrode active material; The first capacity ratio NP1 of the battery cell satisfies 1.019≤NP1≤1.089, and the relative capacity ratio Satisfy 0.002≤ ≤0.04; The calculation formula of the first capacity ratio NP1 is: , the relative capacity ratio The calculation formula is: ; C1 is the capacity of the first active substance in the safety coating per unit area. The calculation formula of C1 is: C1=k×c w ×a, 0<k<1, 0<a≤300, c w is the single-sided coating density of the safety coating, a is the theoretical gram capacity of the first active substance, and k is a constant; C2 is the capacity of the positive electrode active material in the positive electrode active material layer per unit area; C0 is the capacity of the negative electrode active material per unit area of ​​the negative electrode active material layer.

[0007] The battery cell according to the embodiment of the present invention has at least the following beneficial effects: the battery cell provided by the present invention introduces a safety coating in the positive electrode sheet, and limits the capacity of the first active substance in the safety coating, so that the mechanical safety performance, hot box performance and cycle performance of the battery cell can be taken into account without changing the original process, and the low-temperature discharge performance and rate discharge performance can be improved.

[0008] In the present invention, C1 is defined as the capacity of the first active substance in the safety coating per unit area, and the calculation formula of C1 is: C1=k×c w ×a, 0<k<1, 0<a≤300, c w is the single-sided coating surface density of the safety coating, a is the theoretical gram capacity of the first active material, and k is a constant related to the battery system and discharge depth. Generally speaking, the larger a is, the worse the stability of the active material. The present invention limits it to 0<a≤300. At this time, the thermal stability of the first active material is better, and it is not easy to collapse or deform the structure. It is also not easy to decompose when the battery cell is subjected to mechanical abuse tests such as acupuncture, which reduces the risk of thermal runaway of the battery cell and improves the safety of the battery. In addition, the first active material not only reduces the possibility of contact between the positive and negative electrodes and improves the mechanical safety performance of the battery cell, but also can exert a certain capacity, thereby reducing the N / P ratio (ratio of negative electrode capacity to positive electrode capacity) of the battery cell, reducing the potential of the positive electrode when fully charged, and improving the thermal abuse performance and cycle performance of the battery. Define C2 as the capacity exerted by the positive electrode active material per unit area in the positive electrode active material layer, and C0 as the capacity exerted by the negative electrode active material per unit area in the negative electrode active material layer. The present invention defines the ratio of C0 to C2 as the N / P ratio (the ratio of the negative electrode capacity to the positive electrode capacity, N / P ratio = C0 / C2), because the change in NP value caused by the introduction of the safety coating is defined as (Relative capacity ratio), The calculation formula is: , the corresponding cell capacity ratio is NP1, and the calculation formula of NP1 is: The present invention defines The value range is 0.002~0.04. When it is lower than 0.002, the corresponding c w When the thickness is relatively small, not only is the processing difficult, the adjustment of the NP value is not obvious, but the safety coating is thin, which will have an adverse effect on the mechanical safety performance of the battery cell; when When it is greater than 0.04, the corresponding c w It is also relatively large, which will have an adverse effect on the energy density of the battery cell. The present invention also limits the value range of NP1. When NP1 is less than 1.019, it indicates that the capacity of the negative electrode is lower than the capacity of the positive electrode, and the battery cell is at risk of lithium precipitation; when the value is greater than 1.089, it indicates that the negative electrode has sufficient margin, which will cause greater irreversible lithium loss during formation, reduce the initial efficiency of the battery cell, and the negative electrode is not fully utilized, which will lead to a decrease in the energy density of the battery cell. In addition, it will deepen the charging depth of the positive electrode, increase the potential of the fully charged positive electrode, and make the cycle performance and hot box performance of the battery cell worse. Considering the need to leave a certain margin to cope with process fluctuations, the present invention limits the value range of NP1 to 1.019~1.089.

[0009] Finally, the present invention provides a battery cell with good mechanical safety performance, hot box performance and cycle performance, while being able to improve low-temperature discharge performance and cycle performance by limiting relevant parameters.

[0010] In the present invention, C1 is the capacity of the first active material in the safety coating per unit area, C2 is the capacity of the positive active material in the positive active material layer per unit area, and C0 is the capacity of the negative active material in the negative active material layer per unit area. "Unit area" can refer to "per square meter", "per square centimeter", "per square millimeter" or other suitable units, and it is sufficient to use the same unit for C1, C2 and C0. The calculation formula is: , the calculation formula of the first capacity ratio NP1 is: , we can see that the units of C1, C2, and C0 will not affect or the value of NP1.

[0011] In some embodiments of the present invention, the first capacity ratio NP1 of the battery cell satisfies 1.028≤NP1≤1.053.

[0012] In some embodiments of the present invention, the calculation formula of C1 is: C1=k×c w ×a, 0<k<1, 0<a≤300, c wis the single-sided coating surface density of the safety coating, a is the theoretical gram capacity (constant) of the first active material, and k is a constant related to the battery system and discharge depth. Preferably, 100≤a≤200. When a is greater than 200, the stability of the active material is poor; when a is less than 100, the amount of the first active material needs to be increased to reduce the same N / P ratio.

[0013] In some embodiments of the present invention, c w The value range is 3 mg / 1540.25 mm 2 ~18 mg / 1540.25 mm 2 The present invention finds that when c w Less than 3 mg / 1540.25mm 2 When c is less than 0.05, it will not affect the NP value of the system, and the processing is more difficult, the safety coating is thinner, and it will also have an adverse effect on the mechanical safety performance of the battery cell; when c is less than 0.05, it will not affect the NP value of the system, and the processing is more difficult, the safety coating is thinner, and it will also have an adverse effect on the mechanical safety performance of the battery cell; w Higher than 18 mg / 1540.25 mm 2 When the value is lower than 0.05, the safety performance of the battery cell has not been improved (the pass rate of the battery cell puncture test has reached 100% when the value is lower than 0.05), but it will have an adverse effect on the energy density of the battery cell. Based on the above considerations, the present invention c w The value range is 3 mg / 1540.25 mm 2 ~18 mg / 1540.25 mm 2 .

[0014] In some embodiments of the present invention, the first active material includes one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium iron manganese phosphate and ternary materials, preferably one or more of active materials with good thermal stability such as lithium iron phosphate, lithium manganese phosphate and lithium iron manganese phosphate. The crystal structure of the active material with good thermal stability is a very stable olivine structure, which is not prone to structural collapse or deformation, and is not prone to decomposition when the battery cell is subjected to mechanical abuse tests such as needle puncture, thereby reducing the risk of thermal runaway of the battery cell and improving the safety of the battery. In addition, the first active material can also exert a certain capacity, thereby reducing the N / P ratio (ratio of negative electrode capacity to positive electrode capacity) of the battery cell, reducing the potential of the positive electrode when fully charged, and improving the thermal abuse performance and cycle performance of the battery.

[0015] In some embodiments of the present invention, the median particle size D of the first active material is v50 The range is 0.1~15μm, and the specific surface area is 2~50 m 2 / g. The median particle size D of the first active material v50 Less than 0.1 μm, or with a specific surface area greater than 50 m 2 / g, it is very easy to agglomerate when the slurry is stirred, and when D v50Greater than 15 μm, or when the specific surface area is less than 2 m 2 / g, it is difficult to obtain a thinner safety coating due to the large particle size, which affects the energy density of the battery cell, and the primer is easily missed when applying the safety coating, affecting the safety of the battery cell.

[0016] In some embodiments of the present invention, the battery cell includes at least one of the following: A1) the first active material is a ternary material, and the ternary material includes at least one of a nickel-cobalt-manganese ternary material and a nickel-cobalt-aluminum ternary material; A2) When including A1), the nickel-cobalt-manganese ternary material includes at least one of NCM333, NCM523, NCM613, NCM622 and NCM811; A3) the surface of the first active material is coated with an inorganic ceramic material; A4) When A3) is included, the inorganic ceramic material includes silicon dioxide, aluminum oxide or titanium oxide.

[0017] In some embodiments of the present invention, the ternary material includes at least one of a nickel-cobalt-manganese ternary material (NCM) and a nickel-cobalt-aluminum (NCA) ternary material. The ternary material used in the present invention may be a common ternary material in the art, and no limitation is made here. For example, the nickel-cobalt-manganese ternary material may include at least one of NCM333, NCM523, NCM613, NCM622, and NCM811.

[0018] In some embodiments of the present invention, the surface of the first active material is coated with an inorganic ceramic material.

[0019] In some embodiments of the present invention, the inorganic ceramic material includes silicon dioxide, aluminum oxide or titanium oxide.

[0020] The first active material can be coated with a layer of inorganic ceramic materials such as silicon dioxide, aluminum oxide or titanium oxide on the surface of its particles. These ceramic materials can inhibit the migration of free lithium ions on the surface of the first active material into the solution, reduce the pH of the coating slurry, and reduce the corrosion of the current collector aluminum foil.

[0021] In some embodiments of the present invention, the dispersant includes one or more of an ionic dispersant, a nonionic dispersant, an amphoteric dispersant and a fluorosurfactant.

[0022] In some embodiments of the present invention, the ionic dispersant includes one or more of polyacrylic acid and its salts, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and polyethyleneimine.

[0023] In some embodiments of the present invention, the nonionic dispersant includes one or more of polyvinyl pyrrolidone, polyethylene glycol, polyvinyl alcohol, polyethylene oxide and carboxymethyl cellulose.

[0024] In some embodiments of the present invention, the amphoteric dispersant comprises betaine.

[0025] Because the first active material is insoluble in water, has small particles and a large specific surface area, it is very easy to agglomerate when stirring and dispersing, so a dispersant must be added. The dispersant can improve the dispersion of the first active material with poor dispersibility in the slurry, and can be one or more of the following dispersants: ionic dispersants, such as polyacrylic acid (PAA) and its salts, sodium dodecylbenzene sulfonate (SDBS), sodium dodecyl sulfate (SDS), polyethyleneimine (PEI), etc.; non-ionic dispersants, such as polyvinyl pyrrolidone (PVP), polyethylene glycol (PEG), polyvinyl alcohol (PVA), polyoxyethylene (POE), carboxymethyl cellulose (CMC), etc.; amphoteric dispersants represented by betaine; and fluorosurfactants. The dispersant can reduce the mutual attraction between inorganic filler particles, thereby improving the dispersibility of the particles in the rubber. Good dispersibility can ensure the uniform distribution of inorganic filler particles, reduce agglomeration, reduce the viscosity of the slurry, improve the uniformity of the coating, and help improve the electrochemical performance of the battery cell. Preferably, the dispersant is selected from polyacrylic acid (PAA) and its salts, or polyvinylpyrrolidone (PVP).

[0026] In some embodiments of the present invention, the safety coating further comprises a first conductive agent, a first binder and an inorganic filler.

[0027] In some embodiments of the present invention, the safety coating satisfies at least one of the following: B1) The mass ratio of the first conductive agent, the first binder, the inorganic filler, the first active material, and the dispersant is (0.5-5): (1-21.2): (1-50): (1-95): (0.01-1); B2) The median particle size D of the inorganic filler v50 The range is 0.1~5μm, and the specific surface area is 8~15m 2 / g; B3) the inorganic filler comprises one or more of alumina, boehmite, aluminum hydroxide, magnesium hydroxide, silicon dioxide or titanium dioxide; B4) The first binder includes one or more of polyvinylidene fluoride binder, sodium carboxymethyl cellulose binder or polyacrylate binder.

[0028] In some embodiments of the present invention, the mass ratio of the first conductive agent, the first binder, the inorganic filler, the first active material, and the dispersant is (0.5-5): (1-21.2): (1-50): (1-95): (0.01-1). For example, in terms of weight, the first conductive agent may be 0.5-5 parts, preferably 1.5-3 parts, the first binder may be 1-21.2 parts, preferably 5-15 parts, the inorganic filler may be 1-50 parts, the first active material may be 1-95 parts, and the dispersant may be 0.01-1 parts.

[0029] In some embodiments of the present invention, the median particle size D of the inorganic filler is v50 The range is 0.1~5μm, and the specific surface area is 8~15m 2 / g. When the inorganic filler D v50 Less than 0.1 μm, and the specific surface area is greater than 15 m 2 / g, the inorganic filler is prone to agglomeration and difficult to disperse; when the inorganic filler D v50 Greater than 5μm, and specific surface area less than 8m 2 / g, it is difficult to obtain a thin safety coating due to the large particle size, which affects the energy density of the battery cell, and the primer is easily missed when the safety coating is applied, affecting the safety of the battery cell. When the median particle size and specific surface area of ​​the inorganic filler are within the above range, a good balance can be achieved between the processability of the safety coating and the energy density of the battery cell.

[0030] In some embodiments of the present invention, the inorganic filler includes one or more of alumina, boehmite, aluminum hydroxide, magnesium hydroxide, silicon dioxide or titanium dioxide. Boehmite is preferably used. Compared with other inorganic fillers, boehmite is not only cheap, but also has a lower Rockwell hardness and less wear on the gravure roller, thereby reducing manufacturing costs.

[0031] In some embodiments of the present invention, the mass fraction of the inorganic filler in the safety coating is 1% to 50%.

[0032] In some embodiments of the present invention, the first binder includes one or more of a polyvinylidene fluoride (PVDF) binder, a sodium carboxymethyl cellulose (CMC) binder, or a polyacrylate (PAA) binder.

[0033] In some preferred embodiments of the present invention, the first adhesive is a polyacrylate adhesive, which can reduce the corrosion of the active substance to the aluminum foil, has good bonding performance, is cheap, and the solvent is deionized water, which is environmentally friendly.

[0034] In some embodiments of the present invention, the structural formula of the polyacrylate binder is: ; wherein each occurrence of R1 is independently selected from H, Li or Na; Each occurrence of R2 is independently selected from substituted or unsubstituted C1~C 10 The alkyl group; And 5≤(x+z) / y≤20, 1.2≤z / x≤2, x, y, z are all not 0.

[0035] The polyacrylate adhesive provided by the present invention achieves good bonding performance by limiting the content of cyano (-CN), ester (-COOR2) and carboxylate (-COOR1) in the adhesive molecular chain; and the adhesive is water-soluble, the solvent is water, no harmful organic solvents such as NMP are needed, it is harmless to the human body and environmentally friendly; the source is abundant, the price is cheap, and it can be widely used in industrial production. The above-mentioned adhesive is introduced into the electrode sheet as a raw material for the water-based safety coating. Based on its excellent bonding performance, the safety coating can be firmly adhered to the collector surface of the electrode sheet, which can not only reduce the surface contact resistance, but also reduce the generation of collector burrs when the battery cell is tested for safety, and reduce the contact short circuit between the collector burrs and the active material in the unstable charging state, thereby improving the safety of the battery cell. In addition, by limiting the molecular weight of the adhesive and the content of cyano, ester and carboxylate in the molecular chain, the absorption rate of the adhesive electrolyte can be adjusted, which can significantly improve the rate performance and high and low temperature discharge performance of the battery cell, and improve the safety performance and cycle performance of the battery.

[0036] The binder provided by the present invention has a molecular chain containing a cyano group (-CN, the number of which accounts for n1 in all side chain groups, n1=z / (x+y+z)), a carboxylate group (-COOR1, R1 each time appears is independently selected from H, Li, Na, the number of which accounts for n2 in all side chain groups, n2=x / (x+y+z)) and an ester group (-COOR2, R2 each time appears is independently selected from substituted or unsubstituted C1~C 10 The number of alkyl groups in all side chain groups is n3, n3=y / (x+y+z)), n1+n2+n3=1.

[0037] Among them, -CN is a strongly polar group with good electrolyte affinity and electrochemical stability, and can provide greater adhesion. However, this group is very rigid and cannot cope with the huge volume changes that occur when lithium ions are embedded in / out of the active material.

[0038] Among them, -COOR1 carries a negative charge and repel each other, which helps the stretching of the binder molecules and promotes the uniform dispersion of the conductive agent. At the same time, it can also regulate the swelling degree of the binder in the electrolyte solvent, reduce the erosion of the adhesive by the electrolyte dissolution, and better maintain the bonding ability and bonding effect.

[0039] Among them, -COOR2 has a polarity and solubility parameter close to that of carbonate solvents in the electrolyte, which is conducive to the binder's moderate absorption of the electrolyte. The absorption of the electrolyte will plasticize the binder, making it elastic and flexible to adapt to the periodic volume changes of the electrode active material during the charging and discharging process as lithium ions are inserted and extracted. At the same time, the absorption of the electrolyte will also increase the ionic conductivity of the water-based safety coating and promote the improvement of the low-temperature discharge performance of the battery cell.

[0040] Binders are essential to maintaining the integrity of the electrode, and are very important for improving battery specific capacity, cycle stability and other performance. Polyacrylic acid is used as a binder for the positive and negative electrodes of lithium batteries because it contains more polar functional groups, is soluble in water and has good adhesion. However, the polar groups of polyacrylic acid cause the hydrogen bonds formed between the molecular chains to result in greater chain rigidity, which is not conducive to maintaining the integrity of the electrode during charging and discharging. Therefore, it is imperative to control the number of polyacrylic acid functional groups, change the type of functional groups and the structure of the polyacrylic acid molecular chain in order to improve the electrical performance of lithium batteries. The present invention limits the content of cyano, ester and carboxylate groups in the binder molecular chain: (1) 1.2≤z / x≤2, that is, n1 and n2 satisfy 1.2≤n1 / n2≤2; when n1 / n2<1.2, the adhesive strength of the binder is insufficient; and when n1 / n2>2, the molecular chain is in a curled state, which is not conducive to the dispersion of the conductive agent, and the binder is more susceptible to the swelling of the electrolyte; (2) 5≤(x+z) / y≤20, that is, n1, n2, and n3 satisfy 5 ≤(n1+n2) / n3≤20; when (n1+n2) / n3<5, the binder contains excessive -COOR2, at which time the binder easily absorbs excessive electrolyte, the bonding force decreases rapidly, the elasticity deteriorates, and the performance of the battery cell deteriorates; and when (n1+n2) / n3>20, the -COOR2 content in the binder is too low, at which time the elasticity of the binder is insufficient, the ionic conductivity of the water-based safety coating is low, and the low-temperature discharge performance and rate discharge performance of the battery cell are significantly reduced. Finally, the present invention achieves good bonding force of the binder by regulating the content of cyano, ester and carboxylate groups in the binder molecular chain, and adjusts the electrolyte absorption rate of the binder, thereby improving the rate and high and low temperature discharge performance of the battery cell.

[0041] In some embodiments of the present invention, each occurrence of R2 is independently selected from C1 to C 10 A straight chain alkyl, branched chain alkyl or cycloalkyl group, preferably C1~C 10The straight chain alkyl group is more preferably a C1~C4 alkyl group.

[0042] In some embodiments of the present invention, the electrolyte absorption rate c of the polyacrylate binder at 80° C. is 10% to 50%, for example, 10% to 20%, 20% to 30%, 30% to 40%, or 40% to 50%.

[0043] The present invention achieves the adjustment of the electrolyte absorption rate of the binder by limiting the content of cyano, ester and carboxylate groups in the binder molecular chain. The electrolyte absorption rate c of the binder at 80°C satisfies 10%≤c≤50%. When c<10%, the binder absorbs insufficient electrolyte, has poor elasticity, and cannot buffer the periodic volume changes caused by the insertion and extraction of lithium ions from the active material. In addition, the ionic conductivity of the water-based safety coating is low, and the low-temperature discharge performance and rate discharge performance of the battery cell deteriorate. When c>50%, the binder absorbs excessive electrolyte, the water-based safety coating expands, the bonding force decreases, and the internal resistance increases, which also leads to the deterioration of the battery cell performance.

[0044] In some embodiments of the present invention, the weight average molecular weight M of the polyacrylate binder is w The range is 200000~500000, for example, it can be 200000, 250000, 300000, 350000, 400000, 450000, and 500000.

[0045] In some embodiments of the present invention, the number average molecular weight M of the polyacrylate binder is n The range is 100000~400000, for example, it can be 100000, 150000, 200000, 250000, 300000, 350000, and 400000.

[0046] In some embodiments of the present invention, the weight average molecular weight M of the polyacrylate binder is w and number average molecular weight M n The ratio satisfies M w / M n ≤3, preferably M w / M n The range is 1.5~1.9.

[0047] If the molecular weight of the binder is too low, not only will the bonding force be too low, but it will also lead to an increase in the amount of binder used; if the molecular weight is too high, the viscosity will be too high and processing will be difficult. w / M n >3. The molecular weight distribution of the binder is too dispersed, which deteriorates the performance of the water-based safety coating.

[0048] In some embodiments of the present invention, the mass fraction of the polyacrylate binder in the safety coating is 1wt%~21.2wt%, preferably 5wt%~15wt%. When the amount of binder in the safety coating is less than 1%, the safety coating has insufficient adhesion and is prone to fall off during later use; when the amount of binder is greater than 21.2%, the safety coating will be difficult to process during gravure printing, and the internal resistance of the battery cell will also be deteriorated. In addition, the amount of binder is 1%~21.2%, which can also adjust the pH of the slurry to below 8.5, thereby reducing the corrosion of the alkaline active substance aqueous solution to the current collector aluminum foil.

[0049] The polyacrylate binder can be prepared by conventional preparation methods in the art, for example, by any one of emulsion polymerization, solution polymerization, bulk polymerization and suspension polymerization.

[0050] In a specific embodiment, the present invention also provides a method for preparing the above-mentioned polyacrylate adhesive, comprising the steps of: S1. Adding a dispersion medium into a reaction vessel and deoxygenating the vessel; S2, adding a certain amount of acrylonitrile, monomer A providing -COOR1, and monomer B providing -COOR2 into the reaction container according to the ratio of x, y, and z; S3, adding initiator and heating to initiate reaction; S4. After the reaction is completed, the product is filtered, dried, crushed and sieved to obtain a polyacrylate adhesive.

[0051] In some embodiments of the present invention, the monomer A includes at least one of acrylic acid, lithium acrylate, and sodium acrylate, but is not limited thereto. The purpose of adding monomer A is to provide -COOR1, where R1 is selected from H, Li, or Na. Those skilled in the art can select a suitable monomer A according to their needs, which should be regarded as a reasonable change within the scope of the present invention.

[0052] In some embodiments of the present invention, the monomer B includes at least one of methyl acrylate, ethyl acrylate, and butyl acrylate, but is not limited thereto, and may also be C1~C 10 The purpose of adding monomer B is to provide -COOR2, R2 is selected from substituted or unsubstituted C1~C 10 Those skilled in the art can select suitable monomer B according to their needs, which should be regarded as reasonable changes within the scope of the present invention.

[0053] In some embodiments of the present invention, in step S1, distilled water is added to the reaction container, stirring is started, and high-purity nitrogen is introduced for deoxygenation.

[0054] In some embodiments of the present invention, in step S2, after adding acrylonitrile, monomer A providing -COOR1, and monomer B providing -COOR2, the mixture is heated to 65° C. and maintained at a constant temperature under an inert atmosphere.

[0055] In some embodiments of the present invention, the initiator includes 20% ammonium persulfate, but is not limited thereto.

[0056] In some embodiments of the present invention, the mass fraction of the first conductive agent in the safety coating is 0.5% to 5%. Preferably, it is 1% to 3.5%. If the conductive agent content is too low, the water-based safety coating film resistance will be too large and the battery cell cycle performance will be poor; if the content is too high, the water-based safety coating film resistance will be too low and the battery cell safety will be poor. When the content of the conductive agent is between 0.5wt% and 5wt%, both safety and cycle can be taken into account.

[0057] In some embodiments of the present invention, the first conductive agent includes at least one of acetylene black, graphene, graphyne, carbon nanotubes, carbon fibers, and conductive carbon black. The present invention has no special requirements for the first conductive agent, and any conventional conductive agent in the art can be used, such as conductive carbon black or carbon nanotubes, and more specifically, super dense high conductive carbon black SUPER P Li.

[0058] In some embodiments of the present invention, the positive electrode sheet also includes a positive electrode current collector, the safety coating is coated on at least one side surface of the positive electrode current collector, and the positive electrode active material layer is coated on the side surface of the safety coating away from the positive electrode current collector and / or the side surface of the positive electrode current collector away from the safety coating.

[0059] In some embodiments of the present invention, the negative electrode sheet further includes a negative electrode current collector, and the negative electrode active material layer is coated on at least one side surface of the negative electrode current collector.

[0060] In the positive electrode provided by the present invention, the safety coating is closer to the current collector, and its structure is "current collector-safety coating-active material layer". Figure 1 As shown, the positive electrode sheet 01 includes the following structures: a current collector 022; a safety coating 023, which is arranged on at least one surface of the current collector 022; and a positive electrode active material layer 011, which is arranged on the surface of the safety coating 023 away from the current collector 022.

[0061] The internal short circuit of lithium-ion batteries can generally be divided into several types: 1) short circuit between positive and negative current collectors; 2) short circuit between positive and negative active materials; 3) short circuit between negative active material and positive current collector; 4) short circuit between positive active material and negative current collector. Among them, the impedance of the short circuit point between the negative active material and the positive current collector is small, and the trigger temperature of the negative exothermic reaction is low. Therefore, the short circuit between the negative active material and the Al foil is the most dangerous. The present invention introduces a safety coating with high adhesion to the surface of the positive current collector to reduce the probability of contact between the positive current collector and the negative active material, which can effectively improve the safety performance of the battery cell.

[0062] In some embodiments of the present invention, the single-sided coating density of the safety coating is 3 mg / 1540.25 mm 2 ~18 mg / 1540.25 mm 2 . For example, it can be 3~6mg / 1540.25mm 2 , 6~9mg / 1540.25mm 2 , 9~12mg / 1540.25mm 2 12~15mg / 1540.25mm 2 15~18mg / 1540.25mm 2 When less than 3 mg / 1540.25mm 2 Although it will not affect the NP value of the system, it is more difficult to process, and the safety coating is thin, which will also have an adverse effect on the mechanical safety performance of the battery cell; and above 18 mg / 1540.25mm 2 When the value is less than 30%, the safety performance of the battery cell will not be improved (the pass rate of the battery cell needle puncture test has reached 100% when the value is lower than this value), but it will have an adverse effect on the energy density of the battery cell. Based on the above considerations, the single-sided coating surface density of the safety coating of the present invention is in the range of 3 mg / 1540.25 mm 2 ~18mg / 1540.25mm 2 .

[0063] In some embodiments of the present invention, the safety coating is applied to both sides of the current collector. The safety coating satisfies at least one of the following conditions: C1) The double-sided thickness of the safety coating is 1-20 μm; C2) The double-sided diaphragm resistance of the safety coating tested under a pressure of 0.4t is 0.5~5Ω; C3) The double-sided thickness d of the safety coating and the value of the double-sided diaphragm resistance R under a pressure of 0.4t satisfy the condition: 2≤R×d≤50; C4) along the direction perpendicular to the unwinding direction of the positive electrode current collector, the distance W between the left edge of the safety coating on the A side of the positive electrode current collector and the left edge of the positive electrode current collector A1 The range is 2mm~30mm, and the distance W between the right edge and the right edge of the positive electrode collector is A2 The range is 2mm~30mm; the distance W between the left edge of the safety coating on the B side of the positive electrode collector and the left edge of the positive electrode collector B1 The range is 3mm~30mm, and the distance W between the right edge and the right edge of the positive electrode collector is B2 The range is 3mm~30mm; and W B1 -W A1 ≥1mm, W B2 -W A2 ≥1mm.

[0064] In some embodiments of the present invention, the double-sided thickness d of the safety coating (ie, the sum of the thicknesses of the safety coatings coated on both sides of the current collector surface) is 1-20 μm, for example, 1-7 μm, 7-14 μm, or 14-20 μm.

[0065] In some embodiments of the present invention, the double-sided membrane resistance R of the safety coating under a pressure of 0.4 t (i.e., the sum of the membrane resistances of the safety coating on both sides coated on the surface of the current collector) is 0.5~5Ω, for example, 0.5~2Ω, 2~3.5Ω, 3.5~5Ω. The membrane resistance of the safety coating is the primary factor affecting the safety performance of the battery cell. If the value is too small, the safety performance of the battery cell will deteriorate, and if it is too large, the cycle performance of the battery cell will deteriorate. The value is between 0.5~5Ω@0.4 t, which can take into account both safety performance and cycle performance.

[0066] In some embodiments of the present invention, the double-sided thickness d (in μm) of the safety coating and the double-sided membrane resistance R (in Ω) under a pressure of 0.4t satisfy the condition: 2≤R×d≤50. Generally speaking, the parameters R and d are positively correlated with the safety of the battery cell, and negatively correlated with the cycle performance of the battery cell. When the relationship 2≤R×d≤50 is satisfied, a good balance can be achieved between the safety performance and electrochemical performance of the battery cell.

[0067] In some embodiments of the present invention, the bonding force between the safety coating and the current collector is not less than 100 N / m. If the bonding force is less than 100 N / m, there is a risk that the safety coating will fall off during subsequent use.

[0068] In some embodiments of the present invention, the raw material of the positive electrode active material layer includes a positive electrode active material, a second conductive agent and a second binder.

[0069] In some embodiments of the present invention, the mass percentage of the positive electrode active material in the positive electrode active material layer is 90% to 98%.

[0070] The positive electrode active material is not limited, and can be one or more of common lithium cobalt oxide, lithium iron phosphate and ternary materials, and the amount used is 90wt% to 98wt% of the total weight of the active material layer. Under the condition of ensuring that the active material has a certain conductivity and adhesion, the higher the content of the active material, the better, so that the battery cell has a higher energy density.

[0071] In some embodiments of the present invention, the mass percentage of the second conductive agent in the positive electrode active material layer is 0.5% to 5%, preferably 0.5% to 2%. If the content of the second conductive agent is too low, the battery cell cycle performance is poor; if the content is too high, it is good for improving the cycle performance, but will lead to poor safety performance of the battery cell.

[0072] In some embodiments of the present invention, the second conductive agent includes at least one of acetylene black, graphene, graphyne, carbon nanotubes, carbon fibers, and conductive carbon black. The present invention has no special requirements for the second conductive agent, and any conventional conductive agent in the art can be used, such as conductive carbon black or carbon nanotubes, and more specifically, super dense high conductive carbon black SUPER P Li.

[0073] In some embodiments of the present invention, the mass percentage of the second binder in the active material layer is 0.5% to 5%. If the amount of the second binder is too little, the active material layer will not have sufficient bonding strength and will easily fall off during later use; if the amount of the second binder is too much, the active material layer will be difficult to process and the internal resistance of the battery cell will also be deteriorated.

[0074] In some embodiments of the present invention, the second binder includes at least one of polyvinylidene fluoride PVDF, sodium carboxymethyl cellulose CMC, styrene butadiene rubber SBR, and PAA-based binders. The present invention has no special requirements for the second binder, and any conventional binder in the art can be used.

[0075] The second binder is not limited and can be a common cathode binder, including polyvinylidene fluoride PVDF, sodium carboxymethyl cellulose CMC and PAA binders, and the amount used is 0.5wt%~5wt% of the total weight of the active material layer. If the amount of the second binder is too little, the active material layer will not have enough adhesion and will easily fall off during later use; if the amount of the second binder is too much, the active material layer will be difficult to process and the internal resistance of the battery will also be deteriorated. Considering that it does not directly contact the current collector, the upper limit of its amount can be appropriately reduced to ensure that the positive active material does not fall off during the use of the battery. At the same time, a lower amount can also improve the cycle performance of the battery, increase the amount of positive active material, and improve the energy density of the battery.

[0076] In some embodiments of the present invention, the positive electrode sheet further includes a positive electrode current collector. The positive electrode current collector is not limited and can be a common positive electrode current collector, such as aluminum foil or composite aluminum foil.

[0077] In some embodiments of the present invention, the dyne value of the positive electrode current collector is not less than 30 dyn / cm, preferably, the dyne value of the positive electrode current collector is not less than 38 dyn / cm. When the dyne value of the current collector is less than 30 dyn / cm, on the one hand, it is not conducive to the wetting of the current collector by the safety coating slurry, resulting in leakage of the primer, and on the other hand, it will reduce the adhesion between the safety coating and the current collector, causing the safety coating to easily fall off during subsequent use, which has an adverse effect on the safety of the battery cell. When the dyne value of the current collector is not less than 38 dyn / cm, it can ensure that the primer has a good appearance and morphology, and the safety coating and the current collector have good adhesion.

[0078] In some embodiments of the present invention, the raw material of the negative electrode active material layer includes a negative electrode active material, a third conductive agent and a third binder.

[0079] In some embodiments of the present invention, the mass percentage of the negative electrode active material in the negative electrode active material layer is 90% to 98%.

[0080] The negative electrode active material is not limited and can be one or more of common artificial graphite, natural graphite, modified graphite, silicon oxide compounds, silicon carbon composites and other silicon negative electrode materials, and the amount used is 90wt%~98wt% of the total weight of the negative electrode active material layer.

[0081] In some embodiments of the present invention, the mass percentage of the third conductive agent in the negative electrode active material layer is 0.5% to 5%, preferably 0.5% to 2%. If the content of the third conductive agent is too low, the battery cell cycle performance is poor; if the content is too high, it is good for improving the cycle performance, but will lead to poor safety performance of the battery cell.

[0082] In some embodiments of the present invention, the third conductive agent includes at least one of acetylene black, graphene, graphyne, carbon nanotubes, carbon fibers, and conductive carbon black. The present invention has no special requirements for the third conductive agent, and any conventional conductive agent in the art can be used, for example, conductive carbon black or carbon nanotubes, more specifically, super dense high conductive carbon black SUPER P Li.

[0083] In some embodiments of the present invention, the mass percentage of the third binder in the negative electrode active material layer is 0.5% to 5%. If the amount of the third binder is too little, the active material layer will not have sufficient bonding strength and will easily fall off during later use; if the amount of the third binder is too much, the active material layer will be difficult to process and the internal resistance of the battery cell will also be deteriorated.

[0084] In some embodiments of the present invention, the third binder includes at least one of polyvinylidene fluoride PVDF, sodium carboxymethyl cellulose CMC, styrene butadiene rubber SBR, and PAA-based binders. The present invention has no special requirements for the third binder, and any conventional binder in the art can be used.

[0085] In some embodiments of the present invention, the negative electrode sheet further comprises a negative electrode current collector. The negative electrode current collector is not limited and can be a common negative electrode current collector, copper foil, or composite copper foil.

[0086] In some embodiments of the present invention, the dyne value of the negative electrode current collector is not less than 30 dyn / cm, preferably, the dyne value of the negative electrode current collector is not less than 38 dyn / cm. When the dyne value of the current collector is less than 30 dyn / cm, on the one hand, it is not conducive to the wetting of the current collector by the safety coating slurry, resulting in leakage of the primer, and on the other hand, it will reduce the adhesion between the safety coating and the current collector, causing the safety coating to easily fall off during subsequent use, which has an adverse effect on the safety of the battery cell. When the dyne value of the current collector is not less than 38 dyn / cm, it can ensure that the primer has a good appearance and morphology, and the safety coating and the current collector have good adhesion.

[0087] In some embodiments of the present invention, the battery cell further includes a separator spaced between the positive electrode sheet and the negative electrode sheet.

[0088] The second aspect of the present invention provides a method for preparing the above-mentioned battery cell, comprising the steps of: S100, mixing raw materials for preparing the safety coating in a solvent to obtain a safety coating slurry; S200, applying the safety coating slurry to at least one side surface of a positive electrode current collector to obtain a positive electrode current collector containing a safety coating; S300, coating a positive electrode active material layer on a side of the safety coating away from the positive electrode current collector or on a side of the positive electrode current collector away from the safety coating to obtain a positive electrode sheet; S400, coating a negative electrode active material layer on the negative electrode current collector to obtain a negative electrode sheet; S500, assembling the positive electrode sheet and the negative electrode sheet to obtain a battery cell.

[0089] The method for preparing the battery cell according to the embodiment of the present invention has at least the following beneficial effects: by introducing a safety coating into the positive electrode sheet and limiting the capacity of the active material in the safety coating, the present invention can take into account the mechanical safety performance, hot box performance and cycle performance of the battery cell without changing the original process, and improve the low-temperature discharge performance and rate discharge performance. This method is not only simple in process, but also has non-harsh reaction conditions, is compatible with the original preparation process, and has the potential for large-scale application.

[0090] In some embodiments of the present invention, the safety coating comprises at least one of the following: D1) The solid content of the safety coating slurry is ≥ 10%; D2) the viscosity of the safety coating slurry is ≥50 mPa·s; D3) the dyne value of the positive electrode current collector is ≥30 dyn / cm; D4) applying the safety coating slurry to one or both sides of the positive electrode current collector by gravure printing; D5) When D4) is included, the oven temperature during gravure printing is 90-110°C and the printing speed is 10-50 m / min.

[0091] In some embodiments of the present invention, the raw materials of the safety coating include a first conductive agent, a first binder, an inorganic filler, a first active material, a dispersant and a co-solvent.

[0092] In some embodiments of the present invention, the mass ratio of the first conductive agent, the first binder, the inorganic filler, the first active material, the dispersant, and the co-solvent is (0.5-5): (1-21.2): (1-50): (1-95): (0.01-1): (1-20). For example, in terms of weight, the first conductive agent may be 0.5-5 parts, preferably 1.5-3 parts, the first binder may be 1-21.2 parts, preferably 5-15 parts, the inorganic filler may be 1-50 parts, the first active material may be 1-95 parts, the dispersant may be 0.01-1 parts, and the co-solvent may be 1-20 parts.

[0093] In some embodiments of the present invention, the co-solvent includes one or more of isopropanol, ethanol, ethylene glycol, acetone and ethyl acetate. The co-solvent can optimize the slurry performance and can be one or more of isopropanol (IPA), ethanol, ethylene glycol, acetone and ethyl acetate. The co-solvent can reduce the viscosity of the slurry, improve the wettability of the slurry to the current collector, ensure that the slurry can be evenly covered on the surface of the current collector, and form a more uniform and dense safety coating, thereby improving the coating quality. In addition, in the production process of the safety coating, the volatilization rate of the co-solvent is usually faster than that of the main solvent, which helps to quickly form a uniform coating and reduce coating defects. Preferably, the co-solvent is selected from isopropanol (IPA), which is a commonly used co-solvent with good solubility and volatility, and can effectively improve the performance of the slurry.

[0094] In some embodiments of the present invention, the solid content of the safety coating slurry is ≥10%, preferably 10% to 21%.

[0095] In some embodiments of the present invention, the viscosity of the safety coating slurry is ≥50 mPa·s.

[0096] The solid content of the safety coating slurry should not be less than 10%, and the viscosity should not be less than 50 mPa·s. Too low solid content will not only reduce the production efficiency, but also make it difficult to obtain a water-based safety coating with a specified thickness and surface density, while too low viscosity will be detrimental to the gravure printing process.

[0097] In some embodiments of the present invention, the dyne value of the positive electrode current collector and / or the negative electrode current collector is ≥30 dyn / cm, preferably ≥38 dyn / cm. When the dyne value of the current collector is lower than 30 dyn / cm, on the one hand, it is not conducive to the wetting of the current collector by the safety coating slurry, resulting in leakage of the primer, and on the other hand, it will reduce the adhesion between the safety coating and the current collector, causing the safety coating to easily fall off during subsequent use, which has an adverse effect on the safety of the battery cell. The dyne value of the current collector is not less than 38 dyn / cm, which can ensure that the primer has a good appearance and morphology, and the safety coating and the current collector have good adhesion.

[0098] In some embodiments of the present invention, the safety coating slurry is coated on one or both sides of the surface of the positive electrode current collector by gravure printing.

[0099] In some embodiments of the present invention, the temperature of the oven during gravure printing is 90-110° C.; the printing speed is not less than 10 m / min, preferably 10-50 m / min.

[0100] When gravure printing is performed, the oven temperature should be 90~110℃ and the printing speed should be 10~50 m / min. If the oven temperature is lower than 90℃, the production efficiency will be reduced. If it is higher than 110℃, there may be problems such as cracking and migration of the conductive agent to the surface. If the printing speed is too low, the production efficiency will also be reduced. If it is too high, the safety coating will be missed, which will have a negative impact on the safety performance of the battery cell.

[0101] In some embodiments of the present invention, the method for preparing the positive electrode sheet comprises the steps of: (10) mixing the first binder and the solvent and performing gluing to obtain a glue solution; (20) uniformly mixing the glue, the first conductive agent, the inorganic filler, the first active material, the dispersant, and the co-solvent to obtain a safety coating slurry; (30) The safety coating slurry obtained in step (20) is transferred to one or both sides of the current collector by gravure printing to obtain a positive electrode sheet in which the safety coating area and the non-safety coating area are alternately arranged along the unwinding direction of the current collector.

[0102] Among them, the non-safety coating area corresponds to the head and / or tail of the positive electrode sheet of the battery cell, usually one side of which is an active material and the other side is a blank foil, or a separately set ceramic layer. The ceramic layer usually contains only inorganic fillers and binders, which can reduce the generation of positive current collector burrs in the non-safety coating area during battery cell testing, reduce the probability of contact between the positive current collector and the negative active material, and thus improve the safety performance of the battery cell. However, the ceramic layer needs to be coated in an additional process after the safety coating is set, which not only reduces production efficiency, but also increases production costs.

[0103] In some embodiments of the present invention, the first binder is a polyacrylate binder.

[0104] In some embodiments of the present invention, the solid content of the glue solution is 10% to 30%, for example, 10% to 20%, 20% to 25%, or 25% to 30%.

[0105] In some embodiments of the present invention, the viscosity of the glue is 1×10 3 ~3×10 4 mPa·s, preferably 1.5×10 4 ~2.5×10 4 mPa·s, more preferably 1.6×10 4 ~2.2×10 4 mPa·s, for example, can be 2×10 4 mPa·s.

[0106] If the solid content and viscosity of the adhesive liquid are too low, it will not only reduce the processing efficiency, but also may cause insufficient adhesion of the safety coating; if the solid content and viscosity are too high, it may make the safety coating difficult to process.

[0107] In some embodiments of the present invention, the total length of the positive electrode current collector containing the safety coating is L, the length of the safety coating area is L1, the length of the non-aqueous safety coating area is L2, and L1>L2, L1+L2=L.

[0108] In some embodiments of the present invention, a safety coating may be applied to both sides (side A and side B) of the positive electrode current collector, wherein the length of the safety coating area on side A is L A1 , the length of the non-safety coating area is L A2 , and L A1 >L A2 , L A1 +L A2 =L A ; The length of the safety coating area on the B side is L B1 , the length of the non-safety coating area is L B2 , and L B1 >L B2 , L B1 +L B2 =L B .

[0109] In some preferred embodiments of the present invention, in order to improve production efficiency and reduce costs, a ceramic layer can be provided only on the non-safety coating area of ​​the B surface, and a safety coating can also be provided on the non-safety coating area of ​​the A surface, that is, a single-sided continuous coating structure is provided. A2 is 0, that is, L B1 +L B2 =L B =L A1 =L A =L.

[0110] Figure 2 The figure shows a cross-sectional view of a current collector coated with a safety coating along the unwinding direction in one of the specific embodiments of the present invention. In the figure, 02-positive current collector with safety coating; 021-reserved slot; 022-current collector; 023-safety coating; 024-non-safety coating area. The safety coating area and non-safety coating area on the A side and B side of the positive electrode sheet can be arranged opposite to each other, as shown in Figure (a); one side can also be provided with a non-safety coating area and the other side with a safety coating area, as shown in Figure (b). The total length of the current collector with safety coating is L, and the length of the safety coating area on the B side is L. B1 , the length of the non-safety coating area is L B2 , and L B1 >L B2 , LB1 +L B2 =L B =L A1 =L A =L; the non-safety coating area can also be provided with a safety coating, L A2 and L B2 are all set to 0, that is, L A1 =L B1 =L A =L B , as shown in Figure (c).

[0111] In some embodiments of the present invention, when applying the safety coating, N1 slots for electrode tab welding need to be reserved in the safety coating area or non-safety coating area along the unwinding direction of the current collector, where N1≥0.

[0112] In some embodiments of the present invention, when applying the safety coating, N2 slots for electrode tab welding need to be reserved in the safety coating area or non-safety coating area perpendicular to the unwinding direction of the current collector, where N2≥0.

[0113] In some embodiments of the present invention, when applying the safety coating, N3 strips of the safety coating may be simultaneously applied along the unwinding direction of the current collector, where N3≥1.

[0114] When the safety coating is applied, the slot for the electrode tab welding may be reserved or not reserved as required, such as Figure 3 shown.

[0115] In some embodiments of the present invention, if both sides of the current collector are coated with a safety coating, the slots reserved for the tab welding should be kept opposite to each other, and the horizontal and vertical misalignment should be kept. None exceed 2mm.

[0116] In some embodiments of the present invention, the safety coating is coated on both sides of the positive current collector, and the distance W between the left edge of the safety coating on the A side of the positive current collector and the left edge of the positive current collector is perpendicular to the unwinding direction of the positive current collector. A1 The range is 2mm~30mm, and the distance W between the right edge and the right edge of the positive electrode collector is A2 The range is 2mm~30mm; the distance W between the left edge of the safety coating on the B side of the positive electrode collector and the left edge of the positive electrode collector B1 The range is 3mm~30mm, and the distance W between the right edge and the right edge of the positive electrode collector is B2 The range is 3mm~30mm; and W B1 -W A1 ≥1mm, W B2 -W A2That is to say, if both sides of the positive electrode current collector are coated with a safety coating, the distance between the left edge of the safety coating on side A and the left edge of the current collector perpendicular to the unwinding direction of the positive electrode current collector is W. A1 (That is, the left side of A is blank as W A1 ), the blank on the right side of A is W A2 , the left side of B is blank for W B1 , the blank on the right side of B is W B2 , satisfying 2mm≤W A1 , W A2 ≤30mm, 3mm≤W B1 , W B2 ≤30mm, and W B1 -W A1 ≥1mm, W B2 -W A2 ≥1mm. Figure 4 The figure shows a cross-sectional view of the safety coating perpendicular to the unwinding direction in a specific embodiment of the present invention. In the figure, 021 is a reserved slot; 022 is a current collector; 023 is a safety coating. This arrangement enables the width of the safety coating on side A to be more than 2 mm wider than that on side B, thereby reducing the bulging of the edge of the primer when it is rolled up.

[0117] In a third aspect of the present invention, a lithium-ion battery is provided, comprising the battery cell as described above or the battery cell obtained by the preparation method as described above.

[0118] Since the lithium-ion battery adopts all the technical solutions of the battery cell of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment. That is, the lithium-ion battery introduces a safety coating in the electrode sheet and limits the capacity of the first active material in the safety coating, so that the mechanical safety performance, hot box performance and cycle performance of the battery cell can be taken into account without changing the original process, and the low-temperature discharge performance and rate discharge performance can be improved.

[0119] In some embodiments of the present invention, the battery cell includes: a positive electrode sheet, a negative electrode sheet, and a separator between the positive electrode sheet and the negative electrode sheet.

[0120] In some embodiments of the present invention, the positive electrode sheet is an electrode sheet as described above. The positive electrode sheet includes the positive electrode current collector containing the safety coating and a positive electrode active material layer coated on at least one surface of the positive electrode current collector. The positive electrode current collector is a common positive electrode current collector in the art, such as aluminum foil, but not limited thereto. The positive electrode active material layer includes a positive electrode active material, which is a common positive electrode active material currently used in lithium-ion batteries, including but not limited to a chemical formula such as Li x Ni h Co y M zO 2-d N d (wherein 0.95≤x≤1.2, h>0, y≥0, z≥0, and h+y+z=1, 0≤d≤1, M is selected from a combination of one or more of Mn and Al, and N is selected from a combination of one or more of F, P, and S) The positive electrode active material may also be, but is not limited to, LiCoO2, LiNiO2, LiVO2, LiCrO2, LiMn2O4, LiCoMnO4, Li2NiMn3O8, LiNi 0.5 Mn 1.5 O4, LiCoPO4, LiMnPO4, LiFePO4, LiNiPO4, LiCoFSO4, CuS2, FeS2, MoS2, NiS, TiS2, etc. The positive electrode active material may also be subjected to a modification treatment, and the method for modifying the positive electrode active material should be known to those skilled in the art. For example, the positive electrode active material may be modified by coating, doping, etc. The material used for the modification treatment may include but is not limited to a combination of one or more of Al, B, P, Zr, Si, Ti, Ge, Sn, Mg, Ce, W, etc.

[0121] In some embodiments of the present invention, the negative electrode sheet is an electrode sheet as described above. The negative electrode sheet includes the negative electrode current collector containing the safety coating and the negative electrode active material layer coated on at least one surface of the negative electrode current collector. The negative electrode current collector has no special requirements and can be a copper foil commonly used in the industry. The negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a silicon-based material, which can be selected from one or more of elemental silicon, silicon oxide compounds, silicon carbon composites, and silicon alloys, or a mixture of silicon negative electrode materials and other commonly used negative electrode active materials. The other negative electrode active materials include but are not limited to one or more of graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microspheres, tin-based materials, lithium titanate or other metals that can form alloys with lithium. Among them, the graphite can be selected from one or more of artificial graphite, natural graphite and modified graphite; the tin-based material can be selected from one or more of elemental tin, tin oxide compounds, and tin alloys.

[0122] In some embodiments of the present invention, the diaphragm may be any material suitable for lithium-ion battery diaphragms in the art, for example, it may be a combination of one or more of polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fiber, etc. In actual production, the material and structure of the diaphragm are not strictly limited, for example, it may be a multi-layer structure formed by stacking the above materials, it may be a single-layer structure formed by mixing the above materials, or it may be a single-layer structure formed by a single material; as long as it can play the basic role of a diaphragm.

[0123] In some embodiments of the present invention, the lithium-ion battery further comprises an electrolyte, and the electrolyte infiltrates the positive electrode, the negative electrode and the separator. The electrolyte comprises an organic solvent, an electrolyte lithium salt and an additive. Among them, the electrolyte lithium salt can be LiPF6 and / or LiBOB used in high-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, and LiPF6 used in low-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, LiPF6, and LiTFSI used in anti-overcharge electrolytes; it can also be at least one of LiClO4, LiAsF6, LiCF3SO3, and LiN(CF3SO2)2. The organic solvent can be a cyclic carbonate, including PC and EC; it can also be a chain carbonate, including DEC, DMC or EMC; it can also be a carboxylic acid ester, including PP, MA, EA, EP, etc. The additives include, but are not limited to, at least one of film-forming additives, conductive additives, flame retardant additives, overcharge prevention additives, additives for controlling the content of H2O and HF in the electrolyte, additives for improving low temperature performance, and water-based safety additives.

[0124] The present invention also provides a secondary battery, including the battery cell as described above or the battery cell obtained by the preparation method as described above. The battery cell provided by the present invention can be applied not only to the above-mentioned lithium-ion battery, but also to other secondary batteries, including sodium-ion batteries, potassium-ion batteries, etc., without any limitation.

[0125] A fourth aspect of the present invention provides an application of the above-mentioned lithium-ion battery in an energy storage device, an electrical device or an electronic device. BRIEF DESCRIPTION OF THE DRAWINGS

[0126] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein: Figure 1 A schematic diagram of the structure of a positive electrode sheet including a safety coating provided by the present invention, wherein 01-positive electrode sheet; 011-positive electrode active material layer; 022-current collector; 023-safety coating; Figure 2A schematic diagram of the cross-sectional structure of a current collector containing a safety coating provided by the present invention along the unwinding direction, wherein 02-positive current collector containing a safety coating; 021-reserved slot; 022-current collector; 023-safety coating; 024-non-safety coating area; Figure 3 A top view of a current collector (not striped) including a safety coating provided by the present invention; Figure 4 A schematic diagram of the cross-sectional structure of a current collector including a safety coating provided by the present invention along the unwinding direction, wherein 021 - reserved slot; 022 - current collector; 023 - safety coating. DETAILED DESCRIPTION

[0127] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0128] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0129] In the description of the present invention, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, wherein a and b are real numbers. Unless otherwise specified, each reaction or operation step may be performed in sequence or not. Preferably, the reaction method of the present invention is performed in sequence.

[0130] If no specific techniques or conditions are specified in the following examples, the techniques or conditions described in the literature in the art or the product instructions are used. All reagents or instruments without manufacturer specified are conventional products that can be purchased commercially.

[0131] Example 1 This embodiment provides a lithium-ion battery, wherein the positive electrode sheet includes a safety coating, wherein the safety coating includes a first active material, lithium iron phosphate (LFP), a first binder, a first conductive agent, Super P Li, and an inorganic filler, boehmite; Wherein, the structural formula of the first binder is:

[0132] (1) Preparation of the first binder: a) adding 1000 parts by weight of distilled water into a reaction vessel, starting stirring, introducing high-purity nitrogen to deoxygenate for 1 hour, then adding 50 parts by weight of acrylonitrile, 35 parts by weight of lithium acrylate, and 15 parts by weight of methyl acrylate, and heating to 65° C. and maintaining the temperature under an inert atmosphere; b) then adding 5 parts by weight of a 20% ammonium persulfate solution as an initiator to initiate the reaction, and reacting for 5 hours; c) After the reaction is completed, the mixture is filtered, dried, crushed and sieved to obtain a binder. In the binder, the proportion of -CN in n1 is 50%, the proportion of -COOLi in n2 is 35%, the proportion of -COOCH3 in n3 is 15%, and the weight average molecular weight M w 3.5×10 5 , number average molecular weight M w 1.8×10 5 , M w / M n =1.94, electrolyte absorption rate c=23%.

[0133] (2) Preparation of positive electrode current collector including safety coating: Deionized water was used as solvent, and 10 parts of the above-mentioned adhesive was added for gluing. The amount of deionized water was adjusted until a solid content of 15% and a viscosity of 2.0×10 4 mPa·s glue; then 58 parts of the first active material lithium iron phosphate (median particle size D v50 The surface area is 0.9 μm and the specific surface area is 10.9 m 2 / g), 30 parts of inorganic filler boehmite (median particle size D v50 The surface area is 0.4 μm and the specific surface area is 9.5 m 2 / g), 1.8 parts of the first conductive agent Super P Li, 0.2 parts of the dispersant polyvinyl pyrrolidone (PVP) and 10% of the total weight of the slurry co-solvent isopropyl alcohol (IPA) were mixed evenly to obtain a safety coating slurry with a solid content of 28% and a viscosity of 50-400 mPa·s. The safety coating slurry was coated on both sides of the aluminum foil by gravure printing. A2 Set to 0, that is, L A1 =L A = L, N1 = N3 = 1, N2 = 4. Safety coating single-sided coating density c w 9 mg / 1540.25 mm 2In addition, the oven temperature during printing should be set to 95 °C and the printing speed should be 30 m / min. The final double-sided coating surface density is 18 mg / 1540.25 mm 2 The double-sided thickness is 10 μm, the double-sided film resistance is 1.1Ω @0.4 T, and the bonding force between the safety coating and the current collector is 225 N / m of the primer. The capacity of lithium iron phosphate in each square meter of safety coating is C1=k×c w ×a, k is 0.306, a is 170, c w 9 mg / 1540.25 mm 2 , then C1 is 468 mAh.

[0134] (3) Preparation of positive electrode sheet: The positive electrode active material lithium cobalt oxide, the second conductive agent (a mixture of conductive carbon black and carbon nanotubes, mass ratio 6:5), PVDF binder and NMP were mixed at a mass ratio of 97.6:1.1:1.3:35 to form a positive electrode slurry with a solid content of 75% and a viscosity of 7000mPa·s. The positive electrode slurry was coated on one side of the current collector aluminum foil containing the safety coating, and the coated surface density was 214mg / 1540.25 mm 2 After drying and rolling at 85°C, the positive electrode slurry is coated and dried on the other side of the current collector aluminum foil containing the safety coating according to the above method, and then the positive electrode sheet coated with the positive electrode active material layer on both sides is cold pressed; then the edges are trimmed and stripped to make lithium-ion battery positive electrode sheets. The capacity C2 of lithium cobalt oxide per square meter of the positive electrode sheet is 24409 mAh.

[0135] (4) Preparation of negative electrode sheet: Using water as solvent, graphite, thickener and SBR binder were mixed evenly in a mass ratio of 97.7:1.1:1.2 to prepare a lithium ion battery negative electrode slurry with a solid content of 50% and a viscosity of 5000 mPa·s, which was then coated on one side of the current collector copper foil with a coating surface density of 115 mg / 1540.25 mm 2 , and dried and rolled at 80°C, and then the negative electrode slurry was coated and dried on the other side of the copper foil according to the above method to obtain a negative electrode sheet with active materials coated on both sides. The capacity C0 of graphite in each square meter of the negative electrode sheet is 25750 mAh.

[0136] (5) Preparation of electrolyte: Lithium hexafluorophosphate (LiPF6) was dissolved in a mixed solvent of dimethyl carbonate (DMC), ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (the mass ratio of DMC, EC and EMC was 3:5:2) to obtain an electrolyte.

[0137] (6) Preparation of batteries: The prepared positive electrode sheet, negative electrode sheet and separator are wound into a battery cell with a capacity of about 5 Ah. The separator is located between the adjacent positive electrode sheet and negative electrode sheet, the positive electrode is spot welded out with an aluminum tab, and the negative electrode is spot welded out with a nickel tab; the battery cell is then placed in an aluminum-plastic packaging bag, baked, and injected with the above electrolyte, and finally made into a lithium-ion battery through packaging, formation, capacity division and other processes.

[0138] Example 2 The difference from Example 1 is that when preparing the positive electrode sheet, the surface density of the positive electrode slurry coating is 218 mg / 1540.25 mm 2 The capacity C2 of lithium cobalt oxide in each square meter of positive electrode sheet is 24865mAh.

[0139] The rest is the same as Example 1 and will not be described again here.

[0140] Example 3 The difference from Example 1 is that when preparing the positive electrode sheet, the surface density of the positive electrode slurry coating is 208.5 mg / 1540.25 mm 2 The capacity C2 of lithium cobalt oxide in each square meter of positive electrode sheet is 23781 mAh.

[0141] The rest is the same as Example 1 and will not be described again here.

[0142] Example 4 The difference from Example 1 is that when the positive electrode is prepared, the single-sided coating density of the safety coating is c w 18 mg / 1540.25 mm 2 The capacity C1 of lithium iron phosphate in each square meter of safety coating is 936 mAh; the surface density of the positive electrode slurry coating is 200 mg / 1540.25 mm 2 The capacity C2 of lithium cobalt oxide in each square meter of positive electrode sheet is 22812 mAh.

[0143] The rest is the same as Example 1 and will not be described again here.

[0144] Example 5 The difference from Example 1 is that when the positive electrode is prepared, the single-sided coating density of the safety coating is c w 3 mg / 1540.25 mm 2 The capacity C1 of lithium iron phosphate in each square meter of safety coating is 156 mAh.

[0145] The rest is the same as Example 1 and will not be described again here.

[0146] Example 6 The difference from Example 1 is that when the positive electrode is prepared, the single-sided coating density of the safety coating is c w 6 mg / 1540.25 mm 2 The capacity C1 of lithium iron phosphate in each square meter of safety coating is 312 mAh.

[0147] The rest is the same as Example 1 and will not be described again here.

[0148] Example 7 The difference from Example 1 is that when the positive electrode is prepared, the single-sided coating density of the safety coating is c w 12 mg / 1540.25 mm 2 The capacity C1 of lithium iron phosphate in each square meter of safety coating is 624 mAh.

[0149] The rest is the same as Example 1 and will not be described again here.

[0150] Example 8 The difference from Example 1 is that when the positive electrode is prepared, the single-sided coating density of the safety coating is c w 18 mg / 1540.25 mm 2 The capacity C1 of lithium iron phosphate in each square meter of safety coating is 936 mAh.

[0151] The rest is the same as Example 1 and will not be described again here.

[0152] Example 9 The difference from Example 1 is that the first active material is replaced by lithium iron phosphate (LFP) with lithium iron manganese phosphate (LMFP), and the rest remains unchanged. The capacity of lithium iron manganese phosphate in each square meter of the safety coating is C1=k×c w ×a, k is 0.306, a is 170, c w 9 mg / 1540.25 mm 2 , then C1 is 468 mAh.

[0153] The rest is the same as Example 1 and will not be described again here.

[0154] Example 10 The difference from Example 1 is that the first active material is replaced by lithium iron phosphate (LFP) with lithium cobalt oxide (LCO), and the rest remains unchanged. The capacity of lithium cobalt oxide in each square meter of safety coating is C1=k×c w ×a, k is 0.399, a is 274, c w 9mg / 1540.25 mm 2 , then C1 is 984 mAh.

[0155] The rest is the same as Example 1 and will not be described again here.

[0156] Embodiment 11 The difference from Example 1 is that: in the first binder, the proportion of -CN in n1 is 55%, the proportion of -COOLi in n2 is 30%, the proportion of -COOCH3 in n3 is 15%, and the weight average molecular weight M w 3.6×10 5 , number average molecular weight M w 2.1×10 5 , M w / M n =1.7, electrolyte absorption rate c=22%.

[0157] The rest is the same as Example 1 and will not be described again here.

[0158] Example 12 The difference from Example 1 is that: in the first binder, the proportion of -CN in n1 is 53%, the proportion of -COOLi in n2 is 37%, the proportion of -COOCH3 in n3 is 10%, and the weight average molecular weight M w 3.4×10 5 , number average molecular weight M w 2.0×10 5 , M w / M n =1.7, electrolyte absorption rate c=17%.

[0159] The rest is the same as Example 1 and will not be described again here.

[0160] Embodiment 13 The difference from Example 1 is that the median particle size D of the first active material lithium iron phosphate (LFP) is v50 2 μm.

[0161] The rest is the same as Example 1 and will not be described again here.

[0162] Embodiment 14 The difference from Example 1 is that the median particle size D of the first active material lithium iron phosphate (LFP) is v50 is 15 μm.

[0163] The rest is the same as Example 1 and will not be described again here.

[0164] Embodiment 15 The difference from Example 1 is that the first binder is replaced by PVDF binder, and the solvent is replaced by NMP (N-methylpyrrolidone) from deionized water.

[0165] The rest is the same as Example 1 and will not be described again here.

[0166] Comparative Example 1 The difference from Example 1 is that when the positive electrode is prepared, the single-sided coating density of the safety coating is c w 30 mg / 1540.25 mm 2 The capacity C1 of lithium iron phosphate in each square meter of safety coating is 1561 mAh; the surface density of the positive electrode slurry coating is 200 mg / 1540.25 mm 2 The capacity C2 of lithium cobalt oxide in each square meter of positive electrode sheet is 22812 mAh.

[0167] The rest is the same as Example 1 and will not be described again here.

[0168] Comparative Example 2 The difference from Example 1 is that when the positive electrode is prepared, the single-sided coating density of the safety coating is c w 2.5mg / 1540.25 mm 2 The capacity C1 of lithium iron phosphate in each square meter of safety coating is 130 mAh.

[0169] The rest is the same as Example 1 and will not be described again here.

[0170] Comparative Example 3 The difference from Example 1 is that when the positive electrode is prepared, the single-sided coating density of the safety coating is c w 18 mg / 1540.25 mm 2 The capacity C1 of lithium iron phosphate in each square meter of safety coating is 936 mAh; the surface density of the positive electrode slurry coating is 218 mg / 1540.25 mm 2 The capacity C2 of lithium cobalt oxide in each square meter of positive electrode sheet is 24865mAh.

[0171] The rest is the same as Example 1 and will not be described again here.

[0172] Comparative Example 4 The difference from Example 1 is that when preparing the positive electrode sheet, the surface density of the positive electrode slurry coating is 202.5 mg / 1540.25 mm 2 The capacity C2 of lithium cobalt oxide in each square meter of positive electrode sheet is 23097 mAh.

[0173] The rest is the same as Example 1 and will not be described again here.

[0174] Comparative Example 5 The difference from Example 1 is that when the positive electrode sheet is prepared, the safety coating does not contain the first active material.

[0175] The rest is the same as Example 1 and will not be described again here.

[0176] Comparative Example 6 The difference from Example 1 is that when the positive electrode sheet is prepared, the safety coating does not contain a dispersant.

[0177] The rest is the same as Example 1 and will not be described again here.

[0178] Comparative Example 7 The difference from Example 1 is that the surface of the positive electrode current collector is not coated with a safety coating.

[0179] The rest is the same as Example 1 and will not be described again here.

[0180] Test Case In order to verify the effect of the introduction of the safety coating of the present invention on the performance of the battery cell, the electrolyte absorption rate c of the first adhesive, as well as the acupuncture, 132°C / 136°C hot box, low temperature discharge performance, rate performance and cycle performance of the battery cell were tested.

[0181] Electrolyte absorption rate c test method: Pour the binder solution into a polytetrafluoroethylene plate, bake it to volatilize the deionized water and obtain an adhesive polymer film. The thickness of the film is controlled at 100μm, and it is cut into a 50mm long × 50mm wide film. After that, the film is vacuum dried for 24 hours and weighed. Then, the completely dried film is immersed in an electrolyte at 80℃ for 12 hours and then taken out. After wiping off the electrolyte attached to the surface of the film, the weight of the film after absorbing the electrolyte is weighed. The increase rate (%) of the weight of the film before and after immersion in the electrolyte is the 80℃ absorption rate of the binder. o C of electrolyte absorption rate.

[0182] Needle penetration test method: charge to 4.45 V at 1.0 C constant current and constant voltage at room temperature, with a cut-off rate of 0.05 C, and then subject the fully charged cell to a needle penetration test. During the test, the deep pit side of the cell faces upward, and a steel nail with a diameter of 4.0 mm is used to completely pierce the cell at a speed of 40 mm / s. The nail penetration position is located at the left, middle, and right positions of the largest surface of the cell (5 cells are tested at each position). Keep for 1 hour. The cell passes the test if it does not catch fire or explode.

[0183] 132℃ / 136℃ hot box test method: discharge at 0.2 C constant current to 3 V at room temperature and leave for 5 min; charge at 1.0 C constant current and constant voltage to 4.45 V, with a cut-off rate of 0.05 C, and then conduct a hot box test on the fully charged cell. During the test, the cell is hung in the oven, and the oven temperature is raised to 132℃ or 136℃ at a rate of 5±2℃ / min, and stopped after 60 min. During the test, the cell surface temperature, ambient temperature and voltage need to be monitored. The cell passes the test if it does not catch fire or explode.

[0184] Low-temperature discharge performance test method: discharge at 1 C constant current to 3 V, and let it stand for 5 min; set the incubator to 25℃ and let it stand for 60 min; charge at 1.0 C constant current and constant voltage to 4.45 V, with a cutoff rate of 0.02 C; let it stand for 5 min, discharge at 0.2 C constant current to 3 V, and record the capacity when discharged to 3 V at 0.2 C as the initial capacity C0; set the incubator to 25℃ and let it stand for 60 min; charge at 1.0 C constant current and constant voltage to 4.45 V, with a cutoff rate of 0.02 C; let it stand for 5 min, set the incubator to -10℃, let it stand for 120 min, then discharge the cell at 0.2 C to 3.0 V, and record the capacities C1 and C2 when discharged to 3.4 V and 3.0 V. The ratio of C1 to C0 is the capacity retention rate when discharged to 3.4 V at -10℃.

[0185] Rate discharge performance test method: discharge at 1 C constant current to 3 V, and let it stand for 5 min; charge at 1.0 C constant current and constant voltage to 4.45 V, with a cut-off rate of 0.02 C, and let it stand for 5 min; discharge at 0.2 C constant current to 3 V, and record the capacity when discharged to 3 V at 0.2 C as the initial capacity C3; charge at 1.0 C constant current and constant voltage to 4.45 V, with a cut-off rate of 0.02 C, and let it stand for 5 min; then discharge the battery cell at 0.2 C to 3.0 V, and record the capacities C4 and C5 when discharged to 3.4 V and 3.0 V. The ratio of C4 to C3 is the capacity retention rate when discharged to 3.4 V at 2C.

[0186] Cycling performance test method: Under the condition of ambient temperature of 25±2℃, discharge the battery cell at 0.2 constant current to 3.0V, then charge it to 4.45V at 3C constant current and constant voltage, with a cut-off rate of 0.05C, and record the voltage, internal resistance, capacity and thickness of the battery cell when it is fully charged for the first time (600gPPG is used for thickness measurement). The cycling process is in accordance with the following HFC standard: discharge to 3V at 0.2C constant current; charge to 4.25V at 3.0C constant current; charge to 4.25V at 2.5C constant current; charge to 4.45V at 2.0C constant current; charge to 4.50V at 1.4C constant current and constant voltage, with a cut-off rate of 0.3C; charge to 4.45V at 2A constant current and constant voltage, with a cut-off rate of 0.05C; discharge to 3V at 1.0C constant current. The above steps are considered one cycle. After 49 cycles, low current recovery is performed according to the following system: charge to 4.25 V at 3.0 C constant current; charge to 4.25 V at 2.5 C constant current; charge to 4.45 V at 2.0 C constant current; charge to 4.50 V at 1.4 C constant current and constant voltage, with a cut-off rate of 0.3 C; charge to 4.45 V at 2 A constant current and constant voltage, with a cut-off rate of 0.05 C; discharge to 3 V at 0.2 C constant current; charge to 4.45 V at 3.0 C constant current and constant voltage, with a cut-off rate of 0.05 C. Record the fully charged cell voltage, internal resistance, and thickness (600 gPPG is used for thickness measurement) every 100 cycles.

[0187] The parameter settings of Examples 1-15 and Comparative Examples 1-7 are shown in Table 1 below: Table 1

[0188] The test results of Examples 1-15 and Comparative Examples 1-7 are shown in Table 2 below: Table 2

[0189] From the comparison of the parameter settings in Tables 1-2 and the cell test results, it can be seen that compared with Comparative Examples 1-7, the safety coating in Examples 1-15 meets the requirement of 0.002≤ ≤0.04, and 1.019≤NP1≤1.089, the puncture performance of the corresponding battery cell is significantly improved, the pass rate of the puncture test is increased from 0% to more than 80%, the hot box is improved by 4℃, and the low-temperature discharge performance, rate discharge performance and cycle performance are also improved. The capacity retention rate after 800 cycles at 25℃ is not less than 90%, the discharge capacity at -10℃ is not less than 70% @3.4 V, and the discharge capacity at 2 C is not less than 70% @3.4 V.

[0190] It can be seen from Comparative Example 1 that although the performance of the battery cell is not significantly deteriorated compared with Example 1, is 0.067, c w 30 mg / 1540.25 mm 2 , which will lead to a decrease in its energy density and poor practicality.

[0191] From Comparative Example 2, it can be seen that is only 0.001, corresponding to c w 2.5 mg / 1540.25 mm 2 , the coating process requires high precision and the needle punching performance deteriorates.

[0192] It can be seen from Comparative Example 3 that NP1 is only 1.003, the residual capacity of the negative electrode is insufficient, and lithium plating is very likely to occur during the cycle, resulting in the battery cell failing due to cycle dive.

[0193] From Comparative Example 4, it can be seen that NP1 is 1.098, and the potential is higher when fully charged. It is found that both its hot box and cycle performances are deteriorated.

[0194] Comparative Examples 5-7 show that if the safety coating does not contain the first active substance or dispersant, or if the safety coating is not applied, the performance of the battery cell will deteriorate.

[0195] In summary, the safety coating provided by the present invention contains the first active material, and by limiting the coating surface density and capacity of the first active material, the mechanical safety performance, thermal abuse performance and cycle performance of the battery cell are improved, while the low temperature discharge performance and rate discharge performance of the battery are improved. The battery cell provided by the present invention has a safety coating that satisfies 0.002≤ When ≤0.04 and 1.019≤NP1≤1.089, the puncture pass rate can be greater than 80%, the hot box temperature is improved by 4°C, and the capacity retention rate after 800 cycles at 25°C is not less than 90%, the discharge capacity at -10°C is not less than 70% @3.4V, and the discharge capacity at 2 C is not less than 70% @3.4 V.

[0196] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A battery cell, characterized in that: include: A positive electrode sheet and a negative electrode sheet; the positive electrode sheet comprises a safety coating and a positive electrode active material layer, the safety coating comprises a first active material and a dispersant, and the positive electrode active material layer comprises a positive electrode active material; The negative electrode sheet comprises a negative electrode active material layer, and the negative electrode active material layer comprises a negative electrode active material; The first capacity ratio NP1 of the battery cell satisfies 1.019≤NP1≤1.089, and the relative capacity ratio Satisfy 0.002≤ ≤0.04; The calculation formula of the first capacity ratio NP1 is: , the relative capacity ratio The calculation formula is: ; C1 is the capacity of the first active substance in the safety coating per unit area. The calculation formula of C1 is: C1=k×c w ×a, 0<k<1, 0<a≤300, c w is the single-sided coating density of the safety coating, a is the theoretical gram capacity of the first active substance, and k is a constant; C2 is the capacity of the positive electrode active material in the positive electrode active material layer per unit area; C0 is the capacity of the negative electrode active material per unit area of ​​the negative electrode active material layer.

2. The battery cell according to claim 1, characterized in that: The first active material includes one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate and ternary materials; and / or, the median particle size D of the first active substance v50 The range is 0.1~15μm, and the specific surface area is 2~50 m 2 / g.

3. The battery cell according to claim 2, characterized in that: Include at least one of the following: A1) the first active material is a ternary material, and the ternary material includes at least one of a nickel-cobalt-manganese ternary material and a nickel-cobalt-aluminum ternary material; A2) When including A1), the nickel-cobalt-manganese ternary material includes at least one of NCM333, NCM523, NCM613, NCM622 and NCM811; A3) the surface of the first active material is coated with an inorganic ceramic material; A4) When A3) is included, the inorganic ceramic material includes silicon dioxide, aluminum oxide or titanium oxide.

4. The battery cell according to claim 1, characterized in that: The dispersant includes one or more of an ionic dispersant, a nonionic dispersant, an amphoteric dispersant and a fluorine surfactant.

5. The battery cell according to claim 4, characterized in that: The ionic dispersant includes one or more of polyacrylic acid and its salts, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and polyethyleneimine; and / or, the nonionic dispersant comprises one or more of polyvinyl pyrrolidone, polyethylene glycol, polyvinyl alcohol, polyoxyethylene and carboxymethyl cellulose; And / or, the amphoteric dispersant comprises betaine.

6. The battery cell according to claim 1, characterized in that: The safety coating further comprises a first conductive agent, a first binder and an inorganic filler; and the safety coating satisfies at least one of the following: B1) The mass ratio of the first conductive agent, the first binder, the inorganic filler, the first active material, and the dispersant is (0.5-5): (1-21.2): (1-50): (1-95): (0.01-1); B2) The median particle size D of the inorganic filler v50 The range is 0.1~5μm, and the specific surface area is 8~15m 2 / g; B3) the inorganic filler comprises one or more of alumina, boehmite, aluminum hydroxide, magnesium hydroxide, silicon dioxide or titanium dioxide; B4) The first binder includes one or more of polyvinylidene fluoride binder, sodium carboxymethyl cellulose binder or polyacrylate binder.

7. The battery cell according to claim 6, characterized in that: The first binder is a polyacrylate binder, and the structural formula of the polyacrylate binder is: ; wherein each occurrence of R1 is independently selected from H, Li or Na; Each occurrence of R2 is independently selected from substituted or unsubstituted C1~C 10 The alkyl group; And 5≤(x+z) / y≤20, 1.2≤z / x≤2, x, y, z are not 0; And / or, the weight average molecular weight M of the polyacrylate binder w The range is 200000~500000, the number average molecular weight M n The range is 100000~400000; And / or, the weight average molecular weight M of the polyacrylate binder w and number average molecular weight M n The ratio M w / M n ≤3; and / or, the electrolyte absorption rate of the polyacrylate binder at 80° C. is 10% to 50%; And / or, the mass fraction of the polyacrylate binder in the safety coating is 1% to 21.2%.

8. The battery cell according to claim 1, characterized in that: The positive electrode sheet further includes a positive electrode current collector, the safety coating is coated on at least one side of the positive electrode current collector, and the positive electrode active material layer is coated on the side of the safety coating away from the positive electrode current collector or the side of the positive electrode current collector away from the safety coating; the negative electrode sheet further includes a negative electrode current collector, and the negative electrode active material layer is coated on at least one side of the negative electrode current collector; And / or, the single-sided coating density of the safety coating is 3 mg / 1540.25 mm 2 ~18mg / 1540.25mm 2 .

9. The battery cell according to claim 8, characterized in that: The safety coating is coated on both sides of the positive electrode current collector; the safety coating satisfies at least one of the following: C1) The double-sided thickness of the safety coating is 1-20 μm; C2) The double-sided diaphragm resistance of the safety coating tested under a pressure of 0.4t is 0.5~5Ω; C3) The double-sided thickness d of the safety coating and the value of the double-sided diaphragm resistance R under a pressure of 0.4t satisfy the condition: 2≤R×d≤50; C4) along the direction perpendicular to the unwinding direction of the positive electrode current collector, the distance W between the left edge of the safety coating on the A side of the positive electrode current collector and the left edge of the positive electrode current collector A1 The range is 2mm~30mm, and the distance W between the right edge and the right edge of the positive electrode collector is A2 The range is 2mm~30mm; the distance W between the left edge of the safety coating on the B side of the positive electrode collector and the left edge of the positive electrode collector B1 The range is 3mm~30mm, and the distance W between the right edge and the right edge of the positive electrode collector is B2 The range is 3mm~30mm; and W B1 -W A1 ≥1mm, W B2 -W A2 ≥1mm.

10. A method for preparing a battery cell according to any one of claims 1 to 9, characterized in that: Includes steps: Mixing the raw materials for preparing the safety coating in a solvent to obtain a safety coating slurry; Applying the safety coating slurry to at least one side of the surface of the positive electrode current collector to obtain a positive electrode current collector containing the safety coating; Coating a positive electrode active material layer on a side surface of the safety coating layer away from the positive electrode current collector or a side surface of the positive electrode current collector away from the safety coating layer to obtain a positive electrode sheet; coating a negative electrode active material layer on the negative electrode current collector to obtain a negative electrode sheet; The positive electrode sheet and the negative electrode sheet are assembled to obtain a battery cell.

11. The method for preparing a battery cell according to claim 10, characterized in that: Include at least one of the following: D1) The solid content of the safety coating slurry is ≥ 10%; D2) the viscosity of the safety coating slurry is ≥50 mPa·s; D3) the dyne value of the positive electrode current collector is ≥30 dyn / cm; D4) applying the safety coating slurry to one or both sides of the positive electrode current collector by gravure printing; D5) When D4) is included, the oven temperature during gravure printing is 90-110°C and the printing speed is 10-50 m / min.

12. A lithium ion battery, characterized in that: The invention comprises a battery cell according to any one of claims 1 to 9 or a battery cell obtained by the preparation method according to any one of claims 10 to 11.

13. Use of the lithium-ion battery according to claim 12 in an energy storage device, an electrical device or an electronic device.

Citation Information

Patent Citations

  • Positive plate of high power lithium ionic cell and lithium ionic cell containing the same

    CN101388449A

  • Acrylonitrile copolymer adhesive and application thereof in lithium ion batteries

    CN106220779A

  • Multilayer positive plate electrode structure, preparation method thereof, and positive and negative electrode battery structure

    CN111129428A

  • Lithium battery positive pole piece and preparation method thereof and lithium battery adopting positive pole piece

    CN112510168A

  • Coating mode of short negative electrode of winding type polymer lithium ion battery

    CN112750970A

Cited By

  • Safety coating and application thereof, electrode plate and lithium ion battery

    CN118970023A

  • A safety coating and its application, electrode sheet and lithium ion battery

    CN118970023B

  • Lithium ion battery and method for predicting, regulating and controlling diaphragm resistance of lithium ion battery

    CN119627034A

  • 3D printing overhang slurry, electrode plate, battery cell and preparation method thereof, and solid-state battery

    CN120413675A

  • Preparation method of lithium ion battery cell

    CN122091783A