A lithium ion battery

By using lithium aluminum titanium phosphate (LATP) and phosphoric anhydride compounds to form a low-resistance passivation layer in lithium-ion batteries, combined with optimized electrolyte composition, the performance degradation problem of lithium-ion batteries in extremely low temperature environments has been solved, achieving improved high-rate discharge and long-cycle performance.

CN118676373BActive Publication Date: 2024-11-22SHENZHEN HIGHPOWER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411147243.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-22
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Lithium-ion batteries degrade in performance at extremely low temperatures, leading to cell polarization, reduced discharge capacity, and safety hazards. Existing improvement methods, such as using carboxylic acid ester solvents, result in increased battery impedance and lithium plating, and cannot effectively solve the limitations of low-temperature applications.

Method used

Lithium aluminum titanium phosphate (LATP) is added to the positive electrode and phosphoric anhydride compounds are added to the electrolyte to form a stable and low-impedance passivation layer, which improves conductivity and reduces polarization. Combined with a low-viscosity solvent and a high-conductivity lithium salt, the electrolyte composition is optimized to improve lithium-ion migration.

Benefits of technology

It achieves high-rate discharge and long-cycle performance of lithium-ion batteries in extremely low-temperature environments, reduces polarization, and improves the application performance of batteries under low-temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118676373B_ABST
    Figure CN118676373B_ABST
Patent Text Reader

Abstract

The present application relates to a lithium-ion battery. The lithium-ion battery comprises a positive electrode plate, a negative electrode plate, a separator and an electrolyte. The positive electrode plate comprises a positive current collector and a positive electrode material layer coated on the surface of the positive current collector, and the positive electrode material layer comprises lithium aluminum titanium phosphate; the electrolyte comprises an additive A, and the chemical structure of the additive A is shown in Formula I: #imgabs0#; wherein R1, R2, and R3 are each independently selected from hydrocarbon groups with no more than 4 carbon atoms substituted or unsubstituted by fluorine. The technical solution of the present application can form a stable and low-impedance passivation layer at the interface between the positive and negative electrodes, improve the electrical conductivity at low temperatures, and reduce the polarization effect on the positive and negative electrode sides in low temperature environments, thereby improving the low-temperature high-rate discharge and low-temperature long-cycle performance of lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a lithium-ion battery. Background Art

[0002] Lithium-ion batteries have become the preferred energy storage carrier for consumer electronics such as laptops, mobile phones, cameras, and new energy vehicles due to their high energy density and long cycle life.

[0003] With the continuous development of application products, the performance requirements for lithium-ion batteries are becoming higher and higher, especially when the operating conditions deviate from room temperature, such as under extremely low temperature conditions (≤-10℃), the ionic conductivity of the electrolyte decreases, and the solvation / desolvation of lithium ions in the electrolyte becomes more difficult. At the same time, the migration rate of lithium ions in the solid phase of positive and negative electrode materials and the interface between electrode materials and electrolytes (including SEI membranes and CEI membranes) will also be greatly reduced, causing polarization of the battery cell; during discharge, the battery cell voltage will reach the set cut-off voltage in advance, which will lead to a reduction in actual discharge capacity, serious deterioration of battery performance, and may even cause battery failure and safety hazards. The deterioration of the performance of lithium-ion batteries in low temperature environments will limit the use scenarios of application products.

[0004] To address the problem of deteriorating low-temperature performance of lithium-ion batteries, current improvement measures mainly focus on developing low-viscosity solvents, such as using carboxylates instead of carbonates. However, the electrochemical window of carboxylates is narrower than that of carbonates, resulting in an accumulation of battery impedance in the later stages of the cycle, which in turn causes lithium plating and leads to battery failure. This still cannot effectively solve the application limitations of lithium-ion batteries in extremely low temperature environments. Summary of the invention

[0005] In order to solve or partially solve the problems existing in the related art, the present application provides a lithium-ion battery that can form a stable and low-impedance passivation layer at the interface between the positive and negative electrodes, improve the electrical conductivity at low temperatures, and at the same time reduce the polarization effect on the positive and negative electrode sides in a low temperature environment, thereby improving the low-temperature high-rate discharge and low-temperature long-cycle performance of the lithium-ion battery.

[0006] The present application provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode material layer coated on the surface of the positive electrode current collector, wherein the positive electrode material layer comprises lithium aluminum titanium phosphate;

[0007] The electrolyte includes an additive A, and the chemical structural formula of the additive A is shown in Formula I:

[0008] ;

[0009] Wherein, R1, R2, and R3 are each independently selected from a hydrocarbon group having no more than 4 carbon atoms, which may be substituted or unsubstituted with fluorine.

[0010] In some optional embodiments, the positive electrode plate and the electrolyte satisfy:

[0011] ;

[0012] Wherein, c (%) represents the mass percentage of additive A in the electrolyte;

[0013] L (%) represents the mass percentage of lithium aluminum titanium phosphate in the positive electrode material layer;

[0014] f (g / Ah) represents the injection coefficient of the electrolyte in the lithium-ion battery;

[0015] D (μm) represents the D50 particle size of lithium aluminum titanium phosphate in the positive electrode material layer.

[0016] In some optional embodiments, the mass percentage c% of the additive A in the electrolyte satisfies: 0.3≤c≤1.2.

[0017] In some optional embodiments, the mass percentage L% of lithium aluminum titanium phosphate in the positive electrode material layer satisfies: 0.5≤L≤1.0.

[0018] In some optional embodiments, the injection coefficient f (g / Ah) of the electrolyte in the lithium-ion battery satisfies: 1.5≤F≤1.8.

[0019] In some optional embodiments, the D50 particle size D (μm) of the lithium aluminum titanium phosphate in the positive electrode material layer satisfies: 0.2≤D≤0.5.

[0020] In some optional embodiments, the additive A is selected from at least one of the following compounds: n-methyl phosphoric anhydride, n-ethyl phosphoric anhydride, n-propyl phosphoric anhydride, n-butyl phosphoric anhydride, and pentafluoroethyl phosphoric anhydride.

[0021] In some optional embodiments, the electrolyte further includes a lithium salt, and the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium bisfluorooxalatoborate, lithium bisoxalatoborate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethylimide, lithium difluorooxalatophosphate, and lithium perchlorate;

[0022] The mass percentage of lithium salt in the electrolyte is 8% to 15%.

[0023] In some optional embodiments, the lithium salt includes lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, wherein the mass percentage of lithium bis(fluorosulfonyl)imide in the electrolyte is 2% to 6%.

[0024] In some optional embodiments, the electrolyte further includes an organic solvent, and the organic solvent is selected from at least two of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl formate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, and ethyl difluoroacetate; the mass percentage of the organic solvent in the electrolyte is 73% to 85.2%.

[0025] In some optional embodiments, the organic solvent includes at least propylene carbonate and ethyl propionate, wherein the mass percentage of ethyl propionate in the electrolyte is 50% to 65%.

[0026] In some optional embodiments, the electrolyte further includes an additive B, and the additive B includes at least one of a nitrile compound, a carbonate compound, and a sulfate compound.

[0027] In some optional embodiments, the nitrile compound is selected from at least one of hexamethylene dinitrile, succinonitrile, 1,3,6-hexanetricarboxylic acid nitrile, trans-hexamethylene dinitrile, trans-butene dinitrile, 1,2-bis(cyanoethoxy)ethane and 1,2,3-tris(cyanoethoxy)propane; and the mass percentage of the nitrile compound in the electrolyte is 2% to 4%.

[0028] In some optional embodiments, the carbonate compound is selected from at least one of vinylene carbonate, ethylene carbonate, methylene carbonate, fluoroethylene carbonate, trifluoromethylethylene carbonate and difluoroethylene carbonate; the mass percentage of the carbonate compound in the electrolyte is 4% to 6%.

[0029] In some optional embodiments, the sulfate ester compound is selected from at least one of vinyl sulfate, vinyl sulfite, 4-methyl vinyl sulfate, dimethyl sulfite and diethyl sulfite; and the mass percentage of the sulfate ester compound in the electrolyte is 0.5% to 1%.

[0030] The technical solution provided by this application may have the following beneficial effects:

[0031] In the present application scheme, a solid electrolyte lithium aluminum titanium phosphate LATP is added to the positive electrode material. The LATP skeleton has a three-dimensional ion migration channel, which can increase the migration rate of lithium ions at the positive electrode interface, which is beneficial to improving the charge and discharge performance of the battery; at the same time, LATP can also catalyze the additive A phosphoric anhydride compound to form a low-impedance and highly stable interface protection layer at the positive electrode interface, which can increase the conductivity of the lithium-ion battery at low temperatures, and reduce the polarization effect on the positive electrode side in an extremely low temperature environment, so that the lithium-ion battery can achieve high-rate discharge and low-temperature long-cycle performance when used in an extremely low temperature environment.

[0032] Furthermore, the present application, through a low-viscosity solvent system and a lithium salt combination of lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate with high conductivity, when used in combination with additive A, can achieve rapid transmission of lithium ions in the solvent, while achieving the purpose of reducing the polarization of the positive and negative electrodes in an extremely low temperature environment, thereby improving the low-temperature discharge performance and cycle performance of lithium-ion batteries when used in a low-temperature environment.

[0033] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. DETAILED DESCRIPTION

[0034] To make the present invention easy to understand, the present invention will be described in detail below. However, before describing the present invention in detail, it should be understood that the present invention is not limited to the specific embodiments described. It should also be understood that the terms used herein are only for describing specific embodiments and are not intended to be limiting.

[0035] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0036] Where a numerical range is provided, it is to be understood that each intermediate value between the upper and lower limits of the range and any other provisions or intermediate values ​​in the specified range is encompassed within the present invention. The upper and lower limits of these smaller ranges may be independently included in the smaller ranges and are also encompassed within the present invention, subject to any explicitly excluded limits in the specified range. Where a specified range includes one or two limits, the scope excluding any or both of those included limits is also encompassed within the present invention. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically limited.

[0037] Unless otherwise defined, all terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. Although any methods and materials or equivalent methods and materials described herein can also be used in the practice or testing of the present invention, preferred methods and materials are now described.

[0038] At extremely low temperatures, the migration rate of lithium ions in the positive and negative electrode materials, as well as the interface between the electrolyte and the materials, will be severely reduced, causing polarization of the battery cell. During discharge, the overpotential generated by the polarization of the battery cell will cause the battery cell voltage to reach the set cut-off voltage ahead of schedule, resulting in a reduction in the actual discharge capacity. During charging, the overpotential generated by battery polarization will cause the charging capacity to decrease and the negative electrode potential to be lower than the lithium reduction potential, resulting in irreversible lithium deposition. Irreversible lithium deposition will deteriorate the battery cell capacity and may pierce the diaphragm and reduce the electrolyte solvent, thereby generating flammable gases and causing safety hazards. The above factors will deteriorate the performance of lithium-ion batteries in low temperature environments and limit the use scenarios of consumer electronic products.

[0039] In response to the above problems, an embodiment of the present application provides a lithium-ion battery that can form a stable and low-impedance passivation layer at the interface between the positive and negative electrodes, thereby improving the electrical conductivity at low temperatures, while reducing the polarization effect on the positive and negative electrode sides in extremely low temperature environments, thereby improving the extremely low temperature high-rate discharge and low-temperature long-cycle performance of the lithium-ion battery.

[0040] The lithium-ion battery of the embodiment of the present application includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The positive electrode sheet includes a positive electrode current collector and a positive electrode material layer coated on the surface of the positive electrode current collector, and the positive electrode material layer includes lithium aluminum titanium phosphate; the electrolyte includes an additive A, and the chemical structure of the additive A is shown in Formula I:

[0041] ;

[0042] In formula I, R1, R2, and R3 are each independently selected from a hydrocarbon group having no more than 4 carbon atoms and substituted or unsubstituted by fluorine.

[0043] In the embodiment of the present application, a solid electrolyte lithium aluminum titanium phosphate LATP is added to the positive electrode material. The LATP skeleton has a three-dimensional ion migration channel, which can increase the migration rate of lithium ions at the positive electrode interface, which is beneficial to improving the charge and discharge performance of the battery; at the same time, LATP can also catalyze the additive A phosphoric anhydride to form a low-impedance and highly stable interface protection layer at the positive electrode interface, which can improve the conductivity of the lithium-ion battery at low temperatures, and reduce the polarization effect on the positive electrode side in an extremely low temperature environment, so that the lithium-ion battery can achieve high-rate discharge and low-temperature long cycle performance when used in an extremely low temperature environment.

[0044] In some embodiments, R1, R2, and R3 in the additive A may be the same or different; preferably, R1, R2, and R3 are the same group. In some preferred embodiments, the additive A may be selected from at least one of the following compounds: n-methyl phosphoric anhydride (Formula I-1, CAS NO.82593-65-5), n-ethyl phosphoric anhydride (Formula I-2, CAS NO.145007-52-9), n-propyl phosphoric anhydride (Formula I-3, CAS NO.68957-94-8), n-butyl phosphoric anhydride (Formula I-4, CAS NO.163755-62-2), pentafluoroethyl phosphoric anhydride (Formula I-5, CAS NO.103304-98-9), etc.

[0045]

[0046] The electrolyte containing phosphoric anhydride in the embodiment of the present application can form a dense SEI film and CEI film at the interface of the positive and negative electrodes, thereby effectively reducing the decomposition of the electrolyte at the interface of the positive and negative electrodes, and can also absorb the hydrofluoric acid produced by the side reaction in the electrolyte, reduce the damage of hydrofluoric acid to the positive and negative electrode materials, and improve the cycle performance of the battery; at the same time, the interface film formed at the electrode interface has a small impedance, which can effectively reduce the increase of interface impedance during the cycle process, and the application of lithium titanium aluminum phosphate solid electrolyte in the positive electrode plate can promote the film formation of phosphoric anhydride at the positive electrode, reduce the increase of negative electrode impedance caused by excessive participation of phosphoric anhydride in the film formation of the negative electrode, and the combination of the two can effectively improve the migration rate of lithium ions in the battery, and can reduce the increase of interface impedance during the cycle process, thereby improving the high-rate discharge performance and long cycle performance of lithium-ion batteries when used in extremely low temperature environments.

[0047] In some embodiments, in a lithium-ion battery, the positive electrode sheet and the electrolyte satisfy:

[0048] ;

[0049] Wherein, c (%) represents the mass percentage of additive A in the electrolyte; L (%) represents the mass percentage of lithium aluminum titanium phosphate in the positive electrode material layer; f (g / Ah) represents the injection coefficient of the electrolyte in the lithium-ion battery; D (μm) represents the D50 particle size of lithium aluminum titanium phosphate in the positive electrode material layer.

[0050] In the embodiment of the present application, by optimizing the relationship between the positive electrode plate and the electrolyte, the electrolyte is adapted to the composite positive electrode doped with the solid electrolyte LATP, which is conducive to forming a low-impedance and highly stable interface protection layer on the surface of the composite positive electrode, so that lithium ions can quickly migrate between the positive and negative electrodes even in extremely low temperature environments, thereby improving the low-temperature performance of lithium-ion batteries.

[0051] For this lithium-ion battery, the electrolyte injection coefficient f (g / Ah) satisfies: 1.5≤F≤1.8, for example, it can be 1.5g / Ah, 1.6g / Ah, 1.7g / Ah, 1.8g / Ah or any value within the above range. If the electrolyte injection coefficient is too low, it is difficult for the electrolyte to evenly infiltrate the entire battery cell, and it is difficult for the additives in the electrolyte to evenly form a film on the surface of the battery cell, and the local interface protection of the battery cell is insufficient; if the injection coefficient is too high, it is easy to cause problems such as poor packaging and excessive floating liquid, which can easily cause safety problems.

[0052] In the lithium-ion battery, the mass percentage c% of the additive A in the electrolyte satisfies: 0.3≤c≤1.2, for example, it can be 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2% or any value within the above range. If the phosphoric anhydride content in the electrolyte is too low, the content of the low-impedance interface film formed on the electrode surface is limited, and the content of the CEI film at the positive electrode interface is limited, it is difficult to play the effect of reducing the positive electrode interface impedance; if the phosphoric anhydride content is too high, it will increase the negative electrode impedance, which is not conducive to the lithium ion migration of the negative electrode, and at the same time it will increase the viscosity of the electrolyte, deteriorate the low-temperature charge and discharge performance of the battery, and is not conducive to the application of the battery in a low-temperature environment.

[0053] In the lithium-ion battery, the mass percentage content L% of lithium aluminum titanium phosphate in the positive electrode material layer satisfies: 0.5≤L≤1.0, for example, it can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0% or any value within the above range. As an added component of the positive electrode material layer, the lithium aluminum titanium phosphate solid electrolyte is a composite material composed of phosphate, titanate, aluminate and lithium salt, with a stable structure and a large specific surface area, which is conducive to the adsorption and catalysis of phosphoric anhydride to form a low-impedance passivation layer at the positive electrode, thereby reducing the polarization of the positive electrode side under low-temperature discharge. Too low an amount of lithium aluminum titanium phosphate solid electrolyte added has no obvious effect on improving the film-forming catalytic efficiency of phosphoric anhydride, while too high an amount of lithium aluminum titanium phosphate solid electrolyte added will increase the production cost, and at the same time deteriorate the cycle stability of the battery, and cause the content of positive active substances in the positive electrode material layer to decrease, thereby causing the battery energy density to fail to meet the standard, which is not conducive to the low-temperature long cycle performance of the battery.

[0054] In this lithium-ion battery, the D50 particle size D (μm) of lithium aluminum titanium phosphate in the positive electrode material layer satisfies: 0.2≤D≤0.5, for example, it can be 0.2μm, 0.25μm, 0.3μm, 0.35μm, 0.4μm, 0.45μm, 0.5μm or any value within the above range. It can be understood that the D50 particle size of lithium aluminum titanium phosphate is the particle size corresponding to more than 50% of lithium aluminum titanium phosphate. The smaller the particle size of lithium aluminum titanium phosphate, the larger its specific surface area, and the higher the efficiency of catalyzing phosphoric anhydride additive in forming a film at the positive electrode; however, the smaller the particle size of lithium aluminum titanium phosphate, the higher the production cost, and it is easier to contact with lithium metal to undergo redox reaction, resulting in battery failure, which is not conducive to the low-temperature long cycle performance of the battery.

[0055] In some embodiments, the electrolyte further comprises a lithium salt, which may be selected from at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium bisfluorooxalatoborate, lithium bisoxalatoborate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethylimide, lithium difluorooxalatophosphate, and lithium perchlorate.

[0056] The mass percentage of lithium salt in the electrolyte is 8% to 15%, for example, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15% or any value within the above range. As the amount of lithium salt used increases, the viscosity of the electrolyte increases when used in a low-temperature environment. If the amount is too high, the low-temperature discharge performance of the battery will deteriorate; while too low a lithium salt amount will also lead to low lithium ion conductivity in the electrolyte and increased concentration polarization level of the battery cell, which is not conducive to the application of the battery in low-temperature scenarios.

[0057] In some preferred embodiments, the lithium salt includes lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide. The lithium salt combination has good compatibility with organic solvents and additives, and can maintain high conductivity of lithium-ion batteries in low temperature environments; and the two cooperate to participate in the negative electrode film formation, so that the negative electrode SEI film has both stability and low impedance, improves the kinetic performance of the negative electrode, and enhances the low temperature long cycle performance and low temperature charge and discharge performance of the battery. At the same time, when lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide are used in the electrolyte, the film formation of the negative electrode can be better than that of the phosphoric anhydride additive, thereby reducing the increase in negative electrode impedance caused by the phosphoric anhydride additive, which is beneficial to the kinetic performance of the negative electrode and enhances the low temperature cycle and rate performance of the battery.

[0058] In the lithium salt combination, the mass percentage of lithium bis(fluorosulfonyl)imide in the electrolyte is preferably 2% to 6%, for example, 2%, 3%, 3.7%, 4%, 4.5%, 5%, 6% or any value within the above range. If the proportion of lithium bis(fluorosulfonyl)imide is too large, the viscosity of the electrolyte will increase significantly, and the corrosion of the positive electrode current collector aluminum foil will be enhanced; if the proportion of lithium bis(fluorosulfonyl)imide is too low, it will be completely consumed in the formation stage, and the conductivity level of the electrolyte cannot be improved.

[0059] Furthermore, the mass percentage ratio of additive A to lithium bis(fluorosulfonyl)imide in the electrolyte is 0.12-0.8, for example, 0.12, 0.15, 0.18, 0.2, 0.25, 0.3, 0.4, 0.5, 0.6, 0.6, 0.8 or any value within the above range, preferably 0.15-0.25.

[0060] The embodiment of the present application optimizes the total mass of lithium salt and the ratio of lithium bis(fluorosulfonyl)imide in the electrolyte, so that the battery has good rate performance.

[0061] In some embodiments, the electrolyte further comprises an organic solvent. The organic solvent may be selected from at least two of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl formate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, and ethyl difluoroacetate.

[0062] The mass percentage of the organic solvent in the electrolyte is 73% to 85.2%, for example, 73%, 75%, 77.5%, 80%, 82.5%, 85.2% or any value within the above range.

[0063] In some preferred embodiments, the organic solvent includes at least a combination of propylene carbonate and ethyl propionate. The solvent system is used as the base solvent or conventional solvent of the electrolyte of the embodiment of the present application, has a lower melting point and a higher dielectric constant, and can maintain a lower viscosity when used in a low temperature environment, so that the battery has good discharge performance in an extremely low temperature environment.

[0064] In the solvent system, the mass percentage of ethyl propionate in the electrolyte is 50% to 65%, for example, 50%, 55%, 58%, 60%, 65% or any value within the above range.

[0065] The electrolyte of the embodiment of the present application, through a low-viscosity solvent system and a lithium salt combination of lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate with high conductivity, when used in combination with additive A, can achieve rapid transmission of lithium ions in the solvent and improve the low-temperature discharge performance of the lithium-ion battery when used in a low-temperature environment.

[0066] In some embodiments, the electrolyte further includes an additive B, and the additive B includes at least one of a nitrile compound, a carbonate compound, and a sulfate compound. Additive B is a conventional additive for the electrolyte. When used in combination with additive A, additive B synergistically helps to form a stable and low-impedance passivation protective layer at the interface of the positive and negative electrodes, thereby improving the high-rate discharge and long cycle performance of the battery under low temperature, especially extremely low temperature conditions.

[0067] Specifically, the nitrile compound may be selected from at least one of adiponitrile, succinonitrile, 1,3,6-hexanetricarboxylonitrile, trans-hexenedinitrile, trans-butenedinitrile, 1,2-bis(cyanoethoxy)ethane and 1,2,3-tris(cyanoethoxy)propane.

[0068] Furthermore, the nitrile compound accounts for 2% to 4% of the total mass of the electrolyte, for example, it can be 2%, 3%, 4%, etc. or any value within the above range. If the amount of nitrile compound used is too high, it will deteriorate the impedance of the positive electrode of the battery and the low-temperature discharge performance of the battery; while if the amount of nitrile compound used is too low, the positive electrode protection effect is not obvious, and it is easy to cause the positive electrode metal to dissolve, which is not conducive to the low-temperature cycle performance of the battery in low-temperature scenarios.

[0069] The carbonate compound is at least one selected from vinylene carbonate, vinyl ethylene carbonate, methylene vinyl carbonate, fluoroethylene carbonate, trifluoromethylethylene carbonate and bisfluoroethylene carbonate; preferably fluoroethylene carbonate.

[0070] Furthermore, the carbonate compound such as fluoroethylene carbonate accounts for 4% to 6% of the total mass of the electrolyte, such as 4%, 5%, 6%, etc. or any value within the above range. Fluoroethylene carbonate can form a stable and low-impedance SEI film at the negative electrode, which can reduce the side reactions of nitrile compound additives, phosphoric anhydride additives and solvents at the negative electrode, thereby causing the deterioration of the negative electrode impedance.

[0071] The sulfate compound is at least one selected from vinyl sulfate, vinyl sulfite, 4-methylvinyl sulfate, dimethyl sulfite and diethyl sulfite; preferably vinyl sulfate.

[0072] Furthermore, the sulfate compound such as vinyl sulfate accounts for 0.5% to 1% of the total mass of the electrolyte, such as 0.5%, 0.8%, 1%, etc. or any value within the above range. Vinyl sulfate can form a stable and low-impedance SEI film at both the positive and negative electrodes, thereby reducing the side reactions of the solvent at the positive and negative electrodes and reducing the increase in the interface impedance between the positive and negative electrodes.

[0073] As one of the main materials of lithium-ion batteries, electrolyte is one of the important factors that affect the performance of lithium-ion secondary batteries. Among them, organic solvents, lithium salts, and additives are the main components of the electrolyte, which have a great influence on the battery's cycle, impedance, and dynamics. The embodiment of the present application optimizes the composition of the electrolyte, and comprehensively designs the parameters such as the composition of the organic solvent in the electrolyte, the composition of the lithium salt, and the composition of the additive, so that additives such as phosphoric anhydride, fluoroethylene carbonate, vinyl sulfate, and nitrile compounds cooperate to reduce the polarization and impedance of the electrode, reduce the side reactions of the electrolyte on the electrode surface, and also enable lithium ions to maintain good transmission performance in extremely low temperature environments, realize high-power discharge of lithium-ion batteries in extremely low temperature environments, and enable lithium-ion batteries to have good low-temperature long cycle performance.

[0074] In some embodiments, the positive electrode current collector mentioned in the present application is not particularly limited, and it can be any material known to be suitable for use as a positive electrode current collector. In one embodiment, the positive electrode current collector can be a metal material such as aluminum, stainless steel, nickel plating, titanium, tantalum, and a carbon material such as carbon cloth and carbon paper.

[0075] In some embodiments, the positive electrode material layer is formed by coating a positive electrode slurry on the surface of a positive electrode current collector, wherein the positive electrode slurry includes a positive electrode active material, a conductive agent, and a binder in addition to a lithium aluminum titanium phosphate solid electrolyte.

[0076] Positive electrode active materials include but are not limited to lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, ternary LiNi x Co y Mn z One or more of O2 materials (where x+y+z=1, x≥y).

[0077] The conductive agent includes, but is not limited to, at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0078] The binder includes but is not limited to at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin.

[0079] The positive electrode sheet described in the embodiment of the present application is prepared by the following method:

[0080] The positive electrode active material, the aluminum titanium lithium phosphate solid electrolyte, the conductive agent and the binder are mixed according to the mass ratio to form a uniform positive electrode slurry;

[0081] The positive electrode slurry is evenly coated on the surface of the positive electrode collector, and then the positive electrode sheet is obtained through processes such as drying, rolling and compacting.

[0082] The embodiments of the present application achieve high-rate discharge and long cycle of the battery cell in an extremely low temperature environment by optimizing the composition of the electrolyte and the composition of the positive electrode material. For the electrolyte, the combined use of additives such as phosphoric anhydride compounds, fluoroethylene carbonate, nitrile compounds and vinyl sulfate in the electrolyte, and the addition of aluminum titanium phosphate lithium solid electrolyte to the positive electrode material can synergistically improve the problems of decreased electrolyte ion conductivity and severe electrode polarization when the battery is used in low temperature, especially in an extremely low temperature environment, so that the battery has low-temperature long cycle performance and high-power discharge performance when used in low temperature scenarios.

[0083] In some embodiments, the negative electrode plate includes a negative electrode current collector and a negative electrode material layer coated on the surface of the negative electrode current collector. The negative electrode current collector can be selected from a metal foil or a composite current collector, for example, can be selected from a copper foil.

[0084] In some embodiments, the negative electrode material layer includes a negative electrode active material, a binder, and a conductive agent.

[0085] The negative electrode active material includes, but is not limited to, one or more of graphite, hard carbon, silicon, silicon oxide compounds and silicon carbon compounds.

[0086] The conductive agent includes, but is not limited to, one or more of conductive carbon black, acetylene black, Ketjen black, carbon dots, carbon nanotubes, graphene, carbon nanofibers, and superconducting carbon.

[0087] The binder includes, but is not limited to, one or more of styrene-butadiene rubber, water-based acrylic resin, polyvinylidene fluoride, polytetrafluoroethylene, ethylene-vinyl acetate copolymer, polyacrylic acid, carboxymethyl cellulose, polyvinyl alcohol and polyvinyl butyral.

[0088] In some embodiments, the diaphragm described in the present application can be arbitrarily selected from known porous structure diaphragms with good chemical stability and mechanical stability. The material of the diaphragm can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The diaphragm can be a single-layer film or a multi-layer composite film, without particular limitation. When the diaphragm is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0089] The preparation process of the battery is well known to those skilled in the art and is not particularly limited in this application. For example, the electrochemical device can be manufactured by the following process: the positive electrode sheet and the negative electrode sheet are overlapped via a diaphragm, and after winding, folding, etc. as required, they are placed in a housing, and the electrolyte is injected into the housing and sealed, wherein the diaphragm used is the diaphragm provided in this application. In addition, overcurrent protection elements, guide plates, etc. can also be placed in the housing as required to prevent pressure rise and overcharge and discharge inside the electrochemical device.

[0090] The present application also provides an electrical device or various energy storage systems using batteries as energy storage elements. Electrical devices include but are not limited to mobile phones, tablets, computers, electric toys, electric tools, battery cars, electric cars, ships, spacecraft, etc.

[0091] In order to make the present invention easier to understand, the present invention will be further described in detail below in conjunction with examples, which are merely illustrative and are not intended to limit the scope of application of the present invention. The raw materials or components used in the present invention can be obtained by commercial routes or conventional methods unless otherwise specified.

[0092] Example 1

[0093] (1) Preparation of electrolyte

[0094] In a glove box in an argon environment with a water content of <1 ppm, propylene carbonate (PC) and ethyl propionate (EP) were mixed in a mass ratio of 25:75, and based on the total mass of the electrolyte, the following components in percentages of the total mass of the electrolyte as shown in Table 1 were added and mixed evenly to prepare an electrolyte.

[0095] Lithium salt: 13% lithium hexafluorophosphate (LiPF6) + 2% lithium bis(fluorosulfonyl)imide (LiFSI)

[0096] Additive A Phosphoric anhydride compound: 0.3% n-propyl phosphoric anhydride (T3P)

[0097] Additive B: 2% succinonitrile (SN) + 6% fluoroethylene carbonate (FEC) + 0.8% diethylene sulfate (DTD)

[0098] (2) Preparation of positive electrode sheet

[0099] The positive electrode active material lithium cobalt oxide (LiCoO2), lithium aluminum titanium phosphate solid electrolyte (particle size D50 is 0.5 μm), conductive agent carbon black, binder polyvinylidene fluoride PVDF, and carbon nanotubes CNT are fully stirred and mixed in N-methylpyrrolidone solvent at a mass ratio of 97.5:0.5:0.6:1:0.4 to form a uniform positive electrode slurry;

[0100] The positive electrode slurry is evenly coated on the positive electrode current collector Al foil, and then dried, rolled and compacted (the compaction density is 4.28g / cm 3 ) and other processes to obtain the positive electrode sheet.

[0101] (3) Preparation of negative electrode sheet

[0102] The negative electrode active material graphite, the binder styrene-butadiene rubber, and the thickener sodium carboxymethyl cellulose are mixed in a proper amount of deionized water solvent in a mass ratio of 98.2:1:0.8 to form a uniform negative electrode slurry;

[0103] The negative electrode slurry is evenly coated on the negative electrode current collector copper foil, and then dried, rolled and compacted (the compaction density is 1.78 g / cm 3 ) and other processes to obtain the negative electrode sheet.

[0104] (4) Preparation of lithium-ion batteries

[0105] PE porous polymer film is used as the isolation membrane.

[0106] The positive electrode sheet, separator and negative electrode sheet are stacked in order, so that the separator is in the middle of the positive and negative electrodes to play a role of isolation, and then the stacked electrode sheet and separator are wound to obtain a roll core. The bare roll core is placed in the aluminum-plastic film that has been punched and formed, and the electrolyte prepared above is injected into the baked and dried battery cell at an injection coefficient of 1.5g / Ah. After vacuum packaging, standing, formation and other processes, the preparation of the lithium-ion battery is completed.

[0107] Examples 2-19 and Comparative Examples 1-4 use the same method as Example 1, the differences being the type and content of additive A in the electrolyte, the amount and particle size of LATP in the positive electrode sheet, and the injection coefficient of the electrolyte, as shown in Table 1.

[0108] Lithium-ion battery performance test:

[0109] (1) -29℃ rate discharge performance test:

[0110] At room temperature, charge to 4.48V at 0.5C constant current and constant voltage, with a cut-off current of 0.05C, and stand for 10 minutes; discharge to 3V at 0.2C constant current, record the discharge capacity as C1, and stand for 10 minutes. Charge to 80% C1 capacity at 0.5C constant current and constant voltage, with a cut-off current of 0.05C. After standing at -29℃ for 3 hours, discharge at 10.67W for 5s, 14.35W for 1s, 20.49W for 5ms, 11.23W for 3s, 13.20W for 2s, 7.3W for 10s, and 4.21W for 60s. If the discharge process voltage is not less than 3V, it is recorded as "passed" test, otherwise it is recorded as "failed" test. The test results are recorded in Table 1.

[0111] (2) -10℃ cycle performance test:

[0112] At 25℃, discharge at a given current of 0.2C to 3.0V; leave for 5min; charge at a constant current and constant voltage of 0.5C to the upper limit voltage, with a cutoff current of 0.05C; after leaving for 10min, discharge at 0.2C to 3.0V, and record the initial discharge capacity.

[0113] At -10℃, charge the divided battery to 4.48V at 0.5C constant current and constant voltage, with a cut-off current of 0.05C; then discharge it to 3.0V at 0.5C constant current, and repeat this cycle. After 500 cycles of charge and discharge, calculate the battery capacity retention rate after 500 cycles. The calculation formula is as follows:

[0114] 500th cycle capacity retention rate (%) = (500th cycle discharge capacity / initial cycle discharge capacity) × 100%.

[0115] There are 5 batteries in each group, and the average capacity retention rate is recorded in Table 1.

[0116] Table 1

[0117]

[0118] Note: T3P represents n-propyl phosphoric anhydride, T4P represents n-butyl phosphoric anhydride, and T2FP represents pentafluoroethyl phosphoric anhydride.

[0119] The data comparison of Comparative Examples 1-3 shows that when a phosphoric anhydride compound is added to the electrolyte as additive A but the positive electrode plate does not contain LATP, it not only fails to improve the low-temperature rate discharge performance of the battery, but also deteriorates the low-temperature long cycle performance of the battery as the content of the phosphoric anhydride compound in the electrolyte increases.

[0120] The data comparison of Comparative Example 1, Comparative Example 4 and Example 1 shows that when LATP is added to the positive electrode plate, but the phosphoric anhydride compound is not added to the electrolyte as the additive A, the low-temperature rate discharge performance of the battery cannot be improved. When the phosphoric anhydride compound described in the present application is used as the additive A in the electrolyte, and the aluminum titanium phosphate lithium solid electrolyte LATP is added to the positive electrode plate, LATP can catalyze the phosphoric anhydride compound to form a film at the positive electrode, thereby improving the migration rate of lithium ions under low temperature conditions, and reducing the increase in interface impedance during the cycle process, and synergistically improving the low-temperature rate discharge performance and low-temperature long cycle performance of the battery.

[0121] The data comparison of Examples 1-4 shows that the content of phosphoric anhydride compound additive A in the electrolyte is between 0.3% and 1.2%, and meets The battery has good low-temperature rate discharge performance and low-temperature long cycle performance; further, with the increase of the content of the phosphoric anhydride compound additive in the electrolyte, the low-temperature cycle capacity retention rate of the battery will also deteriorate, and the battery performance improvement effect is better when the content of the phosphoric anhydride compound additive in the electrolyte is ≤1.2%.

[0122] Further in combination with Examples 16-17, when the content of phosphoric anhydride compounds in the electrolyte further increases and the formula value exceeds the range value, the negative electrode impedance will be seriously deteriorated, thereby simultaneously deteriorating the low-temperature rate discharge performance and low-temperature long cycle performance of the battery.

[0123] The data of Example 1 and Example 5 show that the content of the positive electrode material LATP is between 0.5% and 1%, and meets When the battery has good low-temperature rate discharge performance and low-temperature long cycle performance; further increase in the LATP content in the positive electrode sheet will lead to a corresponding decrease in the content of positive electrode active material in the positive electrode slurry, which will be not conducive to the battery maintaining a good energy density, and may even fail to meet the battery's energy density requirements.

[0124] The data of Examples 1, 6-7, and 11-15 show that the electrolyte injection coefficient in the electrolyte is between 1.5 and 1.8 g / Ah and meets When the value is lower than the range, such as in Example 6, and the formula value is lower than the range, the battery has good low-temperature rate discharge performance and low-temperature long cycle performance.

[0125] The data of Examples 1 and 8-10 show that the particle size of the positive electrode material LATP satisfies D50 of 0.2-0.5 μm and satisfies When the particle size is higher than the range value, such as in Example 10, and the formula value is lower than the range value, the battery has good low-temperature rate discharge performance and low-temperature long cycle performance.

[0126] The data from Example 18 and Example 19 show that the combination of phosphoric anhydride of the structural formula described in the present application and LATP in the positive electrode plate has the same effect on improving the low-temperature rate discharge or low-temperature long cycle performance of the battery.

[0127] Furthermore, an electrolyte, a positive electrode sheet, a negative electrode sheet and a lithium-ion battery were prepared in the same manner as in Example 15, except for the types and contents of the solvent, lithium salt and additive B in the electrolyte, as shown in Table 2.

[0128] Table 2

[0129]

[0130] Note: LiBF4 represents lithium tetrafluoroborate, and DEC represents diethyl carbonate.

[0131] The data of Example 15 and Examples 20-21 show that the combination of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide in the electrolyte has a better effect on improving the low-temperature performance of the battery.

[0132] The data from Example 15 and Examples 22-23 show that the electrolyte solvent is a combination of propylene carbonate and ethyl propionate, and the mass percentage of ethyl propionate is in the range of 50% to 65%, which has a better effect on improving the low-temperature performance of the battery.

[0133] The data from Example 15 and Examples 24-25 show that, on the basis of the electrolyte containing the phosphoric anhydride compound as additive A, adding nitrile compounds, carbonate compounds and sulfate compounds as additives B as basic additives, and utilizing the synergistic effect between the components, is beneficial to forming an interface film with high stability and good density on the positive and negative pole pieces, thereby protecting the positive and negative pole pieces and having a better effect on improving the low temperature performance of the battery.

[0134] It should be noted that the embodiments described above are only used to explain the present application and do not constitute any limitation to the present application. The present application is described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present application may be modified as specified within the scope of the claims of the present application, and the present application may be revised without departing from the scope and spirit of the present application. Although the present application described therein relates to specific methods, materials and embodiments, it does not mean that the present application is limited to the specific examples disclosed therein. On the contrary, the present application can be extended to all other methods and applications with the same functions.

Claims

1. A lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, characterized in that: The positive electrode plate comprises a positive electrode current collector and a positive electrode material layer coated on the surface of the positive electrode current collector, wherein the positive electrode material layer comprises lithium aluminum titanium phosphate; The electrolyte includes an additive A, and the chemical structural formula of the additive A is shown in Formula I: ; wherein R1, R2, and R3 are each independently selected from a hydrocarbon group having no more than 4 carbon atoms, substituted or unsubstituted with fluorine; The positive electrode sheet and the electrolyte meet the following requirements: ; Wherein, c (%) represents the mass percentage of the additive A in the electrolyte, 0.3≤c≤1.2; L (%) represents the mass percentage of lithium aluminum titanium phosphate in the positive electrode material layer, 0.5≤L≤1.0; f (g / Ah) represents the injection coefficient of the electrolyte in the lithium-ion battery, 1.5≤f≤1.8; D (μm) represents the D50 particle size of lithium aluminum titanium phosphate in the positive electrode material layer, and 0.2≤D≤0.

5.

2. The lithium-ion battery according to claim 1, characterized in that The additive A is selected from at least one of the following compounds: n-methyl phosphoric anhydride, n-ethyl phosphoric anhydride, n-propyl phosphoric anhydride, n-butyl phosphoric anhydride, and pentafluoroethyl phosphoric anhydride.

3. The lithium ion battery according to claim 1 or 2, characterized in that: The electrolyte further comprises a lithium salt, wherein the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium bis(fluorooxalatoborate), lithium bis(oxalatoborate), lithium bis(fluorosulfonylimide), lithium bis(trifluoromethylimide), lithium difluorooxalatophosphate, and lithium perchlorate; The mass percentage of lithium salt in the electrolyte is 8% to 15%.

4. The lithium-ion battery according to claim 3, characterized in that: The lithium salt comprises lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, wherein the mass percentage of lithium bis(fluorosulfonyl)imide in the electrolyte is 2% to 6%.

5. The lithium ion battery according to claim 1 or 2, characterized in that: The electrolyte further comprises an organic solvent, wherein the organic solvent is selected from at least two of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl formate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, and ethyl difluoroacetate; The mass percentage of the organic solvent in the electrolyte is 73% to 85.2%.

6. The lithium-ion battery according to claim 5, characterized in that: The organic solvent comprises at least propylene carbonate and ethyl propionate, wherein the mass percentage of ethyl propionate in the electrolyte is 50% to 65%.

7. The lithium-ion battery according to claim 1, characterized in that: The electrolyte further includes an additive B, and the additive B includes at least one of a nitrile compound, a carbonate compound, and a sulfate compound.

8. The lithium-ion battery according to claim 7, characterized in that: The nitrile compound is selected from at least one of adiponitrile, succinonitrile, 1,3,6-hexanetricarbonitrile, trans-hexenedinitrile, trans-butenedinitrile, 1,2-bis(cyanoethoxy)ethane and 1,2,3-tris(cyanoethoxy)propane; the mass percentage of the nitrile compound in the electrolyte is 2% to 4%; And / or, the carbonate compound is selected from at least one of vinylene carbonate, vinyl ethylene carbonate, methylene carbonate, fluoroethylene carbonate, trifluoromethylethylene carbonate and bisfluoroethylene carbonate; the mass percentage of the carbonate compound in the electrolyte is 4% to 6%; And / or, the sulfate ester compound is selected from at least one of vinyl sulfate, vinyl sulfite, 4-methyl vinyl sulfate, dimethyl sulfite and diethyl sulfite; and the mass percentage of the sulfate ester compound in the electrolyte is 0.5% to 1%.