SiO2 doped Fe-N-C difunctional oxygen electrode and preparation method and application thereof

By doping Fe-N-C oxygen electrode with SiO2, a rich mesoporous structure and solid-liquid-gas three-phase reaction interface are formed, which solves the problem of low active site density of the Fe-N-C catalyst layer and improves the electrocatalytic activity of the oxygen electrode and mass transport capacity, high power density and excellent charging and discharging performance are achieved, and non-precious metal catalysts are promoted in the field of fuel cells.

CN119069725APending Publication Date: 2024-12-03DONGHUA UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411052765.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing Fe-N-C catalyst layer has low active site density, resulting in mass transfer hindered at high current density, and high-temperature pyrolysis and surface fluorination processes will reduce the oxygen catalytic activity of the catalyst, making it difficult to achieve efficient application in fuel cells.

Method used

SiO2-doped Fe-N-C bifunctional oxygen electrode is used to form a rich mesoporous structure and solid-liquid-gas three-phase reaction interface through SiO2 as a carbon support pore-forming agent and surface hydrophobic layer regulator to improve the active position of the catalyst. Point density and mass transport capacity.

Benefits of technology

The electrocatalytic activity of the oxygen electrode is significantly improved, the cathode mass transmission is improved, the oxygen catalytic activity of the catalyst is maintained, the high power density and excellent charging and discharge performance are achieved, and the large-scale application of non-precious metal catalysts in the fuel cell field is promoted.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069725A_ABST
    Figure CN119069725A_ABST
Patent Text Reader

Abstract

The invention relates to a SiO2 doped Fe-N-C bifunctional oxygen electrode and a preparation method and application thereof, the bifunctional oxygen electrode takes doped mesoporous carbon as a carbon carrier, SiO2 is used as a pore forming agent and a surface hydrophobic layer regulator of the carbon carrier, and Fe is anchored on the carbon carrier in a monatomic form as an active site of oxygen reaction. The surface of the bifunctional oxygen electrode has abundant layered pore structures, and the unique microstructure not only provides abundant active sites, but also can effectively improve cathode mass transmission and promote formation of abundant solid-liquid-gas three-phase reaction interfaces, so that the electro-catalytic activity of the oxygen electrode is remarkably improved, and the oxygen electrode has a good application prospect. And the assembled zinc-air battery and proton exchange membrane fuel cell have excellent power generation power density and zinc-air battery charge-discharge performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrocatalysis, and particularly relates to a SiO2-doped Fe-NC bifunctional oxygen electrode and a preparation method and application thereof. Background Art

[0002] Fuel cells (including proton exchange membrane fuel cells and zinc-air batteries) are recognized as one of the most promising technologies for future electric vehicles due to their high efficiency and "zero" greenhouse gas emissions. However, the large-scale application and promotion of fuel cell technology are seriously hindered by the extremely slow kinetics of oxygen reduction reaction (ORR), the high cost of Pt catalysts (especially at the cathode), and the easy poisoning. Therefore, it is urgent to develop efficient and low-cost non-platinum group metal (non-PGM) or even non-precious metal oxygen catalysts.

[0003] Among various non-PGM and non-precious metal catalysts, pyrolytic Fe-NC is one of the most promising candidate catalysts. Significant progress has also been made in the synthesis of highly active Fe-NC catalysts. Despite this, due to the low active site density of Fe-NC catalysts, the mass activity of Fe-NC catalysts is still 4-8 times lower than that of commercial Pt / C catalysts (J.Am.Chem.Soc.136(2014)978-985; Angew.Chem.Int.Ed.Engl.127(2015)10045-10048). For example, under the operating conditions of proton exchange membrane fuel cells (PEMFCs), in order to achieve the same high voltage as Pt / C cathode (0.4 mg / cm2) in the kinetic control region (high operating voltage region), the Fe-NC catalyst has a low mass activity, which is 4-8 times lower than that of commercial Pt / C catalysts. Pt cm -2 , 45.4% Pt / C) with a current density comparable to that of Fe-NC catalyst (3-4 mg Fe-N-C cm -2) usually requires 3 to 6 times the load (Appl. Catal. B: Environ 234 (2018) 357–364; Appl. Catal. B: Environ 264 (2020) 118523). Therefore, the thickness of the Fe-NC catalyst layer is almost 10 times higher than that of the Pt / C catalyst layer (e.g. 100μm vs. 10μm) (Energy Environ. Sci. 11 (2018) 365-382; J. Power Sources 344 (2017) 39-45; J. Electrochem. Soc. 160 (2013) F824–F833), which will inevitably lead to severe mass transfer obstruction (loss) at high current density. Therefore, how to improve the mass transport of the Fe-NC high-load catalyst layer to achieve the ideal state is a huge challenge currently faced. In order to improve the mass transport in the Fe-NC catalyst layer, there are currently two main strategies: one is to enrich the pore structure of the Fe-NC catalyst by introducing more mesopores as effective mass transfer channels; the other strategy is to adjust the hydrophilicity and hydrophobicity of the Fe-NC catalyst layer to achieve better water management. However, both high-temperature pyrolysis and surface fluorination processes will reduce the intrinsic oxygen catalytic activity of the catalyst. Therefore, combining the two to obtain a dual-body improvement of adjusting the pore structure and surface wettability can not only effectively improve the mass transfer problem of the Fe-NC thick catalyst layer, but also maintain its inherent oxygen catalytic activity improvement, which is of great significance for promoting the early large-scale application of non-precious metal catalysts in the field of fuel cell technology. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a SiO2-doped Fe-NC bifunctional oxygen electrode and its preparation method and application, which solves the technical problems of the quality activity of the high-loaded Fe-NC catalyst layer in the prior art and enriching the oxygen reaction gas-solid-liquid three-phase reaction interface.

[0005] The present invention provides a SiO2-doped Fe-NC bifunctional oxygen electrode, wherein the bifunctional oxygen electrode uses doped mesoporous carbon as a carbon carrier, SiO2 as a pore former and a surface hydrophobic layer regulator of the carbon carrier, and Fe is anchored on the carbon carrier in the form of a single atom as an active site for oxygen reaction.

[0006] The present invention provides a method for preparing a SiO2-doped Fe-NC bifunctional oxygen electrode, comprising the following steps:

[0007] (1) Fe(SO4)2·7H2O, polyquaternium-7, and SiO2 are successively added to a HCl solution, stirred and dissolved, and placed in an oven to dry overnight to obtain a dry product;

[0008] (2) The dried product is calcined in a N2 atmosphere to obtain a carbide; the carbide is then alkali washed and acid washed, and the obtained product is calcined again in a N2 atmosphere to obtain a SiO2-doped Fe-NC bifunctional oxygen electrode, denoted as SiO2 / Fe-NC.

[0009] Preferably, the mass volume ratio of Fe(SO4)2·7H2O, polyquaternium-7, SiO2 and HCl solution in step (1) is 10-20g:25-90g:10-30g:40-180mL.

[0010] Preferably, the oven temperature in step (1) is 80-90°C.

[0011] Preferably, the calcination conditions in step (2) are: 800-1100° C., time 1-4 h, and heating rate 5-20° C. / min.

[0012] Preferably, the alkali washing conditions in step (2) are: using NaOH solution, alkali washing at room temperature or heated alkali washing, for 1 to 6 days; alkali washing may also be omitted.

[0013] Preferably, the pickling conditions in step (2) are: using H2SO4 solution, pickling at room temperature or heated pickling, for 1 to 10 hours.

[0014] Preferably, the secondary calcination conditions in step (2) are: 800-1100° C., time 1-4 h, and heating rate 5-20° C. / min.

[0015] The present invention also provides an application of a SiO2-doped Fe-NC bifunctional oxygen electrode in a H2-air fuel cell and a zinc-air battery.

[0016] The present invention first prepares a SiO2-doped carbon precursor through a primary carbonization process, then removes SiO2 through an alkaline washing process to obtain a mesoporous structure, and retains an appropriate amount of SiO2 as a hydrophobic layer; at the same time, excess metallic Fe is removed through an acid washing process, and then a mesoporous carbon-anchored Fe single atom (SiO2 / Fe-NC) is generated through a secondary carbonization process.

[0017] Beneficial Effects

[0018] (1) The surface of the bifunctional oxygen electrode of the present invention has a rich layered pore structure. The unique microstructure not only provides abundant active sites, but also effectively improves the cathode mass transfer and promotes the formation of a rich solid-liquid-gas three-phase reaction interface, thereby significantly improving the electrocatalytic activity of the oxygen electrode.

[0019] (2) The present invention uses SiO2 as a template to manufacture the mesoporous carbon structure. The presence of an appropriate amount of SiO2 on the surface of the mesoporous carbon carrier improves the mass transport in the Fe-NC catalyst layer and forms a rich solid-liquid-gas three-phase reaction interface.

[0020] (3) The presence of more pyridinic nitrogen and SiO2-introduced defects in the SiO2 / Fe-NC catalyst of the present invention will produce more catalytic active sites, thereby compensating for the decrease in catalytic oxygen mass activity caused by the incorporation of inactive SiO2.

[0021] (4) The zinc-air battery and proton exchange membrane fuel cell assembled with the bifunctional oxygen electrode of the present invention have excellent power density and zinc-air battery charge and discharge performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 SEM images of SiO2-doped Fe-NC bifunctional oxygen electrodes prepared in Examples 1-4; wherein (a), (b), (c), and (d) correspond to Example 2, Example 3, Example 1, and Example 4, respectively;

[0023] Figure 2 This is an aberration-corrected STEM image of the SiO2-doped Fe-NC bifunctional oxygen electrode prepared in Example 1;

[0024] Figure 3 This is the N2 adsorption analysis isotherm diagram of the SiO2-doped Fe-NC bifunctional oxygen electrode prepared in Example 1;

[0025] Figure 4 XRD pattern of SiO2-doped Fe-NC bifunctional oxygen electrode prepared in Example 1;

[0026] Figure 5 Power density diagrams of the zinc-air battery (a) and the proton exchange membrane fuel cell (b) assembled with the SiO2-doped Fe-NC bifunctional oxygen electrode prepared in Example 1;

[0027] Figure 6 The zinc-air battery assembled with the SiO2-doped Fe-NC bifunctional oxygen electrode prepared in Example 1 and Pt / C-RuO2 was tested at 10 mA / cm 2 Comparison of charge and discharge performance under constant current;

[0028] Figure 7 It is a schematic structural diagram of the SiO2 doped Fe-NC bifunctional oxygen electrode of the present invention. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0030] The microstructure of the product of the embodiment of the present invention was tested by TEM (JEOL JEM-2100F system), AC-HAADF-STEM (JEOL JEM-ARM 200F TEM) and SEM (Hitachi S-4800). The half-cell performance test was carried out on a Chenhua CHI760D electrochemical workstation using a three-electrode system. The zinc-air battery test was carried out on a CT2001A blue battery test system; the H2-air fuel cell test was carried out on a Module 850e (Scribner Associates Inc.) test system.

[0031] Example 1

[0032] This embodiment provides a method for preparing a SiO2(4) / Fe-NC bifunctional oxygen catalyst / electrode, and the specific preparation steps are as follows:

[0033] Step 1: Add 12 g Fe(SO4)2·H2O to 40 mL 1 M HCl and stir well to ensure complete dissolution;

[0034] Step 2): Add 90 g of polyquaternium-7 to 168 mL of 1 M HCl and stir evenly to ensure complete dissolution;

[0035] Step 3): Add 20 g SiO2 (100 nm) to 100 mL 1 M HCl and stir well to ensure complete dissolution;

[0036] Step 4): Add the solution of step 1) and step 2) into step 3) and mix well;

[0037] Step 5): Pour the uniform solution obtained in step 4) into a beaker and place it in an oven at 85°C to dry overnight until it is dry;

[0038] Step 6): Grind the dried product obtained in step 5) into powder, and heat it to 900° C. at a heating rate of 20° C. / min under N2 atmosphere and calcine it for 1 h;

[0039] Step 7): the carbide obtained in step 6) is washed with alkali in 8M NaOH solution at room temperature for 4 days with stirring, and then filtered until it becomes neutral to collect the carbide;

[0040] Step 8): The carbide obtained in step 7) is heated and acid-washed in a 1M H2SO4 solution at 85°C for 8 hours, and then filtered until it becomes neutral to collect the carbide;

[0041] Step 9): The carbide obtained in step 8) is heated to 900°C in a N2 atmosphere at a heating rate of 20°C / min and calcined for 1 h to obtain the final SiO2(4) / Fe-NC bifunctional oxygen catalyst, the morphology of which is as follows: Figure 1 (c) as shown.

[0042] Figure 1 (c) shows that under the conditions of Example 1, the SiO2(4) / Fe-NC catalyst obtained exhibits a rich pore structure and a rich layered structure on the surface, which not only exposes a large number of oxygen reaction active sites, but also facilitates the formation of a rich solid-liquid-gas three-phase reaction interface. The N2 adsorption analysis isotherm test shows a type IV isotherm, indicating that the mesoporous structure of the carbon carrier mainly exists in the form of mesopores ( Figure 2 ). Bright spots in aberration-corrected STEM indicate that Fe exists in single-atom form and serves as an active site for oxygen reaction ( Figure 3 ).

[0043] Example 2

[0044] This embodiment provides a method for preparing a SiO2(0) / Fe-NC bifunctional oxygen catalyst / electrode, and the specific preparation steps are as follows:

[0045] Step 1: Add 12 g Fe(SO4)2·H2O to 40 mL 1 M HCl and stir well to ensure complete dissolution;

[0046] Step 2): Add 90 g of polyquaternium-7 to 168 mL of 1 M HCl and stir well to ensure complete dissolution;

[0047] Step 3): Add 20 g SiO2 (100 nm) to 100 mL 1 M HCl and stir well to ensure complete dissolution;

[0048] Step 4): Add the solution of step 1) and step 2) into step 3) and mix well;

[0049] Step 5): Pour the uniform solution obtained in step 4) into a beaker and place it in an oven at 85°C to dry overnight until it is dry;

[0050] Step 6): Grind the dried product obtained in step 5) into powder, and heat it to 900° C. at a heating rate of 20° C. / min under N2 atmosphere and calcine it for 1 h;

[0051] Step 7): The carbide obtained in step 6) is heated and acid-washed in a 1M H2SO4 solution at 85°C for 8 hours, and then filtered until it becomes neutral to collect the carbide;

[0052] Step 8): The carbide obtained in step 7) is heated to 900°C in a N2 atmosphere at a heating rate of 20°C / min and calcined for 1 h to obtain the final SiO2(0) / Fe-NC bifunctional oxygen catalyst, the morphology of which is as follows: Figure 1 (a) shown.

[0053] Example 3

[0054] This embodiment provides a method for preparing a SiO2(2) / Fe-NC bifunctional oxygen catalyst / electrode, and the specific preparation steps are as follows:

[0055] Step 1: Add 12 g Fe(SO4)2·H2O to 40 mL 1 M HCl and stir well to ensure complete dissolution;

[0056] Step 2): Add 90 g of polyquaternium-7 to 168 mL of 1 M HCl and stir well to ensure complete dissolution;

[0057] Step 3): Add 20 g SiO2 (100 nm) to 100 mL 1 M HCl and stir well to ensure complete dissolution;

[0058] Step 4): Add the solution of step 1) and step 2) into step 3) and mix well;

[0059] Step 5): Pour the uniform solution obtained in step 4) into a beaker and place it in an oven at 85°C to dry overnight until it is dry;

[0060] Step 6): Grind the dried product obtained in step 5) into powder, and heat it to 900° C. at a heating rate of 20° C. / min under N2 atmosphere and calcine it for 1 h;

[0061] Step 7): the carbide obtained in step 6) is washed with alkali in 8M NaOH solution at room temperature for 2 days with stirring, and then filtered until it becomes neutral to collect the carbide;

[0062] Step 8): The carbide obtained in step 7) is heated and acid-washed in a 1M H2SO4 solution at 85°C for 8 hours, and then filtered until it becomes neutral to collect the carbide;

[0063] Step 9): The carbide obtained in step 8) is heated to 900°C at a heating rate of 20°C / min in a N2 atmosphere and calcined for 1 h to obtain the final SiO2(2) / Fe-NC bifunctional oxygen catalyst, the morphology of which is as follows: Figure 1 (b) as shown.

[0064] Example 4

[0065] This embodiment provides a method for preparing a SiO2(6) / Fe-NC bifunctional oxygen catalyst / electrode, and the specific preparation steps are as follows:

[0066] Step 1: Add 12 g Fe(SO4)2·H2O to 40 mL 1 M HCl and stir well to ensure complete dissolution;

[0067] Step 2): Add 90 g of polyquaternium-7 to 168 mL of 1 M HCl and stir evenly to ensure complete dissolution;

[0068] Step 3): Add 20 g SiO2 (100 nm) to 100 mL 1 M HCl and stir well to ensure complete dissolution;

[0069] Step 4): Add the solution of step 1) and step 2) into step 3) and mix well;

[0070] Step 5): Pour the uniform solution obtained in step 4) into a beaker and place it in an oven at 85°C to dry overnight until it is dry;

[0071] Step 6): Grind the dried product obtained in step 5) into powder, and heat it to 900° C. at a heating rate of 20° C. / min under N2 atmosphere and calcine it for 1 h;

[0072] Step 7): the carbide obtained in step 6) is washed with alkali in 8M NaOH solution at room temperature for 6 days with stirring, and then filtered until it becomes neutral to collect the carbide;

[0073] Step 8): The carbide obtained in step 7) is heated and acid-washed in a 1M H2SO4 solution at 85°C for 8 hours, and then filtered until it becomes neutral to collect the carbide;

[0074] Step 9): The carbide obtained in step 8) is heated to 900°C at a heating rate of 20°C / min in a N2 atmosphere and calcined for 1 h to obtain the final SiO2(6) / Fe-NC bifunctional oxygen catalyst, the microstructure of which is as follows: Figure 1 (d) as shown.

[0075] Comparative Examples 1-4 prepared SiO2 / Fe-NC bifunctional oxygen catalyst microstructure ( Figure 1 (ad)) It can be seen that the microstructures of the bifunctional oxygen catalysts prepared under different alkali washing times are similar. Under the condition of alkali washing for 4 days in Example 1, a layered mesoporous structure can be obtained. The unique structure not only allows the catalyst to expose a large number of oxygen reaction active sites, but also facilitates the OH in the oxygen catalytic reaction. -In addition, no SiO2 and Fe metal particles were observed in the SEM images, but the XRD images showed that SiO2 nanoparticles ( Figure 4 ), and the presence of an appropriate amount of SiO2 on the mesoporous carbon layer can adjust the hydrophilicity and hydrophobicity of the catalyst layer and enrich the solid-liquid-gas three-phase reaction interface.

[0076] Example 5

[0077] 30 mg of the bifunctional oxygen catalyst prepared in Example 1 and Pt / C-RuO2 powder were dissolved in 10 mL of ethanol, 110 μL of 5 wt% Nafion solution was added, and ultrasonicated for 50 minutes to form a uniform catalyst slurry. Then, 5 mL of the slurry was sprayed on a hydrophobic treated carbon paper (loading 15 mg / cm 2 ), and dried on a heating table at 85°C for 40 minutes to obtain an air electrode. Finally, zinc foil was used as the negative electrode, carbon paper sprayed with catalyst slurry was used as the air electrode, and 6M KOH solution was used as the electrolyte to assemble a homemade zinc-air battery, which was tested using a blue power system. The test of hydrogen-air proton exchange membrane fuel cell was carried out at Module850e, Scribner Associates Inc. The test conditions were: membrane electrode (MEA) effective area 5cm 2 , catalyst double-sided loading 4mg / cm 2 , test temperature 80°C, 100% RH, 200 sccm fuel (H2) and oxidant (air) at normal pressure.

[0078] The test results are as follows Figure 5 (a) shows that Example 1 is a comparison of the power generation of the prepared SiO2(4) / Fe-NC bifunctional oxygen electrode and the commercial Pt / C-RuO2 catalyst in a zinc-air battery. It can be seen that when SiO2(4) / Fe-NC is used as the air electrode, 444.1 mW / cm 2 The peak power density is significantly better than that of commercial Pt / C+RuO2 catalyst (176.3mW / cm 2 ) performance, and the voltage has good stability during the test process. At the same time, it is applied to the hydrogen-air proton exchange membrane fuel cell test system. SiO2(4) / Fe-NC can be used as an air electrode to obtain up to 477.93mW cm-2 without backing. -2 Power density( Figure 5 (b)).

[0079] Example 6

[0080] 30 mg of the bifunctional oxygen catalyst prepared in Example 1 and Pt / C-RuO2 powder were dissolved in 10 mL of ethanol, 110 μL of 5 wt% Nafion solution was added, and ultrasonicated for 50 minutes to form a uniform catalyst slurry. Then, 5 mL of the slurry was sprayed on a hydrophobic treated carbon paper (loading 15 mg / cm 2 ) and dried on a heating table at 85°C for 40 minutes to obtain an air electrode. Finally, zinc foil was used as the negative electrode, sprayed slurry carbon paper was used as the air electrode, and 6M KOH solution was used as the electrolyte to assemble the homemade zinc-air battery. It was tested using the blue battery test system. Test conditions 10mA / cm 2 Current density, 10 minutes full electrical cycle time.

[0081] Test results such as Figure 6 As shown, it can be seen that at 10mA / cm 2 During constant current charge and discharge, the SiO2(4) / Fe-NC bifunctional oxygen-oxygen electrode has a larger open circuit voltage and discharge time (228 h), the discharge voltage is maintained at about 1.14 V, the charge voltage is about 2.10 V, and the voltage difference is 0.96 V. After 288 h of charge and discharge cycles, the voltage difference has no significant change, indicating that the electrode has excellent charge and discharge performance stability.

[0082] The above embodiments are only preferred embodiments of the present invention and are not any formal or substantial limitations of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the present invention, and these improvements and supplements should also be regarded as the scope of protection of the present invention.

Claims

1. A SiO2 doped Fe-NC bifunctional oxygen electrode, characterized in that: The bifunctional oxygen electrode uses doped mesoporous carbon as a carbon carrier, SiO2 as a pore former and a surface hydrophobic layer regulator of the carbon carrier, and Fe is anchored on the carbon carrier in the form of a single atom as an active site for oxygen reaction.

2. A method for preparing a SiO2-doped Fe-NC bifunctional oxygen electrode, comprising the following steps: (1) Fe(SO4)2·7H2O, polyquaternium-7, and SiO2 are successively added to a HCl solution, stirred and dissolved, and placed in an oven to dry overnight to obtain a dry product; (2) calcining the dried product in a N2 atmosphere to obtain a carbide; then, the carbide is alkali washed and acid washed successively, and the obtained product is calcined again in a N2 atmosphere to obtain a SiO2-doped Fe-NC bifunctional oxygen electrode.

3. The preparation method according to claim 2, characterized in that: The mass volume ratio of Fe(SO4)2·7H2O, polyquaternium-7, SiO2 and HCl solution in the step (1) is 10-20g:25-90g:10-30g:40-180mL.

4. The preparation method according to claim 2, characterized in that: The oven temperature in step (1) is 80-90°C.

5. The preparation method according to claim 2, characterized in that: The calcination conditions in step (2) are: 800-1100° C., time 1-4 h, and heating rate 5-20° C. / min.

6. The preparation method according to claim 2, characterized in that: The alkali washing conditions in step (2) are: using NaOH solution, alkali washing at room temperature or heating alkali washing, the time is 1-6 days or no alkali washing is performed.

7. The preparation method according to claim 2, characterized in that: The pickling conditions in step (2) are: using H2SO4 solution, pickling at room temperature or heated pickling, for 1 to 10 hours.

8. The preparation method according to claim 2, characterized in that: The secondary calcination conditions in step (2) are: 800-1100° C., time 1-4 hours, and heating rate 5-20° C. / min.

9. Use of the SiO2-doped Fe-NC bifunctional oxygen electrode as claimed in claim 1 in H2-air fuel cells and zinc-air batteries.

Citation Information

Cited By

  • Double-site FeCu-N-C difunctional oxygen electrode as well as preparation method and application thereof

    CN122619823A