Application of nickel tetranitro phthalocyanine modified diaphragm in lithium-sulfur battery and preparation method of modified diaphragm
Through the preparation of a tetranitrophthalocyanine nickel modified separator, the high-active Ni-N4 center is combined with graphene, the problem of polysulfide shuttle effect in lithium-sulfur batteries is solved, the discharge capacity and life of the battery is improved, and the battery is enhanced. Ion permeability and conductivity are improved, and the overall performance of the battery is improved.
Patent Information
- Application Number
- CN202410546674.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lithium-sulfur battery separators have large pores, hydrophobic surfaces and non-conductive results, resulting in severe shuttle effect of soluble polysulfides, affecting battery performance and life.
A tetranitrophthalocyanine-modified separator was used to combine with graphene with high-active Ni-N4 center to prepare a separator with good conductivity and pore size, which was used in lithium-sulfur batteries to reduce the shuttle effect of LiPSs and improve battery performance.
It improves the discharge specific capacity and service life of lithium-sulfur batteries, enhances ion permeability and conductivity, and improves the overall performance of the battery.
Smart Images

Figure CN119069947A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium-sulfur battery diaphragms, and in particular to an application of a nickel tetranitrophthalocyanine modified diaphragm in a lithium-sulfur battery and a preparation method thereof. Background Art
[0002] The theoretical energy density of lithium-sulfur (Li-S) batteries is as high as 2600Wh.kg -1 , which is considered to be one of the most promising high-energy secondary batteries. In the electrochemical reaction process of Li-S batteries, complex phase transition behaviors of soluble lithium polysulfides (LiPSs) and insoluble lithium sulfides (Li2S / Li2S2) are involved. Soluble LiPSs intermediates tend to shuttle between the positive and negative electrodes, resulting in violent phase migration and irreversible loss of coulombic efficiency and battery capacity. Due to the low conductivity of sulfur and the adverse reaction of soluble polysulfides (called the shuttle effect), the widespread application of Li-S batteries is limited by slow kinetics and fast capacity decay. As a key component that interacts with the two electrodes, the separator plays an important role in affecting the overall performance. It ensures the electrical isolation between the cathode and the anode, prevents the battery from electrical short circuit, and has the ability to transfer ions through internal pores.
[0003] Currently, the commonly used commercial battery separators include single-layer polypropylene separator (PP), single-layer polyethylene separator (PE) and three-layer PP / PE / PP composite separator. However, these separators have the disadvantages of large pores, hydrophobic surface, and complete non-conductivity, which are not suitable for the application of long-cycle Li-S batteries. Polysulfides can migrate smoothly to the lithium anode through the highly porous separator, and further reduce on the lithium metal anode to form insoluble Li2S / Li2S2, resulting in the loss of active materials and passivation of the lithium metal anode. In addition, the Li dendrites formed due to the uneven dissolution / deposition of Li may cause internal short circuits, seriously affecting the battery performance. Summary of the invention
[0004] The present invention provides an application of a nickel tetranitrophthalocyanine modified diaphragm in a lithium sulfur battery and a preparation method thereof, wherein nickel tetranitrophthalocyanine with a highly active Ni-N4 center is used to transform the cathode side diaphragm to improve the comprehensive performance of the battery.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a nickel tetranitrophthalocyanine modified diaphragm comprises the following steps:
[0007] S1: Add 4-nitrophthalic anhydride, ammonium molybdate, urea and nickel chloride into an agate mortar and grind and mix them evenly, then add nitrobenzene and heat under reflux while magnetic stirring;
[0008] S2: washing the product obtained in step S1 with ethanol to remove nitrobenzene in the product, adding HCl solution and heating, collecting the solid product by centrifugation, adding NaOH solution to the solid product and heating, washing with acid and alkali alternately in sequence, washing with purified water until neutral, and drying to obtain nickel tetranitrophthalocyanine;
[0009] S3: Dispersing graphene and nickel tetranitrophthalocyanine obtained in step S2 in dimethylformamide respectively to obtain a graphene solution and a nickel tetranitrophthalocyanine solution, then adding the nickel tetranitrophthalocyanine solution to the graphene solution while stirring, ultrasonicating the mixed solution, and then stirring again. After the stirring is completed, vacuum filtering the mixed solution onto a diaphragm to obtain a nickel tetranitrophthalocyanine modified diaphragm.
[0010] Further, in S1, the molar ratio of 4-nitrophthalic anhydride, ammonium molybdate, urea, and nickel chloride is 200:2-3:1000:50, the heating temperature is 185°C, and the heating reflux time is 4.5h;
[0011] Furthermore, in S2, the volume ratio of HCl solution to NaOH solution is 1:1, and the heating temperature after adding HCl solution is 90°C, and the heating time is 1 h. After adding NaOH solution, the heating temperature is 90°C, and the heating time is 1 h.
[0012] Furthermore, in S3, the mass ratio of graphene to nickel tetranitrophthalocyanine is 1:4, the ultrasonic time of the mixed solution is 2 h, and the stirring time is 2 h.
[0013] Application of the nickel tetranitrophthalocyanine modified diaphragm prepared by the above-mentioned method for preparing the nickel tetranitrophthalocyanine modified diaphragm in lithium-sulfur batteries.
[0014] Further, the assembly of the lithium-sulfur battery includes the following steps:
[0015] S10: pouring the carbon nanotubes and the sublimated sulfur into a mortar and grinding them, pouring the ground mixture into a reactor, and introducing argon gas into the reactor to ensure that the mixture is melt-compounded, and then drying the melt-compounded product and cooling it to room temperature to obtain a carbon-sulfur composite material;
[0016] S20: placing polyvinylidene fluoride and N-methylpyrrolidone in a magnetic stirrer, and stirring thoroughly until the polyvinylidene fluoride is completely dissolved to obtain a mixed product;
[0017] S30: putting Ketjenblack and the carbon-sulfur composite material obtained in step S10 into a mortar and grinding them until the color of the sample is uniform, and then placing the sample and the mixed product obtained in step S20 together on a magnetic stirrer and stirring to obtain a positive electrode material;
[0018] S40: Cut the positive electrode material obtained in step S30 into discs to obtain positive electrode sheets, cut the nickel tetranitrophthalocyanine modified diaphragm obtained in step S3 to obtain a battery diaphragm, and assemble them in an argon-filled glove box in the order of negative electrode shell-electrolyte-positive electrode sheet-electrolyte-battery diaphragm-electrolyte-lithium sheet-gasket-shrapnel-positive electrode shell to obtain a button battery.
[0019] Furthermore, in step S10, the mass ratio of carbon nanotubes to sublimated sulfur is 3:7, the grinding time is ≥30 min, the drying temperature is 155° C., and the drying time is 12 h.
[0020] Further, in step S20, the mass ratio of polyvinylidene fluoride to N-methylpyrrolidone is 2:23.
[0021] Further, in step S30, the mass ratio of the carbon-sulfur composite material, Ketjenblack and the mixed product is 7:2:1, and the grinding time is ≥30 min.
[0022] The beneficial effects of the technical solution are:
[0023] 1. The raw materials used in the present invention are abundant, the cost is low, and the preparation process is simple;
[0024] 2. The modified diaphragm of the present invention has a highly active nickel tetranitrophthalocyanine with a Ni-N4 center, which is used as an electrochemical redox catalyst for the conversion of LiPSs in Li-S batteries. Nickel tetranitrophthalocyanine can be easily loaded onto a conductive carbon carrier through interaction, accelerating the electrochemical redox of the conversion of LiPSs in Li-S batteries, reducing the loss of active substances caused by the shuttle of soluble LiPSs intermediates between the positive and negative electrodes, the passivation of the lithium metal anode, or the occurrence of internal short circuits in the battery, and can improve the discharge capacity and service life of the battery, thereby improving the overall performance of the battery;
[0025] 3. The modified diaphragm of the present invention promotes the conversion of LiPSs in Li-S batteries, and at the same time has a certain pore size and porosity, good ionic conductivity, and good permeability to lithium ions, which can improve the specific capacity and charge and discharge performance of the battery, and further improve the comprehensive performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is an X-ray photoelectron energy (XPS) elemental full spectrum of nickel tetranitrophthalocyanine according to an embodiment of the present invention;
[0027] Figure 2 is an X-ray photoelectron energy (XPS) Ni 2p spectrum of nickel tetranitrophthalocyanine according to an embodiment of the present invention;
[0028] Figure 3is a Fourier transform infrared absorption spectrum of nickel tetranitrophthalocyanine according to an embodiment of the present invention;
[0029] Figure 4 It is a rate performance diagram of a battery assembled with a modified diaphragm according to an embodiment of the present invention. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments:
[0031] A method for preparing a nickel tetranitrophthalocyanine modified diaphragm comprises the following steps:
[0032] S1: Add 3.86 g 4-nitrophthalic anhydride, 0.054 g ammonium molybdate, 6 g urea, and 0.648 g nickel chloride into an agate mortar and grind and mix well, then add 60 ml nitrobenzene, and heat under reflux at 185°C with magnetic stirring for 4.5 h;
[0033] The chemical formula of the reaction is as follows:
[0034]
[0035] S2: The product obtained in step S1 is washed with ethanol to remove nitrobenzene in the product, and then 300 ml of 1 mol / L HCl solution is added, and heated at 90°C for 1 hour. Then, the solid product is collected by centrifugation, and then 300 ml of 1 mol / L NaOH solution is added to the solid product, and then heated at 90°C for 1 hour. The product is purified, and then acid and alkali washing are repeated alternately twice, and then washed with pure water until neutral, and dried at 60°C to obtain tetranitrophthalocyanine nickel. The X-ray photoelectron energy (XPS) element spectrum of tetranitrophthalocyanine nickel is as follows: Figure 1 As shown, the X-ray photoelectron energy (XPS) Ni 2p spectrum of nickel tetranitrophthalocyanine is as follows Figure 2 As shown, the Fourier infrared absorption spectrum of nickel tetranitrophthalocyanine is as follows Figure 3 As shown;
[0036] S3: 4 mg of graphene G and 16 mg of nickel tetranitrophthalocyanine obtained in step S2 are dispersed in 30 ml of dimethylformamide respectively to obtain a graphene solution and a nickel tetranitrophthalocyanine solution, and then the nickel tetranitrophthalocyanine solution is added to the graphene G solution while stirring, the mixed solution is ultrasonicated for 2 hours, and then stirred for another 2 hours. After the stirring is completed, the mixed solution is vacuum filtered onto a Celgard 2500 diaphragm to obtain a nickel tetranitrophthalocyanine modified diaphragm.
[0037] The use of the nickel tetranitrophthalocyanine modified diaphragm prepared by the above-mentioned method for preparing the nickel tetranitrophthalocyanine modified diaphragm in a lithium-sulfur battery, the assembly of the lithium-sulfur battery comprises the following steps:
[0038] S10: Weigh carbon nanotubes and sublimed sulfur in a mass ratio of 3:7, pour them into a mortar and grind them manually for more than 30 minutes until the color of the sample is uniform and no yellow particles are observed, then pour the ground mixture into the lining of a high-pressure reactor, pass high-purity argon gas into the reactor through a glove box to ensure that the mixture is melt-compounded under argon gas, then put the melt-compounded product in a blast dryer and keep it at 155°C for 12 hours, wait for the sample to cool naturally to room temperature, then take it out and mark it, and then a carbon-sulfur composite material is obtained;
[0039] S20: Weigh polyvinylidene fluoride and N-methylpyrrolidone in a mass ratio of 2:23 using an electronic balance, then place the sample bottle on a magnetic stirrer and stir thoroughly for several hours until the polyvinylidene fluoride is completely dissolved to obtain a mixed product;
[0040] S30: 20 mg of Ketjen black and 70 mg of the carbon-sulfur composite material obtained in step S10 are put into a mortar and ground for more than 30 min until the color of the sample is uniform, and then the sample and 125 mg of the mixed product obtained in step S20 are placed on a magnetic stirrer and stirred to obtain a positive electrode material. If the slurry is found to be too viscous during the stirring process, a small amount of NMP can be added until it is ground into a black slurry with appropriate thickness and a certain viscosity;
[0041] S40: Cut the positive electrode material obtained in step S30 into discs to obtain positive electrode sheets, cut the nickel tetranitrophthalocyanine modified diaphragm obtained in step S3 to obtain a battery diaphragm, and assemble them in a glove box filled with argon in the order of negative electrode shell-electrolyte-positive electrode sheet-electrolyte-battery diaphragm-electrolyte-lithium sheet-gasket-shrapnel-positive electrode shell to obtain a button battery, wherein the water and oxygen contents in the glove box filled with argon are both less than 1 ppm.
[0042] The button cell obtained from S40 was left to stand for 12 hours, and then the battery charge and discharge test was performed at different rates by the Blue Electric Battery Test System. The test conditions were room temperature, the window start voltage was 1.5V, and the end voltage was 3V. Figure 4 This is the rate performance diagram of the button battery. It can be seen from the figure that the first discharge specific capacity and capacity retention rate of the button battery are relatively high at different rates. The battery assembled with the modified diaphragm has good rate performance, charge and discharge performance and good cycle life.
[0043] The above are only embodiments of the present invention, and common knowledge such as the known specific technical solutions or characteristics in the solution are not described in detail here. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the technical solution of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A method for preparing a nickel tetranitrophthalocyanine modified diaphragm, characterized in that: The following steps are involved: S1: Add 4-nitrophthalic anhydride, ammonium molybdate, urea and nickel chloride into an agate mortar and grind and mix them evenly, then add nitrobenzene and heat under reflux while magnetic stirring; S2: washing the product obtained in step S1 with ethanol to remove nitrobenzene in the product, adding HCl solution and heating, collecting the solid product by centrifugation, adding NaOH solution to the solid product and heating, washing with acid and alkali alternately in sequence, washing with purified water until neutral, and drying to obtain nickel tetranitrophthalocyanine; S3: Dispersing graphene and nickel tetranitrophthalocyanine obtained in step S2 in dimethylformamide respectively to obtain a graphene solution and a nickel tetranitrophthalocyanine solution, then adding the nickel tetranitrophthalocyanine solution to the graphene solution while stirring, ultrasonicating the mixed solution, and then stirring again. After the stirring is completed, vacuum filtering the mixed solution onto a diaphragm to obtain a nickel tetranitrophthalocyanine modified diaphragm.
2. The method for preparing a nickel tetranitrophthalocyanine modified diaphragm according to claim 1, characterized in that: In S1, the molar ratio of 4-nitrophthalic anhydride, ammonium molybdate, urea and nickel chloride is 200:2-3:1000:50, the heating temperature is 185°C, and the heating reflux time is 4.5h.
3. The method for preparing a nickel tetranitrophthalocyanine modified diaphragm according to claim 1, characterized in that: In S2, the volume ratio of HCl solution to NaOH solution is 1:1, and the heating temperature after adding HCl solution is 90°C and the heating time is 1 h. After adding NaOH solution, the heating temperature is 90°C and the heating time is 1 h.
4. The method for preparing a nickel tetranitrophthalocyanine modified diaphragm according to claim 1, characterized in that: In S3, the mass ratio of graphene to nickel tetranitrophthalocyanine is 1:4, the ultrasonic time of the mixed solution is 2 h, and the stirring time is 2 h.
5. Use of a nickel tetranitrophthalocyanine modified diaphragm prepared by the method for preparing a nickel tetranitrophthalocyanine modified diaphragm according to any one of claims 1 to 4 in a lithium-sulfur battery.
6. The use of the nickel tetranitrophthalocyanine modified diaphragm prepared by the method for preparing the nickel tetranitrophthalocyanine modified diaphragm according to claim 5 in a lithium-sulfur battery is applied to the assembly of a lithium-sulfur battery, characterized in that: The following steps are involved: S10: pouring the carbon nanotubes and the sublimated sulfur into a mortar and grinding them, pouring the ground mixture into a reactor, and introducing argon gas into the reactor to ensure that the mixture is melt-compounded, and then drying the melt-compounded product and cooling it to room temperature to obtain a carbon-sulfur composite material; S20: placing polyvinylidene fluoride and N-methylpyrrolidone in a magnetic stirrer, and stirring thoroughly until the polyvinylidene fluoride is completely dissolved to obtain a mixed product; S30: putting Ketjenblack and the carbon-sulfur composite material obtained in step S10 into a mortar and grinding them until the color of the sample is uniform, and then placing the sample and the mixed product obtained in step S20 together on a magnetic stirrer and stirring to obtain a positive electrode material; S40: Cut the positive electrode material obtained in step S30 into discs to obtain positive electrode sheets, cut the nickel tetranitrophthalocyanine modified diaphragm obtained in step S3 to obtain a battery diaphragm, and assemble them in an argon-filled glove box in the order of negative electrode shell-electrolyte-positive electrode sheet-electrolyte-battery diaphragm-electrolyte-lithium sheet-gasket-shrapnel-positive electrode shell to obtain a button battery.
7. Application of the nickel tetranitrophthalocyanine modified diaphragm prepared by the method for preparing the nickel tetranitrophthalocyanine modified diaphragm according to claim 5 in a lithium-sulfur battery, characterized in that: In step S10, the mass ratio of carbon nanotubes to sublimated sulfur is 3:7, the grinding time is ≥30 min, the drying temperature is 155° C., and the drying time is 12 h.
8. Application of the nickel tetranitrophthalocyanine modified diaphragm prepared by the method for preparing the nickel tetranitrophthalocyanine modified diaphragm according to claim 5 in a lithium-sulfur battery, characterized in that: In step S20 , the mass ratio of polyvinylidene fluoride to N-methylpyrrolidone is 2:
23.
9. Application of the nickel tetranitrophthalocyanine modified diaphragm prepared by the method for preparing the nickel tetranitrophthalocyanine modified diaphragm according to claim 5 in a lithium-sulfur battery, characterized in that: In step S30, the mass ratio of the carbon-sulfur composite material, Ketjenblack and the mixed product is 7:2:1, and the grinding time is ≥30 min.
Citation Information
Patent Citations
Graphene / phthalocyanine supercapacitor electrode material, and preparation method thereof
CN106683907A
Functional separator including catalytic state, method for manufacturing same, and lithium secondary
CN112913075A
Lithium-sulfur battery modified diaphragm as well as preparation method and application thereof
CN114583395A
Cited By
Application of metal nickel phthalocyanine modified diaphragm in lithium-sulfur battery
CN118825549A