A nitrogen-phosphorus co-doped metal-free catalyst and its application
Through the preparation of nitrogen and phosphorus co-doped metal-free catalysts, the cost and poor durability of precious metal platinum catalysts are solved, and a low-cost and long-life alternative is provided for cathode oxygen reduction reaction of zinc air batteries, realizing the catalyst The activity and stability of the patient are significantly improved.
Patent Information
- Application Number
- CN202211461492.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-17
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-11-17
AI Technical Summary
The precious metal platinum (Pt) and its alloys are expensive and poor durable as oxygen reduction reaction (ORR) catalysts, limiting their large-scale commercial application in fuel cells and metal air batteries.
Using nitrogen and phosphorus co-doped metal-free catalyst, dicyanide diamine, deionized water, phytic acid and Zn(NO3)2·6H2O are mixed in a specific proportion, and then treated by ultrasonic, stirring, rotary evaporation and procedure heating and calcination , a nitrogen-phosphorus co-doped metal-free catalyst with excellent specific surface area and pore size structure was prepared for cathode oxygen reduction reaction of zinc air battery.
It realizes a low-cost and long-life catalyst, has excellent oxygen reduction activity and stability, reduces the reaction energy barrier, enhances the durability and environmental friendliness of the catalyst, replaces precious metal catalysts, and is suitable for oxygen reduction in zinc air batteries. reaction.
Smart Images

Figure CN115845897B_ABST
Abstract
Description
Technical field:
[0002] The invention belongs to the technical field of catalysts, and in particular relates to a nitrogen-phosphorus co-doped metal-free catalyst and application thereof. Background technology:
[0004] With the accelerated consumption of traditional fossil fuels and the resulting series of environmental pollution problems, advanced energy conversion technologies have attracted widespread attention worldwide. Fuel cells and metal-air batteries are considered to be the next generation of clean energy, which can directly convert the chemical energy of fuels into electrical energy. However, the oxygen reduction reaction (ORR) in the cathode of fuel cells and metal-air batteries has the disadvantages of slow kinetics, high overpotential, and poor stability, and catalysts are needed to improve its reaction activity. In past studies, precious metal platinum (Pt) and its alloys have been considered to be the most advanced ORR catalysts. However, due to limited resources, high prices, easy poisoning (such as methanol poisoning and CO poisoning deactivation) and poor durability, precious metal platinum (Pt) and its alloys cannot be put into large-scale commercial applications. Therefore, in the past few decades, exploring a resource-rich, highly active, and low-cost alternative material has become an important goal of human research.
[0005] Among all candidate materials, functionalized carbon nanomaterials have been intensively studied due to their abundant resources, easy manufacture, excellent activity and low cost, and are considered to be one of the most promising ORR catalysts. Moreover, compared with metal-based catalysts, metal-free catalysts are less susceptible to poisoning and have longer durability. In addition, metal-free catalysts have superior environmental friendliness. Dai et al. (Science, 2009, 323, 760) reported pioneering work on nitrogen-doped vertically aligned carbon nanotubes for ORR in 2009. Since then, researchers have studied various heteroatom (N, B, S, O, P, F, etc.) single / double / multi-doped non-metallic nanocarbon ORR electrocatalysts. Due to the different electronegativity of heteroatoms, the local charge and spin density of the carbon matrix after doping have changed significantly, which can promote oxygen adsorption, reduce the reaction energy barrier, break the OO bond, and enhance the ORR activity. Therefore, heteroatom doping of metal-free catalysts is of great significance to improve the ORR activity. Summary of the invention:
[0007] One object of the present invention is to provide a nitrogen-phosphorus co-doped metal-free catalyst, which is used to solve the problems of expensive price and poor durability of precious metal platinum as ORR catalyst in the prior art. Another object of the present invention is to provide a nitrogen-phosphorus co-doped metal-free catalyst for the cathode oxygen reduction reaction of zinc-air batteries.
[0008] The technical solution adopted by the present invention to solve the technical problem is: the nitrogen-phosphorus co-doped metal-free catalyst is prepared by the following method:
[0009] Step 1, dicyandiamide and deionized water are mixed in a mass ratio of 1:20-1:50, ultrasonicated for 0.5-6 hours, and then stirred for 6-48 hours to fully dissolve the dicyandiamide in the deionized water;
[0010] Step 2: Under stirring, slowly add phytic acid dropwise to the solution prepared in the above step 1, then add Zn(NO3)2·6H2O, and stir for 6-48 hours; the mass ratio of phytic acid to dicyandiamide is 1:1-1:10, and the mass ratio of Zn(NO3)2·6H2O to dicyandiamide is 1:5-1:30;
[0011] Step 3, the solution obtained in the above step 2 is subjected to rotary evaporation at 60-100° C. in a water bath, and further vacuum dried at 70-90° C. for 6-24 hours, and ground to obtain a solid powder;
[0012] Step 4: calcining the solid powder obtained in step 3 in two steps by a programmed temperature method to obtain a nitrogen-phosphorus co-doped metal-free catalyst; the calcination temperature of the first stage is 300-700 ° C, the calcination time is 0.5-3 hours, the heating rate during calcination is 2-10 ° C / min, and the inert gas used during calcination is argon; the calcination temperature of the second stage is 910-1100 ° C, the calcination time is 0.5-3 hours, the heating rate during calcination is 2-10 ° C / min, and the inert gas used during calcination is argon; the prepared nitrogen-phosphorus co-doped metal-free catalyst is composed of carbon, nitrogen, phosphorus and oxygen, wherein the content ratio of nitrogen to phosphorus is 3:1-4:1.
[0013] The nitrogen-phosphorus co-doped metal-free catalyst in the above scheme has a large specific surface area and an excellent pore structure, with a specific surface area of 1000-2000 m 2 g -1 , pore volume is 1.5-2.5 cm 3 g -1 , the pore size is 2-10 nm.
[0014] In the above scheme, the ultrasonic time in step 1 is 3 hours and the stirring time is 24 hours.
[0015] In step 3 of the above scheme, the solution is evaporated to dryness in a water bath at 80°C and then vacuum dried at 80°C for 12 hours.
[0016] The nitrogen-phosphorus co-doped metal-free catalyst in the above scheme has excellent oxygen reduction performance under alkaline and acidic conditions. Under alkaline conditions, the half-wave potential reaches 0.87-0.92 V, and under acidic conditions, the half-wave potential is 0.67-0.70 V. In the zinc-air battery performance test, the peak power density reaches 130-150 mW cm -2 , has excellent charge and discharge cycle stability.
[0017] The nitrogen-phosphorus co-doped metal-free catalyst is used for the cathode oxygen reduction reaction of zinc-air batteries.
[0018] The present invention has the following beneficial effects:
[0019] (1) The present invention uses an impregnation method and a programmed temperature step-by-step calcination method to prepare a nitrogen-phosphorus co-doped metal-free material. The metal-free catalyst preparation method of the present invention is green and environmentally friendly, has a simple preparation process, and can replace the precious metal Pt catalyst. The obtained nitrogen-phosphorus co-doped metal-free catalyst is applied to the oxygen reduction reaction of the cathode of a zinc-air battery and has good catalytic activity and stability.
[0020] (2) The present invention utilizes the synergistic effect between nitrogen and phosphorus heteroatoms to reduce the reaction energy barrier, promote oxygen adsorption, and achieve a significant improvement in catalyst activity and stability.
[0021] (3) The nitrogen-phosphorus co-doped material of the present invention is metal-free, not easily poisoned (such as methanol poisoning and CO poisoning deactivation), and has longer durability; it is more in line with the concept of green development advocated by today's society.
[0022] (4) The preparation method of the nitrogen-phosphorus co-doped metal-free catalyst of the present invention is simple and safe, and the raw materials are abundant and low in price, which greatly reduces the cost of the catalyst.
[0023] (5) The nitrogen-phosphorus co-doped metal-free catalyst of the present invention is applied to oxygen reduction reaction and has good catalytic activity and stability.
[0024] (6) In the second stage of calcination, Zn is volatilized and introduced, which can play a role in forming pores and defects in the nitrogen-phosphorus co-doped metal-free catalyst. Description of the drawings:
[0026] Figure 1 This is the XRD diagram of the nitrogen and phosphorus co-doped metal-free catalyst in Example 1.
[0027] Figure 2 This is the SEM image of the nitrogen and phosphorus co-doped metal-free catalyst in Example 1.
[0028] Figure 3 It is the LSV curve of the nitrogen and phosphorus co-doped metal-free catalyst of Example 1 and other comparison samples under alkaline conditions.
[0029] Figure 4 It is the LSV curve of the nitrogen and phosphorus co-doped metal-free catalyst of Example 1 and other comparison samples under acidic conditions.
[0030] Figure 5 It is the polarization curve and power density diagram of the nitrogen and phosphorus co-doped metal-free catalyst and Pt / C in Example 1. Specific implementation method:
[0032] The present invention will be further described below in conjunction with the accompanying drawings:
[0033] Embodiment 1:
[0034] This embodiment provides a nitrogen-phosphorus co-doped metal-free catalyst, which is prepared by the following method:
[0035] 1. Place 1-10 g of dicyandiamide in 20-200 mL of deionized water, ultrasonicate for 3 hours, and stir for 24 hours until dissolved.
[0036] 2. Under stirring conditions, slowly add 0.5-20 mL of phytic acid dropwise to the above solution, and add 0.1-5 g of Zn(NO0143)2·6H2O, and stir for 12 hours.
[0037] 3. The solution obtained in the above step 2 was evaporated to dryness in a water bath rotary evaporation at 80° C., the solid powder was collected and further vacuum dried at 80° C. for 12 hours, and then ground to obtain a solid powder.
[0038] 4. The solid powder obtained in step 3 was calcined in two steps by programmed temperature method to obtain nitrogen-phosphorus co-doped metal-free catalyst. The first stage of calcination was heated to 600 °C at 5 °C / min and kept at this temperature for 2 hours in an argon atmosphere; the second stage of calcination was heated to 950 °C at 5 °C / min and kept at this temperature for 2 hours in an argon atmosphere.
[0039] A series of structural characterizations were performed on the nitrogen and phosphorus co-doped metal-free catalyst obtained in the above example to verify its structure.
[0040] like Figure 1 The XRD pattern of the nitrogen-phosphorus co-doped metal-free catalyst in Example 1 is shown. In the figure, there are only two broad diffraction peaks at about 23.0° and 43.5°, which correspond to the (002) and (101) crystal planes of graphite carbon, respectively. This shows that the metal-free material has a high degree of graphitization.
[0041] like Figure 2 The SEM image of the nitrogen and phosphorus co-doped metal-free catalyst of Example 1 is shown, which proves that the catalyst obtained in Example 1 is porous and irregular in shape.
[0042] Embodiment 2:
[0043] The difference between this embodiment and embodiment 1 is that, in this embodiment, the ultrasonication time in step 1 is 2 hours.
[0044] Embodiment 3:
[0045] The difference between this embodiment and embodiment 1 is that, in this embodiment, the ultrasonication time in step 1 is 6 hours.
[0046] Embodiment 4:
[0047] The difference between this embodiment and embodiment 1 is that, in this embodiment, the stirring time after adding phytic acid and Zn(NO3)2·6H2O in step 2 is 6 hours.
[0048] Embodiment 5:
[0049] The difference between this embodiment and embodiment 1 is that, in this embodiment, the stirring time after adding phytic acid and Zn(NO3)2·6H2O in step 2 is 48 hours.
[0050] Embodiment 6:
[0051] The only difference between this embodiment and embodiment 1 is that, in this embodiment, the temperature during spin drying in step 3 is 60°C.
[0052] Embodiment 7:
[0053] The only difference between this embodiment and embodiment 1 is that, in this embodiment, the temperature during spin drying in step 3 is 100°C.
[0054] Embodiment 8:
[0055] The difference between this embodiment and embodiment 1 is that, in this embodiment, the vacuum drying time in step 3 is 6 hours.
[0056] Embodiment 9:
[0057] The difference between this embodiment and embodiment 1 is that, in this embodiment, the vacuum drying time in step 3 is 24 hours.
[0058] Embodiment 10:
[0059] The only difference between this embodiment and embodiment 1 is that in this embodiment, the second stage calcination in step 4 is heated to 910°C at 5°C / min under an argon atmosphere and kept at this temperature for 2 hours.
[0060] Embodiment 11:
[0061] The only difference between this embodiment and embodiment 1 is that in this embodiment, the second stage calcination in step 4 is heated to 1000°C at 5°C / min under an argon atmosphere and kept at this temperature for 2 hours.
[0062] Comparative Example 1:
[0063] The only difference between this comparative example and Example 1 is that Zn(NO3)2·6H2O is not added.
[0064] Comparative Example 2:
[0065] The difference between this comparative example and Example 1 is that the spin drying method is not used, and vacuum drying is performed directly after centrifugation.
[0066] Comparative Example 3:
[0067] The difference between this comparative example and Example 1 is that in the last step of calcination, the programmed temperature method is not used, and the temperature is directly increased to 950 ºC at 5 ℃ / min under an argon atmosphere and kept at this temperature for 2 hours.
[0068] In order to test the catalytic performance of the nitrogen-phosphorus co-doped metal-free catalyst of the present application, the present application also provides application examples and catalyst performance tests.
[0069] This nitrogen-phosphorus co-doped metal-free catalyst is applied to the oxygen reduction reaction at the cathode in zinc-air batteries.
[0070] Catalyst oxygen reduction reaction and zinc-air battery performance evaluation: 5 mg of the catalyst prepared in Example 1 was dissolved in 960 μl of anhydrous ethanol + 40 μl of Nafion, ultrasonicated until fully dissolved, and then the performance was tested using an electrochemical workstation.
[0071] like Figure 3 The figure shows the LSV curves of the nitrogen-phosphorus co-doped metal-free catalyst of Example 1 and other comparison samples under alkaline conditions. It can be seen from the figure that under alkaline conditions, the half-wave potential of the nitrogen-phosphorus co-doped metal-free catalyst reaches 0.92 V, which is much higher than commercial Pt / C and other comparison samples, indicating its excellent oxygen reduction activity.
[0072] like Figure 4 The figure shows the LSV curves of the nitrogen-phosphorus co-doped metal-free catalyst in Example 1 and other comparison samples under acidic conditions. It can be seen from the figure that under acidic conditions, the half-wave potential of the metal-free catalyst reaches 0.70 V, indicating its good oxygen reduction performance in an acidic environment.
[0073] like Figure 5 Shown are the polarization curves and power density diagrams of the nitrogen-phosphorus co-doped metal-free catalyst and commercial Pt / C in Example 1. It can be seen from the figure that the discharge polarization curve and power density of the metal-free catalyst are far superior to those of commercial Pt / C, and it has excellent development prospects.
[0074] The metal-free catalyst prepared by the present invention has excellent performance among the same type of metal-free catalysts, and its peak power density exceeds that of most reported metal-free catalysts. This nitrogen-phosphorus co-doped metal-free catalyst has excellent charge-discharge cycle stability when used in zinc-air batteries, and its performance remains stable after 80 hours.
[0075] The above is a detailed introduction to a nitrogen-phosphorus co-doped metal-free catalyst and its preparation method and application disclosed in the embodiments of the present application. Specific examples are used in this article to illustrate the implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for general technicians in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A nitrogen-phosphorus co-doped metal-free catalyst, characterized in that It is prepared by the following steps: Step 1, dicyandiamide and deionized water are mixed in a mass ratio of 1:20-1:50, ultrasonicated for 0.5-6 hours, and then stirred for 6-48 hours to fully dissolve the dicyandiamide in the deionized water; Step 2: Under stirring, slowly add phytic acid dropwise to the solution prepared in the above step 1, then add Zn(NO3)2·6H2O, and stir for 6-48 hours; the mass ratio of phytic acid to dicyandiamide is 1:1-1:10, and the mass ratio of Zn(NO3)2·6H2O to dicyandiamide is 1:5-1:30; Step 3, the solution obtained in the above step 2 is subjected to rotary evaporation at 60-100° C. in a water bath, and further vacuum dried at 70-90° C. for 6-24 hours, and ground to obtain a solid powder; Step 4: calcining the solid powder obtained in step 3 in two steps by a programmed temperature method to obtain a nitrogen-phosphorus co-doped metal-free catalyst; the calcination temperature of the first stage is 300-700 ° C, the calcination time is 0.5-3 hours, the heating rate during calcination is 2-10 ° C / min, and the inert gas used during calcination is argon; the calcination temperature of the second stage is 950-1100 ° C, the calcination time is 0.5-3 hours, the heating rate during calcination is 2-10 ° C / min, and the inert gas used during calcination is argon; the prepared nitrogen-phosphorus co-doped metal-free catalyst is composed of carbon, nitrogen, phosphorus and oxygen, wherein the content ratio of nitrogen to phosphorus is 3:1-4:1, and the pore size of the nitrogen-phosphorus co-doped metal-free catalyst is 10 nm; The nitrogen-phosphorus co-doped metal-free catalyst has excellent oxygen reduction performance under alkaline and acidic conditions. Under alkaline conditions, the half-wave potential reaches 0.87-0.92 V, and under acidic conditions, the half-wave potential is 0.67-0.70 V. In the zinc-air battery performance test, the peak power density reaches 130-150 mW cm -2 , has excellent charge and discharge cycle stability.
2. The nitrogen-phosphorus co-doped metal-free catalyst according to claim 1, characterized in that: The nitrogen-phosphorus co-doped metal-free catalyst has a large specific surface area and an excellent pore structure, with a specific surface area of 1000-2000 m 2 g -1 , pore volume is 1.5-2.5 cm 3 g -1 .
3. The nitrogen-phosphorus co-doped metal-free catalyst according to claim 2, characterized in that: In the step 1, the ultrasonic time is 3 hours and the stirring time is 24 hours.
4. The nitrogen-phosphorus co-doped metal-free catalyst according to claim 3, characterized in that: In the step 3, the mixture is evaporated to dryness in a water bath at 80° C. and then vacuum dried at 80° C. for 12 hours.
5. Use of the nitrogen-phosphorus co-doped metal-free catalyst according to any one of claims 1 to 4, characterized in that: The nitrogen-phosphorus co-doped metal-free catalyst is used for cathode oxygen reduction reaction of zinc-air battery.
Citation Information
Patent Citations
Preparation method and application of nitrogen and phosphorus co-doped porous carbon materials
CN106000438A
Nitrogen-phosphorus double-doped carbon-coated transition metal diphosphide hydrogen evolution catalyst and preparation method thereof
CN107362818A
Preparation method and application for nitrogen phosphorus co-doped porous carbon
CN107425204A
Nitrogen-phosphorus codoped carbon loaded molybdenum carbide or tungsten carbide catalyst and preparing method and application thereof
CN107999108A
Preparation method of bamboo-leaf-based carbon material with high specific surface area
CN111099587A