Coated Substrate

A magnetron-sputtered mixed metal oxide topcoat on transparent substrates, comprising TiO y , ZrO z , and optionally SiO x , addresses the durability issues of functional coatings, enhancing mechanical and chemical resistance while preserving optical properties.

JP2024536031APending Publication Date: 2024-10-04AGC GLASS EUROPE SA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024517171
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-29
Filing Date
2022-09-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing functional coatings, such as magnetron-sputtered dielectric layers, suffer from insufficient mechanical and chemical durability during manufacturing, transportation, and handling, limiting their use in contact with the external environment.

Method used

A coated substrate with a transparent substrate having a functional coating protected by a magnetron-sputtered mixed metal oxide topcoat comprising TiO y , ZrO z , and optionally SiO x , with specific atomic percentages and thickness ranging from 0.1 to 10 nm, providing improved mechanical, chemical, and corrosion resistance without affecting emissivity or aesthetics.

Benefits of technology

The topcoat enhances the durability of the functional coating, increasing abrasion resistance by at least 20% to 40% while maintaining optical properties within acceptable ranges, allowing for use in harsh conditions without adverse effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536031000001
    Figure 2024536031000001
  • Figure 2024536031000002
    Figure 2024536031000002
  • Figure 2024536031000003
    Figure 2024536031000003
Patent Text Reader

Abstract

The present invention provides a coated substrate comprising a transparent substrate having two major opposed first and second surfaces, at least one surface of which is provided with a functional coating, the transparent substrate comprising at least a TiO y and ZrO z and optionally SiO x (where x, y, z are in the range of 1.8-2.2), wherein the topcoat comprises 8-49 atomic % titanium, 51-92 atomic % zirconium, 0-9 atomic % silicon, totaling 100 atomic % metal, and the topcoat has a thickness of 0.1-10 nm; and methods of providing such coated substrates and uses thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a functional coating and at least one TiO y and ZrO z and optionally SiO x and a magnetron sputtered topcoat of a mixed metal oxide comprising the compound of formula (I), a method for providing said coated substrate, and uses of the topcoat. [Background technology]

[0002] It is known that functional coatings, such as those including magnetron sputtered dielectric layers, are typically susceptible to chemical and mechanical damage during their manufacture, transportation, processing, storage, and / or handling, and this limited mechanical, chemical, and corrosion resistance usually limits their feasible uses in contact with the external environment.

[0003] Various attempts have been made to provide glazing with coatings that have high chemical or mechanical durability, or both chemical and mechanical durability.

[0004] WO2009115596A1 relates to an essentially transparent glazing with lightfastness and / or low emission properties, comprising an assembly of thin layers deposited in vacuum by means of a magnetron, in which the surface protective layer comprises a layer comprising titanium oxide and at least one other hard metal oxide selected from the group comprising ZrO2, SiO2, Cr2O3. The disclosed glazing is able to withstand a heat treatment at 550°C for 5 minutes without developing optical defects such as discolouration or pearlescence. In the mixed oxide, titanium oxide is present in an amount of at least 40% by weight. The surface layer comprises zirconium oxide in a proportion of 15 to 50% by weight.

[0005] WO2010031808A1 relates to a glazing comprising at least one layer deposited by cathodic spraying under vacuum, said layer comprising one or more oxides, the weight proportion of titanium oxide being at least 40% and not more than 95%. The thickness of the layer in question, and optionally of another layer containing a metal oxide, is selected so that said layer provides a reflection of at least 15% and a light transmission of at least 60% on a 4 mm thick sheet of transparent "float" glass. The layer or layer system in question furthermore has mechanical and / or chemical resistance comparable to layers produced by pyrolysis to obtain a product with the same type of optical properties. A quantity of titanium oxide of at least 40% by weight typically results in an amount of at least 50 atomic % titanium in the deposited layer.

[0006] However, the above solutions do not provide sufficient mechanical durability against the wear encountered during shipping and storage conditions in a typical dry brush test and / or Automatic Wet Rub Test (AWRT).

[0007] WO 2018202595 A1 relates to a coated substrate comprising a substrate, a soft coating provided on at least a portion of at least one surface of the substrate, a protective sol-gel coating provided on at least a portion of said surface above the soft coating, a method for producing such a coated substrate, and a glazing unit comprising such a coated substrate. The sol-gel coating comprises a mixture of titanium oxide, silicon oxide, and optionally bismuth oxide and / or cerium oxide, in a theoretical weight ratio of titanium oxide TiO2 / silicon oxide SiO2 ranging from 0.10 to 3. If zirconium oxide is present, the ratio of zirconium oxide / silicon oxide ranges from 0.10 to 3. The ratio of titanium oxide / zirconium oxide ranges from 0.10 to 10. The thickness of the sol-gel coating is typically in the range of 50 to 500 nm. This solution has the main drawback that a very thick layer of the protective layer is formed, which entails further manufacturing constraints since an additional mandatory heating step is required to cure the sol-gel coating and modifications of the production line are required. That is, a potentially damaging intermediate step is required before the sol-gel coating can protect the coated substrate.

[0008] Copending application PCT / EP2021 / 058666 relates to a coated substrate comprising a transparent substrate having two major opposed first and second surfaces, at least one surface of which is provided with a functional coating, the transparent substrate being provided with a magnetron sputtered topcoat of a mixed metal oxide comprising at least SiOx, TiOy, and ZrOz (where x, y, z are in the range of 1.8-2.2) over and in contact with the functional coating, the topcoat comprising 10-65 atomic % silicon, 8-38 atomic % titanium, 25-80 atomic % zirconium, totaling 100 atomic % metal, the topcoat having a thickness of 0.1-10 nm, methods of providing such coated substrates, and uses thereof.

[0009] There remains a need to develop coated substrates, particularly glass substrates, provided with functional coatings that have improved mechanical, chemical, and corrosion resistance, but do not significantly affect the emissivity and / or aesthetics of the coating.

[0010] There remains a need to develop coated substrates, particularly glass substrates, on which functional coatings can be provided that have improved mechanical, chemical, and corrosion resistance, but do not significantly affect the emissivity or aesthetics of the coating, i.e., the optical properties of the functional coating are maintained. Summary of the Invention

[0011] The object of the present invention is to provide a coated substrate comprising a transparent substrate having two major opposing first and second surfaces, the first surface being provided with a functional coating, the transparent substrate being provided with at least a TiO y and ZrO z and optionally SiO x wherein x, y, and z are in the range of 1.8 to 2.2; The top coat is - 8 to 49 atomic percent titanium, - 51 to 92 atomic % zirconium, - 0-9 atomic % silicon, and the total amount of the metal is 100 atomic %, and the top coat has a thickness of 0.1 to 10 nm.

[0012] A method for providing the coated substrate is also provided.

[0013] A heat treated coated substrate and a plurality of glazing units are provided.

[0014] The topcoat is composed of at least TiO y , and ZrO zand optionally SiO x where x, y, and z are in the range of 1.8 to 2.2; The top coat is - 8 to 49 atomic % titanium (Ti), - 51 to 92 atomic % zirconium (Zr), - 0 to 9 atomic % silicon (Si), It is 100 atomic % metal including impurities, The topcoat has a thickness of 0.1 to 10 nm.

[0015] Impurities are considered as additional metals that cannot be substantially separated from the metals. This is especially the case for yttrium and / or hafnium, both transition metals. If these additional metals are present, their content remains relatively limited, not exceeding 1 atomic % of the claimed mixed metals, and usually remains below 0.8 atomic %. They are not taken into account in the calculation of the effective metal content of the Ti, Zr and Si topcoats. The effective content is considered as the sum of only the contributions of titanium, zirconium and optional silicon, as mechanical durability is obtained within the scope of the present invention. Aluminum can be present in the titanium-based target or the silicon-based target as a trace element, preferably in an amount of <5.0 atomic %, alternatively <2.0 atomic %, alternatively <1.0 atomic %. Again, such aluminum is considered as an impurity in the present specification and is not taken into account in the effective content of titanium, zirconium and optional silicon.

[0016] Alternatively, the topcoat may comprise at least TiO y , and ZrO z and optionally SiO x where x, y, z are in the range of 1.8 to 2.2; The top coat is - 8 to 49 atomic % titanium (Ti), - 51 to 92 atomic % zirconium (Zr), - 0 to 9 atomic % silicon (Si), - 0-5 atomic % impurities, It is 100 atomic % metal including impurities, The topcoat has a thickness of 0.1 to 10 nm.

[0017] Within the scope of the present invention, elemental Si is considered a metal, even though chemically it is a semi-metallic material, due to its properties in the present topcoat.

[0018] In some embodiments of the invention, the above ranges of Ti, Zr and Si in the topcoat can vary independently of each other. Alternatively, the amount of Ti can range from 10 to 47 atomic %, alternatively from 12 to 46 atomic %. Alternatively, the amount of Zr can range from 53 to 90 atomic %. Alternatively, the amount of Si can range from 1 to 8 atomic %, alternatively from 2 to 7 atomic %. Alternatively, the amount of impurities can range from 0.1 to 3 atomic %, alternatively from 0.2 to 2 atomic %. Thus, these amounts can vary independently for each metal, provided that the total is 100 atomic % metal, including impurities.

[0019] The amount of each metal can be determined by methods available to those skilled in the art, such as X-ray photoelectron spectroscopy (XPS), X-ray fluorescence (XRF), etc. These analyses can be performed on magnetron sputter deposited topcoats using routine procedures well known in the art.

[0020] These amounts, i.e. when the amount of titanium oxide is <40%, in combination with zirconium, optionally in the presence of silicon, result in an optimal topcoat and, surprisingly, excellent mechanical durability against abrasion of functional coatings that require transportation or storage. Contrary to the teaching of WO2009115596A1, it was unexpectedly found that when the amount of titanium oxide is >40%, titanium does not achieve the required durability when combined with zirconium.

[0021] The topcoat may have a thickness in the range of 0.1 to 10.0 nm, alternatively 0.5 to 5.0 nm, alternatively 2.0 to 5.0 nm.

[0022] Such thicknesses can provide improved mechanical durability while at the same time minimizing optical contributions to the underlying functional coating. The topcoat is permanent in that it is not removed or altered by optional heat treatment of the coated substrate. There is also no adverse effect on the optical properties of the underlying functional coating.

[0023] The refractive index, n, of the present topcoat materials within the claimed range depends on their final composition but can range from 1.8 to 2.3 at a wavelength of 550 nm. Silicon can play a role in fine tuning the refractive index of the topcoat material but cannot provide the initial protection function of the topcoat.

[0024] The transparent substrate may be a glass substrate, or a plastic substrate, such as poly(methyl meth)acrylate (PMMA), polycarbonate, polyethylene terephthalate (PET), polyolefin, polyvinyl chloride (PVC), or mixtures thereof. A substrate is considered transparent when T is greater than 10%, or greater than 20%, or greater than 30%.

[0025] In the most preferred cases, the transparent substrate is a glass substrate.

[0026] The glass may be of any type, such as conventional float glass or flat glass, and may be of any composition having any optical property, such as any value of visible transmittance, ultraviolet transmittance, infrared transmittance, and / or total solar energy transmittance greater than 10%.

[0027] The glass substrate may be soda-lime glass, borosilicate glass, lead glass, or aluminosilicate glass. The substrate may be a regular clear, tinted, or ultra-clear (i.e., lower Fe content and higher transmittance) glass substrate. Further examples of glass substrates include clear, green, bronze, or blue-green glass substrates.

[0028] The glass may be annealed glass, tempered glass, or heat strengthened glass.

[0029] The transparent glass substrate can have a thickness ranging from 0.5 mm to about 15 mm, alternatively from 1 mm to about 10 mm, alternatively from 1 mm to about 8 mm.

[0030] A transparent glass substrate may be considered suitable for the present invention if it has a thickness in the range of 0.5 to 2 mm.

[0031] The transparent substrate typically has two major opposed first and second surfaces, with at least a portion of the first surface provided with a functional coating.

[0032] The topcoat is deposited over and in contact with at least a portion of the functional coating provided on at least one surface of the transparent substrate to protect said functional coating from mechanical and / or chemical damage during transportation, storage, handling, processing and / or end use.

[0033] The second surface of the transparent substrate can be coated with the same or a different functional coating, in which case the protective topcoat of the present invention can also be applied over the functional coating applied to the second surface.

[0034] Within the scope of the present invention, the term "functional coating" refers to a coating that changes one or more physical properties of a substrate, such as optical, thermal, chemical, or mechanical properties. Such functional coatings are not intended to be removed from the substrate during subsequent processing. Functional coatings are typically permanent or "non-removable" coatings.

[0035] The functional coating on the first surface, and optionally on the second surface, may independently be a solar control coating, a conductive coating, an anti-reflective coating, a decorative coating, and / or a low-emissivity coating.

[0036] The functional coating may be a single layer or a stack of thin layers, i.e., a multi-layer functional coating, and may include one or more metals, non-metals, semi-metals, dielectrics, semiconductors, or alloys, compounds, composites, combinations, or blends thereof.

[0037] When discussing a stack of thin layers in the present invention, it is understood that typically a first layer is first attached onto the substrate, and then a second layer is attached on top of the first layer on the substrate, with the sequential order of positions being considered proceeding from the substrate to the top layer.

[0038] Within the scope of the present invention, the terms "lower", "bottom" and "lower" refer to the relative position of a layer facing the next layer in the layer sequence starting from the substrate. Within the scope of the present invention, the terms "upper" and "upper" refer to the relative position of a layer facing the next layer in the layer sequence starting from the substrate.

[0039] Within the scope of the present invention, the relative positions of layers in a stack do not necessarily indicate direct contact between the layers. That is, there may be some intermediate layer between the first and second layers. For example, a first layer "deposited on" a substrate does not exclude the presence of one or more other coating layers of the same or different composition located between the film of the first layer and the substrate, unless the object of the present invention is compromised.

[0040] In some cases, a layer may actually be made up of several individual layers.

[0041] The topcoat is understood to be in an upper position relative to the functional coating disposed on the first surface of the transparent substrate, i.e., the topcoat is located furthest from the transparent substrate relative to the first deposition surface of the substrate, and is typically in contact with air.

[0042] The topcoat is the top layer over the functional coating, excluding any non-permanent layers, and is in direct contact with the last layer of said functional coating. In most cases, the last layer of the functional coating does not provide mechanical and / or chemical durability. In such cases, the topcoat provides the mechanical and chemical durability of the functional coating.

[0043] The present topcoat is not intended to be removed and thus is not considered a removable or non-permanent protective layer.

[0044] In some cases, the functional coating may include a top layer that itself provides some degree of mechanical and / or chemical durability. In such cases, the topcoat provides the functional coating with even greater mechanical and chemical durability, particularly in view of abrasion.

[0045] The functional coating may have a thickness in the range of 10 to 1000 nm.

[0046] Unless otherwise stated, all layer thicknesses herein are geometric layer thicknesses.

[0047] In some embodiments of the present invention, the functional coating may be a solar control coating, where the solar control coating includes coatings that reflect or absorb visible, infrared, and / or ultraviolet energy.

[0048] In some embodiments of the present invention, the functional coating may be an electrically conductive coating, for example, an electrically conductive heated window coating, or a single or multi-film coating that can function as an antenna.

[0049] The functional coating may be a low emissivity coating that is typically capable of transmitting visible wavelength energy, e.g., from about 400 nm to about 780 nm, but reflecting shorter wavelength solar and / or thermal infrared energy, typically intended to improve the insulating properties of architectural glazing. "Low emissivity" means an emissivity of less than about 0.3, alternatively less than about 0.2.

[0050] The functional coating may be a single layer metal oxide coating, a multi-layer metal oxide coating, a non-metal oxide coating, or a multi-layer functional coating.

[0051] In certain embodiments of the invention, the single layer metal oxide coatings include coatings including zinc oxide doped with aluminum, gallium, or hafnium; mixed oxides of zinc and tin; tin oxide optionally doped with fluorine or antimony; indium oxide optionally doped with tin, and the like.

[0052] In some embodiments of the present invention, the multilayer metal oxide coating includes a coating comprising at least one layer of a material with a high refractive index and at least one layer of a material with a low refractive index, i.e. a coating having layers of materials with alternating refractive indices. Such coatings are typically represented as coatings comprising a first layer of a material with a low or high refractive index, a second layer of a material with a high or low refractive index, a third layer of a material with a low or high refractive index, a fourth layer of a material with a high or low refractive index, and an optional protective layer. A low refractive index is typically a refractive index <1.7, or typically <1.6, while a high refractive index is typically a refractive index >1.8, or typically ≧1.9 or ≧2.0. Some layers may have an intermediate refractive index comprised between 1.7 and 1.8. The refractive index is typically considered at a wavelength of 550 nm.

[0053] In one embodiment of the invention, the functional coating may be a multi-layer functional coating comprising an alternating arrangement of n infrared-reflective (IR) layers and n+1 dielectric layers, such that each IR layer is surrounded by two dielectric layers, where n≧1.

[0054] The IR layer may be made of silver, gold, palladium, platinum, or alloys thereof. The IR layer may have a thickness of 2-30 nm, alternatively 5-20 nm, alternatively 7-18 nm. These thickness ranges allow for good light transmission while still achieving the desired low emissivity and / or solar control functionality and / or conductivity.

[0055] The dielectric layer may typically comprise an oxide, nitride, oxynitride, or oxycarbide of Zn, Sn, Ti, Zr, Si, In, Al, Bi, Ta, Hf, Mg, Nb, Y, Ga, Sb, Mg, Cu, Ni, Cr, Fe, B, or mixtures thereof.

[0056] In some embodiments of the present invention, the dielectric layer may comprise an oxide, nitride, oxynitride, or oxycarbide of Zn, Sn, Ti, Zr, Si, In, Al, Nb, Sb, Ni, Cr, or mixtures thereof, or the dielectric layer may comprise an oxide, nitride, or oxynitride of Zn, Sn, Ti, Zr, Si, In, Al, Nb, Sb, Ni, Cr, or mixtures thereof.

[0057] These materials can finally be doped, with examples of dopants including aluminum, zirconium, or mixtures thereof. The dopant or mixture of dopants can be present in an amount up to 15% by weight.

[0058] Typical examples of dielectric materials include, but are not limited to, silicon-based oxides, silicon-based nitrides, zinc oxide, tin oxide, mixed zinc tin oxides, silicon nitride, silicon oxynitride, titanium oxide, aluminum oxide, zirconium oxide, niobium oxide, aluminum nitride, bismuth oxide, mixed zirconium silicon nitrides, and mixtures of at least two thereof, such as zirconium titanium oxide.

[0059] The dielectric layer may be comprised of multiple individual layers consisting essentially of the above materials.

[0060] The dielectric layers may each have a thickness in the range of 0.1 to 200 nm, alternatively 0.1 to 150 nm, alternatively 1 to 120 nm, alternatively 1 to 80 nm. The different dielectric layers may have different thicknesses, i.e. a first dielectric layer may have a thickness that is the same or different, greater or less than the thickness of a second or third or any other dielectric layer.

[0061] When there are two IR layers (n=2), the second dielectric layer can be called the "internal dielectric layer" since it is sandwiched between the two IR layers.

[0062] When there are three IR layers (when n=3), the second and third dielectric layers can be referred to as "internal dielectric layers" since they are each sandwiched between two IR layers.

[0063] The multi-layer functional coating may include a seed layer under at least one IR layer and / or the coating may include a barrier layer over at least one IR layer. The seed layer is typically provided to promote the formation of a good quality film of the IR material, i.e. to obtain a uniform and stable layer of the IR material. The barrier layer is typically provided to promote the protection of the IR material from degradation induced by the formation of any layer thereon, for example from oxygen or oxygen-containing species that may degrade the quality of the IR layer, and also from degradation due to heat treatment.

[0064] A given IR layer may be provided with either a seed layer or a barrier layer, or both. A first IR layer may be provided with either a seed layer and a barrier layer, a second IR layer may be provided with either a seed layer and a barrier layer, and so on. Such configurations are not mutually exclusive. The seed layer and / or barrier layer may have a thickness of 0.1 to 35 nm, alternatively 0.5 to 25 nm, alternatively 0.5 to 15 nm, alternatively 0.5 to 10 nm.

[0065] The multi-layer functional coating may also include a thin layer of a sacrificial material having a thickness of <15 nm, or <9 nm, disposed over and in contact with at least one IR layer. Examples of sacrificial materials include titanium, zinc, nickel, chromium, oxides of Ni, oxides of Ni alloys, oxides of Cr, oxides of Cr alloys, NiCrO. x , NiCrO x N y , zinc oxide, tin oxide, or other suitable materials, or mixtures thereof.

[0066] A controlled absorbing layer can be applied to the dielectric layer to selectively change the transmittance of the coated article. In some instances, the thickness of the absorbing layer can be controlled to significantly control the transmittance of the coated article without adversely affecting color. Examples of absorbing layers include Ni, Cr, NiCr, NiCrN, and NiCrN. x , NiCrW, CrN, ZrN, TiN, Ti, Zr, NiO x Such an absorbing layer can be arranged such that at least one IR layer is located above the absorbing layer, and optionally such an absorbing layer can be sandwiched between and in contact with first and second layers comprising silicon nitride. The absorbing layer can have a thickness in the range of 0.5 to 10 nm.

[0067] The multilayer functional coating may optionally already include a top layer comprising an oxide of Ti, Zr, or a mixed oxide of Ti and Zr with 45-65 wt.% Ti; or an oxide of Si, Al; or an oxide of Zr and Al; or a nitride of Si, Al. Such a top layer may be replaced by the present top coat or the present top coat may be applied on top of such a top layer.

[0068] A first example of a multilayer functional coating that functions as a low-emissivity coating includes at least one silver layer and includes the sequence Substrate / MeO / ZnO:AlSi / Ag / AlSi-MeO, where MeO is a metal oxide such as SnO2, TiO2, In2O3, Bi2O3, ZrO2, Ta2O5, SiO2, or Al2O3, or a mixture thereof.

[0069] A second example of a multi-layer functional coating that functions as a low-emissivity coating includes a first dielectric layer comprising silicon nitride; a first layer comprising Ni or NiCr; an infrared (IR) reflective layer comprising silver; a second layer comprising Ni or NiCr; and a second dielectric layer comprising silicon nitride. Such a multi-layer functional coating can optionally include a topcoat of mixed (oxy)nitrides of SiZr or mixed oxides of TiZr.

[0070] A third example of a multi-layer functional coating is an infrared (IR) reflective layer in contact with and sandwiched between the first and second layers, the second layer comprising NiCrOx; At least the second layer, which comprises NiCrOx, is graded oxidized such that a first portion of the second layer proximate the infrared (IR) reflective layer is less oxidized than a second portion of the second layer remote from the infrared (IR) reflective layer.

[0071] A fourth example of a multilayer functional coating includes: a dielectric layer; a first layer including zinc oxide positioned on the dielectric layer; an infrared (IR) reflective layer including silver positioned on and in contact with the first layer including zinc oxide; a layer including an oxide of NiCr positioned on and in contact with the IR reflective layer; a second layer including zinc oxide positioned on and in contact with the layer including an oxide of NiCr; and another dielectric layer positioned on the second layer including zinc oxide.

[0072] A fifth example of a multilayer functional coating includes: a first dielectric layer; a first infrared (IR) reflective layer comprising silver positioned on at least the first dielectric layer; a first layer comprising zinc oxide positioned on at least the first IR reflective layer and the first dielectric layer; a second IR reflective layer comprising silver positioned on and in contact with the first layer comprising zinc oxide; a layer comprising an oxide of NiCr positioned on and in contact with the second IR reflective layer; a second layer comprising zinc oxide positioned on and in contact with the layer comprising an oxide of NiCr; and another dielectric layer positioned on at least the second layer comprising zinc oxide.

[0073] A sixth example of a multilayer functional coating comprises: a first dielectric layer; a first layer comprising zinc oxide located on the dielectric layer; an infrared (IR) reflective layer comprising silver located on and in contact with the first layer comprising zinc oxide; a second layer comprising zinc oxide located on the IR layer; and a second dielectric layer located on the second layer comprising zinc oxide. The first and second dielectric layers can comprise several layers, in particular layers of different compositions in zinc oxide, i.e. layers of zinc oxide, zinc oxide doped with aluminum, or layers of mixed oxides of zinc and tin with a ratio Sn / Zn in the range of 0.5-2 by weight or a ratio Sn / Zn in the range of 0.02-0.5 by weight; layers of silicon nitride; layers of titanium oxide. The first and second layers comprising zinc oxide can also have different compositions in zinc oxide, i.e. layers of zinc oxide, zinc oxide doped with aluminum, mixed oxides of zinc and tin, mixed oxides of zinc, titanium, and aluminum.

[0074] A seventh example of a multilayer functional coating comprises, in order: a first dielectric layer; a first IR layer comprising silver; a second dielectric layer; a second IR layer; a third dielectric layer. The first, second and third dielectric layers can comprise several layers, in particular layers of different compositions in zinc oxide, i.e. layers of zinc oxide, zinc oxide doped with aluminum or layers of mixed oxides of zinc and tin with a ratio Sn / Zn in the range of 0.5-2 by weight or a ratio Sn / Zn in the range of 0.02-0.5 by weight; layers of mixed oxides of zinc, titanium and aluminum; layers of silicon nitride; layers of titanium oxide. In some cases, the IR layer can be provided independently with a metallic barrier layer, such as Ti, Ni, NiCr, etc.

[0075] An eighth example of a multilayer functional coating comprises, in order: a first dielectric layer; a first IR layer comprising silver; a second dielectric layer; a second IR layer; a third dielectric layer; a third IR layer; a fourth dielectric layer. The first, second, third and fourth dielectric layers can comprise several layers, in particular layers of different compositions in zinc oxide, i.e. layers of zinc oxide, zinc oxide doped with aluminum or layers of mixed oxides of zinc and tin with a ratio Sn / Zn in the range of 0.5-2 by weight or a ratio Sn / Zn in the range of 0.02-0.5 by weight; layers of mixed oxides of zinc, titanium and aluminum; layers of silicon nitride; layers of titanium oxide. In some cases, the IR layer can be provided independently with a metallic barrier layer, such as Ti, Ni, NiCr, etc.

[0076] A wide variety of multi-layer functional coatings can be provided with the coated substrate and benefit from the topcoat that provides protection against mechanical damage, while the optical properties such as light transmission, light reflection, and color remain within acceptable limits of change compared to the coating without the topcoat, i.e., Delta T TC <2%, Delta R TC <2% and Delta E * TC <5, where "TC" is the selected optical parameter (T, R, or delta E) of the functional coating. * ) is related to the effect that the topcoat may have on the

[0077] The method for producing the coated substrate is as follows: 1. Providing a transparent substrate having two major opposed first and second surfaces; 2. Depositing a functional coating on at least a portion of a first surface of a transparent substrate; 3. In contact with the functional coating, at least TiO y , ZrO z and optionally SiO xdepositing a topcoat comprising a mixed metal oxide comprising: The top coat is 8-49 atomic percent titanium, 51 to 92 atomic percent zirconium, 0-9 atomic % silicon, %, totalling 100 atomic % metals, the topcoat having a thickness of 0.1 to 10 nm; At least

[0078] The deposition step of the topcoat using magnetron sputtering allows the process to be easily integrated into existing manufacturing lines that first apply functional coatings onto transparent substrates. Magnetron deposition can also deposit topcoat layers having thicknesses of 0.1-10 nm. Such thin layers have been found to be effective in imparting the necessary mechanical durability without adversely affecting the chemical and optical properties of the functional coating.

[0079] Functional coatings can typically be deposited on substrates by chemical vapor deposition (CVD), atmospheric pressure CVD (APCVD), low pressure CVD (LPCVD), plasma enhanced chemical vapor deposition (PECVD), LPCVD (low pressure chemical vapor deposition), physical vapor deposition, magnetron sputtering, ion assisted deposition.

[0080] The individual layers of the same functional coating may be formed by different deposition methods, but typically they are deposited using the same technique.

[0081] In some cases, at least one layer of the functional coating can be deposited by magnetron sputtering. In some cases, all layers of the functional coating are deposited by magnetron sputtering.

[0082] The protective topcoat of the present invention is deposited using magnetron sputtering. Compared to CVD or sol-gel methods, the efficiency of the topcoat for mechanical and chemical durability is optimized when deposited by magnetron sputtering. Layers deposited by magnetron sputtering are available in thicknesses ranging from 0.1 to 10 nm, alternatively 0.5 to 5.0 nm, alternatively 2.0 to 5.0 nm, without prior heating or additional steps. Layers deposited in this manner have low delta T values ​​without significantly affecting the optical properties of the functional coating. TC <2%, Delta R TC <2% and Delta E * TC <5, where "TC" is the selected optical parameter (T, R, or delta E) of the functional coating. * ) is related to the effect that the topcoat may have on the

[0083] Deposition of the topcoat using magnetron sputtering can be carried out using either metallic or ceramic targets to obtain at least three elements of titanium, zirconium, or silicon.

[0084] The at least three elements can be supplied independently from either one or more ceramic or metallic targets. A topcoat deposited by magnetron sputtering on the functional coating comprises at least TiO. y , and ZrO z and optionally SiO x where x, y, and z are in the range of 1.8 to 2.2, The top coat is 8-49 atomic percent titanium, 51 to 92 atomic percent zirconium, 0-9 atomic % silicon, There can be various combinations and co-sputtering alternatives, provided that the total is 100 atomic % metal and the topcoat has a thickness of 0.1-10 nm.

[0085] As discussed above, impurities may be present in the topcoat as a result of impurities present in the selected target. The composition of the topcoat includes impurities in an amount that totals 100 atomic %. However, the effective content of the topcoat only takes into account the amounts of titanium, zirconium, and optional silicon.

[0086] The metal target may include at least one of titanium, zirconium, or silicon. The metal target may include two or more of titanium, zirconium, or silicon.

[0087] The ceramic target can include at least one oxide of titanium, zirconium, or silicon. The ceramic target can include two or more oxides of titanium, zirconium, or silicon.

[0088] The ceramic target can include two elements selected from titanium, zirconium, or silicon, and the metal target can include a third element.

[0089] In some cases, one element of the sputtered topcoat can be obtained from both a ceramic target and a metallic target simultaneously.

[0090] The ceramic target can include at least one oxide of a metal and a metallic form of at least one other metal.

[0091] The ceramic target may include at least one oxide of titanium or zirconium and silicon in metallic form.

[0092] In such cases, the three elements can be obtained from multiple independent targets used in combination, also known as co-sputtering, with each target being either a ceramic or a metallic target.

[0093] Sputtering or deposition from two or more targets has the advantage that different topcoats, including at least silicon, titanium, and zirconium, can be obtained that can be adjusted for the desired mechanical durability. It also has the advantage that the deposition rate can be adjusted and / or the target can be easily exchanged from one target to another depending on the material consumed during the process. It also has the advantage that the stoichiometry of the topcoat can be adjusted as a function of the gas used during sputtering.

[0094] In another case, the three elements Ti, Si and Zr can be obtained from one target.

[0095] The ceramic target may contain oxides of at least the three elements Ti, Si and Zr, or the metallic target may contain at least the three elements in metallic form.

[0096] The ceramic target may include oxides of titanium and zirconium, and silicon in metallic form.

[0097] Sputtering or deposition from one target containing at least silicon, titanium, and zirconium has the advantage of providing a reproducible and uniform topcoat.

[0098] The topcoat is typically sputtered in a gas flow containing argon or oxygen or both. Various mixtures of each gas can be obtained to obtain the required stoichiometry of the topcoat.

[0099] An additional advantage of the present topcoat is that it can be heat treated, thereby protecting the functional coating from such heat treatment.

[0100] Since the topcoat itself provides protection even in the absence of heat treatment, the heat treatment step is only optional and is considered as necessary for the end use of the coated substrate.

[0101] The method for producing a heat-treated coated substrate comprises, in order: 1. Providing a transparent substrate having two major opposed first and second surfaces; 2. Depositing a functional coating on at least a portion of a first surface of a transparent substrate; 3. In contact with the functional coating, at least TiO y and ZrO z and optionally SiO x depositing a topcoat comprising a mixed metal oxide comprising: The top coat is 8-49 atomic percent titanium, 51 to 92 atomic percent zirconium, 0-9 atomic % silicon, %, totalling 100 atomic % metals, the topcoat having a thickness of 0.1 to 10 nm; 4. Heat treatment of the coated substrate; At least

[0102] In some embodiments of the method that are compatible with other embodiments of the invention, the above ranges of Ti, Zr, and Si in the topcoat can be varied independently of each other. Alternatively, the amount of Ti can be in the range of 10-47 atomic %, or alternatively, 12-46 atomic %. Alternatively, the amount of Zr can be in the range of 53-90 atomic %. Alternatively, the amount of Si can be in the range of 1-8 atomic %, or alternatively, 2-7 atomic %. Thus, these amounts can be varied independently for each metal, provided that the total is 100 atomic % metal, including impurities.

[0103] Within the scope of the present invention, when steps are presented in a sequence, it is intended to mean that they are performed in the order stated. However, additional intermediate steps can be added within the sequence. Such additional intermediate steps can be cleaning, transporting, moving, measuring, cutting, etc.

[0104] The heat treatment may be one of bending (also known as curving), annealing (also known as tempering), or occurring during a tempering process.

[0105] One suitable heat treatment involves heating the coated glass sheet in air to a temperature of at least 560°C, for example between 560°C and 700°C, in particular about 640°C to 670°C, for about 3, 4, 6, 8, 10, 12, or even 15 minutes, depending on the type of heat treatment and the thickness of the glass sheet. This treatment can include a rapid cooling step after the heating step to generate a stress difference between the surface and the center of the glass, so that this so-called tempered glass sheet breaks safely into small pieces in the event of an impact. If the cooling step is not too intense, the glass is simply thermally strengthened, which in any case results in better mechanical resistance.

[0106] Further heat treatments may be indicated in process steps such as 1) bending, 2) tempering, 3) sintering of colored ceramic prints or silver busbar prints, 4) vacuum sealing of vacuum double glazing, and 5) firing of wet-applied low-reflection or anti-glare coatings.

[0107] The first method for producing a double-sided coated substrate comprises, in order: 1. Providing a transparent substrate having two major opposed first and second surfaces, the first surface being exposed; 2. Depositing a first functional coating on at least a portion of a first surface of a transparent substrate; 3. Over and in contact with the first functional coating, deposit at least TiO y and ZrO z and optionally SiO x depositing a first topcoat comprising a mixed metal oxide comprising: The first top coat is 8-49 atomic percent titanium, 51 to 92 atomic percent zirconium, 0-9 atomic % silicon, %, totalling 100 atomic % metals, the first topcoat having a thickness of 0.1 to 10 nm; 4. Optionally turning the substrate over so that the second surface is exposed; 5. Depositing a second functional coating onto at least a portion of the second surface of the transparent substrate to form a double-sided coated transparent substrate; 6. Optionally depositing a second topcoat; 7. Optionally subjecting the double-sided coated transparent substrate to a heat treatment; At least

[0108] The second method for producing a double-sided coated substrate comprises, in order: 1. Providing a transparent substrate having two major opposed first and second surfaces, the first surface being exposed; 2. Depositing a first functional coating on at least a portion of a first surface of a transparent substrate; 3. Over and in contact with the first functional coating, deposit at least TiO y and ZrO z and optionally SiO x depositing a first topcoat comprising a mixed metal oxide comprising: The first top coat is 8-49 atomic percent titanium, 51 to 92 atomic percent zirconium, 0-9 atomic % silicon, %, totalling 100 atomic % metals, the topcoat having a thickness of 0.1 to 10 nm; 4. Optionally turning the substrate over so that the second surface is exposed; 5. Depositing a second functional coating onto at least a portion of the second surface of the transparent substrate to form a double-sided coated transparent substrate; 6. Optionally, over and in contact with the second functional coating, at least TiO y and ZrO z and optionally SiO x depositing a second topcoat comprising a mixed metal oxide comprising: The second top coat is 8-49 atomic percent titanium, 51 to 92 atomic percent zirconium, 0-9 atomic % silicon, %, totalling 100 atomic % metals, the topcoat having a thickness of 0.1 to 10 nm; 7. Optionally subjecting the double-sided coated transparent substrate to a heat treatment; At least

[0109] Thus, such first and second methods can provide a transparent substrate having a first functional coating disposed on at least a portion of a first surface and a second functional coating disposed on at least a portion of a second surface, the first and optionally second functional coatings being provided with a protective topcoat of the present invention.

[0110] In such a situation, the first and second functional coatings may be the same or different, and are in particular selected from the functional coatings mentioned above.

[0111] The present topcoats prove to be further useful in that they provide a functional coating that has sufficient mechanical durability to allow coating on a second, opposite surface of the transparent substrate.

[0112] In some cases, consistent with the alternative methods described above, the heat treatment step can occur before or after the optional flipping step, i.e., the coated transparent substrate can be heat treated before applying the second functional coating.

[0113] The present invention therefore also provides a heat treated coated glazing comprising a functional coating and a magnetron sputtered mixed metal oxide topcoat comprising at least titanium, zirconium and silicon, the topcoat comprising at least TiO y and ZrO z and optionally SiO x (where x, y, and z are in the range of 1.8 to 2.2), The top coat is 8-49 atomic percent titanium, 51 to 92 atomic percent zirconium, 0-9 atomic % silicon, It is 100 atomic % metal including impurities, The topcoat has a thickness of 0.1 to 10 nm.

[0114] The functional coating and / or coated substrate can be referred to as "heat treatable" or "temperable" if the coated substrate can withstand a tempering or bending type of heat treatment without impairing the optical and / or energetic properties of the substrate as manufactured.

[0115] In some cases, the functional coating may be "self-matchable," meaning that there is no or only minimal change in optical and / or energetic properties when the coated substrate is subjected to a tempering or bending type heat treatment.

[0116] Typically, CIELAB 1976 values ​​(L * a * b * ) are used. These are measured using illuminant D65 / 10°.

[0117] TIFF2024536031000001.tif13170 represents the color change during heat treatment, i.e., the color difference between before and after heat treatment.

[0118] ΔE in transmission and reflection * HT ≦5, or ≦2, and / or there is no or little change in the values ​​of light transmission (T) and reflection (R) and energy, i.e. T before and after heat treatment in one glazing. HT , R HT , and color values ​​remain ≦5, or ≦2, where “HT” represents the difference between the selected optical parameters (T, R, or delta E) of the functional coating on which the topcoat is applied. * ) is related to the effect that heat treatment can have on the

[0119] If the functional coating is self-compatible, the present topcoat does not alter the self-compatibility of such functional coating disposed underneath.

[0120] This has the advantage that non-heat-treated and heat-treated products can be placed next to each other in the same application, for example on the exterior of a building, and also has the advantage that a topcoat can be provided only on the heat-treated or only on the non-heat-treated products, while self-compatibility as defined is guaranteed between the non-heat-treated and heat-treated products.

[0121] The topcoat is considered to be in contact with the ambient environment furthest from the substrate. Only in certain cases consistent with the other aspects of the present invention, the coated substrate may further be provided with at least one temporary protective layer over and in contact with the topcoat. As explained below, such "temporary" protective layers are typically removed by washing or heat treatment of the substrate.

[0122] In some embodiments of the present invention, the temporary protective layer includes a carbon temporary protective layer, a polymer temporary protective layer, a peelable protective layer.

[0123] Carbon protective layers include layers deposited by magnetron sputtering having a thickness typically between 0.5 and 15 nm, alternatively between 1 and 10 nm, alternatively between 1 and 7 nm, etc. Such carbon protective coatings are typically removed by heat treatment of the transparent substrate, for example at a rate of 99-100% removal as measured by colorimetric methods.

[0124] Polymeric temporary protective layers include layers provided by the products of evaporation or reaction of polymeric coating compositions including polyvinyl alcohol, polyethylene, acrylics, etc., which can be subsequently removed by aqueous washing, solvent washing, vapor stripping, pyrolysis, or combustion. Such polymeric coating compositions can be liquid solutions, emulsions, suspensions, slurries, or dispersions.

[0125] The peelable protective layer may include a coating formed from a polyamide liquid composition.

[0126] The temporary protective coating can be removed, for example, by washing, burning, pyrolysis, or stripping. Before or after removal of the temporary protective coating, the substrate can be processed, for example, cut, trimmed, bent, shaped, and / or incorporated into an article of manufacture.

[0127] Thus, any of the above methods may further comprise the step of depositing a carbon layer on the coated substrate.

[0128] The carbon protective topcoat has the advantage that it can also be deposited by sputtering methods and therefore can be included in the same process without significant technical constraints.

[0129] The present invention provides a multi-layer glazing unit comprising at least one coated substrate as described in the various embodiments above.

[0130] Multi-layer glazing units include double or triple glazing or laminated glazing, in which the coating substrate is associated with one or more other glass sheets, which may or may not be coated. The surfaces of double glazing are typically designated as follows: P1 is the surface of the outer glass sheet, which faces the exterior; P2 is the surface of the outer glass sheet, which faces the interior space between the two glass sheets; P3 is the surface of the inner glass sheet, which faces the interior space between the two glass sheets; P4 is the surface of the inner glass sheet, which faces the interior. Such nomenclature is also applicable to laminated glazing.

[0131] The covering surface of the glazing can be placed in contact with the space between the two glass sheets in the case of double glazing, or in contact with the contact layer in the case of laminated glazing (P2 or P3).

[0132] Due to its mechanical and chemical resistance, the coated surface of the coated substrate before being incorporated into the multi-layer glazing unit does not necessarily need to be edge-removed, but can even be placed on the outer surface of the multi-layer glazing unit, i.e. facing and in contact with the external or internal environment of the building or vehicle (P1 or P4), to obtain sufficient mechanical and chemical resistance therefor. Thus, a stack of thin layers can be provided on the surface of the glass substrate facing the interior of the building or vehicle (P2 for one non-laminated glass sheet, or P4 for laminated glass or double glazing units). In some cases, the coating stack can be placed in contact with the exterior (P1).

[0133] The coated substrates of the present invention may be useful in architectural glazing (doors, windows, display cabinets, insulated glass (IG) window units, etc.), appliance applications (refrigerator doors, oven doors, etc.), and transportation applications (vehicle windows, skylights, windshields, side windows), where there is an increasing need for glass with very pronounced curvatures and / or complex shapes (double curvature, S-curve, etc.).

[0134] In some cases, the coated substrate can be toughened. As a result of its safety and strength, toughened glass is used in a variety of demanding applications such as windows, shower doors, architectural glass doors and tables, refrigerator trays, as a component of bulletproof glass, and in various types of dishes and cooking utensils.

[0135] Thus, the coated substrates are durable, i.e., able to withstand certain chemical and / or mechanical tests, as described below, in some cases both before and after optional heat treatment. Optical parameters can be optimized without losing the durability provided by the functional coatings applied onto the coated substrates claimed herein.

[0136] "Chemical durability" or "chemically durable" is used herein synonymously with the terms "chemical stability" or "chemical resistance."

[0137] "Mechanical durability" or "mechanically durable" is used herein synonymously with the terms "mechanical stability" or "mechanical resistance."

[0138] The present invention provides the use of a topcoat of a transparent substrate provided with a functional coating, wherein the topcoat comprises at least TiO y and ZrO z and optionally SiO x where x, y, and z are in the range of 1.8 to 2.2; The top coat is 8-49 atomic percent titanium, 51 to 92 atomic percent zirconium, 0-9 atomic % silicon, and wherein the topcoat is 0.1 to 10 nm thick; and increases durability by increasing abrasion resistance by at least 20%, alternatively by at least 30%, alternatively by at least 40%.

[0139] Durability is evaluated using the wear test described in the Examples section below.

[0140] In some embodiments of this use, consistent with other embodiments of the present invention, the above ranges of Ti, Zr, and Si in the topcoat can be varied independently of one another. Alternatively, the amount of Ti can range from 10 to 47 atomic %, or alternatively, from 12 to 46 atomic %. Alternatively, the amount of Zr can range from 53 to 90 atomic %. Alternatively, the amount of Si can range from 1 to 8 atomic %, or alternatively, from 2 to 7 atomic %. As discussed above, these amounts can be varied independently in the case of the metals, provided that the total is 100 atomic % metal, including impurities. EXAMPLES

[0141] Using the topcoat according to the present invention, different stacks of functional layers are made.In the following examples section, the composition of the topcoat is shown in atomic percent of the elements Ti, Zr and optional Si, the sum of which amounts to 100 atomic percent as the effective content specified.The effective content is therefore considered to be the sum of only the contributions of titanium, zirconium and optional silicon.The impurities present in the topcoat are therefore not listed, nor are their atomic percents shown.

[0142] Mechanical stability was evaluated by the following wear test method, well known to those skilled in the art.

[0143] The transparent substrate used in this example of glazing provided with one stack of thin layer stacks was a standard float soda lime, transparent, 4 mm thick and thoroughly cleaned prior to coating deposition.

[0144] Further tests of chemical durability were performed, such as the Cleveland test (3, 7 and 10 days), the climate chamber test (3, 7 and 10 days), the salt spray test (2, 5 and 10 days), etc. These results are not outlined in detail, as they were comparable to standard results obtained with top layers such as those in Comparative Examples 1 and 2 below.

[0145] Typical tests of mechanical durability were carried out, such as Automatic Wet Rub Test (AWRT-10, 50, 100, 250, 500 and 1000 cycles) or Dry Brush Test (250, 500, 1000 cycles). All were successfully passed, so the results are not summarized in detail, and the wear tests herein, which are exposed to more severe wear conditions, are carried out.

[0146] Measurements of the emissivity and aesthetics of the functional coating showed no effect from the topcoat.

[0147] Optical properties remain within acceptable limits of change and Delta T measured with a D65 / 2° illuminant when compared to functional coatings without topcoat TC <2%, Delta R TC <2% Delta E measured with D65 / 10° light source * TC <5.

[0148] Dry Brush Test The dry brush test (DBT) is performed according to standard ASTM D2486-00 (Test Method "A") for at least 250 cycles, alternatively at least 500 cycles, and here 1000 cycles. This test can also be performed on samples after they have been heat treated (referred to herein as "post-bake").

[0149] The results of each of the above tests are obtained by visual evaluation of the samples in comparison with a defined grade of a reference sample. The internal grade of the DBT test is set in the range of 0 to 10, with acceptable values ​​being 6 to 10. Typically, one value is the average of at least three samples in one experimental case. Comparative examples in the following table were made along with the examples according to the invention (set in the table below) as an internal validation of the procedure for each "round" of the experiment.

[0150] Abrasion Test The abrasion test is a dry abrasion test carried out as described in the standard ISO 11998:1998, and is carried out for at least 1000 cycles using a 900 g abrasive pad. In the present case, these cycles are carried out on dry feed without adding any liquid.

[0151] This test was also performed on samples after they had been subjected to a heat treatment (referred to herein as "baking"). Typical tests performed consider at least 250 cycles.

[0152] Test results are obtained by visual evaluation of the samples in comparison with a defined grade of a reference sample. An internal grade is set in the range of 0-10 for abrasion tests, with acceptable values ​​of 7-10. One value is typically the average of at least three samples from one experiment. Comparative examples in the table below were made according to the examples according to the invention (set in the table below) as an internal validation of the procedure of each "round" of experiments.

[0153] The present wear test provides more severe and abrasive conditions than the typical AWRT or dry brush tests known in the art.

[0154] The heat treatment conditions (or bake conditions) for DBT and wear testing involved placing the samples inside a convection oven at a temperature of 670° C. for 4-5 minutes.

[0155] In the table below: Ag stands for silver AZO2% represents a layer of zinc oxide doped with aluminum obtained from a ceramic target containing zinc oxide doped with 2% aluminum oxide by weight; SiN represents a layer of silicon nitride Si3N4, TiO is TiO n (n is 1.65-1.85), TZO has a ratio of 65 wt. % TiO2 and 35 wt. % ZrO2 (yielding 74 at. % Ti and 26 at. % Zr). x / ZrO2 composed of TiZrO x a layer of titanium-zirconium mixed oxide obtained from a ceramic target of ZnO represents a layer of zinc oxide without dopants obtained from a zinc metal target; ZSO5 represents a mixed zinc-tin layer obtained from a metal target containing 52 wt.% Zn and 48 wt.% Sn; The barrier layer (on top of and in contact with the silver layer) is made of 85-95% ZnO and TiO x ZnO:TiO with a ratio of 5-15 wt% and Al2O3 with a ratio of 1.5-3 wt%. x Zn:Ti:Al layer obtained from a ceramic target composed of Al2O3, resulting in a composition of Zn:Ti:Al of 86.3:10.4:3.3 atomic % in the contact layer. As a seed layer (below and in contact with the silver layer), ZTAO is a layer of zinc titanium aluminum oxide obtained from a metal target with the following ratios by weight: 88.8% Zn, 9.5% Ti, and 1.7% Al.

[0156] Unless otherwise stated, the standard deposition method for the seed layer is based on a gas flow of an 80 / 20 mixture of oxygen and argon. Silicon nitride was sputtered in a mixed gas flow of argon and N2 with sufficient N2 to obtain sufficient stoichiometry of Si3N4.

[0157] All thicknesses may have a thickness variation of <5% unless otherwise stated.

[0158] Examples 1 to 7 correspond to the sixth example of the multilayer functional coating including the above-mentioned IR layer.

[0159] Example 1 - Comparative Example C1 The following stacks were provided: Glass / ZSO5(17.1nm) / TZO(16.0nm) / ZnO(5.0nm) / Ag(10.5nm) / AZO(7.0nm) / ZSO5(16.1nm) / SiN(17.0nm) / Topcoat(4.0nm)

[0160] In Example 1, a topcoat was prepared according to one embodiment of the present invention using a ceramic target of 20 wt% TiOy and 80 wt% ZrOz to yield a topcoat containing 27.8 at.% Ti and 72.2 at.% Zr within the claimed ranges, as shown in Table 1, where y, z are in the range of 1.8-2.2.

[0161] In Comparative Example 1, the topcoat was a typical TiZrO topcoat (0 atomic % Si) as obtained in the art, sputtered using a ceramic target of 65 wt. % TiOy and 35 wt. % ZrOz.

[0162] The results shown in Table 1 clearly show that the best mechanical resistance is obtained with the glazing of Example 1. This topcoat improves durability by increasing the abrasion resistance by 65.0% (8.3 vs. 5.0) without adversely affecting the optical performance of the coating. TIFF2024536031000002.tif33170

[0163] Examples 2 and 3 and Comparative Example C2 The following stacks were provided: Glass / ZSO5(24.5nm) / ZTAO(9.0nm) / Ag(18.0nm) / ZTAO(5.0nm) / ZSO5(16.5nm) / SiN(20.0nm) / topcoat(5.0nm).

[0164] In Example 2, a topcoat was prepared according to one embodiment of the present invention using co-sputtering of a ceramic target of 20 wt% TiOy and 80 wt% ZrOz and a ceramic target of Si-ZrO2 with a ratio of 65(Si)-35(ZrO2) wt% to yield a topcoat containing Si, Ti, and Zr in atomic percent amounts within the claimed ranges, as shown in Table 2, where x, y, and z are in the range of 1.8 to 2.2.

[0165] In Example 3, a topcoat was prepared according to one embodiment of the present invention using a ceramic target of 20 wt% TiOy and 80 wt% ZrOz to yield a topcoat containing 27.8 at.% Ti and 72.2 at.% Zr within the claimed ranges, as shown in Table 2, where y, z are in the range of 1.8-2.2.

[0166] Comparative Example 2 was a typical TiZrO topcoat (0 atomic % Si) as obtained in the art, sputtered using a ceramic target of 65 wt % TiOy and 35 wt % ZrOz.

[0167] The inventive amounts of each of Si, Ti, and Zr in the mixed metal oxide topcoat can significantly improve the topcoat's performance in terms of abrasion resistance, both before and after baking, to levels not previously achievable.

[0168] The abrasion resistance is combined with comparable performance in all chemical durability tests, and there is no adverse effect on the optical performance of the coating. The increased abrasion resistance of Examples 2 and 3 over Comparative Example 1 as shown in Table 2 (abrasion resistance without baking) indicates that the topcoat improves durability. TIFF2024536031000003.tif46170

[0169] Example 4 and Comparative Examples C3 and C4 The following stacks were provided: Glass / ZSO5(24.5nm) / ZTAO(9.0nm) / Ag(18.0nm) / ZTAO(5.0nm) / ZSO5(16.5nm) / SiN(20.0nm) / topcoat(5.0nm).

[0170] In Example 4, a topcoat was prepared according to one embodiment of the present invention using co-sputtering of a TiOy ceramic target and a ZrOz ceramic target to obtain a topcoat containing 13.2 atomic % Ti and 86.8 atomic % Zr within the claimed ranges as shown in Table 3 (where y, z range from 1.8 to 2.2). The TiOy ceramic target contained aluminum oxide, which is considered here as an impurity and was not considered in the composition of the effective content of the topcoat. The TiOy and ZrOz ceramic targets contained less than 0.5 wt. % impurities and were not considered in the composition of the effective content of the topcoat.

[0171] Comparative Example 3 was a typical TiZrO topcoat (0 atomic % Si) as obtained in the art, sputtered using a ceramic target of 65 wt % TiOy and 35 wt % ZrOz.

[0172] Comparative Example 4 was a ZrO2 topcoat as obtained in the art, sputtered using a ceramic target of ZrOz, where z is in the range of 1.8 to 2.2.

[0173] The abrasion resistance is combined with comparable performance in all chemical durability tests, and there is no adverse effect on the optical performance of the coating. As shown in Table 3, this topcoat improves durability by increasing the abrasion resistance of Example 4 versus Comparative Example 3 (abrasion resistance without baking).

[0174] ZrO z Comparative Example 4, which only had ZrO, could not withstand the heat treatment, and both the DBT after baking and the wear resistance after baking were significantly reduced. z A small proportion of TiO y The addition of helps maintain high DBT resistance and high wear resistance after bake. TIFF2024536031000004.tif45170

[0175] Examples 5 and 6 - Comparative Example C5 The following stacks were provided: Glass / ZSO5(24.5nm) / ZnO(5.0nm) / Ag(17.4nm) / AZO(7.0nm) / ZSO5(21.0nm) / SiN(22.0nm) / top coat(4.0nm).

[0176] In Example 5, a topcoat was prepared according to one embodiment of the present invention using co-sputtering of a TiOy ceramic target and a ZrOz ceramic target to yield a topcoat containing 14.6 at. % Ti and 85.4 at. % Zr within the claimed ranges, as shown in Table 4, where y, z are in the range of 1.8-2.2.

[0177] In Example 6, a topcoat was prepared according to one embodiment of the present invention using a ceramic target of 35 wt% TiOy and 65 wt% ZrOz to yield a topcoat containing 45.4 at.% Ti and 54.6 at.% Zr within the claimed ranges, as shown in Table 4, where y, z are in the range of 1.8-2.2.

[0178] In Comparative Example 5, the topcoat was a typical TiZrO topcoat (0 atomic % Si) as obtained in the art, sputtered using a ceramic target of 65 wt. % TiOy and 35 wt. % ZrOz.

[0179] The results shown in Table 4 clearly show that better mechanical resistance is obtained with the glazings of Examples 5 and 6. This topcoat improves durability by increasing the abrasion resistance, without adversely affecting the optical performance of the coating. TIFF2024536031000005.tif38170

[0180] Example 7 - Comparative Example C6 The following stacks were provided: Glass / TiO(23.5nm) / ZnO(5.0nm) / Ag(11.8nm) / AZO(5.5nm) / ZSO5(16.0nm) / SiN(18.0nm) / Topcoat(4.0nm)

[0181] In Example 7, a topcoat was prepared according to one embodiment of the present invention using a ceramic target of 20 wt% TiOy and 80 wt% ZrOz to yield a topcoat containing 27.8 at.% Ti and 72.2 at.% Zr within the claimed ranges, as shown in Table 5, where y, z are in the range of 1.8-2.2.

[0182] In Comparative Example 6, the topcoat was a typical TiZrO topcoat (0 atomic % Si) as obtained in the art, sputtered using a ceramic target of 65 wt. % TiOy and 35 wt. % ZrOz.

[0183] The results clearly show that the best mechanical resistance is obtained with the glazing of Example 7. This topcoat improves durability by increasing the abrasion resistance by 34.3% (7.8 vs. 5.8) without adversely affecting the optical performance of the coating. TIFF2024536031000006.tif34170

[0184] Example 8 - Comparative Example C7 The following stacks were provided: Glass / ZSO5(24.5nm) / ZnO(5.0nm) / Ag(17.4nm) / AZO(7.0nm) / ZSO5(21.0nm) / SiN(22.0nm) / top coat(4.0nm).

[0185] In Example 8, a topcoat was prepared according to one embodiment of the present invention using a ceramic target of 20 wt% TiOy and 80 wt% ZrOz to yield a topcoat containing 27.8 at.% Ti and 72.2 at.% Zr within the claimed ranges, as shown in Table 6, where y, z are in the range of 1.8-2.2.

[0186] In Comparative Example 7, the topcoat was a typical TiZrO topcoat (0 atomic % Si) as obtained in the art, sputtered using a ceramic target of 65 wt. % TiOy and 35 wt. % ZrOz.

[0187] The results shown in Table 6 clearly show that the best mechanical resistance is obtained with the glazing of Example 8. This topcoat improves durability by increasing the abrasion resistance by 34.3% (8.0 vs. 5.9) without adversely affecting the optical performance of the coating. TIFF2024536031000007.tif33170

[0188] Example 9 and Comparative Example C8 The following stacks were provided: Glass / ZSO5(24.5nm) / ZTAO(9.0nm) / Ag(18.0nm) / ZTAO(5.0nm) / ZSO5(16.5nm) / SiN(20.0nm) / topcoat(5.0nm).

[0189] In Example 9, a topcoat was prepared according to one embodiment of the present invention using a ceramic target of 35 wt% TiOy and 65 wt% ZrOz to yield a topcoat containing 45.4 at.% Ti and 54.6 at.% Zr within the claimed ranges, as shown in Table 7, where y, z are in the range of 1.8-2.2.

[0190] Comparative Example 8 was a typical TiZrO topcoat (0 atomic % Si) as obtained in the art, sputtered using a ceramic target of 65 wt % TiOy and 35 wt % ZrOz.

[0191] The inventive amounts of each of Ti and Zr in the mixed metal oxide topcoat can significantly improve the performance of the topcoat with respect to abrasion resistance, both before and after baking, to previously unattained levels.

[0192] The abrasion resistance is combined with comparable performance in all chemical durability tests, and there is no adverse effect on the optical performance of the coating. As shown in Table 7, this topcoat improves durability by increasing the abrasion resistance of Example 9 versus Comparative Example 8 (abrasion resistance without baking). TIFF2024536031000008.tif43170

Claims

1. 1. A coated substrate comprising a transparent substrate having two major opposed first and second surfaces, at least one surface being provided with a functional coating, The transparent substrate is provided with at least TiO y and ZrO z , and optionally SiO x wherein x, y, z are in the range of 1.8 to 2.2; The top coat is - 8 to 49 atomic % titanium, - 51 to 92 atomic % zirconium, - 0 to 9 atomic % silicon, % metal, and the topcoat has a thickness of 0.1 to 10 nm.

2. 2. The coated substrate of claim 1, wherein the mixed metal oxide of the topcoat comprises 1 to 8 atomic percent silicon.

3. 2. The coated substrate of claim 1, wherein the mixed metal oxide of the topcoat comprises 10 to 35 atomic percent titanium.

4. 2. The coated substrate of claim 1, wherein the mixed metal oxide of the topcoat comprises 25 to 70 atomic percent zirconium.

5. The coated substrate of any one of claims 1 to 4, wherein the functional coating is a solar control coating, a conductive coating, an anti-reflective coating, a decorative coating, and / or a low emissivity coating.

6. The coated substrate of any one of claims 1 to 5, wherein the functional coating is a single layer metal oxide coating, a multi-layer metal oxide coating, a non-metal oxide coating, or a multi-layer functional coating.

7. 7. The coated substrate of claim 6, wherein the single layer metal oxide coating comprises zinc oxide doped with aluminum, gallium, or hafnium; mixed metal oxides of zinc and tin; tin oxide, optionally doped with fluorine or antimony; indium oxide, optionally doped with tin, and the like.

8. The coated substrate of claim 6 , wherein the multi-layer metal oxide coating comprises at least one layer of a high refractive index material and at least one layer of a low refractive index material.

9. 7. The coated substrate of claim 6, wherein the multilayer functional coating comprises an alternating sequence of n infrared-reflective (IR) layers and n+1 dielectric layers, such that each IR layer is surrounded by two dielectric layers, where n>1.

10. The multi-layer functional coating comprises: a. At least one silver layer, comprising the sequence: Substrate / MeO / ZnO:AlSi / Ag / AlSi-MeO, where MeO is SnO 2 , TiO 2 , In 2 O 3 , Bi 2 O 3 , ZrO 2 , Ta 2 O 5 , SiO 2 , or Al 2 O 3 or mixtures thereof; or b. a first dielectric layer comprising silicon nitride; a first layer comprising Ni or NiCr; an infrared (IR) reflective layer comprising silver; a second layer comprising Ni or NiCr; and a second dielectric layer comprising silicon nitride; or c. an infrared (IR) reflective layer in contact with and sandwiched between first and second layers, said second layer comprising NiCrOx; at least said second layer comprising NiCrOx is graded oxidized such that a first portion of said second layer proximate said infrared (IR) reflective layer is less oxidized than a second portion of said second layer remote from said infrared (IR) reflective layer; or d. a dielectric layer; a first layer comprising zinc oxide overlying the dielectric layer; an infrared (IR) reflective layer comprising silver overlying and in contact with the first layer comprising zinc oxide; a layer comprising an oxide of NiCr overlying and in contact with the IR reflective layer; a second layer comprising zinc oxide overlying and in contact with the layer comprising an oxide of NiCr; and another dielectric layer overlying the second layer comprising zinc oxide; or e. a first dielectric layer; a first infrared (IR) reflective layer comprising silver positioned on at least the first dielectric layer; a first layer comprising zinc oxide positioned on at least the first IR reflective layer and the first dielectric layer; a second IR reflective layer comprising silver positioned on and in contact with the first layer comprising zinc oxide; a layer comprising an oxide of NiCr positioned on and in contact with the second IR reflective layer; a second layer comprising zinc oxide positioned on and in contact with the layer comprising an oxide of NiCr; and another dielectric layer positioned on at least the second layer comprising zinc oxide; or f. a first dielectric layer; a first layer comprising zinc oxide overlying the dielectric layer; an infrared (IR) reflective layer comprising silver overlying and in contact with the first layer comprising zinc oxide; a second layer comprising zinc oxide overlying the IR layer; and a second dielectric layer overlying the second layer comprising zinc oxide; or g. comprising a first dielectric layer; a first IR layer comprising silver; a second dielectric layer; a second IR layer; a third dielectric layer, said first, second and third dielectric layers may comprise several layers; or h. The coated substrate of claim 9, comprising a first dielectric layer, a first IR layer comprising silver, a second dielectric layer, a second IR layer, a third dielectric layer, a third IR layer, and a fourth dielectric layer, wherein the first, second, third, and fourth dielectric layers can comprise several layers.

11. 11. The coated substrate of any one of claims 1 to 10, having a first functional coating on at least a portion of the first surface and a second functional coating on at least a portion of the second surface, at least one of the first or second functional coatings being provided with a topcoat of any one of claims 1 to 10.

12. 12. The coated substrate of any one of claims 1 to 11, further comprising at least one temporary protective layer, such as a carbon temporary protective layer, a polymer temporary protective layer, a peelable protective layer, provided over and in contact with the magnetron sputtered topcoat of mixed metal oxide.

13. 1. A heat-treated coated substrate comprising a transparent substrate having two opposing surfaces, at least one surface of which is provided with a functional coating, The transparent substrate is provided with at least TiO y and ZrO z and optionally SiO x wherein x, y, z are in the range of 1.8 to 2.2; The top coat is 8 to 49 atomic percent titanium, 51 to 92 atomic % zirconium, 0-9 atomic % silicon, %, totalling 100 atomic % metal, The coated substrate, wherein the topcoat has a thickness of 0.1 to 10 nm.

14. A multi-layer glazing unit comprising at least one coated substrate according to any one of claims 1 to 12.

15. 1. A method for producing a coated substrate comprising, in order:

1. Providing a transparent substrate having two major opposed first and second surfaces; 2. Depositing a functional coating onto at least a portion of the first surface of the transparent substrate; 3. At least TiO y and ZrO z and optionally SiO x depositing a topcoat comprising a mixed metal oxide comprising: The top coat is 8 to 49 atomic percent titanium, 51 to 92 atomic % zirconium, 0-9 atomic % silicon, %, totalling 100 atomic % metal, the topcoat having a thickness of 0.1 to 10 nm; The manufacturing method includes at least the steps of:

16. 1. A method for producing a heat treated coated substrate, comprising, in order:

1. Providing a transparent substrate having two major opposed first and second surfaces; 2. Depositing a functional coating onto at least a portion of the first surface of the transparent substrate; 3. At least TiO y and ZrO z and optionally SiO x depositing a topcoat comprising a mixed metal oxide comprising: The top coat is 8 to 49 atomic percent titanium, 51 to 92 atomic % zirconium, 0-9 atomic % silicon, %, totalling 100 atomic % metal, the topcoat having a thickness of 0.1 to 10 nm; 4. subjecting the coated substrate to a heat treatment; The manufacturing method includes at least the steps of:

17. 1. A method for producing a double-sided coated substrate comprising, in order:

1. Providing a transparent substrate having two major opposed first and second surfaces, the first surface being exposed; 2. Depositing a first functional coating onto at least a portion of the first surface of the transparent substrate; 3. A TiO y and ZrO z and optionally SiO x depositing a topcoat comprising a mixed metal oxide comprising: The top coat is 8 to 49 atomic percent titanium, 51 to 92 atomic % zirconium, 0-9 atomic % silicon, %, totalling 100 atomic % metal, the topcoat having a thickness of 0.1 to 10 nm; 4. Optionally turning the substrate over so that the second surface is exposed; 5. Depositing a second functional coating onto at least a portion of the second surface of the transparent substrate to form a double-sided coated transparent substrate; 6. Optionally, at least TiO y and ZrO z and optionally SiO xdepositing a topcoat comprising a mixed metal oxide comprising: The top coat is 8 to 49 atomic percent titanium, 51 to 92 atomic % zirconium, 0-9 atomic % silicon, %, totalling 100 atomic % metal, the topcoat having a thickness of 0.1 to 10 nm; 7. Optionally subjecting the double-sided coated transparent substrate to a heat treatment; The manufacturing method includes at least the steps of:

18. 18. The method according to any one of claims 15 to 17, wherein the deposition of the topcoat comprising at least silicon, titanium and zirconium by magnetron sputtering technique is carried out using either metallic or ceramic targets to obtain at least three titanium, zirconium or silicon elements.

19. 18. The method according to any one of claims 15 to 17, wherein the deposition of the topcoat comprising at least silicon, titanium and zirconium by magnetron sputtering technique is carried out using a ceramic target comprising oxides of titanium and zirconium and silicon in metallic form.

20. Use of a topcoat for a transparent substrate provided with a functional coating, the topcoat comprising at least TiO y and ZrO z and optionally SiO x where x, y, z are in the range of 1.8 to 2.2; The top coat is 8 to 49 atomic percent titanium, 51 to 92 atomic % zirconium, 0-9 atomic % silicon, %, totalling 100 atomic % metal, The top coat has a thickness of 0.1 to 10 nm. Use to improve durability by increasing abrasion resistance by at least 10%.

Citation Information

Patent Citations

  • ceramic glass item

    FR3093951A1

  • anti solar glazing

    JP2016513062A

  • Coated article having a protective coating comprising silicon nitride and / or silicon oxynitride

    JP2021513950A

  • Coated glazing

    WO2012110782A1

  • Laminated body and multi-layered glass

    WO2014109369A1