Laminated glass for automobiles

By employing glass plates with controlled compositional and thickness differences, the laminated glass achieves consistent bending and forming, improving optical quality and enabling efficient, cost-effective production of automotive laminated glass.

JP2024536262AActive Publication Date: 2024-10-04FUYAO GLASS IND GROUP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024519759
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-09-01
Publication Date
2024-10-04
Estimated Expiration
2042-09-01

AI Technical Summary

Technical Problem

Automotive laminated glass with asymmetrical glass thicknesses faces challenges in bending and forming due to mismatched softening points, leading to gaps, bulges, and optical defects, especially when the inner glass is chemically strengthened after bending.

Method used

The laminated glass design involves first and second glass plates with specific compositional differences, controlled temperature ranges, and controlled thickness ratios, allowing for simultaneous bending and forming while minimizing gaps and improving optical quality.

Benefits of technology

The solution enables consistent mold matching, reduces center gaps and edge wrinkles, enhances optical performance, and facilitates rapid ion exchange for high surface stress and stress layer depth, suitable for large-scale automotive glass production at reduced costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536262000001
    Figure 2024536262000001
  • Figure 2024536262000002
    Figure 2024536262000002
  • Figure 2024536262000003
    Figure 2024536262000003
Patent Text Reader

Abstract

The present application relates to a laminated glass for automobiles. The manufacturing material of the laminated glass for automobiles includes a first glass sheet, a second glass sheet, and an intermediate layer material, the first glass sheet and the second glass sheet have different compositions, the difference between temperatures Tp1 and Tp2 is 50°C or less, the temperature Tp1 is defined as the sum of a transition point temperature Tg1 of the first glass sheet and a first temperature compensation value Tb1, the temperature Tp2 is defined as the sum of a transition point temperature Tg2 of the second glass sheet and a first temperature compensation value Tb2, and the general formula of the temperature Tp is Tp=Tg+Tb.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to a Chinese patent application bearing application number 2021111635094, filed on September 30, 2021, and entitled "Automotive Laminated Glass," the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to the technical field of laminated glass, in particular to laminated glass for automobiles. [Background technology]

[0003] Automotive laminated glass is asymmetrical, and generally the outer glass is thick and the inner glass is thin. Such special inner and outer laminated glass is different from traditional laminated glass mainly in that the inner glass needs additional chemical strengthening after bending and then bonding with the outer glass to form a laminated glass. Currently, the chemical strengthening method of glass in the electronic display cover industry is generally adopted as the method for chemically strengthening the inner glass. However, when a certain material of inner glass is combined with the outer glass to be bent and formed, and when the inner glass is chemically strengthened after bending, the following problems may occur: (1) The softening point of the inner glass cannot be adapted to the outer glass, so that it is difficult for both to be bent and formed at the same time. (2) Even if it is formed, it is difficult to completely match the shapes of the inner and outer glass sheets after forming, and after bonding, there will be gaps of different sizes between the inner and outer glass sheets, which will affect the optical quality of the product. (3) The forming tendency of the inner and outer glass sheets may not match, so that the bending degree of the center region after hot bending does not match, resulting in bulging or wrinkles at the edges, which will cause sheet cracks or optical defects after joining. Summary of the Invention [Problem to be solved by the invention]

[0004] In view of this, various embodiments of the present application provide a laminated glass for automobiles, the technical solutions of which are as follows: [Means for solving the problem]

[0005] A laminated glass for an automobile, the manufacturing material of which includes a first glass sheet, a second glass sheet, and an interlayer material, The first glass plate and the second glass plate have different compositional components, The difference between the temperatures Tp1 and Tp2 is about 50° C. or less, The temperature Tp1 is defined as the sum of the transition temperature Tg1 of the first glass sheet and the first temperature compensation value Tb1, the temperature Tp2 is defined as the sum of the transition temperature Tg2 of the second glass sheet and the first temperature compensation value Tb2, and the general formula of the temperature Tp is defined as Tp=Tg+Tb; The transition temperature Tg occurs when the viscosity of the glass is about 10 13.4 It is defined as the temperature when the the first temperature compensation value Tb1 and the weight ratio of the composition components of the first glass plate satisfy the condition that Tb1 is equal to approximately 100×(3.5×SiO2+6.5×Al2O3-5×(Na2O+K2O)-3×(CaO+MgO)-6×B2O3-2.5×(ZnO+P2O5)); the second temperature compensation value Tb2 and the weight ratio of the composition components of the second glass plate satisfy the condition that Tb2 is equal to approximately 100×(3.5×SiO2+6.5×Al2O3-5×(Na2O+K2O)-3×(CaO+MgO)-6×B2O3-2.5×(ZnO+P2O5)); In the first glass sheet and the second glass sheet, the content of one or more of Al2O3, K2O, CaO, MgO, B2O3, ZnO, and P2O5 is zero.

[0006] In one embodiment, the second glass sheet has a thickness smaller than that of the first glass sheet, and the composition of the first glass sheet is a preset composition.

[0007] In one embodiment, the weight ratio of Al2O3 in the second glass plate is about 8wt% to 16wt%.

[0008] In one embodiment, the total weight percentage of alkaline earth metal compounds in the second glass sheet does not exceed about 5 wt %.

[0009] In one embodiment, the total weight ratio of the alkali metal compounds in the second glass sheet is about 15wt% to 25wt%.

[0010] In one embodiment, the composition of the second glass sheet includes Na2O, and the content of the Na2O is about 60 wt% or more of the total content of alkali metal compounds in the second glass sheet.

[0011] In one embodiment, the composition of the second glass sheet includes ZnO with a weight ratio of about 2 wt % to 6 wt % and P2O5 with a weight ratio of about 0 to 3 wt %.

[0012] In one embodiment, the material of the second glass sheet is mainly aluminosilicate.

[0013] In one embodiment, the material of the first glass sheet is mainly soda-lime silicate, aluminosilicate or borosilicate.

[0014] In one embodiment, the material of the first glass sheet is mainly soda-lime silicate, and the material of the second glass sheet is mainly aluminosilicate; The weight ratio of Al2O3 in the second glass plate is 8 wt% to 12 wt%, and the total weight ratio of the alkali metal compounds in the second glass plate is 20 wt% to 25 wt%.

[0015] In one embodiment, the material of the first glass sheet is mainly aluminosilicate or borosilicate, and the material of the second glass sheet is mainly aluminosilicate; The weight ratio of Al2O3 in the second glass plate is 12 wt% to 16 wt%, and the total weight ratio of the alkali metal compounds in the second glass plate is 15 wt% to 20 wt%.

[0016] In one embodiment, the first glass sheet has a thickness of about 2.1 mm or greater.

[0017] In one embodiment, the first pane of glass is untinted glass, tinted glass, or painted glass with a painted surface adjacent the interlayer material.

[0018] In one embodiment, the second glass sheet has a thickness of about 1.1 mm or less.

[0019] In one embodiment, the second glass is capable of undergoing ion exchange.

[0020] In one embodiment, the second glass sheet is a colorless glass having a visible light transmittance of about 88% or more.

[0021] In one embodiment, the interlayer material is an organic polymer.

[0022] The details of one or more embodiments of the application are set forth below, and other features, objects and advantages of the application will become apparent from the description and claims. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The technical solutions in the embodiments of the present application are described below clearly and completely. It is obvious that the described embodiments are only some embodiments of the present application, but not all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present application.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains. The terms used herein are for the purpose of describing specific examples only and are not intended to be limiting of this application.

[0025] term Unless otherwise stated or inconsistent, terms or phrases used herein have the following meanings:

[0026] As used herein, the scope of the terms "and / or", "or" and "and / or" includes any one of two or more of the associated listed items, and also includes any and all combinations of the associated listed items, including any two of the associated listed items, any further associated listed items, or all of the associated listed items.

[0027] As used herein, "one or more" refers to one, two, or more than two of any of the listed items. Here, "multiple" refers to two or more than two.

[0028] As used herein, the terms "combinations thereof," "any combination thereof," "any manner of combination thereof," and the like include all appropriate combinations of any two or any two or more of the listed items.

[0029] In this application, the term "appropriate" in terms of "appropriate combination method", "appropriate method", "any appropriate method", etc., is based on whether the technical solution of this application can be implemented, the technical problem of this application can be solved, and the technical effect anticipated by this application can be achieved.

[0030] In addition, in this application, the term "preferably" is only intended to describe an embodiment or example having better effects, and does not constitute a limitation on the scope of protection of the application.

[0031] In this application, technical features described in an open format include closed technical solutions made up of the recited features, and also include open technical solutions including the recited features.

[0032] In this application, when a numerical interval is referred to, both endpoints of the numerical interval are included unless otherwise stated.

[0033] In this application, references to percentage contents refer to mass percentages for solid-liquid and solid-solid mixtures, and volume percentages for liquid-liquid mixtures, unless otherwise specified.

[0034] In the present application, unless otherwise specified, percentage concentration refers to the final concentration. The final concentration refers to the proportion of an added component in a system after the component is added.

[0035] In the present application, unless otherwise specified, when referring to a temperature parameter, it may be a constant temperature process or a process with a constant temperature interval, in which the temperature can vary within the precision of the instrumental control.

[0036] In the present application, unless otherwise specified, the weight ratio refers to the weight ratio of a composition component in the total components. For example, the weight ratio of Al2O3 in the second glass sheet is about 8 wt% to 12 wt%, that is, the weight of Al2O3 in the second glass sheet is the percentage of the weight of the second glass sheet.

[0037] In some embodiments of the present application, a laminated glass for an automobile is provided. The laminated glass for an automobile includes a first glass sheet, a second glass sheet, and an interlayer material, The first glass plate and the second glass plate have different compositional components, The difference between the temperatures Tp1 and Tp2 is 50° C. or less. The difference between temperatures Tp1 and Tp2 is approximately 50°C or less. The temperature Tp1 is defined as the sum of the transition temperature Tg1 of the first glass sheet and the first temperature compensation value Tb1, the temperature Tp2 is defined as the sum of the transition temperature Tg2 of the second glass sheet and the first temperature compensation value Tb2, and the general formula of the temperature Tp is defined as Tp=Tg+Tb; The transition temperature Tg occurs when the viscosity of the glass is about 10 13.4 It is defined as the temperature when the the first temperature compensation value Tb1 and the weight ratio of the composition components of the first glass plate satisfy the condition that Tb1 is equal to approximately 100×(3.5×SiO2+6.5×Al2O3-5×(Na2O+K2O)-3×(CaO+MgO)-6×B2O3-2.5×(ZnO+P2O5)); the second temperature compensation value Tb2 and the weight ratio of the composition components of the second glass plate satisfy the condition that Tb2 is equal to approximately 100×(3.5×SiO2+6.5×Al2O3-5×(Na2O+K2O)-3×(CaO+MgO)-6×B2O3-2.5×(ZnO+P2O5)); In the first glass sheet and the second glass sheet, the content of one or more of Al2O3, K2O, CaO, MgO, B2O3, ZnO, and P2O5 may be zero.

[0038] Preferably, the thickness of the second glass sheet is smaller than the thickness of the first glass sheet, and the composition of the first glass sheet is a preset composition. For example, the first glass sheet is an outer glass sheet, and the second glass sheet is an inner glass sheet. Preferably, the thickness of the first glass sheet is about 2.1 mm or more. Preferably, the thickness of the second glass sheet is about 1.1 mm or less. For example, the thickness of the first glass sheet includes, but is not limited to, about 2.1 mm, about 2.3 mm, about 2.5 mm, about 2.6 mm, about 2.8 mm, about 3.0 mm, about 3.2 mm, about 3.5 mm, about 3.8 mm, about 4.0 mm, about 4.2 mm, about 4.5 mm, about 5.0 mm, and more. The thickness of the second glass sheet includes, but is not limited to, about 0.5 mm, about 0.7 mm, about 0.9 mm, about 1.1 mm, or other thicknesses within the range of about 0.5 mm to 1.1 mm. It is possible to combine different thicknesses and still have the above technical effects of the present application.

[0039] In some cases, the composition and specifications of the outer glass sheet are generally preset. The outer glass sheet largely determines the color, appearance, visible light transmittance, infrared and ultraviolet transmittance, compatibility of inks and adhesive accessories, and the set of glass drawing equipment and process system from the original sheet to the finished product of the glass assembly of the automobile, so the material of the first glass sheet in the present application may be a preset material. Compared with the outer glass sheet, the material of the inner glass sheet has a higher degree of freedom to adjust, and the production process of the original sheet of the inner sheet is more diversified, so that the composition adjustment is relatively feasible, and it is possible to make appropriate adjustments to match the outer glass sheet. In the present application, the material of the second glass sheet can be adjusted according to the preheating material of the first glass sheet, so that the difference in the forming temperature between the two is about 50°C or less.

[0040] In this application, the forming temperature (Tp) of glass is defined as the sum of the glass transition temperature (Tg) of the glass and the temperature compensation value (Tb) of the glass. The calculation formula of Tb is obtained by combining example data according to the effect of different oxide components in glass on the viscosity-temperature curve. In the calculation formula of Tb, for oxides with positive coefficients (e.g., SiO2, Al2O3), the introduction of the oxide improves the high-temperature viscosity of glass and correspondingly improves the forming temperature, and the magnitude of the coefficient indicates the strength of the effect of the oxide on the viscosity. For oxides with negative coefficients, the introduction of the oxide reduces the high-temperature viscosity of glass and correspondingly reduces the forming temperature, and the magnitude of the coefficient similarly indicates the strength of the effect of the oxide on the viscosity. Generally, when the composition components of glass are different, Tg and Tb are also different, and it is necessary to simultaneously control Tg and Tb so that the forming temperatures Tp of both satisfy the above conditions.

[0041] The Tg of the glass can be measured by referring to standard methods, and is determined when the viscosity of the glass is about 10 13.4 It is defined as the temperature at which the

[0042] In the present application, the forming temperature Tp1 of the first glass sheet may be a temperature between the Tg1 and the softening point of the first glass sheet. At this temperature, the glass exhibits an optimal viscosity suitable for hot bending processing, and has a certain ductility to enable bending, but also has too high fluidity and is too soft, which causes various common defects (such as sheet adhesion, die-off, die marks, impurity particle embedment, etc.) in the bending process. Similarly, the forming temperature Tp2 of the second glass sheet may be a temperature between the Tg2 and the softening point of the second glass sheet.

[0043] When the above conditions are satisfied, the processing operation of simultaneously bending the first and second glass sheets can be realized, and the degree of matching between the first and second glass sheets after bending can be improved, the central gap between the first and second glass sheets can be small, there can be no obvious bulge in the middle, and there can be small wrinkles at the edges, and the optical performance of the laminated glass can be improved after bonding.

[0044] In one embodiment, when the difference between the forming temperature Tp1 of the first glass sheet and the forming temperature Tp2 of the second glass sheet satisfies the above condition, the composition of the second glass sheet further satisfies the following requirement: the composition of the second glass sheet contains Al2O3, at least one type of alkali metal compound, and at least one type of alkaline earth metal compound.

[0045] In some embodiments, the content of Al2O3 in the second glass sheet is about 8 wt% to 16 wt% of the second glass sheet.

[0046] In some embodiments, the total content of alkaline earth metal compounds in the second glass sheet does not exceed about 5 wt % of the second glass sheet.

[0047] In some embodiments, the total content of alkali metal compounds in the second glass sheet is about 15% wt-25% wt of the second glass sheet.

[0048] Alkali metals are components of oxides necessary for glass production. They are generally introduced as raw materials such as soda and feldspar, and are used to lower the melting temperature in glass production. On the other hand, they are also used for chemical strengthening ion exchange (K in salt baths). + is Na in the glass + provides the free cations necessary for the exchange of

[0049] In some embodiments, the composition of the second glass sheet includes Na2O, and the content of the Na2O is about 60 wt% or more of the total content of alkali metal compounds in the second glass sheet. The above content of Na2O in the glass is advantageous for achieving rapid ion exchange.

[0050] In some embodiments, the composition of the second glass sheet includes ZnO that is present in a range of about 2 wt % to 6 wt % of the second glass sheet, and P2O5 that is present in a range of about 0 to 3 wt % of the second glass sheet.

[0051] Preferably, the material of the second glass plate is mainly an aluminosilicate.

[0052] As can be appreciated, the second glass sheet is capable of undergoing ion exchange.

[0053] As can be seen, the second glass pane is a colorless glass having a visible light transmittance of about 88% or greater.

[0054] Automotive laminated glass has large dimensions, many varieties, and complicated curvature shapes, and has high requirements for the depth of the stress layer, so it is necessary to carry out rapid ion exchange, i.e., to reach the desired maximum depth of the stress layer within the shortest possible exchange time, thereby improving the production rate. Rapid ion exchange can also shorten the time that the glass is immersed in the molten salt, reduce the impurities in the glass from being ion-exchanged in the salt bath, ensure the durability of the molten salt, and reduce the frequency of molten salt exchange. However, some inner glass sheets cannot reach the desired depth of the stress layer through rapid ion exchange, which results in high costs in both the production rate and the frequency of molten salt exchange.

[0055] If the above conditions are met, the second glass sheet will have sufficiently high surface stress and stress layer depth within a short time during chemical strengthening, and have the effect of rapid ion exchange strengthening, which can meet the large size and mass production requirements of chemically strengthened glass for automobiles, improve the production rate, and further reduce the frequency of replacing molten salt, saving costs, and the process cost can reach a level close to that of traditional physical air-cooling strengthening, which makes it convenient and low-cost for chemically strengthened glass to be better applied in the vehicle market.

[0056] The sufficiently high surface stress and depth of the stress layer mean that the depth of the compressive stress layer of the inner glass sheet after replacement is about 30 μm or more, and the compressive stress is about 500 MPa or more.

[0057] In the present application, the rate of ion exchange is rapid, and in some embodiments, the time of ion exchange strengthening is 4 hours or less, and in some embodiments, the time of ion exchange strengthening is 2 hours or less.

[0058] Preferably, the material of the first glass sheet is mainly soda-lime silicate, aluminosilicate or borosilicate.

[0059] As can be appreciated, the first glass sheet can be annealed low stress glass or physically heat strengthened prestressed glass.

[0060] As can be appreciated, the first pane of glass can be plain glass, tinted glass, or painted glass with a painted surface adjacent the interlayer material.

[0061] In some embodiments, the material of the first glass sheet is primarily soda-lime silicate, the material of the second glass sheet is primarily aluminosilicate, the content of Al2O3 in the second glass sheet is about 8 wt% to 12 wt% of the second glass sheet, and the total content of alkali metal compounds in the second glass sheet is about 20 wt% to 25 wt% of the second glass sheet.

[0062] In some embodiments, the material of the first glass is primarily an aluminosilicate or borosilicate, the material of the second glass sheet is primarily an aluminosilicate, the content of Al2O3 in the second glass sheet is about 12 wt% to 16 wt% of the second glass sheet, and the total content of alkali metal compounds in the second glass sheet is about 15 wt% to 20 wt% of the second glass sheet.

[0063] In some embodiments, the interlayer of the present laminated automotive glass may be single or multi-ply and may be made with any interlayer material.

[0064] Preferably, the interlayer material is an organic polymer, which in some embodiments may be pre-compounded with a special functional layer.

[0065] Preferably, the organic polymer includes, but is not limited to, polymers based on polyvinyl butyral (PVB), polyurethane (PU), polyethylene-vinyl acetate (EVA), and ethylene-methacrylate (SGP), which have excellent aging resistance and sufficient adhesion to glass surfaces.

[0066] In this application, according to the effect of different oxide components in glass on the viscosity-temperature curve, the empirical formula of the temperature compensation value Tb of the glass sheet is obtained by combining the actual data, and the forming temperature Tp of the glass sheet is derived. By limiting the difference between the forming temperatures Tp1 and Tp2 of the first and second glass sheets, the processing possibility of the simultaneous bending of the first and second glass sheets is satisfied, and the matching degree of the first and second glass sheets after bending is improved, so that the central gap between the first and second glass sheets is small, there is no obvious bulge in the middle, the wrinkles at the edges are small, and the optical performance of the laminated glass is improved after bonding.

[0067] The present application further provides a method for producing the above laminated automotive glass.

[0068] This manufacturing method for automotive laminated glass includes the steps of bending the first glass sheet and the second glass sheet at a preset temperature, separating the first glass sheet and the second glass sheet after bending and subjecting the second glass sheet after bending to a chemical strengthening treatment, and disposing the intermediate layer material between the first glass sheet after bending and the second glass sheet after chemical strengthening treatment, and heating and pressurizing the resulting mixture to manufacture laminated glass.

[0069] As can be seen, the step of bending the first and second glass sheets further includes a step of pre-treating the first and second glass sheets, which includes cutting and beveling the first and second glass sheets to form a desired specific contour, pre-setting a dimensional lamination difference between the first and second glass sheets according to the bending shape and dimensions of the final product, and matching the edges of the two layers of glass after lamination and bending.

[0070] Preferably, the step of bending the first glass sheet and the second glass sheet at the preset temperature includes: overlapping the first glass sheet and the second glass sheet, applying a high-temperature resistant insulating powder to the overlapping surfaces of both glass sheets to obtain a laminated glass sheet; and placing the laminated glass in a forming die, and bending the laminated glass at the preset temperature.

[0071] As can be seen, the laminated glass sheet may be bent by thermal bending using the weight of the glass to attach it to a mold, or by using a ring-shaped lower mold and a solid upper mold to assist in pressure bonding to complete the bending.

[0072] Preferably, the laminated glass sheet is heated uniformly and symmetrically on the top and bottom in a continuous furnace or tunnel furnace by presetting the furnace temperature. The forming method may adopt a gravity forming method, in which the laminated glass sheet is bent by gravity and bonded to the contour of a mold to form a desired shape, or a pressure method, in which the laminated glass sheet that is not completely formed by its own weight is placed between a ring-shaped lower mold and a solid upper mold and pressure-formed to form a desired shape. After forming, the laminated glass sheet is gradually cooled to room temperature to complete annealing, and a laminated glass sheet after bending is obtained.

[0073] Preferably, the preset temperature is a forming temperature of the first glass sheet.

[0074] As can be seen, the continuous or tunnel furnace may include one or more chambers. If there is one chamber, the heating step increases the temperature of the chamber to a preset temperature, the preset temperature being the forming temperature of the first glass sheet. If there are multiple chambers, the heating step increases the temperature of each chamber, each chamber may be configured to have a gradient temperature distribution, the highest temperature in the chamber is a preset temperature, the preset temperature being the forming temperature of the first glass sheet.

[0075] Preferably, the high-temperature resistant insulating powder is a powder material that does not react with the surface of the glass plate, including but not limited to diatomaceous earth or calcium carbonate. In one embodiment, the particle size of the diatomaceous earth is about 5 μm to 15 μm.

[0076] Since a high-temperature resistant insulating powder is added between the first glass sheet and the second glass sheet after bending, the two can be separated, and the second glass sheet after bending is subjected to a chemical strengthening treatment.

[0077] Preferably, the chemical strengthening treatment includes the steps of preheating, ion exchange, cooling and washing.

[0078] Specifically, the second glass plate after bending is placed in a chemically strengthened mounting frame of corresponding dimensions, the glass plate is uniformly fixed, the mounting frame is uniformly heated together with the glass plate in the preheating cavity until it is close to the ion exchange temperature (about 350-400°C), and then immersed in a salt bath of molten KNO3 to carry out ion exchange, set the temperature and time of ion exchange, and make the stress and depth reach a specific requirement. After the exchange is completed, the mounting frame is slowly lifted together with the glass plate, and after the sticky liquid KNO3 drops are cleaned, it is placed in a cooling cavity and uniformly cooled to about 100°C or less, and the glass plate after cooling is completed is immersed in deionized water to remove excess KNO3. The second glass plate after chemical strengthening is combined with the first glass plate to be bent at the same time, and then the bonding process is carried out.

[0079] The bonding treatment includes disposing the intermediate layer material between the first glass plate after bending and the second glass plate after chemical strengthening, and heating and pressing the resulting mixture to produce the laminated glass for automobiles.

[0080] After being pre-pressurized (or vacuumed) and processed through a high-temperature and high-pressure process, the two pieces of glass and the polymer interlayer are aligned and uniformly adhered together to obtain a laminated glass for automobiles.

[0081] In one embodiment, the structure of the laminated glass for automobiles has a convex surface, and after being attached to a vehicle body, the convex surface faces the exterior of the vehicle, the first glass sheet is located on the side facing the exterior of the vehicle, and the second glass sheet is located on the side facing the interior of the vehicle.

[0082] Preferably, the laminated glass for automobiles may be front and rear windshields, roof glass, or front and rear door glass of a vehicle body.

[0083] In one embodiment, the preset temperature of the bending is about 593°C, and the preset ion exchange temperature of the chemical strengthening of the second glass sheet after bending is about 420°C.

[0084] In one embodiment, the ion exchange time is about 2 hours, which can meet the stress and depth requirements of the glass.

[0085] The following is a further description with reference to specific examples and comparative examples. Unless otherwise specified, the raw materials involved in the following specific examples can all be obtained commercially, unless otherwise specified, the equipment used can all be obtained commercially, unless otherwise specified, and the processes involved can all be selected by those skilled in the art, unless otherwise specified.

[0086] Examples and Comparative Examples Laminated glass of Examples and Comparative Examples was produced with reference to the oxide components of the glass sheets shown in Table 1 and the combination of the first and second glass sheets shown in Table 2. The thickness of the first glass sheet was about 3.5 mm, and the thickness of the second glass sheet was about 1.1 mm. The specific production method is as follows. (1) The first glass sheet and the second glass sheet were cut and edged to form a desired specific outline. The second glass sheet and the first glass sheet were overlapped, and diatomaceous earth with a particle size of about 5 μm to 15 μm was applied to the overlapping surfaces of the two sheets to obtain a laminated glass sheet. The laminated glass sheet was placed in a ring-shaped lower mold and placed in a continuous furnace. There was one chamber in the continuous furnace, and the temperature of the chamber was raised to about 593°C, and the laminated glass sheet was heated uniformly and symmetrically from the top to the bottom, and was shaped by assisting compression bonding with a solid upper mold and a lower ring-shaped mold. After the shaping was completed, the glass sheet was slowly cooled to room temperature to complete the annealing, and a laminated glass sheet after bending was obtained. (2) The first glass plate and the second glass plate after bending are separated, and the second glass plate after bending is placed in a chemical strengthening mounting frame of corresponding dimensions. The glass plate is uniformly fixed, and the mounting frame together with the glass plate is uniformly heated in a preheating chamber, and then immersed in a salt bath of molten KNO3 to carry out ion exchange, and the ion exchange temperature is about 420°C. After the stress and depth reach certain requirements, the glass plate is cooled, washed and removed. (3) An organic polymer film is placed between the first glass sheet and the second glass sheet after chemical strengthening, and after pre-pressurization (or vacuum drawing) and processing with a high-temperature and high-pressure process, the two pieces of glass and the organic polymer film are aligned and uniformly bonded together to obtain a laminated glass for automobiles. The manufactured laminated glass can be used as a windshield product for automobiles.

[0087] [Table 1]

[0088] [Table 2]

[0089] The technical effects of the above examples and comparative examples are evaluated according to the state of the central gap and edge gap between the first glass sheet and the second glass sheet after forming.

[0090] In addition, compared with electronic display covers, chemically strengthened glass for automobiles has lower requirements for surface stress and higher requirements for stress layer depth. Even if the size of the furnace body is increased, the number of reinforced layers per one time is still low, so it is necessary to obtain a sufficient stress layer depth within as short a time as possible. Therefore, the technical effects of the above examples and comparative examples were evaluated according to the average ion exchange rate for the first 4 hours after the second glass sheet started ion exchange. The results are shown in Table 3.

[0091] [Table 3]

[0092] As can be seen from Table 3, in Examples 1 to 4, the central gap between the first and second glass sheets after bending is small, there is no obvious bulge in the middle region of the first and second glass sheets, the edge gap is small, the edge wrinkles are small, and the mold consistency is high, so that the shape of the final laminated glass can be consistent with the laminated glass after hot bending, which is favorable for improving the optical quality of the entire product. Meanwhile, the second glass sheet according to Examples 1 to 4 has the effect of rapid ion exchange strengthening, and within the first 4 hours after the start of ion exchange, the exchange rate of the average stress layer depth is 12 μm / h or more. In the individual examples, the stress layer depth of about 40 μm is obtained under the exchange condition of about 2 hours, which can meet the large size and mass production requirements of chemically strengthened glass for automobiles, and the process cost reaches a level close to that of traditional physical air cooling strengthening, which is convenient for chemically strengthened glass to be better applied in the automotive market. In addition, the time that the glass is immersed in the molten salt is reduced, the impurities in the glass are ion-exchanged into the salt bath, the durability of the molten salt is ensured, the frequency of replacement of the molten salt is reduced, and costs are saved.

[0093] The technical features of the embodiments described above can be combined in any manner, and for the sake of brevity, not all possible combinations of the technical features in the embodiments described above have been described; however, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope described in this specification.

[0094] The above examples merely show some embodiments of the present application, and although the description is specific and detailed, it should not be understood as limiting the scope of the present invention. It should be noted that a person skilled in the art can make some modifications and improvements within the scope of the present application without departing from the idea of ​​the present application. Therefore, the protection scope of the present application shall be subject to the scope of the attached claims.

Claims

1. A laminated glass for automobiles, comprising: The article of manufacture includes a first glass sheet, a second glass sheet, and an interlayer material; The first glass plate and the second glass plate have different compositional components, The difference between the temperatures Tp1 and Tp2 is about 50° C. or less. The temperature Tp1 is defined as the sum of the transition point temperature Tg1 of the first glass sheet and the first temperature compensation value Tb1, the temperature Tp2 is defined as the sum of the transition point temperature Tg2 of the second glass sheet and the first temperature compensation value Tb2, and the general formula of the temperature Tp is defined as Tp = Tg + Tb, The transition temperature Tg is reached when the viscosity of the glass is about 10 13.4 is defined as the temperature at which the The weight ratio of the first temperature compensation value Tb1 to the compositional components of the first glass plate is about 100×(3.5×SiO 2 +6.5×Al 2 O 3 -5×(Na 2 O+K 2 O)-3×(CaO+MgO)-6×B 2 O 3 -2.5×(ZnO+P 2 O 5 )) is satisfied, The weight ratio of the second temperature compensation value Tb2 to the compositional components of the second glass plate is about 100×(3.5×SiO 2 +6.5×Al 2 O 3 -5×(Na 2 O+K 2 O)-3×(CaO+MgO)-6×B 2 O 3 -2.5×(ZnO+P 2 O 5 )) is satisfied, In the first glass plate and the second glass plate, Al 2 O 3 , K 2 O, CaO, MgO, B 2 O 3 , ZnO and P 2 O 5 The present invention relates to a laminated glass for automobiles, and a method for manufacturing the same.

2. 2. The laminated glass for an automobile according to claim 1, wherein a thickness of the second glass sheet is smaller than a thickness of the first glass sheet, and a composition of the first glass sheet is a preset composition.

3. Al in the second glass plate 2 O 3 3. The laminated glass for automobiles according to claim 1, wherein the weight ratio of said first and second components is about 8 wt % to 16 wt %.

4. 4. The laminated glass for automobiles according to claim 1, wherein the total weight ratio of the alkaline earth metal compounds in the second glass sheet does not exceed about 5 wt %.

5. 5. The laminated glass for an automobile according to claim 1, wherein a total weight ratio of the alkali metal compound in the second glass sheet is about 15 wt % to 25 wt %.

6. The composition of the second glass plate is Na 2 O, and the Na 2 6. The laminated glass for automobiles according to claim 5, wherein the content of O is about 60 wt% or more of the total content of alkali metal compounds in the second glass sheet.

7. The composition of the second glass plate is about 2 wt % to 6 wt % ZnO and about 0 to 3 wt % P. 2 O 5 The laminated glass for automobiles according to any one of claims 1 to 6, comprising:

8. 8. The laminated glass for an automobile according to claim 1, wherein the material of the second glass sheet is mainly an aluminosilicate.

9. 9. The laminated glass for an automobile according to claim 1, wherein the material of the first glass sheet is mainly soda-lime silicate, aluminosilicate, or borosilicate.

10. The material of the first glass sheet is mainly soda-lime silicate, and the material of the second glass sheet is mainly aluminosilicate, Al in the second glass plate 2 O 3 10. The laminated glass for an automobile according to claim 1, wherein a weight ratio of the alkali metal compounds in the second glass sheet is 8 wt % to 12 wt %, and a total weight ratio of the alkali metal compounds in the second glass sheet is 20 wt % to 25 wt %.

11. The material of the first glass is mainly an aluminosilicate or a borosilicate, and the material of the second glass sheet is mainly an aluminosilicate; Al in the second glass plate 2 O 3 10. The laminated glass for an automobile according to claim 1, wherein a weight ratio of the alkali metal compounds in the second glass sheet is 12 wt % to 16 wt %, and a total weight ratio of the alkali metal compounds in the second glass sheet is 15 wt % to 20 wt %.

12. 12. The laminated glass for automobiles according to claim 1, wherein the first glass sheet has a thickness of about 2.1 mm or more.

13. The laminated glass for automobiles according to any one of claims 1 to 12, characterized in that the first glass sheet is a colorless glass sheet, a colored glass sheet, or a painted glass sheet having a painted surface adjacent to the interlayer material.

14. 14. The laminated glass for automobiles according to claim 1, wherein the second glass sheet has a thickness of about 1.1 mm or less.

15. The laminated glass for an automobile according to any one of claims 1 to 14, characterized in that the second glass sheet is capable of performing ion exchange.

16. 16. The laminated glass for an automobile according to claim 1, wherein the second glass sheet is a colorless glass having a visible light transmittance of about 88% or more.

17. The laminated glass for automobiles according to any one of claims 1 to 16, characterized in that the interlayer material is an organic polymer.

Citation Information

Patent Citations

  • Chemically strengthened colored thin glass

    JP2019503965A

  • Method for producing laminated glass

    WO2014054468A1

  • Glass compositions for use in co-formed laminates

    WO2020046668A1

  • Laminated glass for vehicle

    WO2021220996A1