Method for producing positive electrode binder or positive electrode insulating liquid for lithium secondary battery, and lithium secondary battery containing the positive electrode binder or positive electrode insulating liquid produced thereby

By using a non-aqueous organic solvent to replace water in the dispersion of conjugated diene latex particles, the method addresses the issue of short circuits in lithium secondary batteries, ensuring stable coating and preventing thermal runaway while maintaining battery performance.

JP2024536318AInactive Publication Date: 2024-10-04LG CHEM LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024520040
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-04
Filing Date
2023-04-04
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional separators for lithium secondary batteries fail to prevent physical short circuits between positive and negative electrodes due to insufficient heat resistance, leading to thermal runaway, and existing insulating methods either compromise adhesion or prevent lithium ion migration, degrading battery performance.

Method used

A non-aqueous organic solvent, such as N-methyl-pyrrolidone, is used to replace water as a dispersion solvent for conjugated diene latex particles, forming a positive electrode binder or insulating liquid that can coat both the positive electrode mixture and insulating layers simultaneously, maintaining flexibility and insulation properties.

Benefits of technology

This approach prevents separator shrinkage and electrode folding, thereby preventing physical short circuits and maintaining battery stability by ensuring effective coating without compromising adhesion or lithium ion migration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536318000001_ABST
    Figure 2024536318000001_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide an insulating layer composition for a lithium secondary battery, which can perform coating of an insulating liquid simultaneously with coating of a positive electrode by replacing water, which is a dispersion medium of an aqueous conjugated dienes copolymer latex, with a non-aqueous organic solvent (e.g., N-methyl-pyrrolidone). The present invention relates to a method for producing a positive electrode binder or a positive electrode insulating liquid for a lithium secondary battery, the method comprising the steps of adding a non-aqueous organic solvent to a water-dispersed conjugated diene latex, and replacing water, which is a dispersion solvent for the conjugated diene latex particles, with the non-aqueous organic solvent by heating and reducing the pressure, and a lithium secondary battery including the produced positive electrode binder or positive electrode insulating liquid.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a positive electrode binder or a positive electrode insulating liquid for a lithium secondary battery, and a lithium secondary battery including the positive electrode binder or the positive electrode insulating liquid produced thereby. [Background technology]

[0002] As technological development and demand for mobile devices increases, the demand for secondary batteries as an energy source is growing rapidly, and accordingly, much research is being conducted on batteries that can meet various needs.

[0003] Typically, in terms of battery shape, there is high demand for thin rectangular and pouch-shaped batteries that can be used in products such as mobile phones, and in terms of materials, there is high demand for lithium secondary batteries such as lithium-cobalt polymer batteries, which have excellent energy density, discharge voltage, and safety.

[0004] One of the main research topics for such secondary batteries is to improve their safety. The main cause of safety-related accidents in batteries is the reaching of abnormally high temperatures due to short circuits between the positive and negative electrodes. In other words, under normal circumstances, a separator is located between the positive and negative electrodes to maintain electrical insulation, but in abnormal abuse situations such as when the battery is overcharged or overdischarged, internally short-circuited by dendritic growth of the electrode material or foreign matter, pierced by sharp objects such as nails or screws, or subjected to excessive deformation due to external forces, the conventional separator alone shows its limitations.

[0005] Generally, microporous membranes made of polyolefin resin are mainly used as separators, but their heat resistance is insufficient, with a heat resistance of about 120 to 160°C. Therefore, when an internal short circuit occurs, the separator shrinks due to the short circuit reaction heat, expanding the short circuit area, leading to a thermal runaway state in which a larger amount of reaction heat is generated. Therefore, various methods have been studied to reduce the possibility of cell deformation, external impact, or physical short circuit between the positive and negative electrodes.

[0006] For example, in order to prevent a short circuit caused by the electrode tab coming into contact with the upper end of the electrode assembly due to the movement of the electrode assembly in a completed battery, a method of attaching insulating tape of a predetermined size on the electrode tab adjacent to the upper end of the current collector is known. However, the winding of such insulating tape is very cumbersome, and when the insulating tape is wound up to a length that extends slightly downward from the upper end of the current collector, such a portion may cause an increase in the thickness of the electrode assembly. Furthermore, there is a problem that the electrode tab is easily loosened when it is bent.

[0007] There is also a method of forming an insulating layer on the tab portion of the positive electrode using a non-aqueous binder (such as PVDF) or an aqueous styrene butadiene copolymer (SBL). However, when a non-aqueous binder (such as PVDF) is used, there is a problem that the wet adhesion is reduced and the migration of lithium ions cannot be prevented in the overlay region of the electrode, resulting in the development of capacity. In particular, when the capacity is developed in the overlay region of the electrode, lithium ions may be precipitated, which may result in a decrease in the stability of the battery cell. In addition, when an aqueous styrene butadiene copolymer (SBL) binder is used, when it is simultaneously coated with the slurry for the positive electrode mixture layer, there is a problem that the gelation of PVDF, which is an organic binder used as the positive electrode binder, and the deterioration of battery performance due to side reactions caused by moisture occur, and simultaneous coating of the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer is impossible.

[0008] Therefore, there is a strong need to develop an insulating liquid that allows for simultaneous coating of a slurry for a positive electrode mixture layer and a slurry for an insulating coating layer while simultaneously satisfying the requirements for flexibility, insulating properties, and electrolyte resistance. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Korean Patent No. 10-1586530 Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide an insulating layer composition for a lithium secondary battery that can perform insulating liquid coating simultaneously with positive electrode coating by replacing water, which is a dispersion solvent for an aqueous conjugated dienes copolymer latex, with a non-aqueous organic solvent (e.g., N-methyl-pyrrolidone).

[0011] Another object of the present invention is to provide a positive electrode binder or a positive electrode insulating liquid for a lithium secondary battery, which is prepared according to the above-mentioned method.

[0012] Another object of the present invention is to provide a lithium secondary battery including the above-mentioned positive electrode binder or positive electrode insulating liquid for a lithium secondary battery.

[0013] Other objects and advantages of the present invention will be more clearly described in the following detailed description of the invention and the appended claims. [Means for solving the problem]

[0014] In order to achieve the above-mentioned technical objectives, the present invention provides a method for preparing a positive electrode binder or a positive electrode insulating solution for a lithium secondary battery, comprising the steps of adding a non-aqueous organic solvent to a water-dispersed conjugated dienes latex, and heating and reducing the pressure.

[0015] The present invention also provides a positive electrode binder or a positive electrode insulating liquid for a lithium secondary battery, comprising a conjugated dienes copolymer as a binder polymer prepared by the above-mentioned preparation method and a non-aqueous organic solvent as a dispersion solvent.

[0016] The present invention also provides a lithium secondary battery comprising the positive electrode binder or the positive electrode insulating liquid for a lithium secondary battery. Effect of the Invention

[0017] According to one embodiment of the present invention, by replacing water, which is a dispersion solvent for conjugated diene latex particles, with a non-aqueous organic solvent (e.g., N-methyl-pyrrolidone), a positive electrode binder or a positive electrode insulating liquid for a lithium secondary battery can be provided, which can prevent physical short circuit between the positive electrode and the negative electrode when defects such as separator shrinkage and electrode folding occur in the lithium secondary battery.

[0018] The effects of the present invention are not limited to the above examples, and more various effects are described in this specification. [Brief description of the drawings]

[0019] [Figure 1] The slurry for the positive electrode mixture layer and the slurry for the insulating coating layer produced in each of Examples 1 to 6, Comparative Examples 1 to 2, and Comparative Examples 4 to 5 were simultaneously applied to a current collector using a doctor blade so as to be overlaid, and the results were compared immediately after application and after 1 minute had elapsed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention will be described in detail below.

[0021] All terms used in this specification (including technical and scientific terms) may be used in the sense commonly understood by those having ordinary skill in the art to which the present invention belongs, unless otherwise defined. Furthermore, terms defined in commonly used dictionaries are not to be interpreted ideally or excessively, unless clearly and specifically defined.

[0022] Throughout this specification, when a part is said to "comprise" certain elements, this should be understood as an open-ended term that does not exclude other elements, but rather includes the possibility of further including other elements, unless specifically stated to the contrary.

[0023] As used herein, "preferred" and "preferably" refer to embodiments of the invention that may provide certain advantages, under certain circumstances. However, other embodiments may also be preferred, under the same or different circumstances. Furthermore, reference to one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude other embodiments from the scope of the invention.

[0024] In the present invention, the term "insulating coating layer" refers to an insulating member formed by coating and drying from at least a portion of the uncoated portion of the electrode current collector to at least a portion of the electrode mixture layer.

[0025] <Method for producing positive electrode binder or positive electrode insulating liquid for lithium secondary battery>

[0026] The present invention provides a method for preparing a positive electrode binder or a positive electrode insulating solution for a lithium secondary battery, comprising the steps of adding a non-aqueous organic solvent to a water-dispersed conjugated dienes latex, and heating and reducing the pressure.

[0027] In the heating and depressurizing step, water, which is a dispersion medium for the conjugate diene latex particles, is replaced with a non-aqueous organic solvent.

[0028] The step may be a step of heating to a temperature of 40° C. to 100° C. Preferably, the temperature may be, but is not limited to, 60° C. to 95° C.

[0029] The step may be a step of reducing the pressure to less than 200 Torr, preferably, but not limited to, 60 Torr or less.

[0030] In this step, the decompression may be carried out for 1 hour to 20 hours.

[0031] In one embodiment of the present invention, the step may be a step of heating to a temperature of 40° C. to 100° C. and reducing the pressure to less than 200 torr for 1 hour to 20 hours.

[0032] The experimental results showed that when the pressure was reduced to 200 torr or more at a temperature of 40℃~100℃, the final moisture content exceeded 10,000 ppm even after 20 hours of reduced pressure. Also, when the pressure was reduced to 10 torr but the temperature was less than 40℃, the moisture content exceeded 10,000 ppm within 20 hours.

[0033] Even after replacing the water, which is the dispersion medium of the conjugate diene latex particles, with a non-aqueous organic solvent, the conjugate diene latex particles maintain their particle shape. Whether or not the particle shape is maintained can be confirmed by particle size measurement. The size of the particles can be confirmed by, but is not limited to, a DLS particle size analyzer, a laser diffraction particle size analyzer, or an electron transmission microscope.

[0034] In one embodiment of the present invention, the step may be one in which the pressure, temperature and time satisfy the following correlation:

[0035] [Equation 1]

[0036] y (Minimum pressure, torr) / x (Temperature, K) 17.4 * 10 44 <z (Time, h) 0.5 <8

[0037] When the relationships among the pressure, temperature, and time during the replacement process do not satisfy Relational Expression 1, the final moisture content can exceed 10,000 ppm.

[0038] When water, which is a dispersion solvent of conjugated diene latex particles, is replaced with a non-aqueous organic solvent under the above conditions, the moisture content becomes 10,000 ppm or less, and excellent effects can be exhibited when used as a positive electrode binder or an insulating liquid.

[0039] The conjugated diene copolymer may include a polymer of (a) a conjugated diene monomer or a conjugated diene polymer, (b) one or more monomers selected from the group consisting of acrylate monomers, vinyl monomers, and nitrile monomers, and (c) one or more monomers selected from the group consisting of unsaturated carboxylic acid monomers and hydroxy group-containing monomers.

[0040] The conjugated diene monomer may be one monomer selected from the group consisting of 1,3-butadiene, isoprene, chloroprene, and piperylene.

[0041] The conjugated diene polymer may be, for example, a polymer of two or more monomers selected from the group consisting of 1,3-butadiene, isoprene, chloroprene, and piperylene, a styrene-butadiene copolymer, an acrylonitrile-butadiene copolymer, a styrene-isoprene copolymer, an acrylate-butadiene rubber, an acrylonitrile-butadiene-styrene rubber, an ethylene-propylene-diene polymer, or a polymer in which these polymers are partially epoxidized or brominated, or a mixture thereof.

[0042] The acrylate monomer may be one or more monomers selected from the group consisting of methyl ethacrylate, methyl methacrylate, methacryloxyethyl ethylene urea, β-carboxyethyl acrylate, aliphatic monoacrylate, dipropylene diacrylate, ditrimethylolpropane tetraacrylate, dipentaerythriol hexaacrylate, pentaerythriol triacrylate, pentaerythriol tetraacrylate, and glycidyl methacrylate.

[0043] The vinyl monomer may be at least one monomer selected from the group consisting of styrene, α-methylstyrene, β-methylstyrene, pt-butylstyrene, and divinylbenzene.

[0044] The nitrile monomer may be at least one monomer selected from the group consisting of acrylonitrile, methacrylonitrile, and allyl cyanide.

[0045] The unsaturated carboxylic acid monomer may be at least one monomer selected from the group consisting of maleic acid, fumaric acid, methacrylic acid, acrylic acid, glutaric acid, itaconic acid, tetrahydrophthalic acid, crotonic acid, isocrotonic acid, and nadic acid, but is not limited thereto.

[0046] The hydroxy group-containing monomer may be one or more monomers selected from the group consisting of hydroxyacrylate, hydroxyethyl acrylate, hydroxybutyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate, but is not limited thereto.

[0047] Preferably, the conjugate diene latex can be, but is not limited to, a styrene-butadiene latex.

[0048] The method for producing the conjugate diene copolymer particles is not particularly limited, and may be carried out by a known suspension polymerization method, emulsion polymerization method, seed polymerization method, etc. The mixture of monomers for producing the copolymer particles may contain one or more other components such as a polymerization initiator, a crosslinking agent, a coupling agent, a buffer solution, a molecular weight regulator, and an emulsifier. Specifically, the copolymer particles may be produced by an emulsion polymerization method, and in this case, the average particle size of the copolymer particles may be adjusted by the amount of an emulsifier. In general, the particle size tends to become smaller as the amount of the emulsifier increases, and the particle size tends to become larger as the amount of the emulsifier decreases. The desired average particle size can be achieved by adjusting the amount of the emulsifier used in consideration of the desired particle size, reaction time, reaction stability, etc. The polymerization temperature and polymerization time may be appropriately determined depending on the polymerization method, the type of polymerization initiator, etc. For example, the polymerization temperature may be 10°C to 150°C, and the polymerization time may be 1 to 20 hours.

[0049] The polymerization initiator may be an inorganic or organic peroxide, for example, a water-soluble initiator including potassium persulfate, sodium persulfate, ammonium persulfate, etc., or an oil-soluble initiator including cumene hydroperoxide, benzoyl peroxide, etc. In addition, an activator may be further included to promote the initiation reaction of the peroxide together with the polymerization initiator, and the activator may be at least one selected from the group consisting of sodium formaldehyde sulfoxylate, sodium ethylenediaminetetraacetate, ferrous sulfate, and dextrose.

[0050] The crosslinking agent is a substance that promotes crosslinking of the binder, and examples of the crosslinking agent include amines such as diethylene triamine, triethylene tetramine, diethylamino propylamine, xylene diamine, and isophorone diamine, dodecyl succinic anhydride, and phthalic anhydride. Examples of suitable grafting agents include acid anhydrides such as aryl methacrylate, polyamide resins, polysulfide resins, phenolic resins, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol dimethacrylate, trimethylolpropane trimethacrylate, trimethylolmethane triacrylate, and glycidyl methacrylate. Examples of suitable grafting agents include aryl methacrylate (AMA), triaryl isocyanurate (TAIC), triarylamine (TAA), and diarylamine (DAA).

[0051] The coupling agent is a material for increasing the adhesive strength between the active material and the binder, and is characterized by having two or more functional groups, one of which reacts with a hydroxyl group or a carboxyl group on the surface of the silicon, tin or graphite-based active material to form a chemical bond, and the other functional group is a material that forms a chemical bond through a reaction with the nanocomposite according to the present invention, and is not particularly limited. For example, silane-based coupling agents such as triethoxysilylpropyl tetrasulfide, mercaptopropyl triethoxysilane, aminopropyl triethoxysilane, chloropropyl triethoxysilane, vinyltriethoxysilane, methacryloxypropyl triethoxysilane, glycidoxypropyl triethoxysilane, isocyanatopropyl triethoxysilane, and cyanatopropyl triethoxysilane may be used.

[0052] The buffer (buffering agent) is, for example, NaHCO 3 , Na 2 CO 3 , K 2 HPO 4 , K.H. 2 PO 4 , Na 2 HPO 4 , NaOH and NH 4 It may be one selected from the group consisting of OH.

[0053] As the molecular weight regulator, for example, mercaptans, terfins such as terpinolene, dipentene, and t-terpiene, and halogenated hydrocarbons such as chloroform and carbon tetrachloride can be used.

[0054] The emulsifier is a substance having both a hydrophilic group and a hydrophobic group. In one specific example, the emulsifier may be at least one selected from the group consisting of anionic emulsifiers and nonionic emulsifiers.

[0055] Nonionic emulsifiers, when used with anionic emulsifiers, can help control particle size and distribution and provide additional colloidal stabilization through van der Waals forces of the polymer particles in addition to the electrostatic stabilization of the ionic emulsifiers. Nonionic emulsifiers are not often used alone because they produce less stable particles than anionic emulsifiers.

[0056] The anionic emulsifier may be selected from the group consisting of phosphates, carboxylates, sulfates, succinates, sulfosuccinates, sulfonates and disulfonates. For example, the anionic emulsifier may be selected from the group consisting of sodium alkyl sulfate, sodium polyoxyethylene sulfate, sodium lauryl ether sulfate, sodium polyoxyethylene lauryl ether sulfate, sodium lauryl sulfate, sodium alkyl sulfonate, sodium alkyl ether sulfonate, sodium alkyl benzene sulfonate, sodium linear alkyl benzene sulfonate, sodium alpha olefin sulfonate, sodium alcohol polyoxyethylene ether sulfonate, sodium dioctyl sulfosuccinate, sodium perfluorooctane sulfonate, sodium perfluorobutane sulfonate, alkyl diphenyloxide disulfonate, sodium dioctyl sulfosuccinate (DOSS), sodium alkyl-aryl phosphate, alkyl ether phosate, and sodium lauryl sarcosinate. However, the anionic emulsifier is not limited to these, and all known anionic emulsifiers may be included in the scope of the present invention.

[0057] The nonionic emulsifier may be an ester type, an ether type, an ester-ether type, etc. For example, it may be polyoxyethylene glycol, polyoxyethylene glycol methyl ether, polyoxyethylene monoallyl ether, polyoxyethylene bisphenol-A ether, polypropylene glycol, polyoxyethylene alkenyl ether, etc. However, it is not limited thereto, and all known nonionic emulsifiers may be included in the content of the present invention.

[0058] The conjugate diene latex may contain, based on the total weight, 20 to 45% by weight of the (a) conjugated diene monomer or conjugated diene polymer, 50 to 70% by weight of the (b) one or more monomers selected from the group consisting of acrylate monomers, vinyl monomers, and nitrile monomers, and 1 to 20% by weight of the (c) one or more monomers selected from the group consisting of unsaturated carboxylic acid monomers and hydroxyl group-containing monomers. Other components such as the emulsifier, buffer, and crosslinker may be optionally contained within the range of 0.1 to 10% by weight.

[0059] Meanwhile, the average particle size of the conjugate diene latex particles may be 50 nm to 500 nm or less. Here, if the average particle size is less than 50 nm or more than 500 nm, it is not preferable because the dispersion stability may be reduced.

[0060] Meanwhile, when the conjugated diene latex particles in the composition according to the present invention exist as an independent phase, the effect of improving the adhesive strength is improved, so it is very important to prevent the occurrence of agglomeration between the particles. Therefore, the composition according to the present invention includes a dispersion solvent for dispersing the particles. In the present invention, a non-aqueous organic solvent is used as the dispersion solvent.

[0061] The non-aqueous organic solvent may be at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol.

[0062] Preferably, N-methyl-pyrrolidone (NMP) can be used as the non-aqueous organic solvent, but is not limited thereto.

[0063] The moisture content of the insulating layer composition for a lithium secondary battery according to an embodiment of the present invention may be 10,000 ppm or less, preferably 5,000 ppm or less, and more preferably 3,000 ppm or less. When the moisture content is within the above range, the insulating layer composition may be coated separately from the electrode mixture layer, and the physical properties of the electrode may not deteriorate.

[0064] <Positive electrode binder or positive electrode insulating liquid for lithium secondary batteries>

[0065] Another embodiment of the present invention provides a positive electrode binder or a positive electrode insulating liquid for a lithium secondary battery, comprising a conjugated diene copolymer as a binder polymer prepared according to the above-mentioned preparation method and a non-aqueous organic solvent as a dispersion solvent.

[0066] In the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to the present invention, conjugated dienes copolymer particles having an average particle size of 50 nm to 500 nm exist as an independent phase.

[0067] In one embodiment of the present invention, the conjugate diene copolymer may be a styrene-butadiene copolymer, and the non-aqueous organic solvent may be NMP (N-methyl-pyrrolidone).

[0068] In one embodiment of the present invention, the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery may have a water content of 10,000 ppm or less.

[0069] <Lithium secondary battery>

[0070] Another example of the present invention is a lithium secondary battery including the positive electrode binder for lithium secondary batteries or the positive electrode insulating liquid.

[0071] In addition to the electrodes, the lithium secondary battery generally further includes a separator and a non-aqueous electrolyte containing a lithium salt.

[0072] The separation membrane is interposed between the positive and negative electrodes, and is a thin insulating membrane having high ion permeability and mechanical strength. The pore size of the separation membrane is generally 0.01 to 10 μm, and the thickness is generally 5 to 300 μm. As such a separation membrane, for example, a sheet or nonwoven fabric made of an olefin polymer such as polypropylene, which is chemically resistant and hydrophobic, glass fiber, or polyethylene, etc. is used. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte can also serve as the separation membrane.

[0073] The lithium-containing non-aqueous electrolyte solution comprises a non-aqueous electrolyte solution and a lithium salt.

[0074] As the non-aqueous electrolyte, for example, non-quantum organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydroxyfuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate may be used.

[0075] The lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte solution, and is, for example, LiCl, LiBr, LiI, LiClO 4 , LiBF 4 , LiB 10 Cl 10 , LiPF 6 , LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiSbF 6 , LiAlCl 4 , C.H. 3 SO 3 Li, (CF 3 SO 2 ) 2 NLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium 4-phenylborate, imide, etc. are used.

[0076] In some cases, an organic solid electrolyte, an inorganic solid electrolyte, or the like may be used.

[0077] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ionic dissociation groups.

[0078] The inorganic solid electrolyte may be, for example, Li 3 N, LiI, Li 5 NI 2 , Li 3 N-LiI-LiOH, LiSiO 4 , LiSiO 4 -LiI-LiOH, Li 2 SiS 3 , Li 4 SiO 4 , Li 4 SiO 4 -LiI-LiOH, Li 3 PO 4 -Li 2 S-SiS 2 Nitrides, halides, sulfates, etc. of Li such as Li may be used.

[0079] In addition, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. may be added to the non-aqueous electrolyte solution in order to improve charge / discharge characteristics, flame retardancy, etc. In some cases, a halogen-containing solvent such as carbon tetrachloride or ethylene trifluoride may be further added to impart non-flammability, carbon dioxide may be further added to improve high-temperature storage characteristics, and FEC (Fluoro-Ethylene Carbonate), PRS (Propenesultone), etc. may be further added.

[0080] The secondary battery according to the present invention is not only used as a battery cell used as a power source for small devices, but is also preferably used as a unit battery for medium- to large-sized battery modules containing a large number of battery cells used as a power source for medium- to large-sized devices.

[0081] Preferred examples of the medium- to large-sized devices include, but are not limited to, power tools that are driven by a battery motor, electric vehicles including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), etc., electric bicycles (E-bikes), electric scooters (E-scooters), electric golf carts, and energy storage systems.

[0082] The present invention will be described in detail below with reference to examples. However, the following examples are merely illustrative of the present invention and are not intended to limit the present invention.

[0083] [Example 1]

[0084] 5 parts by weight of styrene-butadiene seed latex with a particle size of 55 nm was placed in a reactor and heated to 80 ° C., and then 38 g of 1,3-butadiene as a monomer, 59 g of styrene, 3 g of acrylic acid, and NaHCO as a buffer were added. 30.5g of styrene butadiene copolymer, 1g of alkyldiphenyloxide disulfonate as emulsifier, 1g of dodecyl mercaptan as molecular weight regulator, and 1g of potassium persulfate as polymerization initiator were added to the reactor for 4 hours, and the reaction was continued for another 4 hours at 80°C to produce a styrene butadiene copolymer latex with a solid content of 50%. At this time, the pH was adjusted to neutral (7) using sodium hydroxide. After polymerization, the size of the copolymer particles was analyzed using a submicron particle sizer (Nicomp TM 380), and the average particle size of the polymerized copolymer particles was 150 nm.

[0085] 100g of the prepared styrene butadiene copolymer latex was placed in a reactor, 600g of NMP (N-methyl-pyrrolidone) was added, mixed, and heated to 90℃. The pressure was reduced to 60 torr within 8 hours to replace the water, which is the dispersion solvent of the styrene butadiene copolymer particles, with NMP, and a composition containing a styrene butadiene copolymer dispersed in NMP was prepared. At this time, the final water content was 10,000ppm or less and the solid content was 7.8%. The remaining water was vaporized using a heating and decompression device, and the vaporized water was collected in a receiver reactor in a liquid state through a cooling device. At this time, excess NMP was also vaporized together with the water, and further NMP was added to adjust the final solid content.

[0086] [Example 2]

[0087] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that the temperature was raised to 90° C. and the pressure was reduced to 15 torr for 4 hours.

[0088] [Example 3]

[0089] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that the temperature was raised to 80° C. and the pressure was reduced to 10 torr for 8 hours.

[0090] [Example 4]

[0091] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that the temperature was raised to 70° C. and the pressure was reduced to 10 torr for 15 hours.

[0092] [Example 5]

[0093] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that the temperature was raised to 100° C. and then the pressure was reduced to 180 torr for 20 hours.

[0094] [Example 6]

[0095] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that 600 g of NMP was added, the temperature was raised to 50° C., and the pressure was reduced to 10 torr for 12 hours.

[0096] [Comparative Example 1]

[0097] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that 600 g of NMP was added, the temperature was raised to 95° C., and the pressure was reduced to 200 torr for 20 hours.

[0098] [Comparative Example 2]

[0099] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that the temperature was raised to 70° C. and the pressure was reduced to 60 torr for 15 hours.

[0100] [Comparative Example 3]

[0101] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that the temperature was raised to 110° C. and the pressure was reduced to 10 torr for 8 hours.

[0102] [Comparative Example 4]

[0103] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that 600 g of NMP was added, the temperature was raised to 39° C., and the pressure was reduced to 10 torr for 20 hours.

[0104] The temperature, time, pressure and solid content conditions of Examples 1 to 4 and Comparative Examples 1 to 4 are summarized in Table 1 below.

[0105] [Comparative Example 5] Preparation of a composition containing styrene butadiene latex without replacing the dispersion solvent

[0106] To compare with a composition containing styrene-butadiene latex without solvent replacement, the styrene-butadiene latex prepared in Example 1 was mixed with carboxymethyl cellulose in a weight ratio of 9:1 without solvent replacement to prepare a composition. Carboxymethyl cellulose is used as a thickener to improve the coatability of styrene-butadiene latex without solvent replacement.

[0107] [Table 1]

[0108] The compositions containing the styrene-butadiene copolymer dispersed in NMP produced in Examples 1 to 6 and Comparative Examples 1 to 4 were evaluated for viscosity and water content.

[0109] [Experimental Example 1] Viscosity

[0110] The viscosity of the compositions containing the styrene-butadiene copolymer dispersed in NMP prepared in Examples 1 to 6 and Comparative Examples 1 to 4 was measured. The viscosity was measured at 25° C. using a Brookfield LV viscometer with a No. 63 spindle, rotated at 12 rpm, and then measured 1 minute later. When the viscosity was outside the measurement range, the rpm was lowered and the measurement was performed, and the results are shown in Table 2 below. In Table 2 below, the viscosity means the viscosity at a solid content of 7.8%.

[0111] [Experimental Example 2] Moisture content

[0112] The moisture content of the compositions prepared in Examples 1 to 6 and Comparative Examples 1 to 4 was measured by weighing 0.1 to 0.4 g of each sample using a Metrohm 899 Coulometer connected to an 860KF Thermoprep oven at 220° C. The measurement results are shown in Table 2 below.

[0113] [Experimental Example 3] Particle size measurement

[0114] The particle sizes of the compositions prepared in Examples 1 to 6 and Comparative Examples 1 to 4 were measured using a Nicom N3000 DLS particle size analyzer, and the results are shown in Table 2 below. The compositions containing styrene-butadiene copolymer dispersed in NMP prepared in Examples 1 to 6 and Comparative Examples 1 to 4 were diluted to 0.12±0.02 wt% with NMP, and the viscosity and refractive index of NMP were input into the DLS device and then measured. Although it was difficult to measure the absolute particle size due to scattering from the NMP solvent, it was possible to make a relative comparison of the particle sizes.

[0115] [Table 2]

[0116] [Experimental Example 4] Moisture effect evaluation

[0117] LiNi as the positive electrode active material 0.8 Co 0.2 Mn 0.2 O 2 96 parts by weight of the positive electrode mixture layer, 2 parts by weight of PVdF as a binder, and 2 parts by weight of carbon black as a conductive material were weighed and mixed in N-methylpyrrolidone (NMP) solvent to produce a slurry for the positive electrode mixture layer.

[0118] The slurry for the positive electrode mixture layer and the slurry for the insulating coating layer, which is a composition containing a styrene-butadiene copolymer prepared in each of Examples 1 to 6 and Comparative Examples 1 and 5, were simultaneously applied to a current collector using a doctor blade so as to be overlaid, and the results were compared immediately after application and after 1 minute had elapsed. In the case of Comparative Example 3, gelation occurred, making coating impossible. Here, gelation refers to a state in which the viscosity of the composition increases excessively, reducing fluidity and making it impossible to coat with a certain thickness.

[0119] As a result of comparing the results immediately after application and 1 minute after application, in the case of the slurries for insulating coating layers prepared in Examples 1 to 4, the initial coated state was maintained without penetration into the overlay both immediately after application and 1 minute after application, as shown in Figure 1, but in the case of the slurries for insulating coating layers prepared in Comparative Examples 1 to 5, which have a moisture content of 10,000 ppm or more, the electrode slurry penetrated into the insulating layer side 1 minute after application, making it impossible to reliably maintain the coating boundary. In the case of the slurry for insulating coating layer of Comparative Example 5, which did not have a solvent replacement, it was confirmed that the boundary where the positive electrode slurry and the insulating liquid come into contact was coagulated by moisture immediately after application, which confirmed that simultaneous coating was impossible.

[0120] As shown in Table 2, gelation occurred when the solvent was replaced with NMP at 110°C or higher as in Comparative Example 3. It was confirmed that at high temperatures of 110°C or higher, the stability of styrene-butadiene copolymer particles decreased and they aggregated together to form a gel, regardless of the pressure reduction level.

[0121] When a gel is formed, the particles lose stability and aggregate together, which can be confirmed by measuring the average particle size, and it can be confirmed that the average particle size of the composition prepared in Comparative Example 3 is significantly larger than that of the compositions prepared in Examples 1 to 4. When the particles aggregate together, the coating properties decrease, and when a gel is finally formed, there is no fluidity and coating is impossible, so it cannot be used as an insulating liquid.

[0122] When the pressure was reduced to 200 torr or more as in Comparative Example 1, the final moisture content exceeded 10,000 ppm even after a long period of reduced pressure of 20 hours. When the pressure was reduced to 10 torr but the temperature was less than 40°C as in Comparative Example 4, the moisture content exceeded 10,000 ppm even after a period of reduced pressure of 20 hours. Furthermore, even if the temperature during the substitution step was 40°C to 100°C or less and the reduced pressure was less than 200 torr, if the relationship between pressure, temperature and time does not satisfy Relational Formula 1 as in Comparative Example 2, the moisture content cannot be kept below the expected level in the process.

Claims

1. The method comprises adding a non-aqueous organic solvent to a water-dispersed conjugate diene latex, and heating and reducing the pressure. A method for producing a positive electrode binder or a positive electrode insulating liquid for a lithium secondary battery.

2. In the heating and depressurizing step, water, which is a dispersion medium for the conjugated diene latex particles, is replaced with a non-aqueous organic solvent. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 1.

3. The conjugate diene latex particles maintain their particle shape even after the dispersion solvent is replaced with a non-aqueous organic solvent. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 2.

4. The step is characterized in that the heating step is performed at a temperature of 40°C to 100°C. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 1.

5. The step is characterized in that the pressure is reduced to less than 200 torr. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 1.

6. The step is carried out for 1 hour to 20 hours. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 1.

7. The step is characterized in that the temperature is raised to 40°C to 100°C and the pressure is reduced to less than 200 torr for 1 hour to 20 hours. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 1.

8. The step is characterized in that the pressure, temperature and time satisfy the following relationship 1: A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 1. [Relationship 1] y (minimum pressure, torr) / x (temperature, K) 17.4 * 10 44 / z(time, h) 0.5 <8

9. The conjugate diene latex contains (a) a conjugated diene monomer or a conjugated diene polymer, (b) at least one monomer selected from the group consisting of an acrylate monomer, a vinyl monomer, and a nitrile monomer, and (c) a polymer of at least one monomer selected from the group consisting of an unsaturated carboxylic acid monomer and a hydroxyl group-containing monomer. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 1.

10. the conjugated diene monomer is one monomer selected from the group consisting of 1,3-butadiene, isoprene, chloroprene, and piperylene; The conjugated diene polymer is a polymer of two or more monomers selected from the group consisting of 1,3-butadiene, isoprene, chloroprene and piperylene, a styrene-butadiene copolymer, an acrylonitrile-butadiene copolymer, a styrene-isoprene copolymer, an acrylate-butadiene rubber, an acrylonitrile-butadiene-styrene rubber, an ethylene-propylene-diene polymer, a partially epoxidized or brominated polymer of these polymers, or a mixture thereof. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 9.

11. The acrylate monomer is at least one monomer selected from the group consisting of methyl ethacrylate, methacryloxyethyl ethylene urea, β-carboxyethyl acrylate, aliphatic monoacrylate, dipropylene diacrylate, ditrimethylolpropane tetraacrylate, dipentaerythriol hexaacrylate, pentaerythriol triacrylate, pentaerythriol tetraacrylate, and glycidyl methacrylate. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 9.

12. The vinyl monomer is one or more monomers selected from the group consisting of styrene, α-methylstyrene, β-methylstyrene, pt-butylstyrene, and divinylbenzene; A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 9.

13. The nitrile monomer is one or more monomers selected from the group consisting of acrylonitrile, methacrylonitrile, and allyl cyanide. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 9.

14. The unsaturated carboxylic acid monomer is one or more monomers selected from the group consisting of maleic acid, fumaric acid, methacrylic acid, acrylic acid, glutaric acid, itaconic acid, tetrahydrophthalic acid, crotonic acid, isocrotonic acid, and nadic acid. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 9.

15. The hydroxy group-containing monomer is one or more monomers selected from the group consisting of hydroxyacrylate, hydroxyethyl acrylate, hydroxybutyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 9.

16. The conjugate diene latex contains, based on the total weight, 25 to 45% by weight of (a) a conjugated diene monomer or a conjugated diene polymer, 50 to 70% by weight of (b) one or more monomers selected from the group consisting of an acrylate monomer, a vinyl monomer, and a nitrile monomer, and 1 to 20% by weight of (c) a polymer of one or more monomers selected from the group consisting of an unsaturated carboxylic acid monomer and a hydroxyl group-containing monomer. A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 9.

17. The non-aqueous organic solvent is at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethylmethyl carbonate (EMC), dimethylcarbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol; A method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 1.

18. the conjugate diene latex is a styrene-butadiene latex; The non-aqueous organic solvent is NMP (N-methyl-pyrrolidone); The method for producing the positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 1 .

19. A dispersion medium comprising a conjugated dienes copolymer as a binder polymer and a non-aqueous organic solvent as a dispersion solvent, the dispersion medium being produced according to the production method of any one of claims 1 to 18. Positive electrode binder or positive electrode insulating liquid for lithium secondary batteries.

20. Conjugated dienes copolymer particles having an average particle size of 50 nm to 500 nm are present as a separate phase; The positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 19.

21. the conjugate diene copolymer is a styrene-butadiene copolymer; The non-aqueous organic solvent is NMP (N-methyl-pyrrolidone); The positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 19.

22. The moisture content is 10,000 ppm or less. The positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 19.

23. The positive electrode binder or positive electrode insulating liquid for a lithium secondary battery according to claim 19 is provided. Lithium secondary battery.

Citation Information

Patent Citations

  • Method of manufacturing lithium ion secondary battery, electrode and battery

    JP2001176517A

  • Negative electrode mixture paste for nonaqueous secondary battery, negative electrode and nonaqueous secondary battery using it as well as manufacturing method of negative electrode mixture paste

    JP2007234418A

  • Method for manufacturing slurry for lithium ion secondary battery heat-resistant layer and method for manufacturing electrode for lithium ion secondary battery

    JP2014165096A

  • Binder composition for secondary battery, electrode for secondary battery containing same, and lithium secondary battery

    JP2019537232A

  • Binder composition for secondary battery, electrode slurry composition containing the same, electrode, and secondary battery

    JP2020516021A