Method for forming low resistivity tungsten features
A method using a boron-tungsten nucleation layer and differential inhibition in a single processing chamber addresses voids and seams in tungsten deposition, achieving low resistivity and reliable tungsten features in semiconductor manufacturing.
Patent Information
- Application Number
- JP2024520809
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-04-27
- Filing Date
- 2022-07-25
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2042-07-25
AI Technical Summary
Conventional tungsten deposition processes in semiconductor manufacturing face challenges in forming voids and seams, leading to device performance and reliability issues as feature sizes shrink, making it difficult to achieve low resistivity and void-free tungsten features.
A method involving a nucleation layer with boron and tungsten, a differential inhibition profile, and a filler layer is used to form tungsten features with a resistivity of 16 μΩ·cm or less, utilizing a single processing chamber for nucleation, inhibition, and gap-filling without substrate transfer, and subsequent annealing to enhance grain growth and reduce resistivity.
The method results in seamless, low-resistivity tungsten features with reduced surface roughness and improved device reliability by minimizing voids and seams, achieving resistivities as low as 10-16 μΩ·cm across various film thicknesses.
Smart Images

Figure 2024536376000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE Embodiments herein relate to methods used in electronic device manufacturing, and more particularly, to methods used to form tungsten features in semiconductor devices. [Background technology]
[0002] Tungsten (W) is widely used in integrated circuit (IC) device fabrication to form conductive features where relatively low electrical resistance and relatively high resistance to electromigration are desired. For example, tungsten may be used as a metal fill material to form source contacts, drain contacts, metal gate fill, gate contacts, interconnects (e.g., horizontal features formed on the surface of a dielectric material layer), and vias (e.g., vertical features formed through a dielectric material layer to connect other interconnect features located above or below the dielectric material layer). Due to its relatively low resistivity, tungsten is also commonly used to form bit lines and word lines used to address individual memory cells in memory cell arrays of dynamic random access memory (DRAM) devices.
[0003] As circuit density increases and device features continue to shrink to meet the demands of next generation semiconductor devices, it is becoming increasingly difficult to reliably manufacture tungsten features. Problems such as voids and seams that form during traditional tungsten deposition processes are amplified as feature sizes shrink and can adversely affect device performance and reliability, or even render the device inoperable.
[0004] Therefore, there is a need for a process for filling contact features that is free or substantially free of voids and seams and has low resistivity for a variety of film thicknesses. Summary of the Invention
[0005] A structure is provided that includes a tungsten-containing layer including a nucleation layer and a fill layer. The nucleation layer is disposed along a sidewall of an opening. The nucleation layer includes boron and tungsten. The fill layer is disposed within the opening over the nucleation layer. The tungsten-containing layer includes a resistivity of about 16 μΩ·cm or less. The tungsten-containing layer has a thickness of about 200 Å to about 600 Å. The thickness of the tungsten-containing layer is half the width of the tungsten-containing layer disposed within the opening between opposing sidewall portions of the opening.
[0006] A structure on a substrate is provided that includes an opening in the substrate. An adhesion layer is disposed on sidewalls of the opening and a tungsten-containing layer is disposed on the adhesion layer in the sidewalls. The tungsten-containing layer has a resistivity of about 16 μΩ·cm or less, and the tungsten-containing layer has a thickness of about 200 Å to about 600 Å. The thickness of the tungsten-containing layer is half the width of the tungsten-containing layer disposed in the opening between opposing sidewall portions of the opening.
[0007] A method of forming a structure is provided. The method includes exposing a substrate to a tungsten-containing precursor gas at a precursor gas flow rate. The substrate is exposed to a reducing agent including boron at a reducing agent flow rate. The tungsten-containing precursor gas and the reducing agent are cyclically alternated to form a nucleation layer on the substrate in at least one opening in the substrate. The method includes depositing a fill layer on the nucleation layer in the at least one opening. The substrate is annealed at about 600°C to about 1000°C.
[0008] So that the above-mentioned features of the present disclosure can be understood in detail, a more particular description of the present disclosure summarized above can be made by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings depict only exemplary embodiments and therefore should not be considered as limiting its scope, as other equally effective embodiments may be recognized. [Brief description of the drawings]
[0009] [Figure 1A]1 is a schematic cross-sectional view of a portion of a substrate illustrating undesirable void or seam formation in a conventionally formed tungsten feature. [Figure 1B] 1 is a schematic cross-sectional view of a portion of a substrate illustrating undesirable void or seam formation in a conventionally formed tungsten feature. [Figure 2A] 1 is a schematic side view of a processing system that can be used to perform the methods described herein, according to one embodiment. [Figure 2B] 2B is an enlarged cross-sectional view of a portion of the processing system shown in FIG. 2A, according to one embodiment. [Diagram 3] 2B is an enlarged cross-sectional view of a portion of the processing system shown in FIG. 2A, according to one embodiment. [Figure 4] 1 is a schematic side view of a rapid thermal processing system that can be used to perform the methods described herein, according to one embodiment. [Diagram 5] 1 illustrates a method of processing a substrate, according to one embodiment. [Figure 6A] 1 is a schematic cross-sectional side view of a substrate prior to processing, according to one embodiment. [Figure 6B] 1A-1D are schematic cross-sectional side views of a substrate at one stage of processing, according to one embodiment. [Figure 6C] 1A-1D are schematic cross-sectional side views of a substrate at one stage of processing, according to one embodiment. [Figure 7] 1 is a comparative curve showing the resistivity of film layers formed using methods described herein and comparative methods at various film thicknesses, according to some embodiments. [Figure 8] 1 is a comparative curve showing the resistivity of a film layer formed using the methods described herein before and after annealing at various temperatures, according to some embodiments. [Figure 9] 1 is a comparative curve showing the resistivity of a film layer formed using the methods described herein before and after annealing at various film thicknesses, according to some embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] For ease of understanding, the same reference numbers have been used, where possible, to designate identical elements common to the figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further description.
[0011] SUMMARY OF THE DISCLOSURE
[0003] Embodiments herein are directed generally to electronic device manufacturing, and more particularly, to systems and methods for forming low resistivity tungsten features in semiconductor device manufacturing schemes.
[0012] FIG. 1A is a schematic cross-sectional view of a substrate 10A showing an undesired void 20 formed during a conventional tungsten deposition process. Here, substrate 10A includes a patterned surface 11 including a dielectric layer 12 having a high aspect ratio opening (shown filled with a portion of tungsten layer 15) formed therein, a barrier material layer 14 deposited on dielectric layer 12 to line the opening, and a tungsten layer 15 deposited on barrier material layer 14. Tungsten layer 15 is formed using a conventional deposition process, e.g., a chemical vapor deposition (CVD) or atomic layer deposition (ALD) process, to conformally deposit (grow) tungsten on patterned surface 11 to fill the opening. Tungsten layer 15 forms tungsten features 15A in the opening and forms an overburden of material (tungsten overburden layer 15B) over the fields of patterned surface 11.
[0013] In FIG. 1A, the opening has a non-uniform profile that is narrower at the surface of the substrate 10A and becomes wider (bows outward) as the opening extends inward from the surface into the dielectric layer 12. As shown, the overhanging portions of the conformal tungsten layer 15 grow together to block or "pinch off" the entrance to the opening before the opening is completely filled, causing an undesired void 20, i.e., loss of tungsten material, in the tungsten feature 15A. If the void 20 opens (exposes) during a subsequent CMP process, polishing fluid can penetrate the tungsten feature 15A, and the chemically active components of the polishing fluid can cause further loss of tungsten material, e.g., undesired coring (keyholing) of the feature by corrosion and / or static etching of the tungsten material. This undesired loss of tungsten can lead to device performance and reliability issues, or ultimately complete failure of the device. Even without void formation, undesirable seam formation in tungsten features is almost unavoidable when using conventional tungsten deposition processes such as that shown in FIG. 1B.
[0014] FIG. 1B is a schematic cross-sectional view of a substrate 10B showing an undesired seam 24 formed during a conventional tungsten deposition process. Here, the patterned surface 11 includes an opening (filled with a portion of the tungsten layer 15) having a substantially uniform profile as the opening extends from the surface of the substrate 10B into the dielectric layer 12. The opening is filled with tungsten and no voids are formed. Nevertheless, an undesired seam 24 is formed in the opening that extends through the center of the tungsten feature 15A due to the conformal growth of the tungsten layer 15 outward from the walls of the opening. Similar to the void 20 shown in FIG. 1A, the seam 24 is vulnerable to attack by chemically active components of the tungsten polishing solution and may cause undesired loss of tungsten material from the feature 15A if the seam 24 is exposed during the CMP process.
[0015] Accordingly, embodiments herein provide a processing system configured to perform a combination of individual aspects of the present methods without transferring substrates between processing chambers, thus improving the overall substrate processing throughput and capacity of the tungsten gap fill processing scheme described herein.
[0016] In general, the gap-fill processing scheme includes forming a differential tungsten deposition inhibition profile in a feature opening formed in a surface of a substrate, filling the opening with a tungsten material according to the inhibition profile, and depositing an overburden of tungsten on the field surface of the substrate. Forming a tungsten deposition inhibition profile typically includes forming a tungsten nucleation layer and treating the tungsten nucleation layer with active nitrogen species, e.g., treatment radicals. The nitrogen treatment radicals are incorporated into a portion of the nucleation layer, e.g., by adsorption of the nitrogen species and / or by reaction with the metallic tungsten of the nucleation layer to form tungsten nitride (WN). The adsorbed nitrogen and / or the nitrided surface of the tungsten nucleation layer desirably retard (inhibit) tungsten nucleation and thus retard (inhibit) subsequent tungsten deposition.
[0017] In some embodiments, the treatment radicals are formed remotely from the substrate processing chamber by using a remote plasma source fluidly coupled to the substrate processing chamber. The desired inhibition effect on the fields of the patterned surface and the desired inhibition profile in the openings formed in the patterned surface are achieved by controlling the process conditions in the process chamber, such as temperature and pressure, and controlling the concentration, flux, and energy of the treatment radicals at the substrate surface. Typically, the treatment radicals are formed from a non-halogen nitrogen-containing gas, such as N2, NH3, NH4, or a combination thereof.
[0018] The tungsten nucleation and deposition process of the gap-fill processing scheme generally involves flowing a tungsten-containing precursor and a reducing agent into a processing chamber and exposing a substrate surface to the tungsten-containing precursor and the reducing agent, which react at the substrate surface in one of a chemical vapor deposition (CVD) process, a pulsed CVD process, an atomic layer deposition (ALD) process, or a combination thereof, to deposit a tungsten material on the substrate surface.
[0019] The processing systems described herein are configured to periodically perform chamber cleaning operations in which undesirable tungsten residues are removed from the interior surfaces of the processing chamber using cleaning chemistries, such as cleaning chemistries that include activated halogen species, e.g., fluorine or chlorine (cleaning) radicals, formed remotely from the processing chamber.
[0020] A chamber cleaning operation generally involves flowing halogen cleaning radicals into the processing chamber, reacting the cleaning radicals with tungsten residues to form volatile tungsten species, and exhausting the volatile tungsten species from the processing chamber through an exhaust. Chamber cleaning operations are typically performed between substrate processing, i.e., after a processed substrate has been removed from the processing chamber and before a next processed substrate is received into the processing chamber for processing.
[0021] 2A-2B illustrate generally a processing system 200 that may be used to perform the bottom-up tungsten gap-fill substrate processing methods described herein, where the processing system is configured to provide different processing conditions desired for each of the nucleation, inhibition treatment, selective gap-fill, and overburden deposition processes within a single processing chamber 202, i.e., without transferring the substrate between multiple processing chambers.
[0022] As shown in Figure 2A, the processing system 200 includes a processing chamber 202, a gas delivery system 204 fluidly coupled to the processing chamber 202, and a system controller 208. The processing chamber 202 (shown in cross-section in Figure 2A) includes a chamber lid assembly 210, one or more sidewalls 212, and a chamber base 214, which collectively define a processing volume 215. The processing volume 215 is fluidly coupled to an exhaust 217, such as one or more vacuum pumps, which are used to maintain the processing volume 215 at sub-atmospheric pressure and to evacuate processing gases and processing by-products therefrom.
[0023] The chamber lid assembly 210 includes a lid plate 216 and a showerhead 218 coupled to the lid plate 216 and defining a gas distribution volume 219 therewith, where the lid plate 216 is maintained at a desired temperature using one or more heaters 229 thermally coupled thereto. The showerhead 218 faces a substrate support assembly 220 disposed within the processing volume 215. As described below, the substrate support assembly 220 is configured to move a substrate support 222, and thus a substrate 230 disposed on the substrate support 222, between an elevated substrate processing position (shown) and a lowered substrate transfer position (not shown). When the substrate support assembly 220 is in the elevated substrate processing position, the showerhead 218 and the substrate support 222 define a processing region 221.
[0024] The gas supply system 204 is fluidly coupled to the processing chamber 202 via a gas inlet 223 (FIG. 2B) disposed through the lid plate 216. Processing or cleaning gases supplied by use of the gas supply system 204 enter the gas distribution volume 219 through the gas inlet 223 and are distributed to the processing region 221 through a plurality of openings 232 (FIG. 2B) in the showerhead 218. In some embodiments, the chamber lid assembly 210 further includes a perforated shield plate 225 disposed between the gas inlet 223 and the showerhead 218. In these embodiments, gases entering the gas distribution volume 219 are first diffused by the shield plate 225, which, together with the showerhead 218, provides a more uniform or desired distribution of gas flow to the processing region 221.
[0025] Process gases and process by-products are exhausted radially outward from the processing region 221 through an annular channel 226 that surrounds the processing region 221. The annular channel 226 may be formed in a first annular liner 227 disposed radially inward of the one or more sidewalls 212 (as shown) or may be formed in the one or more sidewalls 212. In some embodiments, the processing chamber 202 includes one or more second liners 228 used to protect the inner surface of the one or more sidewalls 212 or the chamber base 214 from corrosive gases and / or undesirable material deposition.
[0026] In some embodiments, a purge gas source 237 in fluid communication with the process volume 215 is used to flow a chemically inert purge gas, such as argon (Ar), through an opening in the chamber base 214 surrounding the support shaft 262, into a region disposed below the substrate support 222. The purge gas can be used to create a region of positive pressure (compared to the pressure in the process region 221) below the substrate support 222 during substrate processing. Typically, the purge gas introduced through the chamber base 214 flows upward therefrom, around the edge of the substrate support 222, and is exhausted from the process volume 215 through the annular channel 226. The purge gas reduces and / or prevents the flow of material precursor gases into the substrate support 222, thereby reducing undesired material deposition on surfaces below the substrate support 222.
[0027] The substrate support assembly 220 includes a movable support shaft 262 that extends through the chamber base 214 in a sealed manner, such as surrounded by a bellows 265 in an area below the chamber base 214, and a substrate support 222 disposed on the movable support shaft 262. To facilitate transfer of a substrate to and from the substrate support 222, the substrate support assembly 220 includes a lift pin assembly 266 that includes a plurality of lift pins 267 coupled to or disposed in engagement with a lift pin hoop 268. The plurality of lift pins 267 are movably disposed in openings formed through the substrate support 222. When the substrate support 222 is disposed in a lowered substrate transfer position (not shown), the plurality of lift pins 267 extend above a substrate receiving surface of the substrate support 222 to lift a substrate 230 from the substrate receiving surface and provide access to a backside (non-active) surface of the substrate 230 by a substrate handler (not shown). When the substrate support 222 is in the raised or processing position (as shown), the plurality of lift pins 267 are retracted below the substrate receiving surface of the substrate support 222 to allow the substrate 230 to rest on the substrate receiving surface.
[0028] Substrates 230 are transferred to and from the substrate support 222 through a door 271, e.g., a slit valve disposed in one of the one or more side walls 212, where one or more openings in the area surrounding the door 271, e.g., an opening in the door housing, are fluidly coupled to a purge gas source 237, e.g., an Ar gas source. The purge gas is used to prevent process and cleaning gases from contacting and / or degrading the seal surrounding the door, thus extending its useful life.
[0029] The substrate support 222 is configured for vacuum chucking, in which the substrate 230 is secured to the substrate support 222 by applying a vacuum to an interface between the substrate 230 and the substrate receiving surface. The vacuum is applied using a vacuum source 272 fluidly coupled to one or more channels or ports formed in the substrate receiving surface of the substrate support 222. In other embodiments, the substrate support 222 may be configured for electrostatic chucking, for example, when the processing chamber 202 is configured for direct plasma processing. In some embodiments, the substrate support 222 includes one or more electrodes (not shown) coupled to a bias voltage power supply (not shown), such as a continuous wave (CW) RF power supply or a pulsed RF power supply, that provides a bias voltage.
[0030] As shown, the substrate support assembly 220 features a dual-zone temperature control system for providing independent temperature control in different regions of the substrate support 222. The different temperature control regions of the substrate support 222 correspond to different regions of the substrate 230 disposed on the substrate support 222. Here, the temperature control system includes a first heater 263 and a second heater 264. The first heater 263 is disposed in a central region of the substrate support 222, and the second heater 264 is disposed radially outward from the central region to surround the first heater. In other embodiments, the substrate support 222 can have a single heater or more than two heaters.
[0031] In some embodiments, the substrate support assembly 220 further includes an annular shadow ring 235 that is used to prevent undesired material deposition on the beveled circumferential edges of the substrate 230. During substrate transfer to and from the substrate support 222, i.e., when the substrate support assembly 220 is disposed in a lowered position (not shown), the shadow ring 235 rests on an annular ledge in the processing volume 215. When the substrate support assembly 220 is disposed in a raised or processing position, a radially outer surface of the substrate support 222 engages the annular shadow ring 235 such that the shadow ring 235 circumscribes the substrate 230 disposed on the substrate support 222. Here, the shadow ring 235 is shaped such that a radially inward portion of the shadow ring 235 is disposed above the beveled edges of the substrate 230 when the substrate support assembly 220 is in the raised, substrate processing position.
[0032] In some embodiments, the substrate support assembly 220 further includes an annular purge ring 236 disposed on the substrate support 222 to circumscribe the substrate 230. In these embodiments, the shadow ring 235 may be disposed on the purge ring 236 when the substrate support assembly 220 is in the elevated substrate processing position. Typically, the purge ring 236 features a plurality of radially inward openings that are in fluid communication with a purge gas source 237. During substrate processing, purge gas flows into the annular region defined by the shadow ring 235, the purge ring 236, the substrate support 222, and the beveled edge of the substrate 230 to prevent process gas from entering the annular region and causing undesired material deposition on the beveled edge of the substrate 230.
[0033] In some embodiments, the processing chamber 202 is configured for direct plasma processing. In these embodiments, the showerhead 218 may be electrically coupled to a first power source 231, such as an RF power source, that provides power via capacitive coupling to ignite and maintain a plasma of the processing gases flowing into the processing region 221. In some embodiments, the processing chamber 202 includes an inductive plasma generator (not shown), and the plasma is formed by inductively coupling RF power to the processing gases.
[0034] The processing system 200 is advantageously configured to perform each of the tungsten nucleation process, the inhibition treatment process, and the bulk tungsten deposition process of a void-free and seam-free tungsten gap-fill process scheme without removing the substrate 230 from the processing chamber 202. Gases used to perform the individual processes of the gap-fill process scheme and to clean residues from the interior surfaces of the processing chamber are supplied to the processing chamber 202 using a gas supply system 204 that is fluidly coupled to the processing chamber 202.
[0035] Generally, the gas supply system 204 includes one or more remote plasma sources, here first and second radical generators 206A-206B, a deposition gas source 240, and a conduit system 294 (e.g., multiple conduits 294A-294F) that fluidly couples the radical generators 206A-206B and the deposition gas source 240 to the lid assembly 210. The gas supply system 204 further includes multiple isolation valves, here first and second valves 290A-290B, respectively, disposed between the radical generators 206A-206B and the lid plate 216, which can be used to fluidly isolate each of the radical generators 206A-206B from the processing chamber 202 and from each other.
[0036] Each of the radical generators 206A-206B features a chamber body 280 that defines a respective first and second plasma chamber volume 281A-281B (FIG. 2B). Each of the radical generators 206A-206B is coupled to a respective power source 293A-293B. The power sources 293A-293B are used to ignite and maintain a plasma 282A-282B of gas supplied to the plasma chamber volume 281A-281B from a corresponding first or second gas source 287A-287B fluidly coupled to the plasma chamber volume 281A-281B. In some embodiments, the first radical generator 206A generates radicals used in a differential inhibition process. For example, the first radical generator 206A can be used to ignite and maintain a processing plasma 282A from a halogen-free gas mixture supplied to the first plasma chamber volume 281A from the first gas source 287A. The second radical generator 206B may be used to generate cleaning radicals used in the chamber cleaning process by igniting and sustaining a cleaning plasma 282B from a halogen-containing gas mixture supplied from a second gas source 287B to the second plasma chamber volume 281B.
[0037] Typically, nitrogen processing radicals are relatively short-lived (when compared to halogen cleaning radicals) and may exhibit a relatively high susceptibility to recombination through collisions with surfaces in the gas delivery system 204 and / or other species in the processing plasma effluents. Thus, in embodiments herein, the first radical generator 206A is typically positioned closer to the gas inlet 223 than the second radical generator 206B, for example, to provide a relatively short travel distance from the first plasma chamber volume 281A to the processing region 221.
[0038] In some embodiments, the first radical generator 206A is also fluidly coupled to a second gas source 287B, which supplies a halogen-containing conditioning gas to the first plasma chamber volume 281A for use in the plasma source conditioning process. In these embodiments, the gas delivery system 204 can further include a plurality of diverter valves 291 operable to direct the halogen-containing mixed gas from the second gas source 287B to the first plasma chamber volume 281A.
[0039] Suitable remote plasma sources that may be used for either or both of the radical generators 206A-206B include radio frequency (RF) or very high frequency (VHRF) capacitively coupled plasma (CCP) sources, inductively coupled plasma (ICP) sources, microwave induced (MW) plasma sources, electron cyclotron resonance (ECR) chambers, or high density plasma (HDP) chambers.
[0040] As shown, the first radical generator 206A is fluidly coupled to the process chamber 202 by using first and second conduits 294A-294B that extend upward from the gas inlet 223 and connect with the outlet of the first plasma chamber volume 281A. A first valve 290A disposed between the first conduit 294A and the second conduit 294B is used to selectively fluidly isolate the first radical generator 206A from the process chamber 202 and other portions of the gas delivery system 204. Typically, the first valve 290A is closed during a chamber cleaning process to prevent activated cleaning gas, e.g., halogen radicals, from entering the first plasma chamber volume 281A and damaging its surfaces.
[0041] The second radical generator 206B is fluidly coupled to the second conduit 294B, and thus to the processing chamber 202, by using third and fourth conduits 294C-294D. The second radical generator 206B is selectively isolated from the processing chamber 202 and other portions of the gas delivery system 204 by using a second valve 290B disposed between the third conduit 294C and the fourth conduit 294D.
[0042] Deposition gases, e.g., a tungsten-containing precursor and a reducing agent, are supplied to the process chamber 202 from the deposition gas source 240 using a fifth conduit 294E. As shown, the fifth conduit 294E is coupled to the second conduit 294B in proximity to the gas inlet 223 such that the first and second radical generators 206A-206B, respectively, can be isolated from the deposition gases introduced into the process chamber 202 using the first and second valves 290A-290B. In some embodiments, the gas supply system 204 further includes a sixth conduit 294F coupled to the fourth conduit 294D in proximity to the second valve 290B. The sixth conduit 294F is fluidly coupled to a bypass gas source 238, e.g., an argon (Ar) gas source, which can be used to periodically purge undesirable residual cleaning gas, residual inhibiting gas, and / or residual deposition gas from a portion of the gas supply system 204.
[0043] The operation of the processing system 200 is facilitated by a system controller 208. The system controller 208 includes a programmable central processing unit, here a CPU 295, operable with memory 296 (e.g., non-volatile memory) and support circuits 297. The CPU 295 may be any form of general-purpose computer processor used in industrial environments, such as a programmable logic controller (PLC), for controlling various chamber parts and sub-processors. The memory 296 coupled to the CPU 295 facilitates operation of the processing chamber. The support circuits 297 conventionally include caches, clock circuits, input / output subsystems, power supplies, etc., and combinations thereof coupled to the CPU 295 and to various components of the processing system 200, which facilitate control of substrate processing operations.
[0044] The instructions in the instruction memory 296 are in the form of a program product, such as a program that performs the methods of the present disclosure. In one example, the present disclosure may be implemented as a program product stored on a computer-readable storage medium for use with a computer system. The program of the program product defines the functions of the embodiments (including the methods described herein). Thus, a computer-readable storage medium is an embodiment of the present disclosure when it carries computer-readable instructions that direct the functions of the methods described herein.
[0045] The processing system 200 described above can be used to perform each of the nucleation, inhibition, and gap-fill depositions, thus providing a single chamber seamless tungsten gap-fill solution.
[0046] 3 is an enlarged cross-sectional view of the deposition gas source 240 of the processing system shown in FIG. 2A, according to one embodiment. The deposition gas source 240 includes a first gas source 302, such as a reducing agent gas source, and a second gas source 314, such as a tungsten-containing precursor. The reducing agent gas source 302 is in fluid communication with a reservoir 306. The reservoir 306 is continuously filled with the reducing gas source 302 or is refilled using a refill valve 304. The pressure of the reservoir 306 is monitored using a pressure gauge 308. It has been found that the use of the reservoir 306 allows for a large amount of gas to be rapidly released into the processing chamber 202. The large amount of gas is released at a large gas flow rate (e.g., about 200 sccm or more, such as about 300 sccm or more) of the reducing gas flowing into the processing chamber 202 during operation, such as during pulsing. The reducing gas is released from the reservoir 306 to the chamber 202 via a valve 310 disposed along the conduit 294E. A second gas source 314 is in fluid communication with the chamber 202 via conduit 294E. The second gas source 314 flows a tungsten-containing precursor into the chamber 202 via valve 312. One or more of the valves 304, 310, and 312 are controlled using a controller, such as the system controller 208. In some embodiments, one or more of the valves are switched between an open and closed state for a predetermined time at predetermined intervals depending on operating parameters.
[0047] After processing the substrate in the processing chamber 202, the substrate is transferred to a second processing system for annealing the substrate, such as the substrate processing system 400 shown in FIG. 4. The substrate processing system 400 may be a rapid thermal processing (RTP) apparatus. The substrate processing system 400 includes a thermal processing chamber 402 and a process gas source 404 coupled to the thermal processing chamber 402 and used to supply process gas to a processing region 406 of the thermal processing chamber 402. The processing region 406 is surrounded by one or more sidewalls 408 (e.g., four sidewalls or a single sidewall for a circular processing region 406) and a base 410. The top of the sidewall 408 may be sealed to a window assembly 412 (e.g., using an "O" ring). A radiant energy assembly 414 is disposed above and coupled to the window assembly 412. The radiant energy assembly 414 has a number of lamps 416, which may be tungsten halogen lamps, each lamp mounted in a receptacle 418 and positioned to emit electromagnetic radiation into the processing region 406. Although the window assembly 412 of FIG. 4 has a number of light pipes 420, the window assembly 412 may only have a flat solid window without light pipes. The window assembly 412 has an outer wall 422 (e.g., a cylindrical outer wall) that forms a rim surrounding the window assembly 412 on its periphery. The window assembly 412 also has a first window 424 covering a first end of the number of light pipes 420 and a second window 426 covering a second end of the number of light pipes 420 opposite the first end. The first window 424 and the second window 426 extend to and engage the outer wall 422 of the window assembly 412 to enclose and seal the interior of the window assembly 412 including the number of light pipes 420. When light pipes are used in this manner, a vacuum can be created within the plurality of light pipes 420 by applying a vacuum to one of the plurality of light pipes 420 via a conduit 428 that passes through the outer wall 422, with the light pipe 420 being fluidly connected to the remaining light pipes.
[0048] The substrate W is supported in the thermal treatment chamber 402 by a support ring 430 in the processing region 406. The support ring 430 is attached to a rotatable cylinder 432. Rotating the rotatable cylinder 432 rotates the support ring 430 and the substrate W during processing. The base 410 of the thermal treatment chamber 402 has a reflective surface 434 for reflecting energy to the backside of the substrate W during processing. Alternatively, a separate reflector (not shown) can be disposed between the base 410 of the thermal treatment chamber 402 and the support ring 430. The thermal treatment chamber 402 can include a number of temperature probes 436 disposed through the base 410 of the thermal treatment chamber 402 to detect the temperature of the substrate W. If a separate reflector is used as described above, the temperature probes 436 are also disposed through the separate reflector to optically access the electromagnetic radiation coming from the substrate W.
[0049] The rotatable cylinder 432 is supported by a magnetic rotor 438, which is a cylindrical member having a ledge 440 on which the rotatable cylinder 432 rests when both members are installed in the thermal treatment chamber 402. The magnetic rotor 438 has a plurality of magnets in a magnet region 442 below the ledge 440. The magnetic rotor 438 is disposed in an annular well 444 located in a peripheral region of the thermal treatment chamber 402 along the base 410. A cover 446 rests on the peripheral portion of the base 410 and extends over the annular well 444 toward the rotatable cylinder 432 and the support ring 430, leaving a tolerance gap between the cover 446 and the rotatable cylinder 432 and / or the support ring 430. The cover 446 generally protects the magnetic rotor 438 from exposure to process conditions in the processing region 406.
[0050] The magnetic rotor 438 rotates due to magnetic energy from a magnetic stator 448 disposed about the base 410. The magnetic stator 448 has a plurality of electromagnets 450 and is powered according to a rotational pattern during processing of the substrate W to create a rotating magnetic field that provides the magnetic energy to rotate the magnetic rotor 438. The magnetic stator 448 is coupled to a linear actuator 452 by a support 454. Activation of the linear actuator 452 moves the magnetic stator 448 along an axis 456 of the thermal processing chamber 402, thereby moving the magnetic rotor 438, the rotatable cylinder 432, the support ring 430, and the substrate W along the axis 456.
[0051] Process gases are supplied to the thermal treatment chamber 402 through a chamber inlet 458 and exhausted through a chamber outlet oriented out of the plane of the paper and generally coplanar with the chamber inlet 458 and the support ring 430 (not shown in FIG. 4). Substrates enter and exit the thermal treatment chamber 402 through an access port 460 formed in the sidewall 408 and shown at the rear of FIG.
[0052] 4, additional gas sources are contemplated. The gas source 404 may also be coupled to a plasma initiator (not shown) to remotely provide radicals to the process volume. The gas source 404 may be or include one or more of a nitrogen-containing gas, an oxygen-containing gas, a silicon-containing gas, a hydrogen-containing gas, or a plasma-forming gas, such as argon or helium.
[0053] Figure 5 illustrates a method 500 for processing a substrate according to one embodiment that can be performed using processing system 200 and processing system 400. Figures 6A-6C are schematic cross-sectional views of a portion of a substrate 600 illustrating aspects of method 500 at different stages of a void-free and seam-free tungsten gap-fill process scheme.
[0054] Substrate 600 features a patterned surface 601 including a dielectric material layer 602 having a plurality of openings 605 (one shown) formed therein. In some embodiments, the plurality of openings 605 includes one or a combination of high aspect ratio via or trench openings having a width of about 1 μm or less, e.g., about 800 nm or less or about 500 nm or less, and a depth of about 2 μm or more, e.g., about 3 μm or more or about 4 μm or more. In some embodiments, an individual opening of openings 605 can have an aspect ratio (ratio of depth to width) of about 3:1 or more, e.g., about 5:1 or more, 10:1 or more. In some embodiments, the via or trench openings are between about 20 nm and about 50 nm and have an aspect ratio of about 3:1 to about 10:1.
[0055] As shown, patterned surface 601 includes a barrier or adhesion layer 603, such as a titanium nitride (TiN) layer, deposited on dielectric material layer 602 to conformally line openings 605 and facilitate subsequent deposition of tungsten nucleation layer 604. In some embodiments, adhesion layer 603 is deposited to a thickness of about 20 angstroms (Å) to about 150 Å, such as about 30 Å to about 100 Å.
[0056] In operation 502, the method 500 includes exposing a substrate having an adhesion layer 603 to a tungsten-containing precursor gas at a precursor gas flow rate. In operation 504, the substrate is exposed to a reducing agent at a reducing agent flow rate. Operations 502 and 504 are cyclically alternated starting with either 502 or 504. In some embodiments, operations 502 and 504 are cyclically alternated starting with operation 502 and ending with operation 504. Operations 502 and 504 together form a nucleation layer 604 on the substrate using a nucleation process. The ratio of the reducing agent gas flow rate to the precursor agent flow rate is about 5:1 or more by volume, such as about 6:1 to about 10:1. A portion of an exemplary substrate 600 having a nucleation layer 604 formed thereon is shown generally in FIG. 6A.
[0057] In some embodiments, the nucleation layer 604 is deposited using an atomic layer deposition (ALD) process. The ALD process includes alternating cycles of exposing the substrate 600 to a tungsten-containing precursor and exposing the substrate 600 to a reducing agent. In some embodiments, the processing region 221 is purged between alternating exposures. In some embodiments, the processing region 221 is purged continuously during operations 402 and 404. Examples of suitable tungsten-containing precursors include tungsten halides, such as tungsten hexafluoride (WF6), tungsten hexachloride (WCl6), or combinations thereof. In some embodiments, the tungsten-containing precursor includes WF6 and the reducing agent includes a boron-containing agent, such as B2H6. In some embodiments, the tungsten-containing precursor comprises an organometallic precursor and / or a fluorine-free precursor, such as MDNOW (methylcyclopentadienyl-dicarbonylinitrosyl-tungsten), EDNOW (methylcyclopentadienyl-dicarbonylinitrosyl-tungsten), tungsten hexacarbonyl (W(CO)6), or a combination thereof.
[0058] During the nucleation process, the processing volume 215 is maintained at a pressure of less than about 120 Torr, such as about 900 mTorr to about 120 Torr, about 1 Torr to about 100 Torr, or, for example, about 1 Torr to about 50 Torr. Exposing the substrate 600 to the tungsten-containing precursor includes flowing the tungsten-containing precursor from the deposition gas source 240 to the processing region 221 at a flow rate of about 100 sccm or less, such as about 10 sccm to about 60 sccm, or about 20 sccm to about 80 sccm. Exposing the substrate 600 to the reducing agent includes flowing the reducing agent from the deposition gas source 240 to the processing region 221 at a flow rate of about 200 sccm to about 1000 sccm, such as about 300 sccm to about 750 sccm. The deposition gas source 240 depicted in FIG. 3 has been found to be particularly useful for flowing a gas flow rate from the reducing gas source 302 through the reservoir 306 at about 100 seem or greater, such as about 300 seem or greater.
[0059] It should be noted that the flow rates for the various deposition and treatment processes described herein are for a processing system 200 configured to process a 300 mm diameter substrate. Appropriate scaling can be used for processing systems configured to process substrates of different sizes.
[0060] The tungsten-containing precursor and reducing agent are each flowed into the processing region 221 for a period of about 0.1 seconds to about 10 seconds, such as about 0.5 seconds to about 5 seconds. The processing region 221 can be purged between alternating exposures by flowing a purge gas, such as argon (Ar) or hydrogen gas, into the processing region 221 for a period of about 0.1 seconds to about 10 seconds, such as about 0.5 seconds to about 5 seconds. The purge gas may be supplied from the deposition gas source 240 or the bypass gas source 238. Typically, the repeated cycles of the nucleation process continue until the nucleation layer 604 is about 10 Å to about 200 Å thick, such as about 10 Å to about 150 Å or about 20 Å to about 150 Å thick. The nucleation layer 604 is disposed along the sidewalls of the opening 605, such as over the barrier or adhesion layer 603. The nucleation layer has an atomic ratio of boron to tungsten of about 1:n, where n is about 5 or less, such as from about 1:4.5 to about 1:1, such as from about 1:4 to about 1:2, or from about 1:3 to 3:4, such as from about 1.1:1 to about 2:1.
[0061] In operation 506, the method 500 includes treating the nucleation layer 604 to inhibit tungsten deposition on the field surface of the substrate 600 and form a differential inhibition profile in the plurality of openings 605 by use of a differential inhibition process. Typically, forming the differential inhibition profile includes exposing the nucleation layer 604 to an active species of a process gas, such as the process radicals 606 shown in FIG. 6B. Suitable process gases that can be used for the inhibition process include N2, H2, NH3, NH4, O2, CH4, or combinations thereof. In some embodiments, the process gas includes nitrogen, such as N2, H2, NH3, NH4, or combinations thereof, and the active species includes nitrogen radicals, such as atomic nitrogen. In some embodiments, the process gas is combined with an inert carrier gas, such as Ar, He, or combinations thereof, to form a process gas mixture.
[0062] Without being bound by theory, it is believed that the active nitrogen species (processing radicals 606) are incorporated into a portion of the nucleation layer 604 by adsorption of the active nitrogen species and / or by reaction with the metallic tungsten of the nucleation layer 604 to form a tungsten nitride (WN) surface. The adsorbed nitrogen and / or nitrided surface of the tungsten nucleation layer 604 desirably retards (inhibits) further tungsten nucleation and thus retards subsequent tungsten deposition onto the tungsten nucleation layer.
[0063] In some embodiments, exposing the nucleation layer 604 to the processing radicals 606 includes forming a processing plasma 282A of a substantially halogen-free processing gas mixture using the first radical generator 206A and flowing effluents of the processing plasma 282A into the processing region 221. In some embodiments, the flow rate of the processing gas mixture into the first radical generator 206A, and therefore the flow rate of the processing plasma effluents into the processing region 221, is between about 1 sccm and about 3000 sccm, e.g., between about 1 sccm and about 2500 sccm, between about 1 sccm and about 2000 sccm, between about 1 sccm and about 1000 sccm, between about 1 sccm and about 500 sccm, between about 1 sccm and about 250 sccm, between about 1 sccm and about 100 sccm, or between about 1 sccm and about 75 sccm, e.g., between about 1 sccm and about 50 sccm.
[0064] In some embodiments, the inhibition treatment process includes exposing the substrate 600 to the treatment radicals 606 for a period of about 2 seconds or more, such as about 4 seconds or more, about 6 seconds or more, about 8 seconds or more, about 9 seconds or more, about 10 seconds to about 20 seconds.
[0065] In some embodiments, the concentration of the substantially halogen-free process gas in the process gas mixture is from about 0.1 vol.% to about 50 vol.%, e.g., from about 0.2 vol.% to about 40 vol.%, from about 0.2 vol.% to about 30 vol.%, from about 0.2 vol.% to about 20 vol.%, or for example, from about 0.2 vol.% to about 10 vol.%, e.g., from about 0.2 vol.% to about 5 vol.%.
[0066] In other embodiments, the processing radicals 606 can be formed using a remote plasma (not shown) that is ignited and maintained in a portion of the processing volume 215 separated from the processing region 221 by the showerhead 218, such as between the showerhead 218 and the lid plate 216. In these embodiments, the activated processing gas may be flowed through an ion filter to remove substantially all ions from the processing gas before the processing radicals 606 reach the processing region 221 and the surface of the substrate 600. In some embodiments, the showerhead 218 may be used as an ion filter. In other embodiments, the plasma used to form the processing radicals is an in situ plasma formed in the processing region 221 between the showerhead 218 and the substrate 600. In some embodiments, for example, when using an in situ processing plasma, the substrate 600 may be biased to control the directionality of the ions, e.g., charged processing radicals, formed from the processing gas and / or to accelerate them toward the substrate surface.
[0067] In some embodiments, the inhibition treatment process includes flowing an activation treatment gas into the treatment volume 215 while maintaining the treatment volume 215 at a pressure less than about 100 Torr. For example, during the inhibition treatment process, the treatment volume 215 may be maintained at a pressure less than about 75 Torr, such as less than about 50 Torr, less than about 25 Torr, less than about 15 Torr, or between about 0.5 Torr and about 120 Torr, such as between about 0.5 Torr and about 100 Torr, or between about 0.5 Torr and about 50 Torr, or such as between about 1 Torr and about 10 Torr.
[0068] In operation 508, the method 500 includes depositing a tungsten gap-fill material 608 (FIG. 6C) in the plurality of openings 605 according to the differential inhibition profile provided by the inhibition treatment in operation 206. In one embodiment, the tungsten gap-fill material 608 is formed using a chemical vapor deposition (CVD) process that includes simultaneously flowing (parallel flowing) a tungsten-containing precursor gas and a reducing agent into the processing region 221 and exposing the substrate 600 to them. The tungsten-containing precursor and reducing agent used in the tungsten gap-fill CVD process may include any combination of the tungsten-containing precursor and reducing agent described with reference to operations 502 and 504. In some embodiments, the tungsten-containing precursor includes WF6 and the reducing agent includes hydrogen gas.
[0069] The tungsten-containing precursor is flowed into the processing region 221 at a flow rate between about 10 sccm and about 1000 sccm, or greater than about 50 sccm, or less than about 1000 sccm, or between about 100 sccm and about 900 sccm. The reducing agent is flowed into the processing region 221 at a flow rate greater than about 500 sccm, such as greater than about 750 sccm, greater than about 1000 sccm, or between about 500 sccm and about 10,000 sccm, such as between about 1000 sccm and about 9,000 sccm, or between about 1000 sccm and about 8,000 sccm.
[0070] In some embodiments, tungsten gap-fill CVD process conditions are selected to provide tungsten characteristics with relatively low residual film stress compared to conventional tungsten CVD processes. For example, in some embodiments, the tungsten gap-fill CVD process includes heating the substrate to a temperature of about 250° C. or higher, e.g., about 300° C. or higher, or from about 250° C. to about 600° C., or from about 300° C. to about 500° C. During the CVD process, the processing volume 215 is typically maintained at a pressure of less than about 500 Torr, less than about 600 Torr, less than about 500 Torr, less than about 400 Torr, or from about 1 Torr to about 500 Torr, e.g., from about 1 Torr to about 450 Torr, or from about 1 Torr to about 400 Torr, or e.g., from about 1 Torr to about 300 Torr.
[0071] In another embodiment, an atomic layer deposition (ALD) process is used to deposit the tungsten gap-fill material 608 in operation 508. The tungsten gap-fill ALD process includes repeating cycles of alternatingly exposing the substrate 600 to a tungsten-containing precursor gas and a reducing agent, with purging of the processing region 221 between the alternating exposures.
[0072] The tungsten-containing precursor and reducing agent are each flowed into the processing region 221 for a period of about 0.1 seconds to about 10 seconds, such as about 0.5 seconds to about 5 seconds. The processing region 221 is typically purged between alternating exposures by flowing an inert purge gas, such as argon (Ar) or hydrogen, into the processing region 221 for a period of about 0.1 seconds to about 10 seconds, such as about 0.5 seconds to about 5 seconds. The purge gas may be supplied from the deposition gas source 240 or the bypass gas source 238.
[0073] In another embodiment, the tungsten gap-fill material 608 is deposited using a pulsed CVD method that includes repeated cycles of exposing the substrate 600 to alternating tungsten-containing precursor gases and reducing agents without purging the processing region 221. The processing conditions for the tungsten gap-fill pulsed CVD method may be the same, substantially the same, or within the same range as those described above for the tungsten gap-fill ALD process.
[0074] It has been discovered that forming a nucleation layer 604 having a high concentration of boron relative to tungsten reduces film resistivity and reduces surface roughness of the tungsten-containing layer while maintaining a seam-free or substantially seam-free gap fill at various thicknesses 620, e.g., thicknesses of about 2000 Å or less, e.g., film thicknesses of about 600 Å or less, e.g., thicknesses of about 200 Å to about 600 Å. The film thickness 620 is measured as half the width of the tungsten-containing layer (e.g., nucleation layer 604 and tungsten gap fill material 608) disposed within the opening between opposing sidewall portions of the opening 605. Alternatively, the film thickness 620 is the distance between the centerline of the opening 605 and the interface between the adhesion layer 603 and the nucleation layer 604. In some embodiments, the nucleation layer 604 and the fill layer 608 are monolithic and there is no interface between them. The tungsten gap-fill material 608 and the nucleation layer 604 together form a tungsten-containing layer having a resistivity of about 25 μΩ·cm or less depending on the thickness 620 of the tungsten-containing layer. The tungsten-containing layers 604, 608 include a resistivity of about 20 μΩ·cm or less with a tungsten-containing layer thickness of about 200 Å or more. In some embodiments, the tungsten-containing layers 604, 608 include a resistivity of about 17.5 μΩ·cm or less with a tungsten-containing layer thickness of about 200 Å to about 600 Å. In some embodiments, the tungsten-containing layers 604, 608 include a resistivity of about 15 μΩ·cm or less with a tungsten-containing layer thickness of about 450 Å or more, e.g., about 450 Å to about 600 Å. In some embodiments, the tungsten-containing layers include a surface roughness calculated by root mean square of about 3.5 nm or less, e.g., about 2 nm to about 3 nm.
[0075] Without being bound by theory, it is believed that the increased boron in the nucleation layer allows for bulk tungsten grain growth in the thin region (e.g., thickness 620 of about 600 Å or less, such as about 200 Å to about 500 Å), reducing electron scattering at tungsten grain boundaries and resulting in reduced resistivity. The retardation of bulk tungsten growth during processing operation 506 allows for reduced seam size in the contact fill.
[0076] In operation 510, the substrate 600 is annealed. Annealing the substrate 600 further reduces the resistivity of the substrate. In some embodiments, the substrate 600 is annealed for about 1 second to about 10 minutes, such as about 5 seconds to about 120 seconds, such as about 10 seconds to about 100 seconds, such as about 30 seconds to about 60 seconds. In some embodiments, the substrate 600 is annealed at a temperature of about 600° C. or higher, such as about 700° C. to about 1200° C., such as about 800° C. to about 1000° C., such as about 850° C. to about 950° C., and at a chamber pressure of about 30 Torr to about 70 Torr, such as about 50 Torr. In some embodiments, the substrate 600 is annealed in the presence of a gas comprising a nitrogen-containing gas, such as N2 gas, an argon-containing gas, such as Ar gas, a hydrogen-containing gas, such as H2 gas, or a combination thereof. In some embodiments, the gas is flowed at a volumetric flow rate of about 5 L / min, such as 15 L / min, for example 10 L / min.
[0077] The annealed substrate includes a nucleation layer 604 that has been modified by annealing. The modified nucleation layer has an atomic ratio of boron to tungsten of about 1:n, where n is about 4 or less, e.g., about 1:3 to about 1:1, e.g., about 1:2 to about 1:1. In some embodiments, the modified nucleation layer includes an atomic boron concentration of about 10% or more relative to tungsten, e.g., about 2 to 3 times the amount of boron relative to tungsten, compared to the nucleation layer 604 before annealing. By way of example, in one embodiment, the nucleation layer before annealing includes an atomic boron to tungsten ratio of about 1:4 to 1:5, e.g., about 1:4.5, and after annealing, the modified nucleation layer includes a boron to tungsten ratio of about 1:1 to about 1:3, e.g., about 1:2.
[0078] The annealed substrate includes a tungsten-containing layer 604, 608 modified by annealing. The modified tungsten-containing layer includes a resistivity of about 20 μΩ·cm or less depending on the thickness 620 of the modified tungsten-containing layer. The modified tungsten-containing layer includes a resistivity of about 17 μΩ·cm or less with a tungsten-containing layer thickness of about 200 Å or more. In some embodiments, the modified tungsten-containing layer includes a resistivity of about 10 μΩ·cm to 16 μΩ·cm with a modified tungsten-containing layer thickness of about 200 Å to about 600 Å. In some embodiments, the modified tungsten-containing layer includes a resistivity of about 10 μΩ·cm to 14 μΩ·cm with a tungsten-containing layer thickness of about 450 Å or more, e.g., about 450 Å to about 600 Å. In some embodiments, the tungsten-containing layer comprises a surface roughness calculated by root mean square of about 3.5 nm or less, e.g., about 2 nm to about 3 nm. In some embodiments, the resistivity of the modified tungsten-containing layer is reduced by 10% or more, e.g., about 20% to about 40%, relative to the tungsten-containing layer prior to annealing.
[0079] Without being bound by theory, it is believed that annealing the substrate 600 increases the grain size of the structure of the tungsten-containing layer, contributing to the reduction in resistivity. In some embodiments, the grain size of the tungsten-containing layers 604, 608 increases by about 5% or more, such as about 10% to about 30%, such as about 15% to about 20%, after annealing, as measured by X-ray diffraction (XRD) imaging. It has been further observed that the modified tungsten content comprises alpha phase tungsten and is substantially free of beta phase tungsten. Alpha phase tungsten is stable and has good electrical conductivity. It has also been discovered that the process described herein includes an incubation growth of about 50 Å to about 300 Å, such as about 70 Å to about 100 Å, compared to conventional SSW of about 1150 Å to about 1250 Å.
[0080] In a typical semiconductor fabrication scheme, after depositing tungsten gap-fill material 608 in opening 605, a chemical-mechanical polishing (CMP) process may be used to remove the overburden of tungsten material (and any barrier layers disposed thereunder) from the field surface of the substrate. EXAMPLES
[0081] FIG. 7 shows comparative curves illustrating the resistivity of film layers formed using the methods described herein and comparative methods, according to some embodiments. Curves 702, 704, 706, 708 show the film resistivity results as a function of film thickness for each film sample. As used herein, film resistivity is measured using ASTM B193-20(2020) using a KLA Rs-200 resistivity mapping system to measure sheet resistance with a four-point probe. Film thickness is measured using a Rigaku MFM65 in-line XRF wafer inspection system. Multiplying the sheet resistance by the film thickness gives the film resistivity.
[0082] Curve 702 corresponds to a film formed using a process similar to that described herein prior to annealing and having a nucleation layer with a boron to tungsten atomic ratio of about 1:4.5 or less, e.g., about 1:4.6 to about 1:6. The sample film of curve 702 can be formed using operations 502-508 of method 500. The sample film of curve 702 was formed by exposing the sample to a nitrogen plasma from a remote plasma source as described in operation 508. Curve 704 corresponds to a film deposited using a conventional CVD process. The conventional CVD process illustrated by curve 704 resulted in a relatively low resistivity across the entire thickness range, but the film contained voids and seams within the openings and did not provide good structural properties. The film of curve 702 provided good gap-filling properties that were substantially free of voids and seams, but resistivity increased to about 20 μΩ·cm or more at film thicknesses less than 500 Å. Curve 706 corresponds to a film formed using a conventional CVD process with an increased concentration of boron in the nucleation layer, such as the nucleation layer having a boron to tungsten atomic ratio of about 1:4 or greater, such as from about 1:3 to about 1:2. As can be seen, the resistivity after increasing the boron concentration in the nucleation of a film formed using a conventional CVD process results in a decrease in film resistivity. The resistivity of a thin film having a thickness between 200 Å and 600 Å does not achieve a resistivity below about 16 μΩ·cm.
[0083] Curve 708 corresponds to a film formed using a process described herein (e.g., method 500, operations 502-508) prior to annealing and having a nucleation layer with a boron to tungsten atomic ratio of about 1:4 or greater, such as from about 1:3 to about 1:2. The film of curve 708 was similar to the film of curve 702, except that the film of curve 708 included a higher boron concentration in the nucleation layer. The film of curve 708 provided good gap-filling properties with no or substantially no voids and seams, and also resulted in low resistivity for thicknesses less than 500 Å and greater than 500 Å. Compared to the film corresponding to curve 702, the film corresponding to curve 708 experienced a 10-70% reduction in film resistivity for thicknesses from about 200 Å to about 2000 Å, while also suppressing gap-filling used in post-nucleation layer treatment processes. The reduction in film resistivity is greater for thin films compared to thick films. Compared to samples formed by conventional CVD processes, samples formed using operations 502-508 of method 500, which have a higher concentration of boron in the nucleation layer, surprisingly resulted in reduced resistivity with much lower roughness and much lower resistivity.
[0084] FIG. 8 illustrates the effect of annealing temperature on samples having a tungsten-containing layer approximately 300 Å thick, where the tungsten-containing layer on each sample can be formed using operations 502-508 of method 500 as a control, and a corresponding sample can be formed using operations 502-510 with annealing. Each pair of data points corresponds to resistivity measurements at annealing temperatures ranging from 600° C. to 850° C., at 50 degree intervals, compared to a control sample that was not annealed. As can be seen, higher annealing temperatures generally corresponded to a greater decrease in resistivity. In addition to improved resistivity, the annealed films maintained low surface roughness. Without being bound by theory, it is believed that grain growth, as observed by microscopic imaging, occurred in a planar manner with some increase in film thickness, rather than rough vertical growth.
[0085] 9 illustrates the effect of annealing on samples having tungsten-containing layers of various thicknesses. Curve 902 includes resistivity measurements as a function of film thickness for a sample formed using operations 502-508 of method 500 as a control, and curve 904 includes resistivity measurements for a corresponding sample formed using operations 502-510 with annealing. As can be seen, for thinner films, such as less than 300 Å, a greater effect of annealing is observed.
[0086] Table 1 shows a comparison of grain size before and after annealing. A first sample (s1) was formed using operations 502-508 of method 500. Before annealing, s1 had a thickness of 227.7 Å and a resistivity of 45.6 μΩ·cm. The grain size was measured to be 225 Å. A second sample (s2) was formed in the same manner as the first sample s1 and then annealed at 850°C for 60 seconds. The film thickness of the sample expanded by less than 5% and the grain size expanded to 252 Å. The roughness remained substantially the same between the first and second samples. Without wishing to be bound by theory, it is believed that the grain expansion occurred in a planar manner such that the roughness remained substantially the same and the film thickness expansion was minimized, as evidenced by topology imaging. As a result of the grain growth, the second sample s2 exhibited a reduced resistivity compared to the first sample.
[0087] A third sample (s3) was formed using operations 502-508 of method 500. Before annealing, s3 had a thickness of 324.4 Å and a resistivity of 16.3 μΩ·cm. The grain size was measured to be 265 Å. A fourth sample (s4) was formed similarly to the third sample s3 and then annealed at 850° C. for 60 seconds. The sample's film thickness increased by less than 6% and the grain size increased to 316 Å. The roughness remained substantially the same between the first and second samples. As a result of the grain growth, the fourth sample s4 had a reduced resistivity compared to the third sample. It was observed that the reduction in resistivity was much greater for thinner films, as demonstrated by the second sample compared to the first sample.
[0088] [Table 1]
[0089] Additional Features The present disclosure can include the following non-limiting aspects and / or embodiments.
[0090] Clause 1. A structure on a substrate, the structure comprising: an opening in the substrate; and a tungsten-containing layer, the nucleation layer disposed along a sidewall of the opening, the nucleation layer comprising boron and tungsten; and a filler layer disposed over the nucleation layer in the opening, the tungsten-containing layer having a resistivity of about 16 μΩ·cm or less, the tungsten-containing layer having a thickness of about 200 Å to about 600 Å, the thickness of the tungsten-containing layer being one-half of a width of the tungsten-containing layer disposed in the opening between opposing sidewall portions of the opening.
[0091] Clause 2. The structure of clause 1, wherein the nucleation layer comprises a boron to tungsten ratio of about 1:4 to about 1:1.
[0092] Clause 3. The structure of clause 1 or clause 2, wherein the boron to tungsten ratio is about 1:3 to 1:2.
[0093] Clause 4. The structure of any one of clauses 1-3, further comprising an adhesion layer disposed between the substrate and the nucleation layer.
[0094] Clause 5. The structure of any one of clauses 1-4, wherein the tungsten-containing layer further comprises nitrogen, oxygen, fluorine, or a combination thereof.
[0095] Clause 6. A structure on a substrate, the structure including: an opening in the substrate; an adhesion layer disposed on a sidewall of the opening; and a tungsten-containing layer disposed in the sidewall and over the adhesion layer, the tungsten-containing layer having a resistivity of about 16 μΩ·cm or less and a thickness of about 200 Å to about 600 Å, the thickness of the tungsten-containing layer being half a width of the tungsten-containing layer disposed in the opening between opposing sidewall portions of the opening.
[0096] Clause 7. The structure of clause 6, wherein the tungsten-containing layer has a thickness of about 300 Å to about 600 Å, and the tungsten-containing layer has a resistivity of about 14 μΩ·cm or less.
[0097] Clause 8. The structure of clause 6 or clause 7, wherein the tungsten-containing layer includes a nucleation layer comprising boron.
[0098] Clause 9. The structure of any one of clauses 6 to 8, wherein the ratio of boron to tungsten is about 1:3 to 1:1.
[0099] Clause 10. The structure of any one of clauses 6-9, wherein the tungsten-containing layer comprises a surface roughness calculated by root mean square of about 3.5 nm or less.
[0100] Clause 11. The structure of any one of clauses 6 to 10, wherein the tungsten-containing layer comprises a surface roughness calculated by root mean square of about 2 nm to about 3 nm.
[0101] Clause 12. A method of forming a structure on a substrate, comprising: exposing the substrate to a tungsten-containing precursor gas at a precursor gas flow rate; exposing the substrate to a reducing agent comprising boron at a reducing agent flow rate, wherein the tungsten-containing precursor gas and the reducing agent are applied in a periodic alternating manner to form a nucleation layer on the substrate in at least one opening in the substrate; depositing a fill layer on the nucleation layer in the at least one opening; and annealing the substrate at about 600° C. to about 1000° C.
[0102] Clause 13. The method of clause 12, further comprising transferring the substrate to a rapid thermal processing chamber prior to annealing the substrate.
[0103] Clause 14. The method of clause 12 or clause 13, wherein annealing the substrate comprises exposing the substrate to hydrogen gas.
[0104] Clause 15. The method of any one of clauses 12-14, wherein the reducing agent flow rate is about 300 sccm or greater.
[0105] Clause 16. The method of any one of clauses 12-15, wherein the precursor gas flow rate is about 60 sccm or less.
[0106] Clause 17. The method of any one of clauses 12-16, further comprising filling the reservoir with a reducing agent using a reservoir valve positioned upstream of the reservoir, and flowing the reducing agent from the reservoir to a process volume containing the substrate by opening a mass flow control valve positioned between the process volume and the reservoir.
[0107] Clause 18. The method of any one of clauses 12-17, wherein filling the reservoir further comprises opening a reservoir valve when the pressure in the reservoir falls below a predetermined pressure.
[0108] Clause 19. The method of any one of clauses 12-18, wherein the substrate is annealed for about 1 second to about 10 minutes.
[0109] Clause 20. The method of clause 19, wherein the substrate is annealed for about 10 seconds to about 60 seconds.
[0110] Clause 21. The method of any one of clauses 12-20, wherein annealing the substrate comprises flowing a gas selected from the group consisting of a nitrogen-containing gas, an argon-containing gas, a hydrogen-containing gas, or combinations thereof over the substrate.
[0111] Clause 22. The method of any one of clauses 12-21, wherein the substrate is annealed from a plurality of heat lamps positioned above the substrate.
[0112] Clause 23. The method of any one of clauses 12-22, wherein the substrate is annealed at a temperature of about 700°C to about 900°C.
[0113] Clause 24. The method of any one of clauses 12-23, wherein the reducing agent gas flow rate to precursor agent flow rate ratio is m:1, where m is about 5 or greater by volume.
[0114] Clause 25. A method of forming a structure on a substrate, comprising: exposing the substrate to a tungsten-containing precursor gas at a precursor gas flow rate; exposing the substrate to a reducing agent comprising boron at a reducing agent flow rate, wherein the tungsten-containing precursor gas and the reducing agent are periodically alternated to form a nucleation layer on the substrate in at least one opening in the substrate; depositing a filler layer on the nucleation layer in the at least one opening, wherein the filler layer and the nucleation layer together form a tungsten-containing layer comprising a first resistivity; and annealing the tungsten-containing layer at about 600° C. to about 1000° C. to form a modified tungsten-containing layer having a second resistivity lower than the first resistivity.
[0115] Clause 26. The method of clause 25, wherein the second resistivity is about 10% to 50% lower than the first resistivity.
[0116] While the forgoing is directed to embodiments of the present disclosure, other and further embodiments of the disclosure may be devised without departing from the basic scope thereof, the scope of the disclosure being determined by the claims that follow.
Claims
1. A structure on a substrate, comprising: an opening in the substrate; A tungsten-containing layer comprising: a nucleation layer disposed along a sidewall of the opening, the nucleation layer comprising boron and tungsten; and a filler layer disposed over the nucleation layer in the opening, the tungsten containing layer having a resistivity of about 16 μΩ cm or less, the tungsten containing layer having a thickness of about 200 Å to about 600 Å, the thickness of the tungsten containing layer being half a width of the tungsten containing layer disposed in the opening between opposing sidewall portions of the opening. a tungsten-containing layer comprising: Including, structure.
2. 2. The structure of claim 1, wherein said nucleation layer comprises a ratio of boron to tungsten of about 1:4 to about 1:
1.
3. 3. The structure of claim 2, wherein said boron to tungsten ratio is about 1:3 to 1:
2.
4. The structure of claim 1 further comprising an adhesion layer disposed between the substrate and the nucleation layer.
5. 10. The structure of claim 1, wherein the tungsten-containing layer further comprises nitrogen, oxygen, fluorine, or a combination thereof.
6. A structure on a substrate, comprising: an opening in the substrate; an adhesive layer disposed on a sidewall of the opening; a tungsten-containing layer disposed on the adhesion layer in the sidewall, the tungsten-containing layer having a resistivity of about 16 μΩ cm or less and a thickness of about 200 Å to about 600 Å, the thickness of the tungsten-containing layer being one-half of a width of the tungsten-containing layer disposed in the opening between opposing sidewall portions of the opening; Including, structure.
7. 7. The structure of claim 6, wherein the thickness of the tungsten-containing layer is between about 300 Å and about 600 Å, and the resistivity of the tungsten-containing layer is less than or equal to about 14 μΩ·cm.
8. 7. The structure of claim 6, wherein the tungsten-containing layer comprises a nucleation layer comprising boron.
9. 7. The structure of claim 6, wherein the ratio of boron to tungsten is about 1:3 to 1:
1.
10. 7. The structure of claim 6, wherein the tungsten-containing layer comprises a surface roughness calculated by root mean square of about 3.5 nm or less.
11. 7. The structure of claim 6, wherein the tungsten-containing layer comprises a surface roughness calculated by root mean square of about 2 nm to about 3 nm.
12. 1. A method of forming a structure on a substrate, comprising: exposing the substrate to a tungsten-containing precursor gas at a precursor gas flow rate; exposing the substrate to a reducing agent comprising boron at a reducing agent flow rate, wherein the tungsten-containing precursor gas and the reducing agent are applied alternately in a cyclic manner to form a nucleation layer on the substrate within at least one opening in the substrate; depositing a fill layer over the nucleation layer in the at least one opening; annealing the substrate at about 600° C. to about 1000° C.; A method comprising:
13. The method of claim 12 , further comprising transferring the substrate to a rapid thermal processing chamber prior to annealing the substrate.
14. The method of claim 12 , wherein annealing the substrate comprises exposing the substrate to hydrogen gas.
15. The method of claim 12 , wherein the flow rate of the reducing agent is greater than or equal to about 300 sccm.
16. The method of claim 12 , wherein the precursor gas flow rate is less than or equal to about 60 sccm.
17. 13. The method of claim 12, further comprising filling a reservoir with the reducing agent using a reservoir valve disposed upstream of the reservoir, and flowing the reducing agent from the reservoir to a process volume containing the substrate by opening a mass flow control valve disposed between the process volume and the reservoir.
18. 20. The method of claim 17, wherein filling the reservoir further comprises opening the reservoir valve when the pressure in the reservoir falls below a predetermined pressure.
19. The method of claim 12, wherein the substrate is annealed for about 1 second to about 10 minutes.
20. The method of claim 19, wherein the substrate is annealed for about 10 seconds to about 60 seconds.
Citation Information
Patent Citations
Semiconductor device and manufacturing method thereof
CN103578963A
Semiconductor device
JP1986152067A
Manufacturing method of semiconductor device
JP2003086535A
Method of forming tungsten thin film with low resistivity and robust micro-adhesion characteristic
JP2011192680A
Fluorine-containing conductive film
JP2017521549A