Catalytic cracking catalyst having rich mesopore structure and preparation method thereof
A catalytic cracking catalyst with a balanced composition and preparation method ensures a rich mesopore structure, enhancing heavy oil conversion and coke selectivity while maintaining catalyst strength, addressing the limitations of conventional catalysts.
Patent Information
- Application Number
- JP2024521153
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-09
- Filing Date
- 2022-09-28
- Publication Date
- 2024-10-04
AI Technical Summary
Conventional catalytic cracking catalysts lack sufficient mesopore and macropore structures, leading to high coke yield and poor heavy oil cracking performance, especially with heavier feedstocks, and direct addition of mesoporous and macroporous materials compromises catalyst strength.
A catalytic cracking catalyst composition comprising 10-35% aluminum oxide with mesopores and macropores, 5-30% acidified binder, 2-20% second binder, 20-60% zeolite, and 5-50% clay, with a specific pore structure and preparation method that maintains mesopore and macropore integrity, enhancing heavy oil conversion and coke selectivity.
The catalyst exhibits a rich mesopore structure with improved heavy oil conversion ability and coke selectivity, maintaining strong abrasion resistance and reducing coke yield.
Smart Images

Figure 2024536441000001_ABST
Abstract
Description
Detailed Description of the Invention
[0001] [Technical field] The present invention relates to the field of petroleum refining catalysts, and in particular to a catalytic cracking catalyst having rich mesopore structure and a method for preparing the same.
[0002] [Background technology] The promulgation and implementation of carbon emission regulations and low carbon fuel standards have a great impact on the petroleum refining industry. As a traditional unit in petroleum refining and processing, catalytic cracking units have become the major source of carbon dioxide emissions in the refining industry due to catalyst coking and regeneration. Therefore, reducing the coke yield is the most effective way to reduce carbon emissions from catalytic cracking units. However, as the feedstock becomes heavier and more deteriorated, the coke yield of catalytic cracking catalysts remains high. Catalysts with mesopore and macropore structures can promote the rapid diffusion of reactant and product molecules, reduce the generation of coke precursors, and at the same time, promote the improvement of the stripping performance of the catalyst and the reduction of the coke that can be stripped. Therefore, it is essential to develop catalytic cracking catalysts with abundant mesopore and macropore structures.
[0003] The diameter of heavy oil molecules is about 3nm to 10nm. In order to eliminate the diffusion limitation, the optimal range of the pore size of the catalytic cracking catalyst is 2 to 6 times the diameter of the heavy oil molecules, which corresponds to a pore size range of 6nm to 60nm. However, the pore size of the conventional catalytic cracking catalyst is smaller than 4nm, which cannot meet the needs of heavy oil cracking.
[0004] CN1436835A discloses a catalytic cracking catalyst and its preparation method. The catalyst comprises 5% by weight to 60% by weight of aluminum oxide having mesopores and macropores with an average pore diameter of 3 nm or less, 5% by weight to 60% by weight of zeolite, 5% by weight to 40% by weight of binder, and 5% by weight to 85% by weight of clay. The preparation method of the catalytic cracking catalyst is to uniformly mix zeolite with the aluminum oxide having mesopores and macropores, binder, and clay after undergoing spraying, calcination, washing, and drying. However, the volume of pores with a diameter of more than 2 nm in the catalytic cracking catalyst is still less than 0.2 mL / g.
[0005] CN106179476A discloses a catalytic cracking catalyst, and its preparation method and application. The catalytic cracking catalyst is (0-0.2)Na2O(40-85)Al2O3(10-55)SiO2(0.5-10)P2O5(0.5-10)M x O y The catalytic cracking catalyst has a low coke selectivity and a high catalytic cracking activity, and can obtain a high diesel yield and a low sulfur content gasoline in the catalytic cracking of heavy oil. However, the catalyst prepared lacks mesopore structure and macropore structure.
[0006] CN105688977A discloses a method for preparing a catalytic cracking catalyst containing pseudo-boehmite. The method includes: mixing and stirring a part of the pseudo-boehmite with a silicon-containing solution for more than 15 minutes to prepare modified pseudo-boehmite A; mixing the modified pseudo-boehmite A, the residual pseudo-boehmite B and pulping clay to prepare a matrix slurry containing pseudo-boehmite; mixing, homogenizing, forming, drying and ion-exchanging the matrix slurry and the zeolite slurry to obtain a catalytic cracking catalyst. The catalyst prepared according to the method has a high macropore volume with macropore diameters mainly distributed over 100 nm, and lacks mesopore structure and macropore structure of 5 nm to 100 nm.
[0007] However, since the materials having mesopores and macropores have poor adhesion by themselves, the direct addition of them affects the strength of the catalyst, and the amount of the materials having mesopores and macropores added is limited, so that the increase in the mesopore structure and macropore structure is insignificant. Therefore, the preparation of catalytic cracking catalysts with rich mesopore structure and excellent wear resistance remains a hot topic of research.
[0008] Summary of the Invention In order to solve the above problems, the present invention provides a catalytic cracking catalyst with rich mesopore structure and a preparation method thereof, which has good exhaustion index, rich mesopore structure, strong heavy oil conversion ability and good coke selectivity.
[0009] Meanwhile, the present invention provides a composition for catalytic cracking, the composition comprising, based on the dry weight of the composition, 10 wt%-35 wt% of aluminum oxide having mesopores and macropores, 5 wt%-30 wt% of an acidified binder, 2 wt%-20 wt% of a second binder, 20 wt%-60 wt% of a zeolite, and 5 wt%-50 wt% of a clay, the weight ratio of the acidified binder to the aluminum oxide having mesopores and macropores being 0.5-1.0; the aluminum oxide having mesopores and macropores is an aluminum oxide having a pseudo-boehmite structure, the aluminum oxide having mesopores and macropores has a total pore volume of 0.5 mL / g-2.0 mL / g, an average pore diameter of 5 nm-30 nm, and a specific surface area of 250 m 2 / g~450m 2 / g, wherein the pore volume of pores having a pore diameter of 5 nm to 100 nm accounts for 80% or more of the total pore volume. Preferably, after spray drying and calcination, the composition is -1 Less than 1.0% time, preferably -1 ~3.0% time -1 and a pore volume retention rate of the 5 nm to 100 nm pores of 70% or more, preferably 80% to 100%; and the pore volume retention rate of the 5 nm to 100 nm pores=the pore volume of the 5 nm to 100 nm pores in the catalytic cracking catalyst / (the pore volume of the 5 nm to 100 nm pores in the aluminum oxide having mesopores and macropores×the content of the aluminum oxide having mesopores and macropores in the catalytic cracking catalyst).
[0010] In one embodiment, the composition comprises, based on the dry weight of the composition, 10 wt. % to 30 wt. % of the aluminum oxide having mesopores and macropores, 8 wt. % to 25 wt. % of the acidified binder, 2 wt. % to 15 wt. % of the second binder, 30 wt. % to 45 wt. % of the zeolite, and 10 wt. % to 40 wt. % of the clay, wherein the weight ratio of the acidified binder to the aluminum oxide having mesopores and macropores is 0.5 to 0.8; the aluminum oxide having mesopores and macropores is an aluminum oxide having a pseudoboehmite structure, the aluminum oxide having mesopores and macropores has a total pore volume of 0.7 mL / g to 1.5 mL / g, an average pore diameter of 6 nm to 20 nm, and a pore size of 300 m 2 / g~400m 2 / g, and the pore volume of the pores having a pore diameter of 5 nm to 100 nm accounts for 80% to 95% of the total pore volume.
[0011] In one embodiment, the acidified binder is one or more selected from the group consisting of aluminum sol, silica sol, and silica aluminum sol, and is preferably aluminum sol or silica sol. The second binder is one or more selected from the group consisting of acidified pseudoboehmite, silica sol, aluminum sol, silica aluminum sol, aluminum phosphate sol, and zirconium sol, and is preferably aluminum sol, silica sol, or acidified pseudoboehmite. The weight ratio of the acidified binder to the second binder is 0.5 to 5.0.
[0012] In one embodiment, the zeolite is one or more selected from the group consisting of NaY zeolite, Y zeolite with a high silica-alumina ratio obtained after modifying NaY zeolite (such as HY, REY, REHY, USY, or REUSY), MFI zeolite, and beta zeolite.
[0013] In one embodiment, the clay is any of the various clays that may function as catalytic components, such as kaolin, bentonite, montmorillonite, sepiolite, diatomaceous earth, and the like.
[0014] Meanwhile, the present invention also provides a method for preparing a catalytic cracking catalyst using the composition according to the present invention, the method comprising the following steps, which are preferably carried out in order: (1) homogeneously mixing and stirring aluminum oxide having mesopore and macropore structures, clay and, if necessary, all acidified binders to obtain an acidified slurry; (2) adding zeolite to the acidified slurry and uniformly mixing and stirring to obtain a second slurry; and (3) adding a second binder to the second slurry, mixing and stirring, spray drying the resulting mixed slurry, and calcining it to obtain the catalytic cracking catalyst of the present invention.
[0015] In one embodiment, according to the preparation method provided by the present invention, in the step (1), 10%-35% by weight of the aluminum oxide having mesopore and macropore structure, 5%-50% by weight of the clay, and 5%-30% by weight of the acidified binder are mixed with deionized water based on the dry weight of the catalyst, and pulped for 15 minutes or more to obtain an acidified slurry. The solid content of the obtained acidified slurry is 15%-40% by weight.
[0016] In one embodiment, in the step (2), 20 wt% to 60 wt% of the zeolite is added to the acidified slurry, mixed and pulped for 15 minutes or more to obtain the second slurry having a solid content of 15 wt% to 40 wt%.
[0017] In one embodiment, in the step (3), 2 wt % to 20 wt % of the second binder is added to the second slurry, and the resulting mixed slurry has a solid content of 15 wt % to 40 wt %.
[0018] According to a particularly preferred embodiment of the present invention, in the method of preparing the catalytic cracking catalyst using the composition of the present invention, no other acid is added. For the purposes of the present invention, "no other acid is added" means that the acidification required for the preparation of the catalyst is carried out completely through the acidified binder according to the present invention. Correspondingly, in the method according to the present invention, no other acid, such as hydrochloric acid, which is commonly used, is added, whether for acidification or for other purposes.
[0019] Furthermore, the present invention also provides a catalytic cracking catalyst prepared by the composition of the present invention according to the method described in the present invention.
[0020] In one embodiment, the catalytic cracking catalyst provided according to the present invention has an abundant mesopore structure. The total pore volume of the catalytic cracking catalyst determined by the low-temperature nitrogen adsorption method is 0.200mL / g or more, preferably 0.200mL / g-0.300mL / g, wherein the pore volume of the mesopores and macropores having a pore diameter of 2nm-100nm accounts for 70% or more, preferably 75%-95% of the total pore volume, and the pore volume of the mesopores having a pore diameter of 4nm-50nm accounts for 60% or more, preferably 65%-85% of the total pore volume.
[0021] The present invention has the following advantages over the prior art: on the one hand, in the prior art, the aluminum oxide having mesopores and macropores is acidified to improve the attenuation performance of the catalyst; but the original mesopore structure and macropore structure are lost by the acidification, so that the heavy oil conversion ability and the coke selectivity of the catalyst are reduced; on the other hand, in the prior art, the mesoporous aluminum oxide material and the macroporous aluminum oxide material are directly added to the catalyst without acidification to increase the macropore volume, which leads to the deterioration of the attenuation performance of the catalyst. On the other hand, according to the preparation method of the catalytic cracking catalyst of the present invention, the mesopore structure and macropore structure of the aluminum oxide having mesopores and macropores are maintained, the heavy oil conversion ability and the coke selectivity are improved, and at the same time, the adverse effect of the aluminum oxide having mesopores and macropores on the catalyst strength is overcome.
[0022] Therefore, compared with conventional catalysts, the catalytic cracking catalyst provided by the present invention has a rich mesopore structure of 4 nm to 50 nm, has good wear resistance strength, improves catalytic heavy oil conversion capacity, and significantly improves coke selectivity.
[0023] Description of the drawings FIG. 1 is a pore distribution diagram of the aluminum oxide having mesopores and macropores used in the present invention.
[0024] FIG. 2 is a pore distribution diagram of the catalytic cracking catalyst prepared according to Example 1.
[0025] FIG. 3 is a pore distribution diagram of the catalytic cracking catalyst prepared according to Comparative Example 1.
[0026] [Specific embodiment] The present application will be described in further detail as follows in combination with drawings and examples. Through these illustrations, the features and advantages of the present application will be more clear and obvious.
[0027] Furthermore, the technical features relating to different embodiments of the present application described below can be combined with each other unless they are mutually inconsistent.
[0028] The present invention provides a composition for catalytic cracking, comprising, based on the dry weight of the composition, 10wt%-35wt%, preferably 10wt%-30wt% of an aluminum oxide having mesopores and macropores, 5wt%-30wt%, preferably 8wt%-25wt% of an acidified binder, 2wt%-20wt%, preferably 2wt%-15wt% of a second binder, 20wt%-60wt%, preferably 30wt%-45wt% of a zeolite, and 5wt%-50wt%, preferably 10wt%-40wt% of a clay; the weight ratio of the acidified binder to the aluminum oxide having mesopores and macropores is 0.5-1.0, preferably 0.5-0.8. The aluminum oxide having mesopores and macropores is an aluminum oxide having a pseudo-boehmite structure, and the aluminum oxide having mesopores and macropores has a total pore volume of 0.5 mL / g to 2.0 mL / g, preferably 0.7 mL / g to 1.5 mL / g, an average pore diameter of 5 nm to 30 nm, preferably 6 nm to 20 nm, and a specific surface area of 250 m 2 / g~450m 2 / g, preferably 300m 2 / g~400m 2 / g, wherein the pore volume of the 5 nm to 100 nm pores accounts for 80% or more, preferably 80% to 95% of the total pore volume. Preferably, after spray drying and calcination, the composition is -1 Less than 1.0% time, preferably -1 ~3.0% time -1and a pore volume retention rate of 5 nm to 100 nm pores of 70% or more, preferably 80% to 100%; the pore volume retention rate of 5 nm to 100 nm pores=the pore volume of the 5 nm to 100 nm pores in the catalytic cracking catalyst / (the pore volume of the 5 nm to 100 nm pores in the aluminum oxide having mesopores and macropores×the content of the aluminum oxide having mesopores and macropores in the catalytic cracking catalyst).
[0029] In one embodiment, said aluminum oxide having a pseudoboehmite structure can be prepared according to the methods provided in patents US4010116 and US4206085, the entire text of which is incorporated by reference.
[0030] In one embodiment, the acidified binder may be one or more selected from the group consisting of aluminum sol, silica sol, silica aluminum sol, preferably aluminum sol, and the second binder refers to one or more of acidified pseudoboehmite, silica sol, aluminum sol, silica aluminum sol, aluminum phosphate sol, zirconium sol, preferably acidified pseudoboehmite.
[0031] In one embodiment, the zeolite may be one or more selected from the group consisting of NaY zeolite, Y zeolite with a high silica-alumina ratio obtained after modifying NaY zeolite (REY, HY, REHY, USY, REUSY, etc.), MFI zeolite, and β zeolite.
[0032] In one embodiment, the clay is a variety of clays that can function as a catalytic component, such as kaolin, bentonite, montmorillonite, sepiolite, diatomaceous earth, etc. These clays are commonly known by those skilled in the art.
[0033] The present invention also provides a method for preparing a catalytic cracking catalyst using the composition according to the present invention, said method comprising the following steps, preferably performed in sequence: (1) homogeneously mixing and stirring aluminum oxide having mesopore and macropore structures, clay and an acidified binder to obtain an acidified slurry; (2) adding zeolite to the acidified slurry and uniformly mixing and stirring to obtain a second slurry; and (3) adding a second binder to the second slurry, mixing and stirring, spray drying the resulting mixed slurry, and calcining it to obtain the catalytic cracking catalyst of the present invention.
[0034] In one embodiment, according to the preparation method provided by the present invention, in step (1), the aluminum oxide having mesopore and macropore structure, clay, and acidified binder are mixed with deionized water, and pulped for 15 minutes or more, preferably 20 minutes to 60 minutes, to obtain an acidified slurry having a solid content of 15% by weight to 40% by weight.
[0035] In one embodiment, in the step (2), zeolite is added to the obtained acidified slurry, mixed and pulped for at least 15 minutes, preferably between 20 minutes and 60 minutes, to obtain a second slurry having a solid content of 15% to 40% by weight.
[0036] In one embodiment, in the step (3), a second binder is added to the obtained second slurry, and the obtained mixed slurry has a solid content of 15% to 40% by weight.
[0037] In one embodiment, the spray drying and calcination are carried out according to existing methods, which are not required by the present invention. The method also includes processes such as washing and drying after the catalyst calcination, which can be carried out according to existing methods, which are not required by the present invention.
[0038] The present invention also provides a catalytic cracking catalyst, which is prepared by the composition of the present invention according to the method described in the present invention. The catalytic cracking catalyst provided according to the present invention has an abundant mesopore structure. The total pore volume of the catalytic cracking catalyst determined by the low-temperature nitrogen adsorption method is 0.200mL / g or more, preferably 0.200mL / g to 0.300mL / g, where the pore volume of mesopores and macropores of 2nm to 100nm accounts for 70% or more, preferably 75% to 95% of the total pore volume, and the pore volume of mesopores of 4nm to 50nm accounts for 60% or more, preferably 65% to 85% of the total pore volume.
[0039] [Example] The following examples provide further illustration of the present invention with the aim of enabling the reader to better understand the nature of the invention and the beneficial effects it provides, but should not be construed as any limitation on the operable scope of the invention.
[0040] The raw materials used to prepare the catalytic cracking catalyst in the following examples are listed below: kaolin has a solid content of 76% by weight; aluminum sol has an aluminum oxide content of 21.5% by weight; silica sol has an SiO2 content of 27.0% by weight; the properties of conventional pseudoboehmite and aluminum oxide with mesopores and macropores are shown in Table 1; the acidified pseudoboehmite has a solid content of 12.0% by weight; the molar ratio of acid (HCl) to aluminum oxide when acidified is 0.20; the rare earth ultrafine Y-type zeolite REUSY used has a solid content of 85.0% by weight, a cell constant of 24.51A, and has a Na2O content of 1.6% and a RE2O3 content of 12.0% based on the weight percent content. The aluminum oxides A to D with mesopores and macropores are provided by Sinopec Catalyst Co., Ltd., and their properties are shown in Table 1.
[0041] [Table 1]
[0042] The analytical and evaluation methods are as follows: Analysis of specific surface area and pore volume: Using an automatic adsorption analyzer ASAP 2405N V1.01 manufactured by Micromeritics, USA, the sample was measured according to the low-temperature nitrogen adsorption static volume measurement method to obtain a specific surface area of 1.33 × 10 -2 The adsorption and desorption isotherms of the sample at 77.4 K were measured by vacuum degassing at 100 Pa and 300 °C for 4 h, using N2 as the adsorption medium. The specific surface area of the sample was calculated according to the BET equation. The volume of N2 adsorbed by the sample at a relative pressure of p / p0 = 0.98 was measured and converted to the volume of liquid nitrogen, i.e., the total pore volume. The micropore volume was calculated according to the t-plot method. The difference between the two is the volume of mesopores and macropores from 2 nm to 100 nm, where the pore volumes of both mesopores from 4 nm to 50 nm and mesopores and macropores from 5 nm to 100 nm are obtained using the peak fitting method.
[0043] Catalyst strength: A certain amount of catalyst is placed in a fixed device and blown and crushed under a constant air flow for 5 hours. The average consumption percentage for the last 4 hours excluding the first hour is called the catalyst consumption index, and is measured in % per hour. The method and standard are based on the airlift method Q / SYLS0518-2002.
[0044] Evaluation of the catalytic cracking catalyst: The catalytic cracking catalyst is pre-aged in a fixed bed ageing apparatus at 800°C with 100% steam for 12 hours, and then evaluated in an ACE apparatus. The properties of the reacted crude oil are shown in Table 8. The reaction temperature is 500°C, and the weight ratio of the catalyst to oil is 8.04. Where, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield, and coke selectivity = coke yield / conversion rate.
[0045] Example 1 142g of kaolin and 114g of the aluminum oxide A having mesopores and macropores were added to 291g of water, and the mixture was stirred for 15 minutes, and then 279g of aluminum sol was added, and the mixture was stirred for 60 minutes, to obtain an acidified slurry; 93g of aluminum sol was added to the second slurry, and the mixture was stirred for 30 minutes, and the whole slurry was spray-dried and molded, and then calcined at 500°C for 2 hours, to obtain catalytic cracking catalyst C1 of the present invention. The pore distribution of the obtained catalyst C1 is shown in Figure 2. The composition and properties of the catalyst are shown in Table 2.
[0046] Example 2 153g of kaolin and 86g of the aluminum oxide B having mesopores and macropores are added to 440g of water, and stirred for 30 minutes, then 186g of aluminum sol is added, and stirring is continued for 60 minutes, to obtain an acidified slurry; zeolite slurry (containing 169g of REUSY zeolite, and the solid content in the zeolite slurry is 38% by weight) is added to the acidified slurry, and stirring is continued for 40 minutes, to obtain a second slurry; 333g of the acidified pseudoboehmite is added to the second slurry, and stirring is continued for 60 minutes, and the whole slurry is spray-dried and molded, and then calcined at 500°C for 2 hours to obtain the catalytic cracking catalyst C2 of the present invention. The composition and properties of the catalyst are shown in Table 2.
[0047] Example 3 100g of kaolin and 139g of the aluminum oxide C having mesopores and macropores are added to 578g of water, and stirred for 20 minutes, then 279g of aluminum sol and 74g of silica sol are added, and stirring is continued for 60 minutes, and an acidified slurry is obtained; zeolite slurry (containing 141g of REUSY zeolite, and the solid content in the zeolite slurry is 38% by weight) is added to the acidified slurry, and stirring is continued for 60 minutes, and a second slurry is obtained; 111g of aluminum sol is added to the second slurry, and stirring is continued for 30 minutes, and the whole slurry obtained is spray-dried and molded, and then calcined at 500°C for 2 hours to obtain catalytic cracking catalyst C3 of the present invention. The composition and properties of the catalyst are shown in Table 2.
[0048] Example 4 153g of kaolin, 56g of the aluminum oxide D having mesopores and macropores, and 149g of aluminum sol were added to 179g of water, mixed uniformly, and stirred for 90 minutes to obtain an acidified slurry; zeolite slurry (containing 179g of REUSY zeolite, and the solid content in the zeolite slurry is 35% by weight) was added to the acidified slurry, and stirring was continued for 60 minutes to obtain a second slurry; 500g of the acidified pseudoboehmite was added to the second slurry, and stirring was continued for 60 minutes, and the whole slurry was spray-dried and molded, and then calcined at 550°C for 1.5 hours to obtain the catalytic cracking catalyst C4 of the present invention. The composition and properties of the catalyst are shown in Table 2.
[0049] Example 5 63g of kaolin and 169g of the aluminum oxide D having mesopores and macropores are added to 474g of water, and after stirring for 45 minutes, 372g of aluminum sol is added, and stirring is continued for 60 minutes, and an acidified slurry is obtained; zeolite slurry (containing 155g of REUSY zeolite, and the solid content in the zeolite slurry is 35% by weight) is added to the acidified slurry, and stirring is continued for 60 minutes, and a second slurry is obtained; 74g of silica sol is added to the second slurry, and stirring is continued for 30 minutes, and the whole slurry obtained is spray-dried and molded, and then calcined at 500°C for 2 hours to obtain catalytic cracking catalyst C5 of the present invention. The composition and properties of the catalyst are shown in Table 2.
[0050] Comparative Example 1 In this comparative example, the aluminum oxide having mesopores and macropores is first acidified with hydrochloric acid, and then a conventional acidification method is used to prepare a catalytic cracking catalyst.
[0051] The aluminum oxide A114g having mesopores and macropores was added to 286g of water, and after stirring for 15 minutes, 16g of 36% hydrochloric acid was added for acidification (according to the aluminum acid weight ratio of 0.2), and after stirring for 60 minutes, an acidified slurry was obtained; 142g of kaolin was added to 138g of water, and after stirring for 60 minutes, a zeolite slurry (containing 155g of REUSY zeolite, and the solid content of the zeolite slurry is 35% by weight) was added, and after continuing to stir for 30 minutes, a second slurry was obtained; The acidified slurry was mixed with the second slurry and stirred for 30 minutes, and then 372g of aluminum sol was added and mixed uniformly for 60 minutes. The obtained slurry was spray-dried and molded, and then calcined at 500°C for 2 hours to obtain a comparative catalyst DC1. The pore distribution of the obtained catalyst DC1 is shown in Figure 3. The composition and properties of the catalyst are shown in Table 2.
[0052] Comparative Example 2 In this comparative example, the mesoporous and macroporous aluminum oxide was directly used in the preparation of catalytic cracking catalyst without premixing with an acidified binder.
[0053] The aluminum oxide A having mesopores and macropores (114g) and kaolin (142g) are added to water (811g) and stirred for 60 minutes to obtain an acidified slurry; the zeolite slurry (containing REUSY zeolite (155g), the solid content in the zeolite slurry is 35wt%) is added and stirred for 30 minutes to obtain a second slurry; the aluminum sol (372g) is then added and mixed uniformly for 30 minutes, and the whole slurry is spray-dried and molded, and calcined at 500°C for 2 hours to obtain comparative catalyst DC2. The composition and properties of the catalyst are shown in Table 2.
[0054] Comparative Example 3 A catalytic cracking catalyst was prepared according to the method described in Example 1 of CN1436835A.
[0055] The mesopore- and macropore-containing aluminum oxide A615g, REUSY zeolite 1555g, aluminum sol 1628g, kaolin 2093g, and deionized water 9000g were thoroughly mixed, stirred for 2 hours, homogenized, spray-dried, and molded into microspheres, and the resulting microspheres were calcined at 450°C for 0.5 hours to obtain a control catalyst DC3. The composition and properties of the catalyst are shown in Table 2.
[0056] [Table 2]
[0057] Example 6 The catalysts C1 to C5 prepared in Examples 1 to 5 and the catalysts DC1 to DC3 prepared in Comparative Examples 1 to 3 were pre-aged in a fixed bed aging apparatus at 800°C with 100% steam for 12 hours, and then evaluated in an ACE apparatus. The properties of the reacted crude oil are shown in Table 3. The reaction temperature is 500°C, and the weight ratio of catalyst to oil is 8.02. Here, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield, total liquid yield = liquefied gas yield + gasoline yield + diesel yield, and coke selectivity = coke yield / conversion rate. The evaluation results are shown in Table 4.
[0058] [Table 3]
[0059] [Table 4]
[0060] As shown in Table 2 and the drawings, in Examples 1 to 5, the total pore volume and the proportion of the macropores and mesopores are significantly increased compared to Comparative Examples 1 to 3, but still maintain good wear resistance. Correspondingly, the results in Table 4 show that, compared to the catalysts DC1 to DC3 prepared in Comparative Examples 1 to 3, the catalysts C1 to C5 prepared in the examples of the present invention have a lower heavy oil yield, an increased total liquid yield, a lower coke yield, and a significantly improved coke selectivity. From this, it can be seen that the catalytic cracking catalyst prepared by the present invention has a rich macropore structure and mesopore structure, and this catalytic cracking catalyst provides excellent heavy oil cracking ability and good coke selectivity, as well as good catalytic strength.
[0061] The present application has been exemplified above in combination with preferred embodiments. However, these embodiments are merely illustrative and serve only illustrative purposes. Based on this, various substitutions and improvements can be made to the present application, all of which fall within the protection scope of the present application. [Brief description of the drawings]
[0062] [Figure 1] FIG. 1 is a pore distribution diagram of the aluminum oxide having mesopores and macropores used in the present invention. [Diagram 2] FIG. 2 is a pore distribution diagram of the catalytic cracking catalyst prepared according to Example 1. [Diagram 3] FIG. 3 is a pore distribution diagram of the catalytic cracking catalyst prepared according to Comparative Example 1.
Claims
1. A composition for catalytic cracking, comprising: The composition comprises, based on the dry weight of the composition, 10% to 35% by weight of aluminum oxide having mesopores and macropores, 5% to 30% by weight of an acidified binder, 2% to 20% by weight of a second binder, 20% to 60% by weight of a zeolite, and 5% to 50% by weight of a clay, the weight ratio of the acidified binder to the aluminum oxide having mesopores and macropores being 0.5 to 1.0; the aluminum oxide having mesopores and macropores is an aluminum oxide having a pseudoboehmite structure, the aluminum oxide having mesopores and macropores has a total pore volume of 0.5 mL / g to 2.0 mL / g, an average pore diameter of 5 nm to 30 nm, and a specific surface area of 250 m 2 / g~450m 2 / g, wherein the pore volume of pores between 5 nm and 100 nm accounts for 80% or more of the total pore volume; and wherein after spray drying and calcination, the composition has a pore volume of 3.0%. -1 Less than 1.0% time, preferably -1 ~3.0% time -1 and a pore volume retention of said 5 nm to 100 nm pores of 70% or more, preferably 80% to 100%; said pore volume retention of said 5 nm to 100 nm pores is calculated as follows: The pore volume retention rate of the 5 nm to 100 nm pores=the pore volume of the 5 nm to 100 nm pores in the catalytic cracking catalyst / (the pore volume of the 5 nm to 100 nm pores in the aluminum oxide having mesopores and macropores×the content of the aluminum oxide having mesopores and macropores in the catalytic cracking catalyst).
2. The composition comprises, based on the dry weight of the composition, 10 wt % to 30 wt % of the aluminum oxide having mesopores and macropores, 8 wt % to 25 wt % of the acidified binder, 2 wt % to 15 wt % of the second binder, 30 wt % to 45 wt % of the zeolite, and 10 wt % to 40 wt % of the clay, the weight ratio of the acidified binder to the aluminum oxide having mesopores and macropores being 0.5 to 0.8; the aluminum oxide having mesopores and macropores is an aluminum oxide having a pseudoboehmite structure, the aluminum oxide having mesopores and macropores has a total pore volume of 0.7 mL / g to 1.5 mL / g, an average pore diameter of 6 nm to 20 nm, and a pore size of 300 m 2 / g to 400m 2 / g, wherein the pore volume of the 5 nm to 100 nm pores accounts for 80% to 95% of the total pore volume.
3. 2. The composition of claim 1, wherein the acidified binder is in aqueous form with a pH value of 1.0 to 5.0; and the second binder is the same as or different from the acidified binder.
4. 2. The composition according to claim 1, wherein the acidified binder is one or more selected from the group consisting of aluminum sol, silica sol, and silica aluminum sol; the second binder is one or more selected from the group consisting of acidified pseudoboehmite, silica sol, aluminum sol, silica aluminum sol, aluminum phosphate sol, and zirconium sol; and the weight ratio of the acidified binder to the second binder is 0.5 to 5.
0.
5. 5. The composition of claim 4, wherein said acidified binder is an aluminum sol and said second binder is said acidified pseudoboehmite.
6. 2. The composition of claim 1, wherein the clay is one or more selected from the group consisting of kaolin, bentonite, montmorillonite, sepiolite and diatomaceous earth.
7. The composition according to claim 1, wherein the zeolite is at least one selected from the group consisting of NaY zeolite, Y zeolite with a high silica-alumina ratio obtained by modifying NaY zeolite, MFI zeolite, and β zeolite.
8. 8. The composition according to claim 7, characterized in that the Y zeolite with high silica-alumina ratio obtained after modification of the NaY zeolite is HY, REY, REHY, USY or REUSY.
9. A method for preparing a catalytic cracking catalyst using the composition according to any one of claims 1 to 8, comprising the following steps carried out in order: (1) homogeneously mixing and stirring aluminum oxide having mesopore and macropore structure, clay and optionally all acidified binders, and deionized water to obtain an acidified slurry; (2) adding zeolite to the acidified slurry and uniformly mixing and stirring to obtain a second slurry; and (3) adding a second binder to the second slurry, mixing and stirring, and spray-drying and firing the resulting mixed slurry;
10. Based on the dry weight of the catalyst, In the step (1), 10% to 35% by weight of the aluminum oxide having the mesopore structure and macropore structure, 5% to 50% by weight of the clay, and 5% to 30% by weight of the acidified binder are mixed with deionized water and pulped for 15 minutes or more to obtain an acidified slurry; the solid content of the obtained acidified slurry is 15% to 40% by weight; In the step (2), adding 20% to 60% by weight of the zeolite to the acidified slurry, mixing and pulping for 15 minutes or more to obtain the second slurry having a solid content of 15% to 40% by weight; and / or 10. The method of claim 9, wherein in step (3), 2 wt% to 20 wt% of the second binder is added to the second slurry, and the resulting mixed slurry has a solid content of 15 wt% to 40 wt%.
11. 11. The method according to claim 9 or 10, characterized in that no other acid is added in the method.
12. A catalytic cracking catalyst prepared from the composition according to any one of claims 1 to 8 by the process according to claim 9 or 10.
13. 13. The catalytic cracking catalyst according to claim 12, characterized in that the total pore volume of the catalytic cracking catalyst, determined by low-temperature nitrogen adsorption method, is 0.200 mL / g or more, wherein the pore volume of mesopores and macropores having a pore diameter of 2 nm to 100 nm accounts for 70% or more of the total pore volume, and the pore volume of mesopores having a pore diameter of 4 nm to 50 nm accounts for 60% or more of the total pore volume.
14. the total pore volume of the catalytic cracking catalyst is from 0.200 mL / g to 0.300 mL / g as determined by low temperature nitrogen adsorption; wherein the pore volume of the mesopores and macropores having a pore diameter of 2 nm to 100 nm accounts for 75% to 95%, or 80% to 95% of the total pore volume; and / or The catalytic cracking catalyst according to claim 12 or 13, wherein the pore volume of the 4 nm to 50 nm mesopores accounts for 65% to 85% of the total pore volume.
Citation Information
Patent Citations
Catalytic cracking catalyst and its prepn
CN1436835A
FCC catalysts with enhanced mesoporosity, their preparation and use
JP2021510623A
Balanced alumina matrix in zeolite containing catalyst
US4206085A