Polycarbonate alloy material, its preparation method and use

A polycarbonate alloy with polyethylene terephthalate and metal compounds addresses the limitations of conventional polycarbonate materials by enhancing melt strength and chemical resistance, allowing for the production of stable, thick-walled pharmaceutical packaging containers.

JP2024536619AActive Publication Date: 2024-10-04SHANGHAI KINGFA SCI & TECH +1
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
JP2024526005
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-26
Filing Date
2022-10-12
Publication Date
2024-10-04
Estimated Expiration
2042-10-12

AI Technical Summary

Technical Problem

Conventional polycarbonate materials used in extrusion blow molding lack sufficient chemical resistance and melt strength, making them unsuitable for manufacturing packaging containers, particularly for pharmaceutical products, and require advanced processing techniques.

Method used

A polycarbonate alloy material comprising 40-70 parts of polycarbonate, 20-40 parts of polyethylene terephthalate, and 0.1-2 parts of specific metal compounds, such as titanium or antimony oxides, along with optional additives like carbon nanotubes and reinforcing agents, is formulated to enhance melt strength, chemical resistance, and reduce melt cooling rates.

Benefits of technology

The alloy material achieves high melt strength and low melt cooling rates, enabling the production of thick-walled and large pharmaceutical packaging containers with improved chemical resistance and stability during extrusion blow molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536619000001
    Figure 2024536619000001
  • Figure 2024536619000002
    Figure 2024536619000002
  • Figure 2024536619000003
    Figure 2024536619000003
Patent Text Reader

Abstract

The present invention discloses a polycarbonate alloy material, which comprises, by weight, 40-70 parts of polycarbonate, 20-40 parts of polyethylene terephthalate and 0.1-2 parts of a metal compound, the metal compound being selected from any one of metal oxides, metal bases or metal salts, the metal being selected from any one of copper, iron, magnesium, calcium, titanium, antimony, sodium or potassium. In the present invention, the polycarbonate alloy material obtained by adding a certain amount of polyethylene terephthalate and a specific metal compound to polycarbonate not only has excellent chemical resistance, but also has high melt strength and low melt cooling rate, and is suitable for extrusion blow molding of thick and large packaging container products, providing the packaging field with new material and molding method options, especially to meet the requirements of pharmaceutical packaging containers, and further expanding the application of polycarbonate materials.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of engineering plastics, in particular to a polycarbonate alloy material, its preparation method and application. [Background technology]

[0002] Extrusion blow molding is the largest category of blow molding methods used to produce hollow thermoplastic parts. The molding process mainly involves extruding molten tubular material through an extruder, placing it in the center of an open blow mold while it is hot, closing the mold to clamp the material, and then introducing compressed air in a timely manner to expand it and push it close to the inner wall of the mold cavity to form the part. After cooling and solidifying, the mold is opened and the part is taken out. The most important blow molded products in extrusion blow molding are packaging containers for liquids and solid powders such as food, cosmetics, medicines, and chemicals, and in recent years, their application in automotive parts and household products has also increased. At present, many packaging container products made by extrusion blow molding use conventional plastics such as HDPE and PP, but they have problems such as poor mechanical properties.

[0003] Polycarbonate (PC), an engineering plastic, has excellent overall properties, high mechanical strength and toughness, but its chemical resistance is poor and requires high process requirements during extrusion blow molding, which limits its application in extrusion blow molding packaging containers (especially pharmaceutical packaging containers). At present, there are related technologies using PC materials for extrusion blow molding. Chinese patent application CN106589778A discloses a high molecular weight polymer suitable for blow molding, and by blending PC and ABS to form an alloy, the strength and toughness of the material are improved. Chinese patent application CN108164960A discloses a blow molding PC / ABS composite material, and by adding a melt promoter, styrene-acrylonitrile copolymer, to the material, the melt strength of the material is increased and the extrusion blow molding performance is improved. However, the above-mentioned conventional PC materials are mainly used for small support parts and automobile tail fins, and their chemical resistance has not been improved, and they are not suitable for packaging containers that contain medicines in particular.

[0004] Therefore, the present invention mainly studies the PC material suitable for extrusion blow molding, which can meet the requirements for use of pharmaceutical packaging containers and is of great importance for broadening the application of PC materials. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Chinese patent application CN106589778A [Patent Document 2] Chinese patent application CN108164960A Summary of the Invention [Problem to be solved by the invention]

[0006] In order to overcome the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a polycarbonate alloy material which not only has excellent chemical resistance but also has high melt strength and low melt cooling rate, and is suitable for manufacturing packaging containers by extrusion blow molding, and can also be used for packaging medicines.

[0007] Another object of the present invention is to provide a method for preparing said polycarbonate alloy material.

[0008] Another object of the present invention is to provide uses of the above polycarbonate alloy material. [Means for solving the problem]

[0009] The present invention is realized by the following technical solutions.

[0010] A polycarbonate alloy material comprising, in parts by weight: Polycarbonate 40-70 parts, 20 to 40 parts of polyethylene terephthalate, and Contains 0.1 to 2 parts of a metal compound, The metal compound is selected from any one or more of a metal oxide, a metal base or a metal salt, and the metal is selected from any one or more of copper, iron, magnesium, calcium, titanium, antimony, sodium or potassium.

[0011] Preferably, the polycarbonate alloy material comprises, in parts by weight: Polycarbonate 50-65 parts, 25 to 35 parts polyethylene terephthalate, and Contains 0.3 to 1.2 parts of metal compound.

[0012] It can be seen from the research of the present invention that adding a certain amount of polyethylene terephthalate (PET) and certain metal compounds to polycarbonate can promote the reaction of PC and PET to a certain extent to form a block copolymer, effectively improving the melt strength of the material, and at the same time delaying the crystallization of PET resin and reducing the melt cooling speed of the material; therefore, the molten tubular material extruded from the material in the extrusion blow molding process has high stability and can remain in the molten state during the bending process, and the upper and lower diameters are close to each other without breaking, so that it is possible to produce thick-walled and large-sized packaging container products by blow molding; in addition, the crystallized PET can effectively improve the chemical resistance of the material, ensuring the resistance of the material to chemicals such as drugs.

[0013] Preferably, the metal compound is selected from any one or more of titanium metal oxides or antimony metal oxides, more preferably, the metal compound is selected from any one or more of antimony metal oxides.

[0014] Preferably, the titanium metal oxide may be selected from one or more of TiO, TiO2, or Ti2O3, and the antimony metal oxide may be selected from one or more of Sb2O3, Sb2O4, Sb2O5, Sb6O 13 and SbO.

[0015] Preferably, the viscosity average molecular weight of the polycarbonate is 10,000 to 40,000. If the molecular weight of the polycarbonate is too low, the neck becomes thin during the extrusion process, the material is prone to breakage, and the material has poor corrosion resistance, while if the molecular weight is too high, the rotation of the extruder screw is restricted, making extrusion processing difficult. More preferably, the viscosity average molecular weight of the polycarbonate is 18,000 to 35,000, and even more preferably, the viscosity average molecular weight of the polycarbonate is 25,000 to 33,000.

[0016] The polycarbonate may be selected from any one or more of the aromatic polycarbonates, and the aromatic polycarbonate may be selected from bisphenol A polycarbonate.

[0017] The intrinsic viscosity of the polyethylene terephthalate is 0.65-0.88 dl / g. If the viscosity of the PET is too low, the chemical resistance is poor, and if the viscosity is too high, extrusion processing is difficult. Preferably, the intrinsic viscosity of the polyethylene terephthalate is 0.7-0.88 dl / g. The intrinsic viscosity of the polyethylene terephthalate is measured with reference to standard GT / T1632.5-08, and the time it takes for a PET solution with a concentration of 0.005 g / mL and a solvent at 25°C to flow out of a capillary is measured, and the intrinsic viscosity is calculated based on the measurement time and the solution concentration of the sample.

[0018] The polycarbonate alloy material described in the present invention may further contain 2 to 10 parts by weight of an antistatic agent, the antistatic agent being selected from any one or more types of carbon nanotubes, preferably the antistatic agent being selected from any one or more types of multi-walled carbon nanotubes having a diameter of 1.0 to 80 nm and a length of 2 to 70 μm, more preferably the antistatic agent being selected from any one or more types of multi-walled carbon nanotubes having a diameter of 20 to 60 nm and a length of 10 to 25 μm.

[0019] In the present invention, by adding a certain amount of carbon nanotubes, the melt strength of the material can be further improved and the stability of the molten tubular material extruded during the extrusion blow molding process can be improved, so as to effectively improve the extrusion blow molding processing performance of the material and at the same time endow the material with excellent antistatic properties.

[0020] The polycarbonate alloy material according to the present invention may further comprise 4 to 8 parts by weight of a toughening agent selected from one or more of ethylene-butyl acrylate-glycidyl methacrylate copolymer, ethylene-octene-glycidyl methacrylate copolymer, methyl methacrylate-butadiene-styrene copolymer, methyl methacrylate-acrylic acid copolymer, ethylene-methyl acrylate copolymer or methyl methacrylate-acrylic acid ester-silicone copolymer.

[0021] By adding a certain amount of reinforcing agent, the present invention can effectively improve the low temperature toughness of the material and further improve the chemical resistance of the material.Preferably, the reinforcing agent is obtained by blending ethylene-butyl acrylate-glycidyl methacrylate copolymer and methyl methacrylate-butadiene-styrene copolymer in a weight ratio of 1:2 to 2:1.

[0022] Depending on the performance requirements of the material, the polycarbonate alloy material according to the present invention further comprises 0.01 to 1 part by weight of an antioxidant. The antioxidant is selected from any one or more of octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(nonylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, β-(3,5-di-tert-butyl-4-hydroxyphenyl)n-octadecanol propionate, distearyl pentaerythritol diphosphite, tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane, distearyl thiopropionate, dilauryl thiopropionate, tridecyl thiodipropionate, pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] or β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid amide.

[0023] The present invention further provides a method for preparing the above-mentioned polycarbonate alloy material, which includes the steps of: putting each component into a mixer according to the compounding ratio, blending until uniform to obtain a premix; and then putting the premix into a twin-screw extruder to melt mix and extrude and granulate to prepare a polycarbonate alloy material, wherein the screw length to diameter ratio of the twin-screw extruder is 40:1-50:1, the screw barrel temperature is 240-260°C, and the screw rotation speed is 400-500 rpm.

[0024] The present invention further provides the use of the polycarbonate alloy material in the pharmaceutical packaging field. Specifically, it can be used to manufacture pharmaceutical packaging containers by extrusion blow molding. Effect of the Invention

[0025] Compared with the prior art, the present invention has the following advantages:

[0026] In the present invention, the polycarbonate alloy material obtained by adding a certain amount of polyethylene terephthalate and a specific metal compound to polycarbonate not only has excellent chemical resistance, but also has high melt strength and low melt cooling rate, and is suitable for extrusion blow molding of thick-walled and large packaging container products, especially to meet the use requirements of pharmaceutical packaging containers, providing the packaging field with new material and molding method options, and further expanding the application of polycarbonate materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The present invention will be described in detail below with reference to specific examples. The following examples are useful for those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any manner. It should be noted that those skilled in the art can make some modifications and improvements without departing from the concept of the present invention, all of which fall within the protection scope of the present invention.

[0028] The raw materials used in the examples and comparative examples of the present invention are shown below, but are not limited to these. Polycarbonate 1: Viscosity average molecular weight 28000, PC E-2000F, Mitsubishi Japan, Polycarbonate 2: Viscosity average molecular weight 23000, PC S-3000F, Mitsubishi Japan, Polycarbonate 3: Viscosity average molecular weight 16000, PC H-4000F, Mitsubishi Japan, Polycarbonate 4: Viscosity average molecular weight 35000, PC E-1000F, Mitsubishi Chemical Corporation, Polycarbonate 5: Viscosity average molecular weight 40000, PC K-1000F, Mitsubishi Japan, Polyethylene terephthalate 1: inherent viscosity 0.8 dl / g, PET BG80, characteristic chemical fiber, Polyethylene terephthalate 1: inherent viscosity 0.65dl / g, PET FG600, characteristic chemical fiber, Polybutylene terephthalate: PBT GX112, Ricoh Chemical, Acrylonitrile-butadiene-styrene copolymer: ABS PA-757, Chi Mei, Antimony metal oxide 1: Sb2O3, Sb2O3-99.8, Hunan Huaxing, Antimony metal oxide 2: Sb2O4, Sigma-Aldrich, Antimony metal oxide 3: Sb2O5, Sigma-Aldrich, Titanium metal oxide: TiO2, Sigma-Aldrich, Copper metal oxide: CuO, WSD-T201, Wujiang City Weishida Copper Industry, Iron metal oxide: Fe2O3, Hongwu New Materials, Antimony metal base: Sb(OH)3, Sigma-Aldrich, Antimony metal salts: SbCl3, Sigma-Aldrich; Sodium metal salt: NaCl, Hefei Yingheng Chemical, Calcium metal salts: CaCl2, 94% anhydrous powder, Toshin New Materials, Magnesium metal base: Mg(OH)2, Shanghai Juona, Potassium metal base: KOH, Shandong Feishuo Chemical, Antistatic agent 1: multi-walled carbon nanotubes, diameter 30-50nm, length 10-20μm, CNT106, Beijing Deke Island Metals Technology Co., Ltd. Antistatic agent 2: multi-walled carbon nanotubes, diameter 1.4-8 nm, length 10-30 μm, CNT102, Beijing Deke Island Metals Technology Co., Ltd. Antistatic agent 3: Single-walled carbon nanotube, diameter 1.4-2.2 nm, length 5-30 μm, OCSIAL, Antistatic agent 4: Carbon black, 250G, Imerys, Reinforcement 1: Ethylene-butyl acrylate-glycidyl methacrylate copolymer, commercially available, Reinforcement 2: Methyl methacrylate-butadiene-styrene copolymer, commercially available, Antioxidant: β-(3,5-di-tert-butyl-4-hydroxyphenyl) n-octadecanol propionate, commercially available.

[0029] Preparation methods of examples and comparative examples The process includes the steps of: putting each component into a mixer according to the compounding ratio and blending until uniform to obtain a premix; and then putting the premix into a twin-screw extruder to melt mix and extrude and granulate to prepare a polycarbonate alloy material, the screw length to diameter ratio of the twin-screw extruder being 45:1, the screw barrel temperature being 240-260°C, and the screw rotation speed being 500 rpm.

[0030] Related performance test methods (1) Extrusion blow molding performance test: Huatai Machinery's extrusion molding machine, HT-110, screw diameter 110mm, screw length to diameter ratio 25 / 1, motor power 4.5KW, maximum motor speed 1500m. The five extrusion temperatures are all set at 280℃, and the screw speed is 80r / min. The blow molded product is a drum with a wall thickness of 4mm, a diameter of 300mm, and a height of 500mm, the air source pressure is 0.7MPa, and the clamping force is 500kn.

[0031] A. Melt temperature: When the material extrusion is stable, test the material surface temperature (infrared thermometer) 400m below the die head. The higher the test temperature, the higher the relative yield of blow molding.

[0032] B. Stability of the bent material: When the material is bent by 500mm with the naked eye, the whole material is in a sagging state, the closer the diameter of the top and bottom of the whole tubular material, the higher the melt strength and the easier it is to blow mold, and the thinner the upper neck of the tubular material, the lower the melt strength and the more difficult it is to blow mold. "*" indicates the bent state of the material, the fewer the number of "*", the closer the diameter of the top and bottom of the whole tubular material, and the more the number of "*", the thinner the upper neck, where "*****" means that the neck is thin and will break and fall to the ground.

[0033] (2) Chemical resistance test: After conditioning a 3 mm thick molded square plate at 23°C and 50% humidity for 24 hours, 2 ml of toluene was dropped onto the surface and left to stand for 10 minutes, after which the occurrence of surface cracks was observed and evaluated based on the following criteria: ◎: No change in surface appearance. ○: Slight cracks are observed on the surface. △: Many cracks are observed on the surface. ×: Serious cracks or through-cracks are present on the surface.

[0034] (3) Antistatic performance test: Surface resistivity is used to characterize the antistatic properties of the material. After conditioning a 3 mm thick molded square plate at 23 °C and 50% humidity for 24 hours, the surface resistivity of the square plate is tested according to ASTM D257-93. If the surface resistivity of the material is 10 6 ohm / sq~10 9 If the resistivity is in the ohm / sq range, the material will exhibit better antistatic properties.

[0035] (4) Low temperature toughness test: After leaving the drum obtained by blow molding for 24 hours, 11 kg of gravel is placed inside and left in an environment of -30°C for 24 hours. Then, the drum is allowed to freely fall from a height of 1 m. This is repeated three times, and the cracks on the bottom surface are observed.

[0036] Evaluation was based on the following criteria: ◎: There is no change in the appearance of the bottom surface. ○: Slight cracks are observed on the bottom surface. △: Many cracks are observed on the bottom surface. ×: A significant crack or through-crack is present on the bottom surface.

[0037] [Table 1]

[0038] As can be seen from the above examples and comparative examples, in the present invention, a certain amount of polyethylene terephthalate and a specific metal compound are added to polycarbonate, so that the material not only has excellent chemical resistance, but also has high melt strength and low melt cooling rate, which increases the stability of the molten and bent material extruded during the extrusion blow molding process, and is conducive to blow molding.

[0039] In Comparative Examples 1 and 2, no metal compound was added or the amount of metal compound added was too small, so the cooling speed of the molten material was fast, the strength was low, and the stability of the warped material was low.

[0040] In Comparative Example 3, when the amount of the metal compound added was too large, the cooling rate of the melt became fast, the strength of the melt became low, and the chemical resistance of the material also became low.

[0041] [Table 2]

[0042] Comparing Examples 9 to 17 with Example 1, preferably the metal compound is titanium metal oxide or antimony metal oxide.

[0043] [Table 3]

[0044] In Comparative Example 4, when polybutylene terephthalate (PBT) was added, the melt of the material cooled faster, the strength was lower, and the stability of the warped material was reduced.

[0045] In Comparative Example 5, when acrylonitrile-butadiene-styrene copolymer ABS was added, the chemical resistance of the material was low, the cooling rate of the melt was fast, the strength of the melt was low, and the stability of the warped material was also low.

[0046] [Table 4]

[0047] As can be seen from Examples 23 to 28, in the present invention, a certain amount of antistatic carbon nanotubes and reinforcing agent can be added, which can effectively improve the antistatic properties and low temperature toughness of the material, while also ensuring the chemical resistance of the material, so that the material has a low melt cooling rate and high melt strength, and can effectively realize extrusion blow molding and meet the use requirements of pharmaceutical packaging containers.

[0048] In Comparative Example 6, the use of carbon black is not very effective in improving the antistatic properties of the material, the melt strength of the material is low, the stability of the deflected material is low, and the low temperature toughness of the material is also poor.

Claims

1. A polycarbonate alloy material comprising, in parts by weight: 40 to 70 parts polycarbonate, 20 to 40 parts polyethylene terephthalate, and Contains 0.1 to 2 parts of a metal compound, The metal compound is selected from any one or more of a metal oxide, a metal base, or a metal salt, and the metal is selected from any one or more of copper, iron, magnesium, calcium, titanium, antimony, sodium, or potassium.

2. In parts by weight Polycarbonate 50 to 65 parts, 25 to 35 parts polyethylene terephthalate, and 2. The polycarbonate alloy material according to claim 1, characterized in that it contains 0.3 to 1.2 parts of a metal compound.

3. The polycarbonate alloy material according to claim 1, characterized in that the metal compound is selected from any one or more of titanium metal oxides or antimony metal oxides, preferably, the metal compound is selected from any one or more of antimony metal oxides.

4. The titanium metal oxide is TiO, TiO 2 Or Ti 2 O 3 The antimony metal oxide is selected from one or more of Sb 2 O 3 , Sb 2 O 4 , Sb 2 O 5 , Sb 6 O 13 4. The polycarbonate alloy material according to claim 3, characterized in that the molar ratio of SbO is selected from one or more of SbO.

5. The polycarbonate alloy material according to claim 1, characterized in that the viscosity average molecular weight of the polycarbonate is 10,000 to 40,000, preferably 18,000 to 35,000, more preferably 25,000 to 33,000, and the intrinsic viscosity of the polyethylene terephthalate is 0.65 to 0.9 dl / g, preferably 0.7 to 0.88 dl / g.

6. The polycarbonate alloy material according to claim 1, further comprising 2 to 10 parts by weight of an antistatic agent, the antistatic agent being selected from any one or more types of carbon nanotubes, preferably, the antistatic agent being selected from any one or more types of multi-walled carbon nanotubes having a diameter of 1.0 to 80 nm and a length of 2 to 70 μm, and more preferably, the antistatic agent being selected from any one or more types of multi-walled carbon nanotubes having a diameter of 20 to 60 nm and a length of 10 to 25 μm.

7. The polycarbonate alloy material according to claim 1, further comprising 4 to 8 parts by weight of a toughening agent selected from one or more of ethylene-butyl acrylate-glycidyl methacrylate copolymer, ethylene-octene-glycidyl methacrylate copolymer, methyl methacrylate-butadiene-styrene copolymer, methyl methacrylate-acrylic acid copolymer, ethylene-methyl acrylate copolymer, or methyl methacrylate-acrylic acid ester-silicone copolymer, preferably, the toughening agent is obtained by blending ethylene-butyl acrylate-glycidyl methacrylate copolymer and methyl methacrylate-butadiene-styrene copolymer in a weight ratio of 1:2 to 2:

1.

8. The antioxidant may further comprise 0.01 to 1 part by weight of an antioxidant, the antioxidant being selected from the group consisting of octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(nonylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, β-(3,5-di-tert-butyl-4-hydroxyphenyl)n-octadecanol propionate, distearyl pentaerythritol diphosphite, tetrakis[methylene(3,5-di 3. The polycarbonate alloy material according to claim 1, characterized in that the thiol group is selected from any one or more of the following: thiol group, thiol group-1, thiol group-2, thiol group-3, thiol group-4, thiol group-5, thiol group-6, thiol group-7, thiol group-8, thiol group-9, thiol group-10, thiol group-11, thiol group-12, thiol group-13, thiol group-14, thiol group-15, thiol group-16, thiol group-17, thiol group-18, thiol group-19, thiol group-20, thiol group-21, thiol group-22, thiol group-23, thiol group-24, thiol group-25, thiol group-26, thiol group-27, thiol group-28, thiol group-29, thiol group-30, thiol group-31, thiol group-32, thiol group-33, thiol group-34, thiol group-35, thiol group-36, thiol group-37, thiol group-38, thiol group-39, thiol group-40, thiol group-41, thiol group-42, thiol group-43, thiol group-44, thiol group-45, thiol group-45, thiol group-45, thiol group-45, thiol group-45, thiol group-46, thiol group-47, thiol group-48, thiol group-49, thiol group-51, thiol group-52, thiol group-53, thiol group-54, thiol group-55, thiol group-55, thiol group-55,

9. The method for preparing polycarbonate alloy material according to any one of claims 1 to 8, comprising the steps of: putting each component into a mixer according to the compounding ratio, blending until uniform to obtain a premix; and then putting the premix into a twin-screw extruder to melt mix and extrude and granulate to prepare a polycarbonate alloy material, wherein the ratio of screw length to diameter of the twin-screw extruder is 40:1 to 50:1, the screw barrel temperature is 240 to 260°C, and the screw rotation speed is 400 to 500 rpm.

10. Use of the polycarbonate alloy material according to any one of claims 1 to 8 in the field of pharmaceutical packaging.

Citation Information

Patent Citations

  • Method of manufacturing polycarbonate / polyester alloy

    CN101367992A

  • Polycarbonate / polyethylene glycol terephthalate resin composite and preparation method

    CN101812223A

  • High-fluidity flame-retardant PET / PC resin composition and preparation method thereof

    CN106189114A

  • PC alloy material and preparing method and application thereof

    CN106317827A