Coated quantum dot material, its preparation method and quantum dot optical device
A coated quantum dot material with an inorganic salt coating addresses high-temperature and environmental stability issues, ensuring high quantum yield and reduced light attenuation, suitable for quantum dot devices.
Patent Information
- Application Number
- JP2024515354
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-10
- Filing Date
- 2022-08-26
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-08-26
AI Technical Summary
Existing quantum dot materials face challenges in maintaining fluorescence performance due to poor high-temperature resistance, moisture resistance, and oxygen sensitivity, which are not adequately addressed by current protective methods such as water-oxygen barrier structures or coatings with metal oxides or inorganic salts.
A coated quantum dot material is developed with an inorganic salt coating agent having a specific solubility and thermal decomposition temperature, combined with a quantum dot core material in a defined ratio, to form a dense coating layer that enhances thermal stability and resistance to moisture and oxygen, using a method involving mixing, heating, and reacting cation and anion solutions.
The coated quantum dots exhibit improved quantum yield and reduced light attenuation after high-temperature processing, demonstrating enhanced stability and resistance to environmental factors, allowing for efficient use in quantum dot devices.
Smart Images

Figure 2024536739000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to a Chinese patent application filed with the China Patent Office on September 6, 2021, bearing application number 202111036932.8 and titled "Coated quantum dot material, its preparation method, and quantum dot optical device", and to a Chinese patent application filed with the China Patent Office on November 10, 2021, bearing application number 202111328760.1 and titled "Coated quantum dot material, its preparation method, and quantum dot optical device", the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to the technical field of quantum dot materials, in particular to coated quantum dot materials and their preparation methods and quantum dot optical devices. [Background technology]
[0003] Quantum dots are quasi-zero-dimensional fluorescent semiconductor nanocrystals, and due to their excellent fluorescent performance (high quantum yield, continuously adjustable fluorescent emission wavelength, narrow half-width, etc.), they have great potential for application in the fields of lighting and display. However, during processing and use, quantum dot materials are easily affected by conditions such as light, heat, water, and oxygen, making it difficult to maintain their fluorescent properties for a long period of time. In particular, when forming a quantum dot plate structure, the quantum dots have poor high-temperature resistance, making it difficult to maintain their good fluorescent performance after high-temperature molding or curing steps, which impedes the development of the fields of lighting and display.
[0004] At present, there are two main solutions adopted in the industry. One solution is to use a water and oxygen barrier structure to protect the quantum dot material. For example, in the patent originally applied for by nanosys and 3M, two layers of water and oxygen barrier film are attached outside the quantum dot layer to protect the quantum dot material (CN201480005245.1). However, in this method, the barrier film is expensive and the application process is complicated.
[0005] Another solution is to form a coated quantum dot material to form a protection for the quantum dots. For example, CN108913142A, CN108285792A coat the quantum dot material with metal oxide to improve its stability. However, in the process of processing, as the temperature increases, the ligands (such as fatty acids, thiols, etc.) of the partial quantum dots are oxidized at high temperature to produce other organic substances (such as sulfonic acids, etc.), which become more acidic and react with the oxides on the surface of the quantum dots, further affecting the quantum dot material.
[0006] CN108893103A provides a method for coating quantum dots with inorganic salts, which uses a one-step method to coat the surface of quantum dots by adsorption, and the performance of the coated quantum dots thus formed can be guaranteed to have no obvious light attenuation after 500 hours of blue light irradiation. However, in practical applications, quantum dot devices usually require smooth operation for more than 1000 hours, and the patent does not disclose the thermal stability of the resulting coated quantum dots.
[0007] So far, the prior art still lacks quantum dot materials that meet the needs of high temperature processing and have good water resistance and oxygen ability. Summary of the Invention [Problem to be solved by the invention]
[0008] The purpose of the present application is to provide a coated quantum dot material and a preparation method thereof and a quantum dot device, in order to overcome the defects of the quantum dot materials existing in the prior art, such as being unable to withstand high temperature processing, having poor stability, and poor moisture resistance. The coated quantum dot material of the present application can withstand high temperature processing, has good water resistance, oxygen ability, and has good stability. [Means for solving the problem]
[0009] In order to achieve the above object, according to a first aspect, the present application provides a coated quantum dot material comprising a quantum dot core material and an inorganic salt coating agent, the quantum dots comprising oil-soluble quantum dots, the inorganic salt coating agent having a solubility in water of less than 0.01 g / 100 g and a thermal decomposition temperature of more than 300° C., and the ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent in the coated quantum dot material is 1:0.001 g / mol to 1:0.05 g / mol, preferably 1:0.002 g / mol to 1:0.02 g / mol, and most preferably 1:0.003 g / mol to 1:0.005 g / mol.
[0010] Furthermore, the particle size of the quantum dot core material is 3 to 15 nm, and the coating thickness of the inorganic salt coating agent is 0.5 to 20 nm.
[0011] Furthermore, the coated quantum dot material of the present application has a quantum yield of 70% or more after thermal processing at a high temperature of 200 to 300°C, and the quantum dot device obtained after the thermal processing has a light attenuation of less than 20%, a light attenuation of less than 10%, and more preferably a light attenuation of less than 5% after 1000 hours of high temperature and high humidity blue light accelerated aging measurement.
[0012] Furthermore, the coated quantum dot material has a quantum yield of 80% or more after being thermally processed at a high temperature of 200 to 300° C., and more preferably has a quantum yield of 90% or more.
[0013] Furthermore, the method for preparing the coated quantum dot material includes: S1: Mixing a quantum dot core material, an organic solvent, and an oil-soluble cation precursor to obtain a first mixed solution, the quantum dot core material including oil-soluble quantum dots, and the organic solvent having a boiling point higher than the boiling point of water; S2: Heating the first mixture, the heating temperature being higher than 90°C; S3: Dropping an aqueous anion solution required for growing an inorganic salt into the heated first mixture and reacting the solution to obtain a coated quantum dot material.
[0014] According to a second aspect, the present application provides a preparation method for forming a coated quantum dot material, the coated quantum dot material including a quantum dot core material and an inorganic salt coating agent, the preparation method comprising: S1: Mixing a quantum dot core material, an organic solvent, and an oil-soluble cation precursor to obtain a first mixed solution, the quantum dot core material including oil-soluble quantum dots, and the organic solvent having a boiling point higher than the boiling point of water; S2: Heating the first mixture, the heating temperature being higher than 90°C; S3: Dropping an aqueous anion solution required for growing an inorganic salt into the heated first mixture and reacting the solution to obtain a coated quantum dot material.
[0015] Furthermore, in step S1, the ratio of the mass of the quantum dots to the molar amount of the oil-soluble cation precursor is 1:0.001 g / mol to 1:0.05 g / mol, preferably 1:0.002 g / mol to 1:0.02 g / mol, and most preferably 1:0.003 g / mol to 1:0.006 g / mol.
[0016] Furthermore, in step S2, the heating temperature is 100° C. or higher. There is no particular upper limit to the heating temperature, but it is desirable to set it to 200° C. or lower from the viewpoints of equipment requirements and energy conservation.
[0017] Furthermore, in step S2, the heating time is 10 to 60 minutes.
[0018] Furthermore, in step S3, the dropping speed is 0.5 to 2 mL / min, and preferably 1 to 1.5 mL / min.
[0019] According to a third aspect, the present application provides a coated quantum dot material formed from the preparation method of the second aspect.
[0020] Furthermore, the ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent in the coated quantum dot material is 1:0.001 g / mol to 1:0.05 g / mol, preferably 1:0.002 g / mol to 1:0.02 g / mol, and most preferably 1:0.003 g / mol to 1:0.005 g / mol.
[0021] Furthermore, the coated quantum dot material has a quantum yield of 70% or more, preferably 80% or more, and most preferably 90% or more after thermal processing at a high temperature of 200 to 300°C, and the quantum dot device obtained after the thermal processing has a light attenuation of less than 20%, preferably less than 10%, and most preferably less than 5% after 1000 hours of high temperature, high humidity, blue light accelerated aging measurement.
[0022] According to a fourth aspect, the present application provides a quantum dot device comprising the coated quantum dot material according to the first or third aspect. Effect of the Invention
[0023] In the prior art, the thickness of the coated quantum dot material layer is generally 0.5-20 nm, but the specific effect of the thickness on the light resistance, heat, water and oxygen resistance of the quantum dot material is not clear, and the expression in the stability of the coated quantum dot material with the same coating layer thickness may have obvious differences, and at the same time, no preferred thickness range favorable for the stability of the coated quantum dots has been found. At present, there is no related research on the stability of the coated quantum dot material of the coating structure parameters of the coated quantum dots. The inventors of the present application have found that, in response to the uncertainty of the thickness and stability of the quantum dot material, by optimizing the ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent, the light resistance, heat, water and oxygen resistance of the coated quantum dot material can be effectively improved. By forming a specific amount of coating layer, the high temperature processability of the quantum dot material can be significantly improved, and it has good light resistance, water and oxygen ability, that is, excellent stability. The mechanism by which the current ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent affects the light, heat, water, and oxygen resistance of the coated quantum dots is not clear, but one possible reason is that a coating amount that satisfies the above ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent is more advantageous for forming a coating layer with a density and / or volume that meets the requirements of actual applications, and effectively blocks contact between the quantum dots and water, oxygen, etc., preventing disadvantages such as quenching caused by both, while not significantly affecting the optical performance of the quantum dot core material. This coating amount can directly connect the surface of the quantum dots with a sufficient amount of coating layer on the lattice layer surface, greatly reducing the probability of exposure of defects on the surface of the quantum dots that are likely to be the starting point of reactions such as phase transition, greatly improving the light resistance and heat resistance of the quantum dots, and reducing the impact of light, heat, etc. on the quantum dot core material; at the same time, the coating amount of the coating agent within the above ratio does not cause excessive stress on the contact surface between the inorganic salt structure and the quantum dot structure, which would compress the original lattice structure, generate defects, and affect the transmission of light.
[0024] The quantum dot material of the present application breaks through the technical bottleneck that quantum dot materials cannot withstand high-temperature processing. The material can be directly mixed with pellets such as PS and then thermally processed to prepare optical devices such as quantum dot diffuser plates / light guide plates / functional plates, which greatly reduces the production cost, optimizes the preparation process, reduces the quantum yield loss before and after processing, and improves the optical stability of quantum dot optical devices.
[0025] The present application further provides a method for preparing coated quantum dots, which comprises premixing quantum dots with oil-soluble cation precursors for growing inorganic salts and heating the mixture to adsorb a large amount of cations on the surface of the quantum dots in the oil phase, and then dripping an anion aqueous phase solution therein, which is favorable for dispersing the anion precursor; since the temperature in the first mixture is relatively high, close to or above the boiling point of water, when dripping a small volume of anion droplets, the aqueous solvent evaporates quickly, and at the dripped interface, the anions rapidly combine with the cations on the surface of the quantum dots to form a dense inorganic salt coating layer, thereby obtaining a coated quantum dot material with a high ratio of coating layer to quantum dot core material. This method can obtain a denser and / or larger inorganic salt coating layer than the preparation process that relies only on adsorption to form the coating layer and single-phase coating layer, and the obtained coated quantum dot material has excellent high-temperature resistance and processability compared to other coated quantum dot materials prepared by liquid phase methods, and has good light, water and oxygen resistance and high stability. [Brief description of the drawings]
[0026] The specification drawings which form a part of this application are used to provide a further understanding of this application, and the exemplary embodiments and the description thereof are used to explain this application, and are not intended to unduly limit this application. The drawings are as follows:
[0027] [Figure 1] FIG. 1 is a structural schematic diagram of the coated quantum dot material of the present application. [Diagram 2] FIG. 2 is an electron microscope view of the coated quantum dot material of Example 1 of the present application. [Diagram 3] FIG. 2 is an electron microscope view of a quantum dot material of Comparative Example 1 of the present application. [Figure 4] 1 is a graph of aging measurements of examples and comparative examples of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] The range endpoints and any values disclosed herein are not limited to the precise ranges or values, and should be understood to include values close to these ranges or values. Numerical ranges can be combined between the range endpoints, between the range endpoints and single point values, and between the single point values to obtain one or more new numerical ranges, and these numerical ranges should be considered specifically disclosed herein.
[0029] In this application, "solubility" refers to the solubility of the inorganic salt coating agent in water at 20°C.
[0030] As mentioned above, According to a first aspect, the present application provides a coated quantum dot material comprising a quantum dot core material and an inorganic salt coating agent, the quantum dots comprising oil-soluble quantum dots, the inorganic salt coating agent having a solubility in water of less than 0.01 g / 100 g and a thermal decomposition temperature of more than 300° C., and the ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent in the coated quantum dot material is 1:0.001 g / mol to 1:0.05 g / mol, preferably 1:0.002 g / mol to 1:0.02 g / mol, and most preferably 1:0.003 g / mol to 1:0.005 g / mol.
[0031] In the present application, the coated quantum dot material has a coating structure, and as shown in FIG. 1, specifically, it can be understood that the quantum dot (i.e., A shown in FIG. 1) is coated with the inorganic salt coating agent (i.e., B shown in FIG. 1).
[0032] The coated quantum dot material having the ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent has excellent light resistance, heat, water, and oxygen resistance. In any embodiment, the coated quantum dot material has a quantum yield of 70% or more, preferably 80% or more, and more preferably 90% or more after thermal processing at a high temperature of 200 to 300 ° C. In another embodiment, the quantum dot device obtained after the thermal processing has a light attenuation of less than 20%, preferably less than 10%, and more preferably less than 5% after 1000 h of high temperature and high humidity blue light accelerated aging measurement. The measurement shows that the quantum dot device prepared with the quantum dot material has a light attenuation of less than 20% even after 3500 h of high temperature and high humidity blue light accelerated aging measurement after the thermal processing.
[0033] The conditions for the high temperature, high humidity, blue light accelerated aging measurement were 60°C, 90% humidity, and 40W / m 2 , 450nm blue light.
[0034] The coated quantum dot material of the present application can have the above quantum yield and optical attenuation after thermal processing, whereas under the same conditions, conventional coated quantum dot materials generally have a quantum yield of less than 70% and an optical attenuation of 40% or more after 1000 hours of high temperature, high humidity, blue light accelerated aging measurement.
[0035] In the present application, there is no specific limitation on the type of the quantum dot core material, and any quantum dot material containing conventional oil-soluble quantum dots can be used in the present application, and the quantum dot material, which is the non-ligand portion of the oil-soluble quantum dot, is at least one of the semiconductor compounds of the II-IV, II-VI, II-V, III-V, III-VI, IV-VI, I-III-VI, II-IV-VI, and II-IV-V groups of the periodic table of elements; and / or at least one of the semiconductor compounds having a core-shell structure consisting of at least two of the II-IV, II-VI, II-V, III-V, III-VI, IV-VI, I-III-VI, II-IV-VI, and IIIV-V groups of semiconductor compounds; and / or at least one of the perovskite nanoparticle materials, metal nanoparticle materials, metal oxide nanoparticle materials, and carbon nanomaterials. The quantum dot core material may be commercially available or may be synthesized by a conventional method.
[0036] It is understood that the quantum dot core material may include other non-oil soluble quantum dot components in addition to the oil soluble quantum dots, and preferably the quantum dot core material is only oil soluble quantum dots.
[0037] The inorganic salt coating agent of the present application is not particularly limited as long as it satisfies the above requirements of solubility and thermal decomposition temperature.
[0038] Furthermore, the inorganic salt coating agent may be one or more selected from alkaline earth metal salts, Group IIIA metal salts, Group IVA metal salts, and transition metal salts.
[0039] The alkaline earth metal salt, Group IIIA metal salt, Group IVA metal salt, and transition metal salt may be one or more selected from sulfates, carbonates, molybdates, borates, and halogen salts of the above metals.
[0040] The present application has no specific requirements for the particle size of the quantum dot core material and the thickness of the coating layer formed by the inorganic salt coating agent, and as long as the ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent meets the range limited in the present application, it is possible to obtain better light resistance, heat, water, and oxygen resistance than the prior art. Also, as mentioned above, the specific effect of the thickness on the light resistance, heat, water, and oxygen resistance of the quantum dot material is not clear in the present field, and unless the above limitations of the present application are met, no matter how the thickness is adjusted, it is not possible to ensure better light resistance, heat, water, and oxygen resistance than the prior art.
[0041] Preferably, the particle size of the quantum dot core material is 3-15 nm, and the thickness of the coating layer formed by the inorganic salt coating agent is 0.5-20 nm. The upper limit of the preferred thickness given here is taken into consideration from various aspects such as convenient preparation and economical cost, and it should be emphasized that even if the thickness is not within the preferred range, the technical effect of the present application can be realized as long as the ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent satisfies the above-mentioned limitations of the present application. Within the above range of the particle size of the quantum dot core material and the thickness of the coating layer, the coating layer tends to form a coating layer structure with a moderate density compared to the conventional technology, and can obtain good optical performance while satisfying excellent light resistance, heat, water, and oxygen resistance.
[0042] Preferably, the preparation method of the coated quantum dot material includes the steps of: S1: mixing a quantum dot core material, an organic solvent, and an oil-soluble cation precursor to obtain a first mixed solution, the quantum dot core material containing an oil-soluble quantum dot, and the organic solvent having a boiling point higher than that of water; S2: heating the first mixed solution, the heating temperature being higher than 90° C.; and S3: dropping an anion aqueous solution required for growing an inorganic salt into the heated first mixed solution, and reacting to obtain a coated quantum dot material. The selective scope of the specific process is the same as the preparation method provided by the second aspect of the present application, and specifically, please refer to the subsequent description related to the second aspect.
[0043] The preparation of the coated quantum dot material by the liquid phase method has the advantages of being a simple process, easy to industrialize, etc. The above preparation method is only one method for preparing the coated quantum dot material provided in the present application, and the coated quantum dot material of the present application may be prepared in other ways, and the present application is not limited thereto.
[0044] According to a second aspect, the present application provides a method for preparing a coated quantum dot material, the method comprising: S1: Mixing a quantum dot core material, an organic solvent, and an oil-soluble cation precursor to obtain a first mixed solution, the quantum dot core material including oil-soluble quantum dots, and the organic solvent having a boiling point higher than the boiling point of water; S2: Heating the first mixture, the heating temperature being higher than 90°C; S3: Dropping an aqueous anion solution required for growing an inorganic salt into the heated first mixture and reacting the solution to obtain a coated quantum dot material.
[0045] In the second embodiment, the selective range of the quantum dot core material and the inorganic salt coating agent is the same as that of the quantum dot core material and the inorganic salt coating agent in the first embodiment, and the explanation thereof is omitted here.
[0046] In the present application, in step S1, the quantum dot core material and the oil-soluble cation precursor are mixed in an organic solvent to form a first oil phase mixture, and a large amount of cations can be adsorbed on the surface of the quantum dot core material by utilizing the high solubility of the oil-soluble quantum dots and the oil-soluble cation precursor in the organic solvent, which is more advantageous for subsequently dropping anions to grow a large amount of inorganic salts.
[0047] Furthermore, in step S1, the ratio of the mass of the quantum dots to the molar amount of the oil-soluble cation precursor is 1:0.001 g / mol to 1:0.05 g / mol, preferably 1:0.002 g / mol to 1:0.02 g / mol, and most preferably 1:0.003 g / mol to 1:0.006 g / mol.
[0048] The above-mentioned ratio of the amount of the quantum dots and the oil-soluble cation precursor is advantageous for the quantum dot surface to adsorb the cations in a suitable amount and uniformly.
[0049] In the present application, the organic solvent is not particularly limited as long as its boiling point is higher than that of water. Those skilled in the art can select an appropriate organic solvent according to the solubility of the quantum dots and the oil-soluble cation precursor. The selected organic solvent may or may not undergo a suitable coordination reaction with the quantum dot core material. Non-limiting examples of the organic solvent include liquid paraffin, aromatic hydrocarbons, long-chain alkanes, fatty acids, and octadecene.
[0050] The amount of the organic solvent used may be any amount that allows the quantum dot core material and the oil-soluble cation precursor to be sufficiently mixed, and a person skilled in the art can select an appropriate amount depending on the amounts of the quantum dot core material and the oil-soluble cation precursor used.
[0051] According to the present application, there is no limitation on the mixing method of each raw material in step S1. It may be directly mixed in one step, two of the raw materials may be mixed first and then mixed with another raw material, or they may be mixed in a batch manner.
[0052] In a specific embodiment, in step S1, the quantum dots and the oil-soluble cation precursor are added to the organic solvent to obtain a quantum dot core material solution and an oil-soluble cation precursor solution, and then the two are mixed. In another specific embodiment, the oil-soluble cation precursor may be added to the organic solvent first, and then the quantum dots may be added, or the quantum dot core material may be added to the organic solvent, and then the oil-soluble cation precursor may be added.
[0053] In another specific preferred embodiment, the method includes, before step S1, first preparing the quantum dot core material into a quantum dot oil solution, and then performing step S1.
[0054] In the above preferred embodiment, the quantum dot core material is mixed with the oil-soluble cation precursor and the organic solvent in the form of a quantum dot oil solution, which is advantageous for uniform adsorption of the quantum dot core material and the cation.
[0055] The organic solvent used in preparing the quantum dot oil solution may be the same as or different from the organic solvent used in the subsequent mixing of the quantum dot core material and the oil-soluble cation precursor, and is preferably the same.
[0056] In the present application, by controlling the heating so that the temperature of the first mixed liquid in step S2 approaches or exceeds the boiling point of water, and combining this with the dripping of the anion aqueous solution in step S3, the water solvent can be rapidly evaporated during the dripping process, and at the dripping interface, the anions can rapidly combine with the cations on the quantum dot surface to grow and form an inorganic salt coating layer.
[0057] Compared with conventional methods, the preparation method formed in the above steps can simultaneously utilize the adsorption and ionic bond formation effects to grow more inorganic salt coating agents, more densely and more stably, to form a coating structure on the surface of the quantum dots, thereby achieving the effect that the coated quantum dot material has the comprehensive performance of high temperature resistance, moisture resistance, oxidation resistance and light irradiation resistance.
[0058] Preferably, the heating temperature in step S2 is 100° C. or higher.
[0059] In the present application, the heating time in step S2 is preferably 10 to 60 minutes.
[0060] The above preferred heating conditions are advantageous for the adsorption of the oil-soluble cation precursor and the quantum dot core material, and at the same time, the selection of the heating temperature is advantageous for the rapid evaporation of the aqueous solvent during the dropwise addition, and is advantageous for the growth reaction of the inorganic salt.
[0061] In the present application, preferably, in step S2, the heating is performed under an inert atmosphere, such as argon gas or nitrogen gas, which is more advantageous in preventing the quantum dot core material from being oxidized by contact with oxygen in the air before being coated with the inorganic salt.
[0062] More preferably, in step S2, the heating is performed under stirring, which favors mass transfer and, on the one hand, allows sufficient adsorption of the cation precursor on the quantum dot core material, and, on the other hand, makes the temperature distribution more uniform.
[0063] According to the present application, in step S3, the dropping speed is preferably 0.5-2 mL / min, more preferably 1-1.5 mL / min. If the dropping speed is too fast, the degree of supersaturation at the interface is too large, and the sparingly soluble salt formed tends to self-nucleate, instead of growing on the surface of the quantum dots; if the dropping speed is too slow, the solvent temperature is higher than the boiling point of water, and the solvent evaporates too quickly, which is unfavorable to the chemical reaction at the interface. The preferred specific dropping speed scheme of the present application can encourage the formation of an appropriate amount of coating layer at the dropped interface, and further improve the light resistance, heat resistance, water resistance, and oxygen resistance of the obtained coated quantum dot material.
[0064] In this application, those skilled in the art can select the specific types of cation precursor and anion aqueous solution that form poorly soluble inorganic salt according to the type of inorganic salt coating agent. In particular, this application requires the adoption of oil-soluble cation precursor, which is more advantageous for adsorption to cations on the quantum dot surface.
[0065] Preferably, the oil soluble cation precursor is one or more selected from oil soluble alkaline earth metal salt precursors, oil soluble IIIA metal salt precursors, oil soluble IVA metal salt precursors, oil soluble transition metal salt precursors.
[0066] The specific types of the oil-soluble alkaline earth metal salt precursor, oil-soluble IIIA metal salt precursor, oil-soluble IVA metal salt precursor, and oil-soluble transition metal salt precursor may be any type that can prepare the inorganic salt coating agent. For example, the oil-soluble alkaline earth metal salt, oil-soluble IIIA metal salt precursor, oil-soluble IVA metal salt precursor, and oil-soluble transition metal salt are preferably selected from stearates, phosphonates, oleates, oleylamine salts, and the like containing alkaline earth metals, IIIA metals, IVA metals, and transition metals.
[0067] In the present application, the anion in the anion aqueous solution is determined depending on the type of the target inorganic salt, and the cation in the anion aqueous solution may be any cation that does not affect the growth of the inorganic salt, such as sodium ions, potassium ions, and ammonium ions.
[0068] In the present application, the concentration of the anion in the anion aqueous solution is not particularly limited, as long as it can ensure sufficient dissolution and is favorable for the water solvent in the anion aqueous solution to rapidly evaporate during the dropping process. For example, the anion concentration in the anion aqueous solution may be 0.05 to 10 mol / L.
[0069] The amount of the anionic aqueous solution used may be sufficient to allow sufficient reaction between the cations and anions in the oil-soluble cation precursor. According to the present application, the method preferably further includes, in step S3, continuing the incubation for 15 to 120 minutes after the completion of the dropping. In the continued incubation process, the cations and anions can continue to react, thereby ensuring that sufficient reaction products are obtained.
[0070] According to a third aspect, the present application provides a coated quantum dot material obtained by the method for preparing a coated quantum dot material according to the second aspect.
[0071] Preferably, the coated quantum dot material can obtain a coating structure having a sufficient amount of coating layer similar to that of the first embodiment, and has excellent high-temperature processability and stability to light, heat, water, and oxygen.
[0072] According to a fourth aspect, the present application provides a quantum dot device comprising the coated quantum dot material according to the first or third aspect.
[0073] The present application does not impose any restrictions on the form of the quantum dot device, and includes any form of quantum dot device in the lighting and display fields, such as, but not limited to, quantum dot diffusion plate / light guide plate / functional plate, etc.
[0074] The present application does not impose any restrictions on the method of preparing the quantum dot material to obtain the coated quantum dot device, and the method can be carried out using conventional methods, for example, by directly mixing the coated quantum dot material with pellets such as PS and processing them into a quantum dot device.
[0075] The present disclosure will now be described in more detail with reference to examples.
[0076] Example 1 After selecting and purifying the CdSe / ZnS oil-based quantum dots, 3 g was taken for use.
[0077] 300 mL of liquid paraffin was placed in a flask, 0.01 mol of barium stearate and 3 g of the above quantum dots were added to obtain a first mixed solution, which was then passed through with argon gas, stirred (1000 r / min), heated to 120°C, and kept at that temperature for 30 min.
[0078] Next, 10 mL of an aqueous sodium sulfate solution was added dropwise, with the sulfate ion concentration set to 1 mol / L and the drop rate set to 1 mL / min.
[0079] After the dropping was completed, the mixture was kept warm for 1 hour and purified to obtain a coated quantum dot material having a barium sulfate shell layer on the surface.
[0080] An electron microscope image of the resulting coated quantum dot material is shown in FIG.
[0081] Comparative Example 1 3g quantum dot material selected and purified in Example 1.
[0082] An electron microscope image of the resulting quantum dot material is shown in FIG.
[0083] Comparative Example 2 3 g of quantum dot material obtained by selection and purification according to the method of Example 1 was dissolved in 300 mL of liquid paraffin, heated to 120°C, and 0.01 mol of barium sulfate was added. After sufficient reaction and stirring, a quantum dot material with a barium sulfate shell layer on the surface was obtained after purification.
[0084] Comparative Example 3 A flask was charged with 3 g water-soluble CdSe / ZnS quantum dots, 300 mL of aqueous solution, and 0.01 mol of barium chloride.
[0085] Argon gas was passed through the mixture, which was stirred (1000 r / min), and 10 mL of an aqueous sodium sulfate solution (sodium sulfate concentration: 1 mol / L) was added dropwise at a rate of 1 mL / min.
[0086] After the dropping was completed, stirring was continued for 1 hour, and the mixture was purified to obtain a quantum dot material having a barium sulfate shell layer on the surface.
[0087] Example 2 The procedure of Example 1 was repeated, except that the amount of barium stearate used was 0.005 mol, and the amount of the aqueous sodium sulfate solution (having the same concentration as in Example 1) used was 5 mL.
[0088] Example 3 The procedure of Example 1 was repeated, except that the amount of barium stearate used was 0.05 mol, and the amount of the aqueous sodium sulfate solution (having the same concentration as in Example 1) used was 50 mL.
[0089] Example 4 The procedure of Example 1 was followed, except that the drip rate was 2 mL / min.
[0090] Example 5 The procedure of Example 1 was followed, except that the drip rate was 0.5 mL / min.
[0091] Table 1 shows partial test parameters and measurement results for the above examples and comparative examples.
[0092] Measurement method The coated quantum dot material and PS granule pellets obtained in the examples and comparative examples were mixed at 250°C, and an extruded plate was extruded using a micro extruder and a flat plate vulcanizer to prepare a quantum dot PS device. Next, the following measurements were performed.
[0093] The quantum dot PS devices were subjected to accelerated aging tests under high temperature and high humidity blue light (60°C, 90% humidity, 40 W / m 2 The normalized luminance time curve obtained is shown in FIG. 4.
[0094] Quantum yield measurements were performed on the coated quantum dot material before processing and on the quantum dot PS optical device obtained after the above processing. The quantum yields of the PS quantum dot devices prepared from the coated quantum dot materials of the above examples and comparative examples before processing were all 95%, and the quantum yield results for each example and comparative example after processing are shown in Table 1.
[0095] [Table 1]
[0096] The quantum dot core material selected in the examples and comparative examples is CdSe / ZnS core-shell quantum dot. Due to the protection of the ZnS shell layer, the outside of the ZnS shell layer is coated with an inorganic salt coating agent, which has little effect on the quantum yield. Therefore, the quantum yield of each example and comparative example before heat processing is all 95%. After heat processing, there is an obvious difference between the quantum yields of each example and comparative example. This is because the different coating layers have different protective abilities for the quantum dot core material, that is, the coated quantum dot materials show different heat resistance due to the different inorganic salt coating layers.
[0097] As can be seen from FIG. 4 and Table 1, compared with the comparative example, the coated quantum dot material prepared by the preparation method provided in the present application has a significantly improved coating amount compared with the inorganic salt coating agent in the prior art. The coated quantum dot material in which the ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent is within the limited range of the present application exhibits excellent high temperature resistance performance and good light, moisture and oxygen resistance after high temperature processing, i.e., has good stability.
[0098] Furthermore, by comparing Example 1 with Examples 2 and 3, it is possible to obtain a coated quantum dot material having a more suitable ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent by adjusting the raw material mixing ratio, and the heat resistance, moisture resistance, light resistance, and oxygen stability of the coated quantum dot material can be further improved.
[0099] Furthermore, by comparing Example 1 with Examples 4 and 5, it can be seen that according to the preferred dropping speed scheme of the present application, a coated quantum dot material can be obtained with a more suitable ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent, and the heat resistance, humidity, light, and oxygen stability of the coated quantum dot material can be further improved.
[0100] The above description is only a preferred embodiment of the present application, and does not limit the present application. Those skilled in the art can make various modifications and variations to the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present application should be included in the protection scope of the present application.
Claims
1. A coated quantum dot material comprising a quantum dot core material and an inorganic salt coating agent, wherein the quantum dot core material comprises an oil-soluble quantum dot, and the inorganic salt coating agent has a solubility in water of less than 0.01 g / 100 g and a thermal decomposition temperature of more than 300° C. The ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent in the coated quantum dot material is 1:0.001 g / mol to 1:0.05 g / mol, preferably 1:0.002 g / mol to 1:0.02 g / mol, and most preferably 1:0.003 g / mol to 1:0.005 g / mol.
2. The quantum dot material, which is a non-ligand portion of the oil-soluble quantum dot, is selected from at least one of the group II-IV, group II-VI, group II-V, group III-V, group III-VI, group IV-VI, group I-III-VI, group II-IV-VI, and group II-IV-V semiconductor compounds of the periodic table of elements; and / or at least one of the core-shell structured semiconductor compounds consisting of at least two of the group II-IV, group II-VI, group II-V, group III-V, group III-VI, group IV-VI, group I-III-VI, group II-IV-VI, and group IIIV-V semiconductor compounds; and / or at least one of the perovskite nanoparticle materials, metal nanoparticle materials, metal oxide nanoparticle materials, and carbon nanomaterials; Preferably, the inorganic salt coating agent is one or more selected from alkaline earth metal salts, Group IIIA metal salts, Group IVA metal salts, and transition metal salts. The coated quantum dot material of claim 1 .
3. The coated quantum dot material according to claim 1, wherein the particle diameter of the quantum dot core material is 3 nm to 15 nm, and the coating thickness of the inorganic salt coating agent is 0.5 nm to 20 nm.
4. The coated quantum dot material according to claim 1, wherein the quantum yield is 70% or more after thermal processing at a high temperature of 200°C to 300°C, and the quantum dot device obtained after the thermal processing has a light attenuation of less than 20% after 1000h of high temperature, high humidity, blue light accelerated aging measurement, preferably a light attenuation of less than 10%, more preferably a light attenuation of less than 5%.
5. The coated quantum dot material according to claim 4, wherein the quantum yield of the coated quantum dot material after the thermal processing is 80% or more, preferably 90% or more.
6. The method for preparing the coated quantum dot material includes: S1: Mixing a quantum dot core material, an organic solvent, and an oil-soluble cation precursor to obtain a first mixed solution, the quantum dot core material including oil-soluble quantum dots, and the organic solvent having a boiling point higher than the boiling point of water; S2: Heating the first mixture to a heating temperature higher than 90° C.; S3: Dropping an aqueous anion solution necessary for growing the inorganic salt into the heated first mixture and reacting to obtain a coated quantum dot material. The coated quantum dot material according to any one of claims 1 to 5, comprising the steps of:
7. A method for preparing a coated quantum dot material, the coated quantum dot material including a quantum dot core material and an inorganic salt coating agent, the method comprising: S1: Mixing a quantum dot core material, an organic solvent, and an oil-soluble cation precursor to obtain a first mixed solution, the quantum dot core material including oil-soluble quantum dots, and the organic solvent having a boiling point higher than the boiling point of water; S2: Heating the first mixture to a heating temperature higher than 90° C.; S3: A method for preparing a coated quantum dot material, comprising the steps of: dropping an aqueous anion solution required for growing an inorganic salt into the heated first mixture and reacting the solution to obtain a coated quantum dot material.
8. The organic solvent is at least one of liquid paraffin, aromatic hydrocarbon, long-chain alkane, fatty acid, and octadecene; Preferably, the oil-soluble cation precursor is one or more selected from the group consisting of an oil-soluble alkaline earth metal salt precursor, an oil-soluble IIIA metal salt precursor, an oil-soluble IVA metal salt precursor, and an oil-soluble transition metal salt precursor; The method for preparing a coated quantum dot material according to claim 7, wherein the anion concentration of the anion aqueous solution is preferably 0.05 mol / L to 10 mol / L.
9. 8. The method for preparing a coated quantum dot material according to claim 7, wherein in step S1, the ratio of the mass of the quantum dots to the molar amount of the oil-soluble cation precursor is 1:0.001 g / mol to 1:0.05 g / mol, preferably 1:0.002 g / mol to 1:0.02 g / mol, and most preferably 1:0.003 g / mol to 1:0.006 g / mol.
10. In step S2, the heating temperature is 100° C. or higher, Preferably, in step S2, the heating time is 10 min to 60 min.
11. In the step S3, the dripping speed is 0.5 mL / min to 2 mL / min, more preferably 1 mL / min to 1.5 mL / min; Preferably, the preparation method further comprises, in step S3, continuing the incubation for 15 min to 120 min after the dropping is completed. The preparation method for a coated quantum dot material according to claim 7.
12. A coated quantum dot material prepared by the method for preparing a coated quantum dot material according to any one of claims 7 to 11.
13. The ratio of the mass of the quantum dot core material to the molar amount of the inorganic salt coating agent in the coated quantum dot material is 1:0.001 g / mol to 1:0.05 g / mol, preferably 1:0.002 g / mol to 1:0.02 g / mol, and most preferably 1:0.003 g / mol to 1:0.005 g / mol. The coated quantum dot material according to claim 12.
14. The coated quantum dot material according to claim 12, wherein the quantum yield of the quantum dot material is 70% or more, preferably 80% or more, and most preferably 90% or more after thermal processing at a high temperature of 200 ° C. to 300 ° C., and the quantum dot device obtained after the thermal processing has a light attenuation of less than 20%, preferably less than 10%, and most preferably less than 5% after 1000 h of high temperature, high humidity, blue light accelerated aging measurement.
15. A quantum dot device comprising the coated quantum dot material according to any one of claims 1 to 6 or any one of claims 12 to 14.
Citation Information
Patent Citations
Method for cladding quantum dot and products prepared from quantum dot
CN108893103A
Improving quantum yield using highly reflective materials
JP2015522668A
Luminescent particles, ink formulations, polymer compositions, optical devices, their manufacture, and uses of luminescent particles
JP2018523724A
Compositions and methods for providing fluorescent materials
JP2018532031A
Nanocrystal particles and processes for synthesizing the same
US20150083969A1