Hexagonal Boron Nitride Deposition
By employing boron-containing and nitrogen-containing precursors with controlled plasma power and temperature, hexagonal boron nitride films are formed at low temperatures, addressing the challenges of conventional methods and achieving films with low dielectric constants and high mechanical strength.
Patent Information
- Application Number
- JP2024516878
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-17
- Filing Date
- 2022-09-12
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-09-12
AI Technical Summary
Conventional methods struggle to produce hexagonal boron nitride films with low dielectric constants and high mechanical strength due to high thermal requirements and thickness issues, which affect line resistance and diffusion between layers.
A method involving the use of boron-containing and nitrogen-containing precursors, along with controlled plasma power and temperature, to form hexagonal boron nitride films at temperatures below 500°C, ensuring a thickness of 80 nm or less, thereby maintaining mechanical strength and reducing diffusion.
The method produces hexagonal boron nitride films with low dielectric constants and high Young's modulus, effectively reducing diffusion and line resistance without sacrificing mechanical properties.
Smart Images

Figure 2024536773000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Patent Application No. 63 / 245,508, filed September 17, 2021, the entire disclosure of which is incorporated herein by reference for all purposes.
[0002] The present technology relates to semiconductor processing methods and components. More specifically, the present technology relates to methods for producing low-k films with high mechanical strength. [Background technology]
[0003] Integrated circuits are made possible by processes that fabricate intricately patterned layers of materials on a substrate surface. Fabricating patterned materials on a substrate requires controlled methods to form and remove materials. Material properties can affect how a device operates and can also affect how films are removed relative to each other. Plasma-enhanced deposition can produce films with specific properties. The desired properties of the film can vary depending on its application.
[0004] Thus, there is a need for improved systems and methods that can be used to manufacture high quality devices and structures. These and other needs are addressed by the present technique. Summary of the Invention
[0005] An exemplary method of semiconductor processing may include providing a boron-containing precursor and a nitrogen-containing precursor to a processing region of a semiconductor processing chamber. A substrate may be disposed in the processing region of the semiconductor processing chamber. The method may include forming a plasma of the boron-containing precursor and the nitrogen-containing precursor in the processing region. The temperature of the substrate may be maintained at about 500° C. or less. The method may include forming a layer of material on the substrate. The layer of material may include hexagonal boron nitride.
[0006] In some embodiments, the boron-containing precursor may include at least one of diborane, paradimethylaminobenzaldehyde, tetramethylammonium bromide, tetraethylammonium bromide, or tris(dimethylamino)borane. The nitrogen-containing precursor may include diatomic nitrogen. A flow ratio of the nitrogen-containing precursor to the boron-containing precursor may be maintained at about 100:1 or greater. The method may include delivering a hydrogen-containing precursor along with the boron-containing precursor and the nitrogen-containing precursor. A flow ratio of the hydrogen-containing precursor to the boron-containing precursor may be maintained at about 100:1 or greater. The pressure in the semiconductor processing chamber may be maintained at about 10 Torr or less while forming the layer of material on the substrate. The formation of the plasma of the boron-containing precursor and the nitrogen-containing precursor may be performed at a plasma power of about 500 W or less. The layer of material may be characterized by a boron concentration of about 25.0 atomic % or greater. The boron-containing precursor may include carbon. The layer of material may be characterized by a carbon concentration of about 10.0 atomic % or less. The method may include subsequently forming a layer of material on the substrate for a first period of time, stopping the supply of the boron-containing precursor, and maintaining a flow of the nitrogen-containing precursor for a second period of time. The method may include increasing plasma power while maintaining the flow of the nitrogen-containing precursor. The method may include repeating the semiconductor processing method for at least one additional cycle. The substrate may be a dielectric material.
[0007] Some embodiments of the present technology may include a semiconductor processing method. The method may include providing a boron-containing precursor and a nitrogen-containing precursor to a processing region of a semiconductor processing chamber. A substrate may be disposed in the processing region of the semiconductor processing chamber. The method may include forming a plasma of the boron-containing precursor and the nitrogen-containing precursor in the processing region. The method may include forming a layer of material on the substrate. The layer of material may include hexagonal boron nitride. The method may include subsequently forming the layer of material on the substrate for a first period of time and stopping the supply of the boron-containing precursor. The method may include maintaining a flow of the nitrogen-containing precursor for a second period of time and increasing the plasma power while maintaining the flow of the nitrogen-containing precursor.
[0008] In some embodiments, the boron-containing precursor may include at least one of diborane, paradimethylaminobenzaldehyde, tetramethylammonium bromide, tetraethylammonium bromide, or tris(dimethylamino)borane. The method may include repeating the semiconductor processing method for at least one additional cycle. The method may include increasing the plasma power in the semiconductor processing chamber after stopping the delivery of the boron-containing precursor includes increasing the plasma power to about 600 W or greater. The flow ratio of the nitrogen-containing precursor to the boron-containing precursor may be maintained at about 100:1 or greater.
[0009] Some embodiments of the present disclosure may include a semiconductor structure. The semiconductor structure may include a substrate characterized by a first surface and a second surface opposite the first surface. One or more dielectric materials may cover the first surface of the substrate. One or more recesses may be formed in the one or more dielectric materials. A liner material may extend along a surface defining the one or more recesses. A metallic material may be disposed in each recess of the one or more recesses. The metallic material may be in contact with the liner material. A layer of material may cover the metallic material. The layer of material may include hexagonal boron nitride.
[0010] In some embodiments, the layer of material is characterized by a thickness of about 50 Angstroms to 100 Angstroms.
[0011] Such techniques can provide numerous benefits over conventional systems and techniques. For example, utilizing boron-containing and nitrogen-containing precursors according to embodiments of the present disclosure can enable a layer of hexagonal boron nitride film having a desired thickness, such as less than 80 nm, which is effective in reducing or preventing diffusion between layers adjacent to the hexagonal boron nitride layer. In addition, the layer of hexagonal boron nitride can enable a desired low-k film without sacrificing mechanical strength. These and other embodiments, along with many of their advantages and features, are described in further detail in conjunction with the following description and accompanying drawings.
[0012] A further understanding of the nature and advantages of the disclosed technology may be realized by reference to the remaining portions of the specification and the drawings. [Brief description of the drawings]
[0013] [Figure 1] 1 is a schematic cross-sectional view illustrating an exemplary plasma system in accordance with some embodiments of the present technique. [Diagram 2] 1A-1D illustrate steps of an exemplary method of semiconductor processing in accordance with some embodiments of the present technique. [Diagram 3] 1A-1D show schematic cross-sectional views of exemplary structures that may include layers of material and may be fabricated in accordance with some embodiments of the present technique. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Some of the drawings are included as schematics. It should be understood that the drawings are for illustrative purposes and should not be considered to scale unless specifically indicated as such. Furthermore, as schematics, the drawings are provided to aid in understanding and may not include all aspects or information compared to actual representations and may include exaggerated material for illustrative purposes.
[0015] In the accompanying drawings, similar components and / or features may have the same reference symbol. Furthermore, various components of the same type may be distinguished by following the reference symbol with a letter that distinguishes between the similar components. If only the first reference symbol is used in the specification, the description is applicable to any of the similar components having the same first reference symbol regardless of the letter.
[0016] The layers of material used in the fabrication of semiconductor structures include conventional low-k chemical vapor deposition barrier films, sometimes referred to as BLok. Low-k chemical vapor deposition barrier films are used as an alternative to silicon nitride films. BLok films are silicon carbide films, and compared to silicon nitride films, the barrier film may have a lower dielectric constant to achieve faster and more powerful devices. BLok films, also compared to silicon nitride films, have a dielectric constant less than 5, exhibit leakage 6-7 orders of magnitude less than silicon nitride films, and may have good adhesion to other films. However, BLok can be relatively thick, such as greater than about 80 nm. If the film is too thick, such as the thickness of BLok, the size of the features in the film may decrease and the metal spacing may decrease. The closer the metal spacing, the greater the undesirable increase in line resistance.
[0017] There is a continuing need for materials with low dielectric constant properties that are mechanically strong and thin enough to avoid increasing line resistance. Hexagonal boron nitride films that can be used in place of BLok films can be characterized by thicknesses of about 80 nm or less, such as about 50 nm. However, conventional methods of forming hexagonal boron nitride films require temperatures of about 1,000° C. or more. The present technique can overcome these challenges by forming a layer of hexagonal boron nitride in place of a conventional low-k chemical vapor deposition barrier film. Conventional methods have been unable to form a layer of hexagonal boron nitride as a low-k chemical vapor deposition barrier due to the thermal history of other layers previously deposited on the substrate. The produced hexagonal boron nitride material is characterized by a low dielectric constant value while retaining a useful Young's modulus value, and can be thinner than conventional low-k chemical vapor deposition barrier films. Additionally, the produced hexagonal boron nitride material can be formed at temperatures of about 500° C. or less without the aid of any catalyst.
[0018] In the remaining disclosure, specific deposition processes utilizing the techniques of the present disclosure will be routinely identified and described in one type of semiconductor processing chamber, but it will be readily understood that the processes described are equally applicable to other deposition chambers, and that the processes can be performed in any number of semiconductor processing chambers. Thus, the present technology should not be considered limited to use with only these specific deposition processes or chambers. Before describing the method of semiconductor processing according to the present technology, the present disclosure will describe one possible chamber that can be used to perform the process according to an embodiment of the present technology.
[0019] FIG. 1 illustrates a cross-sectional view of an exemplary semiconductor processing chamber 100 according to some embodiments of the present technology. The figure illustrates an overview of a system that incorporates one or more aspects of the present technology and / or is specifically configured to perform one or more processes according to embodiments of the present technology. Further details of the chamber 100 or the method performed are further described below. The chamber 100 may be utilized to form a film layer according to some embodiments of the present technology, but it should be understood that the method may be performed in any chamber in which film formation may occur as well. The semiconductor processing chamber 100 may include a chamber body 102, a substrate support 104 disposed within the chamber body 102, and a lid assembly 106 connected with the chamber body 102 and enclosing the substrate support 104 within a processing volume 120. The substrate 103 may be provided to the processing volume 120 through an opening 126, which may be conventionally sealed for processing using a slit valve or door. The substrate 103 may be placed on a surface 105 of the substrate support 104 during processing. The substrate support 104 is rotatable, as indicated by arrow 145, along an axis 147 about which the axis 144 of the substrate support 104 is disposed. Alternatively, the substrate support 104 may be elevated and rotated as needed during the deposition process.
[0020] The plasma profile modulator 111 may be disposed in the semiconductor processing chamber 100 to control plasma distribution across a substrate 103 disposed on a substrate support 104. The plasma profile modulator 111 may include a first electrode 108 that may be disposed adjacent to the chamber body 102 and may separate the chamber body 102 from other components of the lid assembly 106. The first electrode 108 may be part of the lid assembly 106 or may be a separate sidewall electrode. The first electrode 108 may be an annular or ring-shaped member or may be a ring electrode. The first electrode 108 may be a continuous loop around the circumference of the semiconductor processing chamber 100 surrounding the processing volume 120 or may be discontinuous at selected locations as desired. The first electrode 108 may also be a perforated electrode, such as a perforated ring or mesh electrode, or may be a plate electrode, such as an auxiliary gas distributor.
[0021] The one or more isolators 110a, 110b may be a dielectric material, such as a ceramic or a metal oxide, e.g., aluminum oxide and / or aluminum nitride, that contacts the first electrode 108 and electrically and thermally isolates the first electrode 108 from the gas distributor 112 and from the chamber body 102. The gas distributor 112 may define an aperture 118 for distributing the process precursors into the processing volume 120. The gas distributor 112 may be connected to a first power source 142, such as an RF generator, an RF power source, a DC power source, a pulsed DC power source, a pulsed RF power source, or any other power source that may be connected to the semiconductor processing chamber 100. In some embodiments, the first power source 142 may be an RF power source.
[0022] The gas distributor 112 may be a conductive gas distributor or a non-conductive gas distributor. The gas distributor 112 may also be formed of conductive and non-conductive components. For example, the body of the gas distributor 112 may be conductive and the faceplate of the gas distributor 112 may be non-conductive. The gas distributor 112 may be powered, such as by a first power source 142 as shown in FIG. 1, or the gas distributor 112 may be connected to ground in some embodiments.
[0023] The first electrode 108 may be connected to a first tuned circuit 128 that may control the ground path of the semiconductor processing chamber 100. The first tuned circuit 128 may include a first electronic sensor 130 and a first electronic controller 134. The first electronic controller 134 may be or include a variable capacitor or other circuit element. The first tuned circuit 128 may be or include one or more inductors 132. The first tuned circuit 128 may be any circuit that allows for variable or controllable impedance of the plasma conditions present in the process volume 120 during processing. In some embodiments as shown, the first tuned circuit 128 may include a first circuit leg and a second circuit leg that are connected in parallel between ground and the first electronic sensor 130. The first circuit leg may include a first inductor 132A. The second circuit leg may include a second inductor 132B that is connected in series with the first electronic controller 134. The second inductor 132B may be disposed between the first electronic controller 134 and a node connecting both the first and second circuit legs to the first electronic sensor 130. The first electronic sensor 130 may be a voltage or current sensor and may be coupled to the first electronic controller 134 which may provide some degree of closed-loop control of the plasma conditions within the process volume 120.
[0024] The second electrode 122 may be connected to the substrate support 104. The second electrode 122 may be embedded in the substrate support 104 or connected to the surface 105 of the substrate support 104. The second electrode 122 may be a plate, a perforated plate, a mesh, a wire screen, or any other distributed arrangement of conductive elements. The second electrode 122 may be a tuning electrode and may be connected to a second tuning circuit 136 by a conduit 146, a cable having a selected resistance, such as 50 Ω, disposed, for example, in the axis 144 of the substrate support 104. The second tuning circuit 136 may have a second electronic sensor 138 and a second electronic controller 140, which may be a second variable capacitor. The second electronic sensor 138 may be a voltage or current sensor and may be connected to the second electronic controller 140 to further control the plasma conditions in the process volume 120.
[0025] The third electrode 124 may be a bias electrode and / or an electrostatic chuck electrode and may be connected to the substrate support 104. The third electrode may be connected to a second power source 150 through an impedance matching circuit, filter 148. The second power source 150 may be DC power, pulsed DC power, RF bias power, pulsed RF source or bias power, or a combination of these or other power sources. In some embodiments, the second power source 150 may be RF bias power. The substrate support 104 may also include one or more heating elements configured to heat the substrate to a processing temperature of about 25° C. to about 800° C. or more.
[0026] The lid assembly 106 and substrate support 104 of FIG. 1 may be used with any processing chamber for plasma or thermal processing. During processing, the semiconductor processing chamber 100 allows for real-time control of plasma conditions within the processing volume 120. The substrate 103 may be placed on the substrate support 104, and processing gases may be flowed through the lid assembly 106 using the inlet 114 according to any desired flow scheme. Gases may be exhausted from the semiconductor processing chamber 100 through the outlet 152. Power is connected to the gas distributor 112 to establish a plasma within the processing volume 120. The substrate may receive an electrical bias using a third electrode 124 in some embodiments.
[0027] When a current is applied to the plasma in the process volume 120, a potential difference may be created between the plasma and the first electrode 108. A potential difference may also be created between the plasma and the second electrode 122. Electronic controllers 134, 140 may then be used to adjust the flow characteristics of the ground paths represented by the two tuned circuits 128 and 136. Set points may be communicated to the first tuned circuit 128 and the second tuned circuit 136 to provide independent control of the deposition rate and center-to-edge plasma density uniformity. In an embodiment in which the electronic controllers are both variable capacitors, an electronic sensor may adjust the variable capacitors to independently maximize the deposition rate and minimize thickness non-uniformity.
[0028] Each tuning circuit 128, 136 may have a variable impedance that can be adjusted using the respective electronic controller 134, 140. If the electronic controller 134, 140 is a variable capacitor, the capacitance range of each of the variable capacitors, as well as the inductance of the first inductor 132A and the second inductor 132B, may be chosen to provide an impedance range. This range may depend on the frequency and voltage characteristics of the plasma and may have a minimum value within the capacitance range of each variable capacitor. Thus, when the capacitance of the first electronic controller 134 is at a minimum or maximum value, the impedance of the first tuning circuit 128 may be high, resulting in a plasma shape that has minimal aerial or lateral coverage above the substrate support 104. When the capacitance of the first electronic controller 134 approaches a value that minimizes the impedance of the first tuning circuit 128, the aerial coverage of the plasma may grow to a maximum value to effectively cover the entire working area of the substrate support 104. As the capacitance of the first electronic controller 134 deviates from the minimum impedance setting, the plasma shape may shrink from the chamber walls, reducing aerial coverage of the substrate support 104. The second electronic controller 140 can have a similar effect, and as the capacitance of the second electronic controller 140 can be changed, the aerial coverage of the plasma above the substrate support 104 can be increased or decreased.
[0029] The electronic sensors 130, 138 can be used to tune the respective circuits 128, 136 in a closed loop. A current or voltage set point can be installed in each sensor, depending on the type of sensor used, and the sensor can be provided with control software that determines adjustments to the respective electronic controllers 134, 140 to minimize deviations from the set point. As a result, the plasma shape can be selected and dynamically controlled during processing. Although the above discussion is based on the electronic controllers 134, 140 being variable capacitors, it should be understood that any electronic component having adjustable characteristics may be used to provide the tuning circuits 128 and 136 with adjustable impedance.
[0030] FIG. 2 illustrates an exemplary process of a processing method 200 according to some embodiments of the present technology. The method 200 may be performed in a variety of processing chambers, including the semiconductor processing chamber 100 described above, as well as any other chambers, including non-plasma chambers. The method 200 may include one or more processes before the start of the method 200, such as front-end processing, deposition, etching, polishing, cleaning, or any other process that may be performed prior to the described processes. The method 200 may include multiple optional processes that may or may not be specifically associated with some embodiments of the method 200 according to embodiments of the present technology. For example, many of the processes are described to provide a broader scope of processes performed, but are not critical to the present technology or may be performed by alternative methodologies as further described below. It should be understood that the figures show only partial schematic views, and the substrate may include any number of additional materials and features having various properties and aspects as shown in the figures.
[0031] Method 200 may include a semiconductor processing method including a process of forming a film or layer of material on a substrate, where the film or layer of material is or includes hexagonal boron nitride. The method may include any process prior to the start of method 200, or the method may include additional processes. For example, method 200 may include processes performed prior to the start of the method, including additional deposition, removal, or treatment processes. In some embodiments, method 200 may include providing one or more precursors in a process chamber at step 205, thereby providing one or more precursors in a processing region of a semiconductor processing chamber in which the substrate may be housed. The substrate may include a dielectric material during a metallization process, and one or more layers of metallic material may be formed on the structure in a back-end-of-line process. The metallic material may be formed in a defined area in the dielectric material, for example, on which a material according to some embodiments of the present technology may be deposited or formed.
[0032] In some embodiments, the precursors may be or include boron-containing and nitrogen-containing precursors that produce low-k dielectric layers, such as hexagonal boron nitride. The boron-containing precursors according to some embodiments of the present technology may include precursors with boron and carbon bonds, may include linear branched precursors, cyclic precursors, or any number of additional precursors. In some embodiments, the precursors may be characterized by a specific ratio of carbon and / or oxygen to boron. For example, in some embodiments, the ratio of either carbon or oxygen to boron may be about 1 or more, may be about 1.5 or more, may be about 2 or more, may be about 2.5 or more, may be about 3 or more, may be about 3.5 or more, may be about 4 or more, or more.
[0033] While any number of precursors may be utilized, in some embodiments of the present technology, exemplary boron-containing precursors include diborane, paradimethylaminobenzaldehyde, tetramethylammonium bromide, tetraethylammonium bromide, or tris(dimethylamino)borane. Any number of other boron-containing precursors are contemplated, such as boron-containing precursors having carbon bonded to boron and nitrogen. Exemplary nitrogen-containing precursors may include diatomic nitrogen. In some embodiments, the nitrogen-containing precursor may be ammonia-free. As further described, it may be easier to form a plasma of ammonia compared to a plasma of diatomic nitrogen, and the slow decomposition of diatomic nitrogen into nitrogen radicals may slow the growth rate of the layer of material, which may contribute to the formation of desirable hexagonal boron nitride as opposed to amorphous boron nitride. According to some embodiments, the method may include providing a hydrogen-containing precursor along with the boron-containing precursor and the nitrogen-containing precursor.
[0034] Various flow rates of the boron-containing precursor, the nitrogen-containing precursor, and optionally the hydrogen-containing precursor can be used depending on the particular semiconductor processing chamber used. In some embodiments of the present technology, the flow rate ratio of the nitrogen-containing precursor to the boron-containing precursor may be maintained at about 100:1 or more, about 200:1 or more, about 300:1 or more, about 400:1 or more, about 500:1 or more, about 600:1 or more, about 700:1 or more, about 800:1 or more, about 900:1 or more, about 1000:1 or more, or more. The nitrogen-containing precursor may be supplied to the processing region of the semiconductor processing chamber 100 at a rate of about 500 sccm or more, and may be supplied at a rate of about 750 sccm or more, about 1,000 sccm or more, about 1,250 sccm or more, about 1,500 sccm or more, about 1,750 sccm or more, about 2,000 sccm or more, or more.
[0035] Similarly, in some embodiments of the present technique, the flow ratio of the hydrogen-containing precursor to the boron-containing precursor may be maintained at about 100:1 or more, about 200:1 or more, about 300:1 or more, about 400:1 or more, about 500:1 or more, about 600:1 or more, about 700:1 or more, about 800:1 or more, about 900:1 or more, about 1000:1 or more, or more. The hydrogen-containing precursor may be delivered to the processing region of the semiconductor processing chamber 100 at a rate of about 500 sccm or more, and may be delivered at a rate of about 750 sccm or more, about 1,000 sccm or more, about 1,250 sccm or more, about 1,500 sccm or more, about 1,750 sccm or more, about 2,000 sccm or more, or more. In some embodiments, the nitrogen-containing precursor and the hydrogen-containing precursor may be delivered to the semiconductor processing chamber 100 at equal flow rates.
[0036] By controlling the flow rate, the layer of material may be formed at a rate such that the layer desirably contains hexagonal boron nitride. For example, a low flow rate of the boron-containing precursor may incorporate more nitrogen into the layer and grow the resulting hexagonal boron nitride layer at a slower rate. The ratio of nitrogen to boron in the layer may be about 1:3 or more, about 1:2 or more, about 2:3 or more, about 1:1 or more, or more. In embodiments, the flow rate of the boron-containing precursor may be about 20 sccm or less, about 15 sccm or less, about 10 sccm or less, about 9 sccm or less, about 8 sccm or less, about 7 sccm or less, about 6 sccm or less, about 5 sccm or less, about 4 sccm or less, about 3 sccm or less, about 2 sccm or less, or less. Additionally, while providing a hydrogen-containing precursor is not necessary for the formation of hexagonal boron nitride, hydrogen may help etch and remove portions of hexagonal boron nitride that may have low mechanical strength or high dielectric properties.
[0037] In step 210, a plasma of the boron-containing precursor and the nitrogen-containing precursor may be formed in the processing region. One or more precursors may be provided to the processing region of the chamber, and a plasma may be formed. The plasma may be generated, such as by providing RF power to a faceplate to generate a plasma in the processing region, although any other processing chamber capable of generating a plasma may be used as well. The formation of the plasma of the boron-containing precursor and the nitrogen-containing precursor may be performed with a plasma power of about 500 W or less, and may be formed with a plasma power of about 450 W or less, about 400 W or less, about 350 W or less, about 300 W or less, about 250 W or less, or less. Using a plasma power of about 500 W or less may result in a slower deposition rate of the layer of material on the substrate, which may result in fewer defects and a more uniform structure in the layer of material. That is, a layer of material with a slower deposition rate may result in a harder material without sacrificing dielectric properties. The deposition rate of the layer of material may be slower due to the hexagonal structure compared to other structures such as amorphous or cubic structures, and due to the ratio of nitrogen to boron in the layer of material. By using the precursors and flow rates specified in this disclosure, the precursors can decompose slowly into plasma effluents and therefore slowly deposit on the substrate to form the layer of material.
[0038] The substrate 305 may be placed in a processing region of the semiconductor processing chamber 100. The substrate 305 may be contacted with the plasma effluent of the precursor to produce a preferred termination. Using diatomic nitrogen as a nitrogen-containing precursor may result in a slower formation of the plasma. The individual nitrogen atoms of diatomic nitrogen are bonded via three covalent bonds and slowly decompose to form individual nitrogen radicals. The slower evolution of the nitrogen plasma from diatomic nitrogen may slow the rate at which a layer of material may be formed on the substrate 305, as compared to a nitrogen-containing precursor that does not have three covalent bonds attached to the nitrogen radical. If the layer of material grows too quickly, amorphous boron nitride may form instead of the desired hexagonal boron nitride. Also, as discussed above, using a plasma power of about 500 W or less may slow the deposition rate of the layer of material on the substrate 305, which may result in a more uniform structure with fewer defects in the layer of material.
[0039] Deposition can be performed at substrate or pedestal temperatures of about 500° C. or less, e.g., the thermal budget in the back-end of line processing. In some embodiments, deposition can be performed at temperatures of about 200° C. or more, about 225° C. or more, about 250° C. or more, about 275° C. or more, about 300° C. or more, about 325° C. or more, about 350° C. or more, about 375° C. or more, about 400° C. or more, about 425° C. or more, about 450° C. or more, about 475° C. or more, or more. Temperatures of about 500° C. or less may be possible with the use of plasma power, such as radio frequency plasma power. Conventional methods may not utilize plasma power and may require higher temperatures to form hexagonal boron nitride films. Deposition may be performed at a pressure of about 10 Torr or less, about 9 Torr or less, about 8 Torr or less, about 7 Torr or less, about 6 Torr or less, about 5 Torr or less, about 4 Torr or less, about 3 Torr or less, about 2 Torr or less, or less. Deposition may be performed at a pressure of about 0.5 Torr or more, about 1 Torr or more, about 2 Torr or more, about 3 Torr or more, about 4 Torr or more, about 5 Torr or more, or more.
[0040] The output of the plasma of the boron-containing precursor and the nitrogen-containing precursor may be deposited on a substrate in step 215, thereby producing a boron-containing material and a nitrogen-containing material, such as hexagonal boron nitride. By utilizing a low-power plasma, such as a plasma formed at a plasma power of about 500 W or less, the amount of precursor decomposition may be reduced, since the decomposition of the boron-containing precursor and the nitrogen-containing precursor may require additional energy and time. This may reduce the deposition rate of the material, which may slow the growth rate of the material on the substrate 305. The reduced deposition rate of the material may allow the formation of hexagonal boron nitride at a temperature below the thermal budget. Although embodiments of the present technology include additional processing following deposition, the properties of the deposited film may include a range of improvements over conventional techniques.
[0041] According to some embodiments, in step 220, the flow of the boron-containing precursor is stopped, and in some embodiments, the flow of the nitrogen and / or hydrogen precursor is continued. Stopping the flow of the boron-containing precursor may allow for further processing of the layer of material already formed on the substrate. If the boron-containing precursor is not provided, the nitrogen-containing precursor and any hydrogen-containing precursor may effectively remove any of the layers of material that are of lower quality. The lower quality material that may be removed by the nitrogen-containing precursor and any hydrogen-containing precursor may be material that was not formed as a well-layered material. The lower quality material is structurally intact and may be more easily removed at lower powers without etching or removing the desired high quality material, such as hexagonal boron nitride, which is highly resistant to the nitrogen-containing precursor and any hydrogen-containing precursor.
[0042] In step 225, the plasma power in the processing region of the semiconductor processing chamber can be increased. The plasma power can be increased in step 225 after the flow of the boron-containing precursor is reduced. In some embodiments, the plasma power can be increased in step 225 after stopping the flow of the boron-containing precursor and maintaining the flow of the nitrogen-containing precursor. During step 225, the plasma power can be increased to about 600 W or more, about 700 W or more, about 800 W or more, about 900 W or more, about 1000 W or more, or more. The increase in plasma power can densify and rearrange the film to improve the mechanical strength of the layer of material on the substrate. In step 225, some portions of the layer of material on the substrate can transition from an amorphous or cubic crystal structure to a hexagonal crystal structure, whereby the layer of material can be characterized as a well-oriented layered structure of hexagonal boron nitride. As the material is rearranged, it may be more aligned, have fewer defects, and diffusion of atoms or molecules through the layer may be reduced or eliminated.
[0043] According to the present technology, hexagonal boron nitride materials may be produced that may be characterized by a dielectric constant of about 4.00 or less, and may be about 3.95 or less, about 3.90 or less, about 3.85 or less, about 3.80 or less, about 3.75 or less, about 3.70 or less, about 3.65 or less, about 3.60 or less, about 3.55 or less, about 3.50 or less, about 3.45 or less, about 3.40 or less, about 3.35 or less, about 3.30 or less, about 3.25 or less, about 3.20 or less, about 3.15 or less, about 3.10 or less, about 3.05 or less, about 3.00 or less, or less. Conventional methods of forming layers of materials for use as low dielectric constant chemical vapor deposition barrier films may sacrifice mechanical strength properties for a low dielectric constant. Furthermore, conventional methods of developing films may exceed the thermal budget in semiconductor processing, making hexagonal boron nitride unsuitable as a barrier film. As discussed above, because conventional methods of depositing hexagonal boron nitride do not utilize plasma power, such as radio frequency plasma power, to deposit hexagonal boron nitride, conventional methods may require temperatures much higher than the thermal budget, on the order of 1000° C. or higher. In contrast, the present inventors have determined that the use of plasma power, such as radio frequency plasma power, can enable the temperatures required to form hexagonal boron nitride to be much lower and within the thermal budget.
[0044] The dielectric constant may be related to the material properties of the film. Traditionally, the lower the dielectric constant, the lower the Young's modulus of the film produced. However, by producing a film according to some embodiments of the present technology, the Young's modulus may be maintained higher than would result in conventional techniques capable of producing a film with a corresponding as-deposited dielectric constant value. For example, in some embodiments, the present technology may produce a material characterized by a Young's modulus of about 55 Gpa or more, and may be characterized by a Young's modulus of about 56 Gpa or more, about 57 Gpa or more, about 58 Gpa or more, about 59 Gpa or more, about 60 Gpa or more, about 61 Gpa or more, about 62 Gpa or more, about 63 Gpa or more, about 64 Gpa or more, about 65 Gpa or more, about 66 Gpa or more, about 67 Gpa or more, about 68 Gpa or more, about 69 Gpa or more, about 70 Gpa or more, or more. As a result, the present technology may be able to produce a film with a lower dielectric constant while maintaining a higher Young's modulus of the material. It should be noted that in embodiments using a boron-containing precursor having a higher amount of carbon, the Young's modulus may be lower than embodiments using a boron-containing precursor having a lower amount of carbon. Depending on the application and desired properties, it may be desirable to select a boron-containing precursor with a lower amount of carbon to limit the amount of carbon in the layer of material formed on the substrate 305.
[0045] The material properties produced by embodiments of the present technology may be related to the amount of boron incorporated within the layer. For example, in some embodiments, the as-deposited materials produced according to the present technology may be characterized by a percentage of boron incorporated or retained within the film of about 25.0 atomic % or more, and may be characterized by boron incorporation within the film of about 27.5 atomic % or more, about 30.0 atomic % or more, about 32.5 atomic % or more, about 35.0 atomic % or more, about 37.5 atomic % or more, about 40.0 atomic % or more, about 42.5 atomic % or more, about 45.0 atomic % or more, about 47.5 atomic % or more, or more.
[0046] Additionally, the percentage of carbon incorporated within the layer may be about 10.0 atomic % or less in the as-deposited material, about 9.0 atomic % or more, about 8.0 atomic % or more, about 7.0 atomic % or more, about 6.0 atomic % or more, about 5.0 atomic % or more, about 4.0 atomic % or more, about 3.0 atomic % or more, about 2.0 atomic % or more, about 1.0 atomic % or more, or less. A smaller amount of carbon in the layer of material may enhance material properties such as Young's modulus of the layer of material. Selection of the boron-containing precursor and the amount of carbon in the precursor may affect the resulting amount of carbon in the layer of material. The particular boron-containing precursor or precursors used may affect all material properties in the layer of material. For example, if the boron-containing precursor also contains a large amount of carbon, Young's modulus may be decreased, such as halved. However, by utilizing a low-power plasma in conjunction with other process characteristics according to embodiments of the present technology, low-k dielectric materials may be produced that are characterized by an increased Young's modulus, among other material properties.
[0047] FIG. 3 illustrates an exemplary schematic cross-sectional structure 300 that includes layers of material and is fabricated according to some embodiments of the present technology. The structure 300 may include multiple layers deposited on a substrate 305. The substrate 305 may include a first surface 306 and a second surface 307 opposite the first surface 306. The substrate may be, for example, silicon. One or more dielectric materials may cover the first surface 306 of the substrate 305. The one or more dielectric materials may include layers such as a first low-k barrier layer 310 and a second low-k barrier layer 340. The one or more dielectric materials, such as the first low-k barrier layer 310 and the second low-k barrier layer 340, may include, but are not limited to, oxide materials such as silicon oxide, or fluorine-doped oxide, carbon, or other low-k materials that may be used in processing. One or more recesses 350 may be formed in the one or more dielectric materials. The layers may also include a low-k material 315, a liner material 320, a metal material 325, and a barrier material 330. The low-k material 315 may be, for example, a silicon-containing material such as silicon oxide or silicon nitride.
[0048] The liner material 320 may extend along the surface defining one or more recesses 350. The liner material 320 may define an opening. In some embodiments, the liner material 320 may be tantalum nitride. The liner material 320 may be a material that is conformal over the dielectric material when deposited. The liner material 320 may include, but is not limited to, tantalum nitride and titanium nitride. A metallic material 325 may be disposed in each recess of the one or more recesses 350. The metallic material 325 may be in contact with the liner material 320 and may be any number of metals, such as copper, cobalt, tungsten, or other metallic materials. The barrier material 330 may be, for example, cobalt. The barrier material 330 may be a material that is selective over the metallic material when deposited.
[0049] A hexagonal boron nitride layer 335, such as the hexagonal boron nitride materials described in this disclosure, may be formed over the low-k material 315, the metal material 325, the barrier material 330, or a combination thereof. Thus, the hexagonal boron nitride layer 335 may be characterized as a blanket that covers all the metal and dielectric materials. In embodiments, the hexagonal boron nitride layer 335 may have a thickness of about 50 angstroms to about 100 angstroms, such as about 50 angstroms to about 80 angstroms. As discussed above, the hexagonal boron nitride material may have desirable properties, such as a low dielectric constant, without sacrificing mechanical strength. In addition, the hexagonal boron nitride material reduces or eliminates diffusion of atoms and molecules between layers separated by the hexagonal boron nitride layer, such as the second low-k barrier layer 340 and the low-k material 315 and / or the barrier material 330.
[0050] In the above description, for purposes of explanation, numerous details have been set forth in order to provide an understanding of various embodiments of the present technology. However, it will be apparent to one skilled in the art that particular embodiments may be practiced without some of these details, or with additional details.
[0051] Although several embodiments have been disclosed, those skilled in the art will recognize that various modifications, alternative configurations, and equivalents may be used without departing from the spirit of the embodiments. In addition, in order to avoid unnecessarily obscuring the technology, many well-known processes and elements have not been described. Thus, the above description should not be considered as limiting the scope of the technology.
[0052] Where a range of values is provided, unless the context clearly indicates otherwise, each intermediate value between the upper and lower limits of that range is also understood to be specifically disclosed, to the smallest fraction of the unit of the lower limit. Any stated or unstated intermediate value in the stated range, and any smaller range between any other stated or intermediate value in that stated range, are also included. The upper and lower limits of those smaller ranges may be independently included or excluded from the range, and each range in which either, neither, or both of the limits are included in the smaller range is also encompassed in the art, subject to any specifically excluded limits in the stated range. If the stated range includes one or both of the limits, then ranges excluding either or both of those included limits are also included.
[0053] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include the plural unless the context clearly indicates otherwise. Thus, for example, reference to a "boron-containing precursor" includes a plurality of such materials, reference to a "precursor" includes reference to one or more precursors and equivalents thereof known to those skilled in the art, and so forth.
[0054] Additionally, the words "comprises," "comprising," "containing," "containing," "including," and "comprising," when used in this specification and the claims that follow, are intended to specify the presence of stated features, integers, components, or operations, but do not preclude the presence or addition of one or more other features, integers, components, operations, operations, or groups.
Claims
1. providing a boron-containing precursor and a nitrogen-containing precursor to a processing region of a semiconductor processing chamber having a substrate disposed therein; maintaining a temperature of the substrate at or below about 500° C. and forming a plasma of the boron-containing precursor and the nitrogen-containing precursor in the processing region; forming a layer of material comprising hexagonal boron nitride on the substrate; 16. A semiconductor processing method comprising:
2. 10. The semiconductor processing method of claim 1, wherein the boron-containing precursor comprises at least one of diborane, paradimethylaminobenzaldehyde, tetramethylammonium bromide, tetraethylammonium bromide, or tris(dimethylamino)borane.
3. The semiconductor processing method of claim 1 , wherein the nitrogen-containing precursor comprises diatomic nitrogen.
4. 10. The semiconductor processing method of claim 1, wherein a flow ratio of said nitrogen-containing precursor to said boron-containing precursor is maintained at about 100:1 or greater.
5. delivering a hydrogen-containing precursor along with the boron-containing precursor and the nitrogen-containing precursor, wherein a flow ratio of the hydrogen-containing precursor to the boron-containing precursor is maintained at about 100:1 or greater; The semiconductor processing method of claim 4 further comprising:
6. 10. The semiconductor processing method of claim 1, wherein a pressure in said semiconductor processing chamber is maintained at about 10 Torr or less while forming said layer of material on said substrate.
7. 10. The semiconductor processing method of claim 1, wherein forming the plasma of the boron-containing precursor and the nitrogen-containing precursor is performed at a plasma power of about 500 W or less.
8. 2. The semiconductor processing method of claim 1, wherein said layer of material has a boron concentration of greater than or equal to about 25.0 atomic percent.
9. 10. The semiconductor processing method of claim 8, wherein the boron-containing precursor comprises carbon, and wherein the layer of material has a carbon concentration of about 10.0 atomic % or less.
10. subsequently forming a layer of the material on the substrate for a first period of time and then terminating the supply of the boron-containing precursor; maintaining a flow of the nitrogen-containing precursor for a second period of time; The semiconductor processing method of claim 1 further comprising:
11. increasing plasma power while maintaining the flow of the nitrogen-containing precursor. The semiconductor processing method of claim 10 further comprising:
12. Repeating the semiconductor processing method for at least one additional cycle. The semiconductor processing method of claim 11 further comprising:
13. The semiconductor processing method of claim 1 , wherein the substrate is a dielectric material.
14. providing a boron-containing precursor and a nitrogen-containing precursor to a processing region of a semiconductor processing chamber having a substrate disposed therein; forming a plasma of the boron-containing precursor and the nitrogen-containing precursor in the processing region; forming a layer of material comprising hexagonal boron nitride on the substrate; subsequently forming a layer of the material on the substrate for a first period of time and then terminating the supply of the boron-containing precursor; maintaining a flow of the nitrogen-containing precursor for a second period of time; increasing plasma power while maintaining the flow of the nitrogen-containing precursor; 16. A semiconductor processing method comprising:
15. 15. The semiconductor processing method of claim 14, wherein the boron-containing precursor comprises at least one of diborane, paradimethylaminobenzaldehyde, tetramethylammonium bromide, tetraethylammonium bromide, or tris(dimethylamino)borane.
16. Repeating the semiconductor processing method for at least one additional cycle.
15. The semiconductor processing method of claim 14 further comprising:
17. 15. The semiconductor processing method of claim 14, wherein increasing the plasma power in the semiconductor processing chamber after stopping the supply of the boron-containing precursor comprises increasing the plasma power to about 600 W or greater.
18. 15. The semiconductor processing method of claim 14, wherein a flow ratio of said nitrogen-containing precursor to said boron-containing precursor is maintained at about 100:1 or greater.
19. a substrate characterized by a first surface and a second surface opposite the first surface; one or more dielectric materials covering the first surface of the substrate, the one or more dielectric materials having one or more recesses formed therein; a liner material extending along a surface defining the one or more recesses; a metallic material disposed in each recess of the one or more recesses and in contact with the liner material; a layer of a material comprising hexagonal boron nitride covering the metallic material; 1. A semiconductor structure comprising:
20. 20. The semiconductor structure of claim 19, wherein said layer of material is approximately 50 to 100 Angstroms thick.
Citation Information
Patent Citations
Semiconductor device
JP2001313335A
Method for forming boron nitride film and film forming apparatus
JP2004186403A
Method and apparatus for forming boron nitride film
JP2006237478A
Memory device with boron nitride liner
US20200287133A1
Interlayer insulating layer formation method and semiconductor device
WO2012011480A1