Submicron surface modified metal oxide particles
The surface modification of metal oxide particles using silicon compounds with specific organic radicals addresses safety and environmental issues of existing methods, achieving improved dispersibility and hydrophobicity with reduced VOCs and energy use.
Patent Information
- Application Number
- JP2024518443
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-24
- Filing Date
- 2022-09-19
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods for surface modification of submicron metal oxide particles, such as those using silazane and hydrosiloxane, are hazardous, require high temperatures, and produce volatile organic compounds (VOCs), leading to non-uniform coverage and safety concerns.
A method involving the use of silicon compounds with specific organic radicals and functional groups to form a layer on the surface of metal oxide particles, ensuring uniform coverage and reducing VOCs, toxicity, and energy consumption.
The method provides improved dispersibility, increased binding sites, and enhanced hydrophobicity, while being environmentally friendly and safer to produce, with reduced agglomeration and VOC emissions.
Smart Images

Figure 2024537022000019 
Figure 2024537022000020 
Figure 2024537022000001
Abstract
Description
[Technical field]
[0001] The present invention relates to surface-modified particles for use in toner compositions, a method for preparing surface-modified particles according to the present invention, a method for treating the surface of a substrate with at least one particle according to the present invention, a substrate having a surface treated with at least one particle according to the present invention, the use of at least one surface-modified particle according to the present invention as an additive in various formulations, and in particular toner compositions comprising surface-modified particles according to the present invention.
[0002] 2. Background of the Invention Submicron particles made from metal oxides are well known in the art, and many methods for their manufacture have been published. The usefulness of such particles depends mainly on their surface, and many attempts have been made to change the properties of such particles by modifying their surface. Typically, surface functionalization of colloidal silica with various functional groups is beneficial for a variety of applications. Silica surfaces can be made hydrophobic using silicone oils (JP 49-042354 A), hydrosiloxanes (US Pat. No. 8,895,145 B1), trialkoxysilanes (US 2008 / 0069753 B1, US 2008 / 0070143 B1, WO 2010 / 005492 B1, US 10,222,717 B1), and silazanes (US 7,083,888 B1, US 2008 / 0070143 B1, JP 2019-043829 B1, EP 3,178,887 B1, US 10,222,717 B1, US 5,013,585 B1). Surface treatment using silazanes, such as hexamethyldisilazane, as disclosed in US Pat. No. 7,083,888, is of particular interest due to their small size and ability to react in aqueous media to impart excellent hydrophobicity. There, an approach is described for silica surface functionalization using monomeric alkoxysilanes, such as methyltrimethoxysilane (MTMS), for toner additives, and silazanes, such as hexamethyldisilizane (HMDS). In this process, MTMS and HMDS are added sequentially to a liquid-phase silica suspension, with intermediate distillation and solvent exchange steps. A major drawback of the silazane approach is the toxicity of this compound and the extensive safety measures that must be implemented when handling it, especially when using large amounts.
[0003] The hydrosiloxanes described in US Patent No. 8,895,145 bind to the particles while liberating hydrogen. This also requires strict safety measures to be implemented, such as the need to work under inert conditions to avoid potential fire and explosion hazards. The reaction of the hydrosiloxanes with the particles requires higher temperatures, resulting in high energy consumption.
[0004] A gentler method for surface functionalization of submicron particles of metal oxides uses monomeric silanes. Amine functionalization can be achieved using trialkoxysilanes (US Pat. No. 9,212,193; Hartono et al., Langmuir, 2009, 25, 6413; An et al., JCIS, 2007, 507) for applications where improved hydrophilicity, molecular adsorption, compatibility with polymers, etc. may be required. Other functional groups such as epoxy (US Pat. App. Pub. No. 2004 / 0102529), polyether (US Pat. App. Pub. No. 2019 / 0375643), acrylate, thiol, and sulfate can also be introduced using alkoxysilanes. However, these procedures often result in non-uniform surface coverage. In addition, the proposed procedures may require high temperatures and solvent exchange steps. They also release large amounts of volatile organic compounds (VOCs), which are undesirable from an ecological point of view.
[0005] CN Patent No. 110272641 reports pearlescent pigments that can be coated with various silicon-based compounds.
[0006] US Patent Application Publication No. 2018 / 112077 discloses a coating composition comprising a silicate binder, a filler, a crosslinker, and a film-forming lubricant. Optionally, a silane-based adhesion promoter is added to the composition.
[0007] In addition, it is desirable to provide an environmentally sustainable surface modification process, which can typically be achieved by reducing energy consumption during the process, for example, by using lower temperatures, using non-toxic surface functionalizing agents, using less solvent, and minimizing the emission of volatile organic compounds (VOCs) and toxic by-products.
[0008] Problem to be solved by the invention It is therefore an object of the present invention to overcome the drawbacks of the prior art.It is a further object of the present invention to provide surface-modified particles with improved dispersibility.
[0009] Summary of the Invention These problems are addressed by providing a surface-modified particle (or particles) for use in a toner composition, comprising: a) a core comprising at least one oxide-based material selected from the group consisting of silicon oxides, metal oxides, and mixtures of one or more of the foregoing; and b) at least one layer, bi) Formula (A): [ka] [In the formula, R 1 is an organic radical, preferably selected from the group consisting of substituted or unsubstituted alkyl groups, substituted or unsubstituted alkenyl groups, and substituted or unsubstituted aryl groups; Each X is independently selected from the group consisting of a hydroxy group, a carboxylic acid group, a chloride, and an alkoxy group; m is selected from 0, 1, and 2. At least one building block according to Formula (B): [ka] [In the formula, R 2is an organic radical, preferably selected from the group consisting of substituted or unsubstituted alkyl groups, substituted or unsubstituted alkenyl groups, and substituted or unsubstituted aryl groups; each Y is independently selected from the group consisting of a hydroxy group, a carboxylic acid group, a chloride, and an alkoxy group; n is selected from 0, 1, and 2. At least one building block by and at least one silicon compound comprising: b.ii) Formula(S): [ka] [In the formula, Each R s At least one R s is independently selected from the group consisting of hydroxy groups, carboxylic acid groups, chloride, alkoxy groups, alkyl groups, and aryl groups, with the proviso that is selected from the group consisting of chloride, carboxylic acid groups, hydroxy groups, and alkoxy groups; R t is selected from the group consisting of alkyl and alkenyl groups. and at least one silane according to Layer obtained from The problem is solved by surface-modified particles, comprising:
[0010] The surface-modified particles according to the present invention allow to improve the coverage of the binding sites of unmodified particles compared to the particles of the prior art.In the context of the present invention, improved coverage means that a higher proportion of binding sites (such as hydroxyl groups and / or silanol groups on the surface of the core) is used to bond the layer on the core surface resulting from treating said core with at least one silicon compound compared to particles produced by the processes of the prior art (e.g. monomeric or long carbon chain silanes or polymers).This improved coverage is usually accompanied by a more uniform statistical distribution of the functional groups present.The improved coverage of binding sites has a number of advantageous effects, namely: Increased cross-linking of surface-modified particles with polymers and resins, Increase in the number of coordination sites per area, Increased wettability, Increased hydrophobicity, or Reduced moisture absorption can be obtained (depending also on the choice of building blocks according to formula (A) and (B)).
[0011] The surface-modified particles according to the present invention have improved dispersion properties compared to other particles, such as those known in the prior art. The production of the surface-modified particles according to the present invention is environmentally friendly, since there are few or no VOCs or toxic / explosives (e.g. ammonia and hydrogen) released during production, and no toxic materials need to be used for this purpose. In addition, the absence of ammonia as a by-product makes the process safer.
[0012] Surface modified particles can be tailored to meet various technical requirements, such as hydrophobicity, making them highly versatile and useful for many technical applications.
[0013] Preferred embodiments which solve the above-mentioned problems particularly well are set forth in the following description and in the dependent claims. [Brief description of the drawings]
[0014] [Figure 1a] FIG. 2 shows a solid-state 29Si NMR spectrum of a suspension containing surface-modified particles according to the present invention. [Figure 1b] FIG. 1 shows the solid-state 29Si NMR spectrum of a suspension containing unmodified particles.
[0015] Detailed Description of the Invention Percentages throughout this specification are weight percent (wt% or wt%) unless otherwise stated. Concentrations given herein refer to the volume of the entire composition, solution, or dispersion unless otherwise stated.
[0016] The term "organic radical" according to the present invention includes, in particular, alkyl groups, aryl groups, and combinations thereof, said groups being substituted or unsubstituted.
[0017] The term "alkyl" according to the present invention includes branched or unbranched alkyl groups containing cyclic and / or acyclic structural elements, the cyclic structural elements of the alkyl group necessarily requiring at least 3 carbon atoms. C1-CX alkyl in the present specification and claims refers to alkyl groups having 1 to X carbon atoms, where X is an integer. For example, C1-C8 alkyl includes, in particular, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, sec-pentyl, tert-pentyl, neopentyl, hexyl, heptyl, 2-ethylhexyl, isooctyl, and n-octyl. Substituted alkyl groups can theoretically be obtained by replacing at least one hydrogen with a functional group. Unless otherwise stated, the alkyl group is preferably selected from substituted or unsubstituted C1-C8 alkyl, more preferably selected from substituted or unsubstituted C1-C4 alkyl.
[0018] An "alkenyl group" is an unsaturated derivative of an alkyl group containing at least one olefinic (C=C double) bond. The preferences given above for the alkyl group also apply mutatis mutandis to the alkenyl group. In the context of the present invention, preferred alkenyl groups are vinyl and allyl groups, unless otherwise stated hereinafter.
[0019] The term "aryl" according to the present invention refers to a cyclic aromatic hydrocarbon residue, such as phenyl or naphthyl, for example benzothiazolyl, in which the individual ring carbon atoms are optionally replaced by N, O, and / or S. Preferably, the carbon atoms are not substituted. Furthermore, the aryl group is optionally substituted in each case by replacing a hydrogen atom with a functional group. The term C5-CX aryl refers to an aryl group having 5 to X carbon atoms (X being of course an integer) in a cyclic aromatic group, which are optionally replaced by N, O, and / or S. Unless otherwise stated, C5-C6 aryl is preferred.
[0020] The carboxylic acid group in the present invention is represented by the formula: [ka] R is preferably an unsubstituted or substituted alkyl group, more preferably an unsubstituted or substituted C1-C4 alkyl group, unless otherwise stated hereinafter. In this context, the functional group is preferably a hydroxyl group. Most preferably, the carboxylic acid group is a lactic acid group ( [ka] ).
[0021] Unless otherwise stated, the above groups are substituted or unsubstituted. Unless otherwise stated below, the functional groups as substituents are preferably selected from the group consisting of hydroxyl group (-OH), amino group (-NR2, where each R is independently H, alkyl group (optionally substituted), or aryl group), ether group (-OR, where R is alkyl group or aryl group or lactate group), and carboxyl group (-CO2H), or salts thereof. Preferably, the above groups are unsubstituted.
[0022] When more than one residue is selected from a given group, each residue is selected independently of the others, unless otherwise stated below. This means that they can be selected to be the same or different members of the group. The methods described herein include the specified method steps. The specified method steps are typically performed in the order shown, unless otherwise stated. The methods optionally include additional method steps performed before, after, and / or between the method steps. The preferences and details described for one aspect of the invention apply mutatis mutandis to other aspects, unless otherwise stated or technically impracticable. At least one means one or more.
[0023] The present invention relates to at least one surface-modified particle (or a plurality of such particles). The surface-modified particles according to the present invention comprise: a) the core; and b) at least one layer obtained (or obtainable) by treating said core with at least one silicon compound comprising at least one building block according to formula (A) and at least one building block according to formula (B) and with at least one silane according to formula (S). Hereinafter, said silicon compound will be referred to as "silicon compound".
[0024] The surface-modified particle optionally comprises one or more additional layers between a) and b) and / or on b). Preferably, the surface-modified particle does not comprise an additional layer, particularly preferably the surface-modified particle according to the invention consists of a) and b). Preferably, the invention relates to a plurality of surface-modified particles according to the invention.
[0025] The core comprises at least one oxide-based material selected from the group consisting of silicon oxide, metal oxide, and mixtures of the foregoing. The at least one oxide-based material is preferably selected from the group consisting of silicon oxide, titanium oxide, zirconium oxide, cerium oxide, aluminum oxide, zinc oxide, molybdenum oxide, and mixtures of the foregoing. The oxide-based material is most preferably silicon oxide.
[0026] Optionally, the core comprises at least one oxide-based material and at least one material other than the at least one oxide-based material. The at least one material other than the at least one oxide-based material is preferably not an oxide-based material. Preferably, the at least one material other than the at least one oxide-based material is not glass, mica, kaolin, and ceramic. Preferably, the at least one material other than the at least one oxide-based material is at least one polymer-based material (and thus derived from organic monomers). The at least one polymer-based material is preferably selected from the group consisting of thermosetting polymers, thermoplastic polymers, and mixtures of the aforementioned. More preferably, the at least one polymer-based material is polystyrene. Preferably, the at least one material other than the at least one oxide-based material forms an inner part of the core, and the oxide-based material coats said inner part, ideally in its entirety. Thus, the surface of the core is preferably at least one oxide-based material (made from at least one oxide-based material). More preferably, the core of the surface-modified particle according to the invention comprises at least 80% by weight, even more preferably at least 90% by weight of an oxide-based material. Most preferably, the core consists of at least one oxide based material.
[0027] The surface-modified particles comprise at least one layer obtained by treating a core with at least one silicon compound and at least one silane according to formula (S). The silicon compound comprises at least one building block according to formula (A) and (B). The at least one building block according to formula (A) and (B) preferably comprises (in total) at least 50% by weight, more preferably 75% by weight, even more preferably at least 90% by weight, based on the total weight of the silicon compound. Ideally, the silicon compound is composed of building blocks according to formula (A) and (B). The at least one silicon compound preferably does not comprise trialkylsilyl groups (e.g. Me3Si-) and / or dialkylsilyl (e.g. -Si(Me)2-) groups.
[0028] R 1 is an organic radical. 1 is preferably selected from the group consisting of substituted or unsubstituted alkyl groups, substituted or unsubstituted alkenyl groups (preferably selected from vinyl and allyl), and substituted or unsubstituted aryl groups. More preferably, R 1 is a substituted or unsubstituted alkyl group. Even more preferably, R 1 R is an unsubstituted alkyl group. The alkyl group is preferably a C1 to C18 alkyl group, more preferably a C2 to C8 alkyl group, even more preferably a C2 to C4 alkyl group, and in particular a propyl group. 1 is particularly preferably an unsubstituted C2-C4 alkyl group, and most preferably an unsubstituted propyl group. The functional group as the substituent is preferably selected from the group consisting of an amino group (primary or secondary), a methacrylate group, an acrylate group, an epoxy group, an anhydride group, a vinyl group, an alkyl group, a polyether group, and a fluorinated alkyl group.
[0029] X is preferably selected from the group consisting of hydroxy and C1-C4 alkoxy groups, more preferably hydroxy, methoxy, and ethoxy groups, to improve coverage of the binding sites and avoid potentially corrosive halides or hydrogen halides such as HCl.
[0030] R 2 is an organic radical. 2 is preferably selected from the group consisting of a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, and a substituted or unsubstituted aryl group. 2 is more preferably selected from the group consisting of substituted alkyl groups and substituted or unsubstituted alkenyl groups. 1 Most preferably, R 2 is an unsubstituted vinyl group.
[0031] Y is preferably selected from the group consisting of hydroxy and C1-C4 alkoxy groups, more preferably hydroxy, methoxy, and ethoxy groups, to improve coverage of the binding sites and avoid potentially corrosive halides or hydrogen halides such as HCl.
[0032] m and n are integers.Preferably, m is selected from 1 and 2, which improves the coverage of binding sites due to the two-dimensional or three-dimensional structure of the silicon compound.At least one silicon compound preferably does not contain trialkoxysilyl groups, which reduces VOC emissions.Preferably, n is selected from 1 and 2, for the reasons described for integer m.
[0033] Preferably, at least one silicon compound contains at least one reactive site per silicon atom, and the reactive site is selected from the group consisting of hydroxyl, carboxylic acid, chloride, and alkoxy groups. This should be understood to mean that the silicon compound contains at least one reactive site per silicon atom on average. More preferably, at least one reactive site is bonded to all silicon atoms of the silicon compound. The reactive site is preferably selected from the group consisting of methoxy, ethoxy, and hydroxyl groups, for the reasons explained for X and Y. This allows for improved coverage of the bond sites compared to the prior art solutions.
[0034] Typically, the silicon compound comprises 1 to 100 building blocks according to formula (A). Preferably, the at least one silicon compound comprises 2 to 50, more preferably 3 to 30, even more preferably 4 to 20 building blocks according to formula (A).
[0035] Typically, the silicon compound comprises 1 to 100 building blocks according to formula (B). Preferably, the at least one silicon compound comprises 2 to 50, more preferably 3 to 30, even more preferably 4 to 20 building blocks according to formula (B).
[0036] The at least one silicon compound preferably comprises a total of 2 to 100, more preferably 4 to 50, even more preferably 5 to 30 building blocks according to formulae (A) and (B).
[0037] To avoid liberation of hydrogen during treatment of the core of the surface modified particles, preferably the silicon compound does not contain a hydrogen atom directly bonded to a silicon atom.
[0038] The silicon compound comprises at least one building block according to formula (A) and at least one building block according to formula (B). The building blocks are preferably bonded to each other by a joint oxygen atom present between two silicon atoms of each building block. When the silicon compound comprises more than one building block according to formula (A) and / or more than one building block according to formula (B), at least one bond as described hereinabove is typically comprised by the silicon compound. The silicon compound comprising a building block according to formula (A) and a building block according to formula (B) typically has the following structure: [ka] It can be expressed as follows.
[0039] Silicon compounds are widely available commercially or can be obtained by standard methods. For example, two or more suitable silanes can be reacted with each other in a (targeted) hydrolysis and condensation reaction. These reactions can be carried out in a suitable solvent (e.g., water, alcohols such as methanol, ethanol, and propanol, or mixtures of water with alcohols or ketones such as methyl isobutyl ketone (MIBK)). Catalysts useful for this type of reaction are known in the art and include inorganic and organic acids (e.g., hydrochloric acid, acetic acid), bases (e.g., ammonia or potassium hydroxide), and metal chelates (e.g., titanates or zirconates). If necessary, the alcohol liberated during the condensation can be removed by standard means such as distillation. Useful methods are described in EP 0 675 128 (see page 2, line 50 to page 5, line 41, especially Example II).
[0040] At least one silane according to formula (S) is R s and R t Preferably, R sis preferably selected from the group consisting of hydroxy and C1-C4 alkoxy groups, more preferably selected from the group consisting of hydroxy, methoxy, and ethoxy groups. This selection allows for improved coverage of the binding sites and avoids potentially corrosive halides or hydrogen halides such as HCl.
[0041] R t is selected from the group consisting of alkyl groups and alkenyl groups. The alkyl groups and alkenyl groups are unsubstituted. R t is preferably an unsubstituted C1 to C18 alkyl group, more preferably an unsubstituted C2 to C8 alkyl group, even more preferably an unsubstituted C2 to C4 alkyl group, and particularly an n-propyl group.
[0042] At least one R s is selected from the group consisting of chloride, carboxylic acid, hydroxy, and alkoxy groups (subject to the above priorities).
[0043] The weight ratio of the at least one silane according to formula (S) to the at least one silicon compound (or a compound derived therefrom) in the layer ranges from 0.1-50, preferably from 0.2-20, more preferably from 1-10.
[0044] The weight of the layer on the surface of the core is preferably in the range of 0.1 to 25% by weight, more preferably 0.5 to 15% by weight, and even more preferably 3 to 8% by weight, based on the weight of the core of the surface-modified particle.
[0045] The means of treatment are described below. The layer obtained by treating the core with at least one silicon compound and at least one silane according to formula (S) advantageously does not change the color of the particle or composition comprising the surface-modified particle according to the present invention. This surface treatment also removes surface hydroxyl groups, thus preventing the formation of hydrogen bonds. Such hydrogen bonds are undesirable because they tend to form permanent aggregates during the drying process of the particle.
[0046] The size of the surface modified particles is preferably in the range of 2-1000 nm, more preferably 5-500 nm, even more preferably 70-200 nm. The size of the surface modified particles can be measured using any suitable technique, preferably X-ray laser diffraction technique. Suitable size measuring devices and their use are described in the experimental section of this specification. It is particularly noted that the size ranges defined above apply to all dimensions of the surface modified particles.
[0047] The shape of the surface-modified particles is not particularly limited. It may be an irregular shape. It is preferably circular, and more preferably spherical.
[0048] The aspect ratio of the surface modified particles is preferably in the range of 1:1 to 5:1, more preferably 1:1 to 3:1, and even more preferably 1:1 to 2:1. In the aspect ratio x:y, x represents the maximum dimension of the surface modified particle and y represents the minimum dimension. The dimensions of the surface modified particles can be measured in two-dimensional photographs obtained by TEM. Usually, at least 100 surface modified particles need to be measured. It is preferred that at least 80%, more preferably at least 90%, and even more preferably 99% of the surface modified particles have the above-mentioned aspect ratio. Surface modified particles having an aspect ratio in the above-mentioned range have improved dispersibility and are particularly suitable for use in toner compositions. The inventors believe that this effect is due to the advantageous volume-to-surface ratio that gives a very high amount of functional groups resulting from the at least one silicon compound and at least one silane according to formula (S) present on the surface of the surface modified particles. Moreover, the above-mentioned aspect ratio has an advantageous effect on the usefulness of the surface modified particles for toner compositions.
[0049] The layer on the surface of the core obtained by treating said core with at least one silicon compound and at least one silane according to formula (S) has turned out to be difficult to characterize. Presumably, it comprises a mixture of compounds formed by reaction of said silicon compound and silane according to formula (S) with one or more binding sites present on the surface of the core, such as hydroxyl groups.
[0050] Generally, the layer in the context of the present invention should be interpreted broadly. The layer can cover the entire surface of the core or one or more parts of the core. For example, it can be a uniform layer on the surface of the core, an island-like structure present on its surface, or simply a surface functionalization of the core, of course, the first mentioned is preferred. The layer on the surface of the core obtained by treating said core with at least one silicon compound and at least one silane according to formula (S) is preferably located directly on the surface of the core. This layer is preferably chemically bonded to the surface of the core, for example by reaction of binding sites such as hydroxyl groups present on the surface of the core with silanol groups of the silicon compound or silane according to formula (S).
[0051] The surface-modified particles according to the invention can be used to impart hydrophobic (i.e. contact angle of 90° or more) and even superhydrophobic (i.e. contact angle of 150° or more) properties to surfaces treated therewith. In this context, any surface can be used. Preferred surfaces are selected from the group consisting of ceramics, fibers, metals, pigments and membranes.
[0052] The present invention further relates to the use of (at least one) surface-modified particle according to the present invention as an additive in toner compositions, adhesives or abrasive slurries, or as a filler in electronic materials, (specialty) coatings or films.Accordingly, the present invention relates to a composition comprising at least one surface-modified particle according to the present invention.Usually, such a composition comprises a plurality of said surface-modified particles, the amount of which depends on various factors and the desired application of the composition.
[0053] The present invention further provides a method for preparing a surface-modified particle according to the invention, comprising the steps of: I) providing at least one unmodified particle; and II) the unmodified particles, II.I) Formula (A): [ka] [In the formula, R 1 is an organic radical, preferably selected from the group consisting of substituted or unsubstituted alkyl groups, substituted or unsubstituted alkenyl groups, and substituted or unsubstituted aryl groups; Each X is independently selected from the group consisting of a hydroxy group, a carboxylic acid group, a chloride, and an alkoxy group; m is selected from 0, 1, and 2. At least one building block according to Formula (B): [ka] [In the formula, R 2 is an organic radical, preferably selected from the group consisting of substituted or unsubstituted alkyl groups, substituted or unsubstituted alkenyl groups, and substituted or unsubstituted aryl groups; each Y is independently selected from the group consisting of a hydroxy group, a carboxylic acid group, a chloride, and an alkoxy group; n is selected from 0, 1, and 2. At least one building block by and at least one silicon compound comprising: II.ii) Formula(S): [ka] [In the formula, Each R s At least one R sis independently selected from the group consisting of hydroxy groups, carboxylic acid groups, chloride, alkoxy groups, alkyl groups, and aryl groups, with the proviso that is selected from the group consisting of chloride, carboxylic acid groups, hydroxy groups, and alkoxy groups; R t is selected from the group consisting of alkyl and alkenyl groups. and at least one silane according to Method steps for treating with The present invention relates to a method comprising the steps of:
[0054] By carrying out method steps I and II, surface-modified particles according to the invention are obtained.
[0055] In method step I, unmodified particles are provided, which comprise at least one oxide-based material. The unmodified particles correspond to the core of the surface-modified particles according to the invention. For that purpose, the unmodified particles can be prepared by known means or commercially available unmodified particles can be used. A useful method for producing unmodified particles is the so-called Stoeber process (Werner Stoeber, Arthur Fink, Ernst Bohn, Controlled growth of monodisperse silica spheres in the micron size range, Journal of Colloid and Interface Science, Vol.26, pp. 62-69 (1968)). The unmodified particles preferably do not comprise a layer on their surface, such as a layer obtained by treating said unmodified particles with silanes or siloxanes, in order to avoid undesired side reactions during method step II. Optionally, the unmodified particles comprise another material other than the oxide-based material (see above). The details and preferences described for the core of the surface-modified particles according to the invention also apply mutatis mutandis to the unmodified particles.
[0056] In method step II, the unmodified particles are treated with at least one silicon compound and at least one silane. The preferences for the silicon compound and the silane according to formula (S) are described above. This results in the formation of a layer on the surface of the unmodified particles. The means of treatment are not particularly limited. For this purpose, the surface of the unmodified particles must be contacted with at least one silicon compound and at least one silane according to formula (S). In the context of the present invention, it is possible to use a solution or dispersion that contains unmodified particles and / or at least one silicon compound and / or silane according to formula (S).
[0057] For example, unmodified particles are immersed in a composition comprising at least one silicon compound and at least one silane according to formula (S), or said silicon compound and at least one silane according to formula (S). Alternatively, unmodified particles are provided (for example as a powder (preferably dried before method step II to remove adhering water therefrom), or as a dispersion), and at least one silicon compound and at least one silane according to formula (S) are added thereto, for example by spraying thereto or immersing therein. It is also possible to use unmodified particles and directly mix them with at least one silicon compound and at least one silane according to formula (S) using a suitable mixing device. Furthermore, it is preferably possible to provide a composition (such as a dispersion) comprising unmodified particles, and then add at least one silicon compound and at least one silane according to formula (S) thereto, and mix the above.
[0058] The order of treatment of unmodified particles with at least one silicon compound and at least one silane according to formula (S) is not particularly limited.Preferably, unmodified particles are first treated with a silicon compound and then treated with a silane according to formula (S).In this connection, when two or more silicon compounds are used, all silicon compounds are used before the first silane according to formula (S).When two or more silane according to formula (S) are used, all said silanes are used after all silicon compounds have been used.This can further improve the coverage of binding sites.Alternatively, unmodified particles are first treated with a silane and then treated with a silicon compound, or unmodified particles are simultaneously treated with a silane according to formula (S) and a silicon compound.
[0059] The at least one silane according to formula (S) is preferably added to the at least one unmodified particle at an addition rate in the range of 0.01-50 g / min / kg of unmodified particle, which further improves the coverage of the bonding sites of the surface-modified particles formed. Preferably, the addition rate is in the range of 0.1-30 g / min / kg of unmodified particle, most preferably 1-10 g / min / kg of unmodified particle.
[0060] The amount of at least one silicon compound and at least one silane according to formula (S) is preferably selected to meet the weight range of the layer described above.Typically, the amount of at least one silicon compound used in method step II is in the range of 0.1-10 wt%, preferably 0.25-8 wt%, more preferably 0.5-4 wt%, based on the total mass of the at least one unmodified particle.
[0061] It is preferred that the weight ratio of the at least one silane according to formula (S) to the at least one silicon compound in process step II ranges from 0.1-50, preferably from 0.2-20, more preferably from 1-10.
[0062] The temperature during method step II is preferably in the range of 5 to 130° C., preferably 20 to 90° C., more preferably 50 to 80° C. The duration of method step II is preferably in the range of 1 to 24 hours, preferably 2 to 18 hours, more preferably 6 to 13 hours.
[0063] Depending on the processing means of method step II, additional optional method steps are optionally added to the method according to the invention. For example, it is possible to disperse the surface-modified particles obtained according to the invention, or to dilute the dispersion, or to increase its concentration, for example by removing excess solvent using standard means, such as distillation. Optionally, the surface-modified particles are dried before and / or after method step II. This can be done by standard means, such as using an oven.
[0064] Optionally, the method for preparing surface-modified particles according to the invention comprises an additional method step III: III) Method step of grinding surface-modified particles Includes.
[0065] This step advantageously reduces the number of secondary particles (so-called agglomerates), resulting in smaller particles. Preferred tools used for this purpose are ball mills or jet mills. The surface-modified particles are preferably dried prior to method step III.
[0066] The method of the present invention allows an easy manufacturing process of the surface-modified particles according to the present invention. The method of the present invention further reduces the release of VOCs and toxic compounds, such as methanol, compared to standard methods using silanes. The use of at least one silicon compound and at least one silane according to formula (S) also results in a homogeneous distribution of the layer obtained on the surface of the core of the surface-modified particles. The use of a silicon compound and at least one silane according to formula (S) also improves the coverage of the binding sites (such as hydroxyl groups) present on the surface of the unmodified particles compared to other methods, such as the use of silanes or hydrosiloxanes or silicon compounds only. The latter requires less material compared to the solutions of the prior art, which offers ecological and economic advantages. In addition, the agglomeration of the particles is also reduced.
[0067] The present invention further relates to a toner composition comprising at least one surface-modified particle according to the present invention. In general, the toner composition and the components used therein are known in the art. The toner composition according to the present invention can be obtained by mixing colored particles and at least one surface-modified particle, preferably as a powder, using a mixer such as a Henschel mixer. The toner according to the present invention has higher humidity resistance, brighter printing, and increased printing efficiency.
[0068] Colored particles typically include at least one binder resin and at least one colorant.The manufacturing method thereof is not particularly limited, but typically, for example, it is manufactured by a grinding process (a process in which a colorant is melted in a thermoplastic resin as a binder resin component, mixed to uniformly disperse, and then this is ground and classified to obtain colored particles), or a polymerization process (a process in which a colorant is melted or dispersed in a polymerizable monomer as a raw material of a binder resin, then suspended in an aqueous dispersion medium containing a dispersion stabilizer after adding a polymerization initiator, and the suspension is heated to a predetermined temperature to start polymerization, and after the polymerization is completed, it is filtered, rinsed, dehydrated, and dried to obtain colored particles).
[0069] The at least one binder resin may be a resin that has been widely used in toners up to now. The at least one binder resin may be, preferably, a polymer of styrene and its substitution products, such as polystyrene, poly-p-chlorostyrene, and polyvinyltoluene, a styrene copolymer, such as styrene-p-chlorostyrene, styrene-propylene, styrene-vinyltoluene, styrene-vinylnaphthalene, styrene-methylacrylate, styrene-ethylacrylate, styrene-butylacrylate, styrene-octylacrylate, styrene-methylmethacrylate, styrene-ethylmethacrylate, styrene-butylmethacrylate, styrene-α-chloromethacrylate, styrene-acrylonitrile, styrene, styrene-α-chloromethacrylate ... The binder resin is selected from the group consisting of styrene-vinyl methyl ether, styrene-vinyl ethyl ether, styrene-vinyl methyl ketone, styrene-butadiene, styrene-isoprene, styrene-acrylonitrile-indene, styrene-maleic acid, and styrene-maleate, polymethyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, polyester, polyurethane, polyamide, epoxy resin, polyvinyl butyral, polyacrylic resin, rosin, modified rosin, terpene resin, phenolic resin, aliphatic or alicyclic hydrocarbon resin, and aromatic petroleum resin, and mixtures of the above. To the at least one binder resin, known release agents, antistatic agents, etc. are optionally added.
[0070] The coloring agent contained in the colored particles can be any pigment and / or dye, such as carbon black or titanium white. The coloring optionally includes at least one magnetic material, preferably selected from the group consisting of iron oxides, such as magnetite, γ-iron oxide, ferrite, and iron-rich ferrite, metals, such as iron, cobalt, and nickel, or alloys of said metals with metals, such as aluminum, copper, magnesium, tin, zinc, calcium, titanium, tungsten, and vanadium, and mixtures thereof.
[0071] Any toner composition according to the present invention can be used as is, i.e. as a one-component toner. It can also be mixed with a carrier for use as a so-called two-component toner.
[0072] The present invention further relates to surface-modified particles obtainable by the method according to the invention.
[0073] The present invention relates to a method for treating a surface of a substrate, B1) the method steps of providing a substrate having a surface; and B2) A method step of treating the surface of a substrate with at least one surface-modified particle according to the invention. The present invention relates to a method for producing a semiconductor device.
[0074] By carrying out the method steps B1 and B2, a substrate with a treated surface is obtained. As previously described herein, the treatment with at least one surface-modifying particle (usually a plurality is used) according to the invention confers a certain functionality to the surface, for example hydrophobicity. The choice of substrate is not particularly limited, and the skilled person can select a suitable substrate according to the technical requirements to be met. Preferred substrates are selected from the group consisting of glass, pigments, fibers, flakes, ceramics, and cellulosic materials, such as paper and cardboard, among others. The surfaces thus treated typically have improved moisture resistance, enhanced mechanical or thermal stability.
[0075] The treatment in method step B2 is not particularly limited. Many methods can be used, such as immersing the substrate in a composition comprising at least one surface-modified particle according to the present invention, and spraying, printing, or painting the composition on the surface of the substrate. Those skilled in the art can select the appropriate temperature and duration based on routine experimentation.
[0076] Furthermore, the present invention also relates to a substrate comprising at least one layer comprising at least one surface-modified particle according to the present invention.
[0077] The invention will now be described with reference to the following non-limiting examples.
[0078] Working Example In the examples, Dynasylan 6598 (co-oligomer of n-propyltriethoxysilane and vinyltriethoxysilane, supplied by Evonik Corp., USA) was used as the silicon compound.
[0079] Preparation of unmodified particles Example 1 (according to the invention) a) Synthesis of 200 nm silica particles (corresponding to method step I): A 1 L reactor was charged with 10.1 g of potassium hydroxide (45 wt % in water), 141.4 g of ethanol, and 518.9 g of water. The solution was vigorously mixed and heated to 78 °C. 329.6 g of TEOS (tetraethoxysilane) was added over a period of 3 h to synthesize silica nanoparticles. After the reaction, the suspension containing the unmodified particles was cooled to room temperature (20 °C).
[0080] b) Functionalization (corresponding to method step II): In the same reactor, 3% (w / v) of Dynasylan 6598 was slowly added to the silica suspension at room temperature. The silicon compound was added dropwise to the suspension over 1 hour. After addition, the temperature was increased to 78°C. The functionalization reaction was carried out for 4 hours. Then, 0.5% (w / v) of n-propyltriethoxysilane (PTEO, supplied by Evonik Corp.) was slowly added to the suspension at 50°C. The reaction was allowed to continue for 3 hours, after which the suspension containing the surface-modified particles was cooled to room temperature.
[0081] c) Drying and grinding (corresponding to optional method step III): The surface-modified particles were then obtained by centrifuging, washing with ethanol, and drying at 50° C. The dried powder samples of the surface-modified particles were ground in a ball mill at 300 RPM (15-30 min).
[0082] Example 2 (Comparison) Silica particles were synthesized as described in Example 1. The silica particles were then functionalized with 3% (w / v) Dynasylan 6598 only using the procedure described in Example 1.
[0083] Example 3 (Comparison) Silica particles were synthesized as described in Example 1. The silica particles were then functionalized with 4% (w / v) n-propyltriethoxysilane using the procedure described in Example 1.
[0084] The resulting products were characterized by the following methods:
[0085] Dispersibility Test The powder samples of Examples 1 to 3 were mixed with various solvents in a weight ratio of 1:5 (20°C). These suspensions were mixed in an ultrasonic disintegrator for 30 minutes and the state of dispersion was visually observed. The results are shown in the table below.
[0086] [Table 1]
[0087] In Example 1 (according to the present invention), stable dispersions were obtained in all organic solvents tested, whereas particles modified only with monomeric silane or silicon compounds could not be completely dispersed.From the results shown above, it can be concluded that the dispersibility of the surface-modified particles according to the present invention in organic solvents is superior to that of particles known from the prior art, such as particles treated with monomeric silane (Example 3) or particles treated only with silicon compounds (Example 2).
[0088] Laser diffraction particle size distribution The particle size distribution of the dispersion containing the surface-modified particles of Example 1 and the dispersion containing unmodified particles in ethanol was measured by a laser diffraction scattering type particle size distribution analyzer (LA950, Horiba). Before the measurement, the dispersion was sonicated for 5 minutes. The peak of Example 1 was narrow and the fraction of particles larger than 1 μm was very small compared to the unmodified particles. This indicates that the wettability and solubility of the surface-modified particles according to the present invention are improved. This also confirms that fewer aggregates are formed during drying of the surface-modified particles according to the present invention compared to the unmodified particles.
[0089] solid 29 Si NMR (Figure 1) solid 29 Si NMR was measured on a Bruker Avance III 300FT-NMR spectrometer. 1 wt% polydimethylsiloxane (PDMS) was added to the powder samples of Example 1 and Example 2, respectively, as an internal standard (see US Patent Application Publication No. 2010 / 0071272, especially the drawings and paragraph 70 et seq.). The area of the PDMS peak and the total area of the silanol peaks in the spectrum were normalized based on the area of the PDMS peak. The ratio of the normalized PDMS peak area to the total area of the silanol peaks provides an estimate for the silanol groups remaining after the functionalization experiment. A higher molar ratio of PDMS to silanol groups indicates a less complete surface coating with the organosilane. The results are shown in the table below.
[0090] [Table 2]
[0091] It is clear that the number of binding sites of the surface modified particles according to the invention is significantly less compared to prior art particles produced using only monomeric silanes or silicon compounds, therefore the method of the invention allows for improved coverage of binding sites.
[0092] Methanol Wettability Test The purpose of this test was to measure the hydrophobicity of the treated samples. The weight percent of the methanol and water mixture that completely wets the sample is a measure of the degree of hydrophobicity and the uniformity of the treatment.
[0093] 0.2 g of surface modified particles were placed into each 15 mL clear conical centrifuge tube (with the first mL marked). Methanol-water mixtures with concentrations varying from 30% to 70% by weight were prepared. To each tube, 8 mL of the methanol-water mixture of the particular concentration was added. The contents were mixed vigorously and then centrifuged at 2500 RPM for 5 minutes. The precipitate levels were then visually analyzed. The results are shown in the table below.
[0094] [Table 3]
[0095] Example 1 of the present invention demonstrated the most hydrophobic surface modified particles.
[0096] Other embodiments of the invention will be apparent to those skilled in the art from consideration of the specification or practice of the invention disclosed herein. It is intended that the specification and examples be considered as exemplary only, with the true scope of the invention being defined only by the following claims.
Claims
1. 1. A surface-modified particle for use in a toner composition, comprising: a) a core comprising at least one oxide-based material selected from the group consisting of silicon oxides, metal oxides, and mixtures of one or more of the foregoing; and b) at least one layer, b.i) Formula (A): 【Chemistry 1】 [In the formula, R 1 is an organic radical, preferably selected from the group consisting of substituted or unsubstituted alkyl groups, substituted or unsubstituted alkenyl groups, and substituted or unsubstituted aryl groups; each X is independently selected from the group consisting of a hydroxy group, a carboxylic acid group, a chloride, and an alkoxy group; m is selected from 0, 1, and 2. At least one building block according to Formula (B): 【Chemistry 2】 [In the formula, R 2 is an organic radical, preferably selected from the group consisting of substituted or unsubstituted alkyl groups, substituted or unsubstituted alkenyl groups, and substituted or unsubstituted aryl groups; each Y is independently selected from the group consisting of a hydroxy group, a carboxylic acid group, a chloride, and an alkoxy group; n is selected from 0, 1, and 2. At least one building block according to At least one silicon compound comprising b.ii) Formula (S): 【Chemistry 3】 [In the formula, Each R s is at least one R s is independently selected from the group consisting of hydroxy groups, carboxylic acid groups, chloride, alkoxy groups, alkyl groups, and aryl groups, with the proviso that is selected from the group consisting of chloride, carboxylic acid groups, hydroxy groups, and alkoxy groups; R t is selected from the group consisting of alkyl and alkenyl groups. and at least one silane according to Layer obtained from A surface-modified particle comprising:
2. The surface-modified particles according to claim 1, characterized in that the size of the surface-modified particles is in the range of 2 to 1000 nm.
3. The surface-modified particles according to claim 2, characterized in that the size of the surface-modified particles is in the range of 5 to 500 nm.
4. 4. The surface-modified particle according to claim 3, wherein the surface height of the modified particle is in the range of 70 to 200 nm.
5. 5. The surface-modified particle of claim 1, wherein the at least one silicon compound comprises at least one reactive site per silicon atom, the reactive site being selected from the group consisting of hydroxyl groups, carboxylic acid groups, chloride, and alkoxy groups.
6. R t The surface-modified particles according to any one of claims 1 to 5, characterized in that is selected from the group consisting of unsubstituted C1 to C18 alkyl groups, preferably unsubstituted C2 to C8 alkyl groups.
7. R t The surface-modified particle according to claim 6, wherein is an unsubstituted C2 to C4 alkyl group.
8. R t 8. The surface-modified particle according to claim 7, wherein is an n-propyl group.
9. 9. Surface modified particles according to any one of claims 1 to 8, characterized in that the weight ratio of the at least one silane according to formula (S) to the at least one silicon compound in the layer is in the range of 0.1 to 50, preferably 0.2 to 20, more preferably 1 to 10.
10. 10. The surface modified particle according to claim 1, characterized in that the weight of the layer on the surface of the core is preferably in the range of 0.1 to 25% by weight, more preferably 0.5 to 15% by weight, even more preferably 3 to 8% by weight, based on the weight of the core of the surface modified particle.
11. 11. Surface-modified particles according to claim 1, characterized in that the layer is obtained by treating unmodified particles first with the at least one silicon compound and then with the at least one silane according to formula (S).
12. The surface modified particle according to any one of claims 1 to 11, characterized in that the aspect ratio of the surface modified particle is in the range of 1:1 to 5:1, preferably 1:1 to 3:1, more preferably 1:1 to 2:
1.
13. A method for preparing a surface-modified particle according to any one of claims 1 to 12, comprising the steps of: I) a method step of providing at least one unmodified particle; and II) subjecting the unmodified particles to II.I) Formula (A): 【Chemistry 4】 [In the formula, R 1 is an organic radical, preferably selected from the group consisting of substituted or unsubstituted alkyl groups, substituted or unsubstituted alkenyl groups, and substituted or unsubstituted aryl groups; each X is independently selected from the group consisting of a hydroxy group, a carboxylic acid group, a chloride, and an alkoxy group; m is selected from 0, 1, and 2. At least one building block according to Formula (B): 【Chemistry 5】 [In the formula, R 2 is an organic radical, preferably selected from the group consisting of substituted or unsubstituted alkyl groups, substituted or unsubstituted alkenyl groups, and substituted or unsubstituted aryl groups; each Y is independently selected from the group consisting of a hydroxy group, a carboxylic acid group, a chloride, and an alkoxy group; n is selected from 0, 1, and 2. At least one building block according to At least one silicon compound comprising II.ii) Formula (S): 【Chemistry 6】 [In the formula, Each R s is at least one R s is independently selected from the group consisting of hydroxy groups, carboxylic acid groups, chloride, alkoxy groups, alkyl groups, and aryl groups, with the proviso that is selected from the group consisting of chloride, carboxylic acid groups, hydroxy groups, and alkoxy groups; R t is selected from the group consisting of alkyl and alkenyl groups. and at least one silane according to Method steps for treating with A method comprising:
14. 14. The method of claim 13, wherein the unmodified particles are first treated with the at least one silicon compound and then with the at least one silane according to formula (S).
15. 15. The method according to claim 13 or 14, characterized in that the at least one silane according to formula (S) is added to the at least one unmodified particle at an addition rate ranging from 0.01 to 50 g per kg of unmodified particle per minute.
16. Surface-modified particles obtainable by the method according to any one of claims 13 to 15.
17. 17. Use of at least one surface-modified particle according to any one of claims 1 to 12 or claim 16 as an additive in a toner composition, an adhesive or an abrasive slurry, or as a filler in an electronic material, (specialty) coating or film.
18. 17. A toner composition comprising at least one surface-modified particle according to any one of claims 1 to 12 or claim 16.
19. 1. A method for treating a surface of a substrate, comprising the steps of: B1) providing said substrate having said surface; and B2) a method step of treating the surface of the substrate with at least one surface-modified particle according to any one of claims 1 to 12 or claim 16. A method comprising:
20. 17. A substrate comprising at least one layer comprising at least one surface-modified particle according to any one of claims 1 to 12 or claim 16.
Citation Information
Patent Citations
Toner
JP2011047988A
Positively-charged toner and method for manufacturing the same
JP2019078802A