Piston ring with particle-containing wear protection layer, method of manufacture and use thereof
A chromium-free piston ring wear protection layer with carbon and hard material particles, formed via galvanic deposition and heat treatment, achieves enhanced hardness, stability, and wear resistance, overcoming toxicity and performance issues of traditional chromium-based layers.
Patent Information
- Application Number
- JP2024519565
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-30
- Filing Date
- 2022-09-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2042-09-28
AI Technical Summary
Existing piston rings for internal combustion engines face challenges with chromium-based wear protection layers due to toxicity concerns and insufficient hardness and wear resistance, necessitating a chromium-free alternative with improved mechanical and thermal performance.
A piston ring with a wear protection layer composed of iron or iron alloy, containing carbon particles and other hard material particles, is formed through a galvanic deposition process using a low pH electrolyte, followed by heat treatment to create cracks and uniform particle distribution, enhancing hardness and wear resistance.
The resulting wear protection layer exhibits high hardness, dimensional stability, and reduced wear, with improved sliding properties and reduced particle detachment, addressing the limitations of chromium-based layers.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a piston ring made of iron or an iron alloy, the iron or iron alloy having solid particles embedded therein. The present invention also relates to a method for making the piston ring and to the use of the piston ring in an internal combustion engine. [Background technology]
[0002] Piston rings for internal combustion engines are exposed to high friction and high temperatures, and therefore must have a surface with high wear resistance and excellent sliding properties. For this purpose, a wear-resistant protective layer, such as an electrolytically deposited hard chromium layer, is usually applied to the outer peripheral surface (running surface) of the piston ring. In addition to high wear resistance, the wear protective layer must have as high a dimensional stability as possible, i.e., it is desirable that the wear protective layer is as durable as possible and not damaged, even if the shape of the piston ring changes during engine operation.
[0003] The wear resistance can be improved by incorporating solid particles into the hard chromium layer. DE-A-3531410 and EP-A-0217126 describe electroplated hard chromium layers in which solid particles are embedded in cracks.
[0004] However, one of the drawbacks of the known hard chromium solid particle layers is that to produce the hard chromium layer, an electrolyte containing hexavalent chromium is required, which is highly toxic. The manufacturing process of hard chromium layers using hexavalent chromium will probably not be permitted within a few years. Therefore, in order to protect the environment and to protect humans and animals, piston rings with a chromium-free wear protection layer are desirable.
[0005] Wear protection layers for steel piston rings with embedded solid particles are known from DE 195 08 419. However, the hardness and wear resistance of these wear protection layers are no longer sufficient for the high thermal and mechanical demands of piston rings in modern internal combustion engines. Summary of the Invention [Problem to be solved by the invention]
[0006] It is therefore an object of the present invention to provide a piston ring having a wear protection layer which overcomes the above-mentioned drawbacks of the prior art and which has high wear resistance, hardness and dimensional stability, the wear protection layer being free of chromium. It is also an object of the present invention to provide a method for producing such a wear protection layer. [Means for solving the problem]
[0007] According to the invention, this object is achieved by a piston ring for an internal combustion engine having a surface on which a wear protection layer of iron or an iron alloy is formed, said wear protection layer having cracks, said cracks having an average density of 10 to 160 cracks per mm of said wear protection layer, and 0.2 to 15% by weight, based on the total weight of said wear protection layer, of carbon particles and 0.2 to 15% by weight, based on the total weight of said wear protection layer, of solid particles that are not carbon particles, embedded in said iron or said iron alloy.
[0008] This objective is further: (a) an iron(II) compound in an amount corresponding to 100 to 500 g / l of FeCl2 and, optionally, a salt of a further metal; placing the piston ring in an aqueous electrolyte solution containing carbon particles and non-carbon solid particles, the aqueous electrolyte solution having a pH of 0 or less; (b) A wear protection layer of iron or iron alloy with a resistance of 10 to 80 A / dm 2 galvanically depositing a cathode current density of 0.1g / mol / L on said piston ring; (c) drying the piston ring together with the wear protection layer; and (d) heating to 300 to 700°C; This is achieved by a method for producing a piston ring, comprising the steps of:
[0009] This object is further achieved by a piston ring obtainable by the above-mentioned method and by the use of said piston ring according to the invention in an internal combustion engine.
[0010] Surprisingly, it has been found in the context of the present invention that the wear protection layer of the piston ring according to the invention has high hardness, high dimensional stability and at the same time high wear resistance.
[0011] The crack density of 10 to 160 cracks per mm of the wear protection layer ensures a high dimensional stability of the wear protection layer, which is achieved, inter alia, by the low pH value of the electrolyte. The heat treatment mainly increases the hardness of the wear protection layer. It is assumed that the carbon particles are partially converted into Fe-C compounds (iron-carbon compounds), which is responsible for the above-mentioned advantageous properties of the wear protection layer, in particular the increased hardness, without the invention being limited by this explanation. On the other hand, the solid particles that are not carbon particles remain in the wear protection layer, and it is assumed that these solid particles that are not carbon particles are mainly responsible for the high wear resistance of the layer, without the invention being limited by this explanation. In this way, a combination of higher hardness and good wear resistance of the wear protection layer according to the invention is achieved.
[0012] Preferably, a piston ring having a surface and comprising a wear protection layer of iron or iron alloy applied to said surface, said wear protection layer having cracks, said cracks having an average density of 10-160 cracks per mm of said wear protection layer, and 0.2-15 wt. % of carbon particles and 0.2-15 wt. % of solid particles that are not carbon particles, based on the total weight of said wear protection layer, are incorporated in said iron or iron alloy, said carbon particles being partially or completely converted to Fe-C compounds. This means that said wear protection layer comprises Fe-C compounds. This conversion is preferably carried out by heating said wear protection layer to 300-700°C.
[0013] In a preferred embodiment, the wear protection layer comprises 0.01-25 wt. % of an iron-carbon compound, more preferably 0.05-10 wt. % of an iron-carbon compound, especially 0.1-5 wt. % of an iron-carbon compound, based on the total weight of the wear protection layer, which is generated from the carbon particles and the surrounding iron when heated to 300-700°C.
[0014] The heat treatment temperature of 300-700° C. is particularly higher than the temperatures to which piston rings are exposed when used in an internal combustion engine, since the temperature of the wear protection layer is always below 250° C. The heat treatment of the piston ring or the wear protection layer before use in an engine is therefore necessary to at least partially convert the carbon particles and improve the properties of the piston ring.
[0015] The temperature in the heat treatment of the piston ring or the wear protection layer is 300-700° C., preferably 320-650° C., more preferably 340-600° C., even more preferably 350-550° C., and in particular 380-540° C. With these temperatures, a particularly advantageous combination of increased hardness and high wear resistance of the wear protection layer can be achieved. The heat treatment is preferably carried out for at least 15 minutes, more preferably at least 30 minutes, and even more preferably for 1 to 4 hours.
[0016] The carbon particles are preferably made of diamond and / or graphite, more preferably diamond particles.
[0017] In order to achieve high wear resistance, hard material particles are preferably used as solid particles that are not carbon particles. For the purposes of the present invention, hard material particles are understood to be particles of materials with a Mohs hardness of 8 or more. Among these, hard material particles with a Mohs hardness of 9 or more are preferred, in particular those with a Mohs hardness of 9.2 to 10. The Mohs hardness is measured according to the Mohs hardness test known in the prior art. Preferred hard material particles are those made of tungsten carbide, chromium carbide, aluminum oxide, silicon carbide, silicon nitride, boron carbide and / or cubic boron nitride. Most preferred is cubic boron nitride (body-centered cubic boron nitride).
[0018] The sliding properties of the wear protection layer can advantageously be further improved by adding solid lubricant particles, examples of which are hexagonal boron nitride or polymer particles.
[0019] The proportion of the carbon particles and the proportion of the non-carbon solid particles are, independently of one another, 0.2 to 15% by weight, preferably 0.5 to 12% by weight, more preferably 1 to 10% by weight, and most preferably 2 to 8% by weight, based on the total weight of the wear protection layer.
[0020] The average particle size (grain size) of the carbon particles and the solid particles that are not carbon particles is 0.02 to 5 μm, preferably 0.05 to 3 μm, particularly preferably 0.1 to 1 μm, and particularly preferably 0.2 to 0.8 μm. 50 The average particle size (d) is measured by a laser diffraction method using a dry disperser (apparatus: Malvern Mastersizer equipped with a Sirocco dispersion unit). 50 ) is the value where 50% by volume of the particle size is smaller and 50% by volume of the particle size is larger than the specified value.
[0021] It is more preferable that not only the average particle size but also all particles are within a predetermined particle size range. Therefore, the particle sizes of the carbon particles and the non-carbon solid particles are preferably 0.02 to 5 μm, more preferably 0.05 to 3 μm, even more preferably 0.1 to 1 μm, and particularly preferably 0.2 to 0.8 μm, independently of each other.
[0022] The wear protection layer is made of iron or an iron alloy. The iron alloy preferably comprises 85% by weight or more of iron, more preferably 95% by weight or more of iron, particularly 98 to 99.8% by weight of iron, based on the total weight of the iron alloy. The alloying components of the iron alloy are typical alloying elements of iron, preferably any of Cr, Ni, Mo, Mn, V, W, Al and / or Nb.
[0023] The Vickers hardness of the wear protection layer according to the present invention is preferably 500 to 750 HV0.1, more preferably 550 to 700 HV0.1, most preferably 600 to 700 HV0.1. The Vickers hardness is measured according to methods known in the prior art for measuring the Vickers hardness.
[0024] Piston rings with cracks in the wear protection layer show improved dimensional stability compared to wear protection layers without cracks. Without limiting the invention, it is assumed that the improved dimensional stability is due to the cracks reducing or distributing the stresses in the layer, so that the layer is not as easily broken, i.e., material loss is avoided. The improved dimensional stability, which results in the avoidance of material loss, also leads to a significant reduction in wear.
[0025] When a piston ring wears on the surface facing the cylinder (the running surface of the piston ring), a distinction is made between adhesive and abrasive wear. Adhesive wear is the transfer of material from the running surface (liner) of the cylinder to the piston ring and vice versa, where the transfer of material essentially takes place from the liner to the ring. Abrasive wear, on the other hand, involves scratches between the running surfaces. The adhesive wear in the wear protection layer according to the invention is improved in particular by the distribution of solid particles in the matrix and, on the other hand, by reduced breakouts as a result of the improved dimensional stability, while abrasive wear is improved in particular by the formation of a lubricating film. Preferably, open cracks formed in the surface that are not filled with material collect engine oil on the one hand and residues from the oil in the form of solid combustion residues on the other hand, which also act as lubricant. Both of these improve the sliding properties of the surface of the wear protection layer and also provide great advantages in cases of too low lubrication, as may occur in engines.
[0026] The process according to the invention, which uses low pH values below 0, results in the abrasion-resistant protective layer being particularly abrasion-resistant and dimensionally stable, since the cracks and particles are very uniformly distributed within the layer.
[0027] The particles are therefore preferably distributed throughout the wear protection layer, i.e. are not restricted to the cracks, as opposed to, for example, hard chromium layers, where the particles are exclusively present in the cracks. Such a uniform distribution means that there are no large areas where the particles are absent or present in very small numbers, which uniformly improves the wear resistance of the layer. Furthermore, the particles are particularly strongly bound in the metal, so that they do not easily fall off the surface during operation, as is the case, for example, with hard chromium layers, where the particles are only present in the cracks. Overall, this results in a high wear resistance.
[0028] To form a wear protection layer on a piston ring according to the invention, the piston ring to be coated is placed in an electrolyte containing iron ions, optionally metal ions of a metal other than iron, carbon particles, and solid particles that are not carbon particles, and is cathodically connected. A direct or pulsating direct current, for example a pulsating direct current with a frequency of 10 kHz, is applied to said piston ring, thus galvanically depositing an iron or iron alloy layer.
[0029] In the present invention, "electrolyte" or "aqueous electrolyte" refers to an aqueous solution in which electrical conductivity is achieved by electrolytic dissociation of the components of the electrolyte into ions. In addition to the components mentioned and any other additives present, the electrolyte comprises water as the balance.
[0030] In the method according to the invention, the solid particles are preferably kept in suspension in the electrolyte. This can be achieved, for example, by intensive stirring and / or by using surface-active substances. Preferably, the electrolyte contains one or more surface-active compounds. These can be ionic, non-ionic and amphoteric surface-active (boundary layer active) compounds. Preferred surface-active compounds are polyfluorinated sulfonates. Preferably, the surface-active compounds do not contain PFOS.
[0031] In the deposition step (step b of the process), cracks are formed in the wear protection layer made of iron or iron alloy. These cracks are generally at least partially interconnected and can be referred to as a crack network. In a preferred embodiment of the invention, the solid particles are not substantially deposited in the cracks in the process according to the invention, even if they fit into the cracks in terms of size. This is in particular due to the pH value of the electrolyte being below 0.
[0032] As mentioned above, in a preferred embodiment of the invention, the carbon particles and / or the non-carbon solid particles are not mainly located in the cracks. Rather, the carbon particles and / or the non-carbon solid particles are substantially embedded in the matrix of the wear protection layer. For the purposes of the present invention, the term matrix refers to the entire metal wear protection layer except the cracks, i.e. the entire material of the wear protection layer that is not present in the form of cracks and is not solid particles. This improves the wear behavior since the solid particles make a significant contribution to the wear resistance, and there are no large areas where they are absent or only present in small amounts. Furthermore, the particles are particularly strongly bound in the matrix and therefore do not easily fall off from the surface during operation.
[0033] In a preferred embodiment of the invention, the proportion of the carbon particles and / or the solid particles which are not carbon particles located in the cracks relative to the total number of the particles in the wear protection layer according to the invention is in each case less than or equal to 0.5%, more preferably in each case less than or equal to 0.1%, even more preferably in each case less than or equal to 0.05% and most preferably in each case less than or equal to 0.02%.
[0034] In a further preferred embodiment of the present invention, the proportion of the sum of the carbon particles and the solid particles that are not carbon particles located in the cracks relative to the total number of the particles in the wear protection layer according to the present invention is less than 0.5%, more preferably less than 0.1%, even more preferably less than 0.05%, and most preferably less than 0.02%.
[0035] The proportion of the particles in the cracks relative to the total number of particles is measured on microscopic images of cross-sections or running surface polishes. For this purpose, particles are counted over an area of at least 10 μm×10 μm and the proportion of the particles in the cracks is measured. This area is selected depending on the size and distribution of the particles so that a sufficient number of particles, preferably at least 200 particles, are visible in the area. The preparation of the microscopic specimen is described in more detail below.
[0036] In a further preferred embodiment of the present invention, surprisingly, the cracks are substantially not filled with iron or iron alloys, i.e. are substantially empty. This has the advantage that, since the cracks are open, engine oil can fill the surface during operation of the piston ring, thus acting as a lubricating film. Furthermore, combustion residues of the engine oil can be deposited in the open cracks, which also improves the sliding properties. In this way, a particularly effective sliding film (tribofilm) is formed.
[0037] When heated to 300-700°C according to step (d) of the method according to the invention, an iron oxide layer is formed on the surface of the crack, because the crack contains air and the oxygen in the air oxidizes the iron surface of the crack. Therefore, preferably the surface of the crack has an iron oxide layer.
[0038] In a preferred embodiment of the present invention, 3% or less by volume of the cracks is filled with iron or iron alloy, based on the total volume of the cracks. More preferably, 2% or less by volume of the cracks is filled with iron or iron alloy, based on the total volume of the cracks, and even more preferably, 1% by volume of the cracks is filled with iron, based on the total volume of the cracks. The volume fraction of the cracks filled with iron or iron alloy can be measured using the color tone of a microscope image in cross-section polishing or running surface polishing. This is because the metal in the cracks, which are dark in color, appears bright, and the crack-free areas of the wear protection layer also appear bright. The percentage of the area is measured over several polishings, preferably 2 to 3 polishings, and corresponds to the volume fraction.
[0039] The pH value of the electrolyte in the process according to the invention is below 0. It has been found in the context of the present invention that this low pH value allows for the formation of an advantageous crack structure, a relatively low crack density, and at the same time particles are preferably not embedded in the cracks of the layer, so that the particle distribution in the layer is very uniform.
[0040] In particular, the crack structure ensures stress relaxation in the layer and therefore high dimensional stability of the wear protection layer according to the invention. As mentioned above, a uniform particle distribution improves the wear behavior, since the solid particles contribute significantly to the wear resistance and there are no large areas where particles are absent or only present in small numbers. Furthermore, the particles are not mainly present in the cracks, but in the so-called matrix, and they are particularly strongly bound to the matrix, so that they do not easily fall off the surface during operation.
[0041] The pH value of the electrolyte is preferably below -0.1, more preferably between -0.5 and -0.1. In a preferred embodiment of the present invention, the pH value is thus negative, i.e., HO + The concentration is less than 1 mol / l.Preferably a strong acid is used to adjust the pH of the electrolyte, preferably hydrochloric acid.
[0042] In a preferred embodiment of the method according to the invention, after the deposition step (b), the direction of the current is reversed in a further step (b1). In this step (b1), also called polarity reversal step, the crack formation is interrupted. Moreover, provided that the polarity reversal step is carried out for a certain time, the crack is enlarged in the polarity reversal step. It is particularly advantageous to interrupt the formation of the crack by reversing the polarity, so that new cracks are formed when the direction of the current is reversed again and a further wear protection layer is deposited. As a result, the incorporation of a polarity reversal step in the manufacturing process of the wear protection layer shortens the cracks in the layer. In contrast to long cracks, these short cracks better disperse the mechanical energy during deformation and increase the dimensional stability of the wear protection layer.
[0043] Therefore, the preferred method is (b1) After step (b), the direction of the current is reversed and the anodic current density is 1-30 A / dm 2 and The direction of the current is again reversed and step (b) above is performed again.
[0044] In the polarity reversal step (b1), the direction of the current is preferably reversed for at least 0.1 seconds, more preferably at least 1 second, even more preferably at least 10 seconds, most preferably at least 30 seconds, in particular 30 to 180 seconds. The current density in the polarity reversal step is preferably 1 to 30 A / dm 2 (amperes per square decimeter), preferably 2 to 20 A / dm 2 , particularly preferably 3 to 10 A / dm 2 It is.
[0045] In a preferred embodiment of the process according to the invention, the direction of the current is reversed at least 5 times, in particular at least 10 times, most preferably 10 to 30 times. In this way, several individual wear protection layers are deposited on top of each other, in each of which new cracks are formed. The multiple layers form a complete wear protection layer.
[0046] Preferably, the electrolyte contains an amount of iron (II) compound equivalent to 150-450 g / l of iron (II) chloride, in particular 200-400 g / l of iron (II) chloride. More preferably, the electrolyte contains less than an amount of iron (III) compound equivalent to 30 g / l of iron (III) chloride, in particular less than an amount of iron (III) compound equivalent to 10 g / l of iron (III) chloride. More preferably, the electrolyte contains less than 50 g / l of iron (III) salt, in particular less than 30 g / l of iron (III) salt.
[0047] In a preferred embodiment of the invention, the electrolyte comprises 20 g / l of a metal salt other than an iron salt, more preferably less than 10 g / l, most preferably less than 5 g / l of a metal salt other than an iron salt. In a preferred embodiment, the iron(II) compound in the electrolyte is FeCl2.
[0048] Preferred electrolytes are 150-500 g / l FeCl2 4H2O, in particular 200-45 g / l FeCl2 4H2O, It contains 1 to 40 g / l each of carbon particles and non-carbon solid particles, and particularly preferably one or more surface-active compounds having a pH value of 0 or less, preferably -0.1 or less.
[0049] The current density in the deposition step (b) is 10 to 80 A / dm 2 , preferably 20 to 70 A / dm 2 , most preferably 30 to 50 A / dm 2 It is.
[0050] The temperature of the electrolyte during the process according to the present invention is preferably below 50°C, more preferably between 15 and 45°C, and most preferably between 20 and 40°C.
[0051] The electrolyte also includes conventional electrolytic additives and catalysts to support the deposition of the iron layer, which may be present in the electrolyte in conventional amounts.
[0052] The duration of the deposition is selected depending on the desired thickness of the wear protection layer; the higher the current density and the longer the deposition is carried out, the thicker the layer. The deposition is preferably carried out for 5 to 240 minutes, in particular for 10 to 120 minutes. The polarity reversal step is advantageously carried out for 0.1 to 600 seconds, in particular for 5 to 200 seconds.
[0053] The wear protection layer according to the invention can be composed of several layers formed one after the other by repeating the deposition step (b) and the polarity reversal step (b1). When several layers are formed and the particles are deposited, a more uniform distribution of the cracks throughout the thickness of the coating can be achieved, since the cracks do not always form in the same place. The number of repetitions of steps (b) and (b1) is preferably 1 to 100 times, in particular 2 to 50 times, more preferably 5 to 30 times.
[0054] The thickness of the wear protection layer is preferably 10 to 600 μm, more preferably 20 to 400 μm, particularly preferably 30 to 200 μm, and most preferably 40 to 150 μm. The layer thickness is measured by measuring the height of the layer by cross-sectional polishing. If the surface is uneven, the layer thickness is measured at at least 5 points, preferably 6 to 10 points, and the arithmetic average value is calculated. This is the layer thickness of the wear protection layer, and is also called the average layer thickness.
[0055] In the process according to the invention, the amount of solid particles (carbon particles and non-carbon solid particles) contained in the electrolyte can vary within wide limits. It has proven advantageous if the electrolyte contains, independently of one another, 0.1 to 200 g / l of carbon particles and non-carbon solid particles respectively. Particularly preferred are 0.5 to 50 g / l, most preferably 2 to 30 g / l, respectively, based on the total amount of the electrolyte.
[0056] Depending on the density of the solid particles, the volume fraction of the solid particles relative to the total volume of the wear protection layer may vary in a slightly wider range than the weight fraction.
[0057] The average width (crack width) of the cracks in the wear protection layer is preferably 0.02 to 2 μm, more preferably 0.05 to 1.5 μm, even more preferably 0.1 to 1 μm, and most preferably 0.1 to 0.8 μm.
[0058] The crack width is measured by measuring the width of at least 10 randomly selected cracks approximately perpendicular to the direction of crack propagation and determining the arithmetic mean of these at least 10 measured crack widths. Microscopic images of surface grinding (running surface grinding) or cross-sectional grinding can be taken for the measurement, preferably cross-sectional grinding is used, as explained in more detail below. Basically, for example, in the case of running surface grinding, the surface is ground with sandpaper and then observed in a microscopic image to measure the crack width. The cracks differ in color tone from the rest of the wear protection layer, the cracks having a darker color tone.
[0059] Furthermore, the surface percentage of cracks on the surface of the wear protection layer can be measured using running surface polishing. To measure the surface area of the cracks, an area of at least 40 μm×40 μm is taken and the percentage of dark coloring, i.e., the percentage of cracks on the surface relative to the total area, is measured. This is done by randomly selecting three squares of at least 40 μm×40 μm and calculating the arithmetic mean of the three measurements. The value thus obtained is the surface percentage of cracks on the surface of the wear protection layer. The surface percentage of cracks on the surface of the wear protection layer according to the present invention is preferably 0.5 to 10%, more preferably 1 to 8%, in any case, relative to the entire surface of the wear protection layer.
[0060] The average crack density of the wear protection layer according to the invention is between 10 and 160 cracks / mm (millimeters). Preferred is an average density between 20 and 140 cracks / mm, more preferably between 30 and 120 cracks / mm, most preferably between 35 and 110 cracks / mm. To measure the average crack density, at least two cut lines at least 1 mm long are placed in different directions on a microscopic image of the surface grind (running surface grind), the crack density (number of cracks intersecting the lines) is measured by counting, and an arithmetic mean value is formed from these at least two counts.
[0061] In a preferred embodiment of the invention, in the polarity reversal step (b1) following the deposition of the wear protection layer, the cracks in the surface can be widened slightly again, which allows the surface area of the cracks in the surface to be higher, so that they can absorb more lubricant, in particular engine oil, and therefore achieve better sliding properties right from the start of use of the wear protection layer according to the invention, which allows the break-in behavior of the wear protection layer to be improved.
[0062] The depth of the cracks in the wear protection layer according to the invention can also be measured. As in the measurement of the crack width, a micrograph is made. For the depth of the cracks, the layer (including the substrate that may be coated) is cut perpendicular to the surface of the wear protection layer, and then the surface is polished with sandpaper in the same manner as in the production of the surface polish to produce a cross-sectional polish. The cross-sectional polish thus produced is observed under a microscope, and the depth of the cracks can be measured from the color intensity of the cracks by measuring the expansion in the direction perpendicular to the surface of the wear protection layer. The arithmetic mean value is measured from at least 10 cracks. The average crack depth of the wear protection layer according to the invention thus obtained is preferably 1 to 40 μm, particularly preferably 3 to 30 μm, more preferably 5 to 20 μm, and most preferably 7 to 15 μm.
[0063] The piston ring is preferably a piston ring having a base body, which has as surfaces an inner circumferential surface, a first flank surface, a second flank surface and a running surface. The wear protection layer according to the invention is applied to at least one of the surfaces, in particular to the running surface. The base body can be made of materials that are customary for piston rings, preferably the base body is made of cast iron or steel, for example chromium steel. Below or above the wear protection layer according to the invention there may be further layers, for example an adhesive layer between the base body and the wear protection layer and / or a running layer above the wear protection layer, which further improves the running-in behavior.
[0064] The present invention also relates to a piston ring obtained by said method according to the invention.
[0065] Preferably, it is a piston ring for an internal combustion engine, (a) a piston ring having a surface and having a wear protective layer of iron or iron alloy applied to said surface, said wear protective layer having cracks, said cracks having an average density of 10 to 160 cracks per mm of said wear protective layer, said iron or iron alloy having incorporated therein 0.2 to 15 weight percent carbon particles, based on the total weight of said wear protective layer, and 0.2 to 15 weight percent solid particles other than carbon particles, based on the total weight of said wear protective layer; and (b) heating the piston ring to 300 to 700°C; It is possible to obtain it through.
[0066] The present invention also relates to the use of the piston ring according to the invention in an internal combustion engine. For this purpose, the piston ring according to the invention is inserted into the piston of an internal combustion engine in a manner known to a person skilled in the art.
[0067] It is understood that the features mentioned above, and those to be described below, can be used not only in the combination shown, but also in other combinations or in separate positions, without going beyond the scope of the invention. [Brief description of the drawings]
[0068] [Figure 1] Figure 1 is a micrograph of abraded running surface of a wear protection layer according to the invention, said surface showing said cracks. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0069] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these.
[0070] Working Example Production of the iron layer according to the invention containing diamond particles and cubic boron nitride particles
[0071] An aqueous iron electrolyte solution of the following composition is provided: 300 g / l FeCl2 4H2O 5g / l polyfluorosulfonate 15g / l, diamond particles with diameter 0.2-0.7μm Cubic boron nitride, 15g / l, diameter 0.2-0.7μm pH value = -0.2 (adjusted with hydrochloric acid)
[0072] Into this iron electrolyte, 15 g / l of crystalline diamond particles with a particle size of 0.2-0.7 μm and 15 g / l of cubic boron nitride particles with a particle size of 0.2-0.7 μm are dispersed with stirring at 30° C. A piston ring made of chromium steel is pickled with hydrochloric acid, degreased, and a nickel layer with a thickness of about 2 μm is formed as a normal pretreatment. The piston ring is placed in the electrolyte and in the first step, it is first switched to the cathode and is charged with 40 A / dm 2 The iron layer is deposited at a current density of 4 A / dm for 5 min. In the second step, the polarity is reversed and the current density is increased to 4 A / dm. 2 The piston ring is switched to the anode at 350° C. for 45 seconds. This cycle, i.e., cathodic chrome plating for 5 minutes and anodic etching for 45 seconds, is repeated a total of 10 times to form an iron-diamond particle layer with a thickness of about 60 μm. The coated piston ring is then heated at a temperature of 400° C. for 1 hour.
[0073] To prepare a microscopic image of the surface, the piston ring is polished on a running surface, and to prepare a microscopic image of a cross section of the layer, the piston ring is polished on a cross section. To prepare the running surface, the surface of the piston ring is polished with SiC wet polishing paper with increasing abrasive grains (220 to 4000 grains), and polished with a 1 μm diamond suspension until the sample is not scratched and the contour is sharp.
[0074] To perform cross-sectional polishing, the piston ring is cut perpendicular to the running surface, and the cut surface is polished with SiC wet abrasive paper in the same manner as in the running surface polishing.
[0075] Thereafter, microscopic images of the traveling surface polishing and the cross-sectional polishing are taken.
[0076] The crack density was 50 cracks / mm.
[0077] Comparative Example 1 : Production of iron layers containing diamond particles without cracks in the layers
[0078] To produce a crack-free iron layer, deposition was performed according to example 1 of DE 19508419 using a conventional ferrous sulfate electrolyte (pH=1.4), which also contained a conventional wetting agent and diamond particles with diameters in the range of 0.2-0.7 μm.
[0079] As a result of the cross-section polishing and the running surface polishing, no cracks were found in the layer according to this comparative example.
[0080] The layers on the piston rings according to the examples and comparative examples were subjected to wear tests and measurements of dimensional stability.
[0081] A rig test was carried out to measure the wear, in which the piston ring was run on a cylinder with engine oil as a running partner at a stroke equivalent to a normal engine stroke for 23 hours, after which the amount of wear between the running surface of the piston ring and the running surface of the cylinder was measured.
[0082] The wear amount of the ring was 9 μm in the above-mentioned Example and 19 μm in the above-mentioned Comparative Example 1. The wear amount of the liner was 7.5 μm in the above-mentioned Example and 16.5 μm in the above-mentioned Comparative Example 1. Thus, in the Examples, both the wear amount of the ring, i.e., the wear amount of the wear protection layer according to the present invention, and the wear amount of the running partner, i.e., the running surface (liner) of the cylinder, are significantly reduced compared to Comparative Example 1.
[0083] To measure the dimensional stability, the piston ring was mechanically clamped and bent in both directions against its original shape until it broke. As a result, it was found that the wear protection layer according to the invention in the above example has a significantly higher dimensional stability than Comparative Example 1. This clearly shows the advantage of the wear protection layer according to the invention in terms of improved dimensional stability and reduced wear.
[0084] Comparative Example 2 : Production of iron layer containing diamond particles in the crack layer
[0085] An aqueous iron electrolyte solution of the following composition is provided: 300 g / l FeCl2 4H2O 5g / l polyfluorosulfonate 15g / l, diamond particles with diameter 0.2-0.7μm pH value = -0.2
[0086] Crystalline diamond particles with a particle size of 0.2-0.7 μm and a concentration of 15 g / l are dispersed in an iron electrolyte at 30° C. under stirring. A chromium steel piston ring is pickled with hydrochloric acid, degreased, and a nickel layer with a thickness of about 2 μm is formed as a conventional pretreatment. The piston ring is placed in the electrolyte and in the first step is first switched to the cathode and is supplied with a current of 40 A / dm. 2 The iron layer is deposited for 5 minutes at a current density of 4 A / dm. In the second stage, the polarity is reversed and 2 The piston ring is switched to the anode at a current density of 0.015 V for 45 seconds. This cycle, i.e., cathodic chrome plating for 5 minutes and anodic etching for 45 seconds, is repeated 10 times in total to form an iron-diamond particle layer with a thickness of about 60 μm. The coated piston ring is then heated at a temperature of 400° C. for 1 hour.
[0087] In order to create a microscopic image of the surface, the piston ring is subjected to running surface polishing as described above, and in order to create a microscopic image of the cross section of the layer, the piston ring is subjected to cross-sectional polishing. Then, microscopic images of the running surface polishing and cross-sectional polishing are created. From the cross-sectional polishing and running surface polishing, it can be seen that cracks have occurred in the layer according to this comparative example. The crack density was 80 cracks / mm.
[0088] The layer on the piston ring according to Comparative Example 2 was also subjected to a wear test. To measure the wear, a rig test as described above was carried out, in which the piston ring was run for 23 hours on a cylinder as a running partner, with engine oil and a stroke corresponding to a normal engine stroke. The amount of wear between the running surface of the piston ring and the running surface of the cylinder was then measured.
[0089] The amount of wear of the ring in Comparative Example 2 was 19.3 μm, and the amount of wear of the liner in Comparative Example 2 was 8.5 μm.
[0090] Overall, it was thus shown that both the wear of the ring of the embodiment according to the invention, i.e. the wear of the wear protection layer, and the wear of its running partner, i.e. the running surface (liner) of the cylinder, are improved compared to both Comparative Examples 1 and 2.
Claims
1. 1. A piston ring for an internal combustion engine, comprising: a surface; and a wear protection layer of iron or an iron alloy formed on said surface, said wear protection layer having cracks, said cracks having an average density of 10 to 160 cracks per mm of said wear protection layer, and 0.2 to 15 wt. % of carbon particles, based on a total weight of said wear protection layer, and 0.2 to 15 wt. % of solid particles that are not carbon particles, based on a total weight of said wear protection layer, embedded in said iron or iron alloy.
2. 2. The piston ring according to claim 1, characterized in that the ratio of the carbon particles and / or the solid particles that are not carbon particles located in the cracks to the total number of particles in the wear protection layer is 0.1% or less at each location.
3. 10. A piston ring according to claim 9, wherein the proportion of the sum of the carbon particles and the non-carbon solid particles located in the cracks relative to the total number of particles in the wear protection layer according to the invention is less than or equal to 0.05%.
4. 10. A piston ring according to claim 9, wherein the carbon particles are partially converted into iron-carbon compounds.
5. 10. A piston ring according to claim 9, wherein the average density of cracks is between 30 and 120 cracks per mm of the wear protection layer.
6. 10. A piston ring according to claim 9, wherein the average width of the cracks is between 0.05 and 1.5 μm.
7. 10. A piston ring according to claim 9, characterized in that the carbon particles and / or the non-carbon solid particles each have, independently of one another, an average particle size of 0.05 to 3 μm.
8. 10. A piston ring according to claim 9, characterized in that the carbon particles consist of diamond and / or graphite and / or the solid particles which are not carbon particles consist of tungsten carbide, chromium carbide, aluminium oxide, silicon carbide, silicon nitride, boron carbide and / or cubic boron nitride.
9. 4. A piston ring according to claim 1, characterized in that the solid particles which are not carbon particles consist of cubic boron nitride.
10. 5. A piston ring according to claim 1, characterized in that the iron alloy contains at least 90% by weight of iron, based on the total weight of the iron alloy.
11. (a) 100 to 500 g / l FeCl 2 and optionally a salt of a further metal, placing the piston ring in an aqueous electrolyte solution containing carbon particles and non-carbon solid particles, the aqueous electrolyte solution having a pH of 0 or less; (b) A wear protection layer of iron or iron alloy is 10 to 80 A / dm 2 galvanically depositing a cathode current density of 0.1g / mol / L on said piston ring; (c) drying the piston ring together with the wear protection layer; and (d) heating to 300-700° C.; The method for producing a piston ring according to any one of claims 1 to 10, comprising:
12. The method according to claim 11, characterized in that the aqueous electrolyte has a pH value of -0.1 or less.
13. After step (b), the direction of the current is reversed and the anodic current density is 1-30 A / dm 2 and The direction of the current is again reversed and step (b) is carried out again. The method according to claim 11 or 12.
14. A piston ring for an internal combustion engine, obtained by the manufacturing method according to any one of claims 11 to 13.
15. Use of a piston ring according to any one of claims 1 to 10 or 14 in an internal combustion engine.
Citation Information
Patent Citations
Piston ring for combustion engines with a wear-resistant coating
EP0731300A1
Sliding member and manufacture thereof
JP1985165389A
Piston ring
JP2000179692A
Iron-phosphorus electroplating bath and method
JP2007525600A
Structured chromium solid particle layer and method for producing the same
JP2011516726A