CATALYST FOR PRODUCING CARBON NANOTUBE AND METHOD FOR PRODUCING CARBON NANOTUBE

A catalyst with a specific metal composition addresses the solubility and dispersibility issues of carbon nanotubes, enabling their use as high-capacity secondary battery conductive materials with improved electrical conductivity and dispersibility.

JP2024537174AActive Publication Date: 2024-10-10KOREA KUMHO PETROCHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024520877
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-12
Filing Date
2022-03-02
Publication Date
2024-10-10
Estimated Expiration
2042-03-02

AI Technical Summary

Technical Problem

Conventional carbon nanotubes face issues with insufficient solubility and dispersibility, making them difficult to use as conductive materials for secondary batteries, and existing catalysts fail to achieve suitable dispersibility for high-capacity batteries.

Method used

A method involving the production of a catalyst with a specific metal composition (Co x :[M1,Zr] y :M2 z ) is used, where Co represents cobalt, M1 represents Al, Ca, Si, Ti, or Mg, Zr represents zirconium, and M2 represents W, V, or Mn, Mo, with controlled molar ratios, to enhance electrical conductivity and dispersibility.

Benefits of technology

The produced carbon nanotubes exhibit excellent electrical conductivity and dispersibility, improving the capacity and lifespan of secondary batteries, and can be easily used as a conductive material with enhanced solubility and dispersibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537174000001_ABST
    Figure 2024537174000001_ABST
Patent Text Reader

Abstract

One embodiment of the present specification provides a method for producing a catalyst for producing carbon nanotubes, comprising: (a) dissolving a metal precursor in a solvent to prepare a precursor solution; (b) spraying the precursor solution into a reactor and pyrolyzing it; and (c) obtaining a catalyst, the catalyst comprising a metal component represented by the following formula 1: <Expression 1> Co x :[M1,Zr] y :M2 z In the above formula, Co represents cobalt, an oxide or a derivative thereof, M1 represents at least one metal selected from Al, Ca, Si, Ti and Mg, an oxide or a derivative thereof, Zr represents zirconium, an oxide or a derivative thereof, M2 represents at least one metal selected from W, V, Mn and Mo, an oxide or a derivative thereof, and 0.2≦x / y≦2.6, 6≦x / z≦13.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present specification relates to a catalyst for producing carbon nanotubes and a method for producing carbon nanotubes. [Background technology]

[0002] As interest and importance of environmentally friendly energy and electric vehicles increases, the demand for secondary batteries is rapidly increasing. High-capacity secondary batteries for electric vehicles are required to have high energy density, long life, and low self-discharge rate, and in order to ensure such physical properties, it is essential to develop a conductive material with high electrical conductivity. The conductive material functions as a path for the movement of charges within the battery, and may be a carbon-based conductive material such as graphite, carbon black, graphene, carbon nanotubes, etc., and conductive carbon black has mainly been used in the past.

[0003] Carbon nanotubes are a material with a tube-like structure consisting of a hexagonal honeycomb lattice in which one carbon atom is bonded to three different carbon atoms, and are in the spotlight as a next-generation conductive material for secondary batteries due to their excellent electrical conductivity. When carbon nanotubes are used as a conductive material, the energy density and lifespan of secondary batteries can be improved and the size of the batteries can be reduced. However, conventional carbon nanotubes have poor solubility in and dispersibility within solvents, making them difficult to use as conductive materials for secondary batteries.

[0004] In order to solve these problems, various attempts have been made, such as physical post-treatment using a ball mill, a pin crusher, etc., but these have resulted in new problems of operational difficulties and increased costs. In addition, catalysts for producing carbon nanotubes having various combinations of metal components and physical properties have been developed, but it is difficult to realize suitable dispersibility as a conductive material for high-capacity secondary batteries. Therefore, there is a need to develop carbon nanotubes that have excellent electrical conductivity and dispersibility and can be used as a conductive material for secondary batteries, and a catalyst for producing the same. Summary of the Invention [Problem to be solved by the invention]

[0005] The present specification is intended to solve the problems of the prior art described above, and one object of the present specification is to provide a method for producing a catalyst for producing carbon nanotubes having excellent electrical conductivity and dispersibility.

[0006] Another object of the present specification is to provide a method for producing carbon nanotubes for use as a conductive material in secondary batteries, which have excellent electrical conductivity and dispersibility. [Means for solving the problem]

[0007] According to one embodiment, there is provided a method for producing a catalyst for producing carbon nanotubes, comprising: (a) dissolving a metal precursor in a solvent to produce a precursor solution; (b) spraying the precursor solution into a reactor and pyrolyzing it; and (c) obtaining a catalyst, the catalyst comprising a metal component represented by the following formula 1:

[0008] <Expression 1> Co x :[M1,Zr] y :M2 z In the above formula, Co represents cobalt, an oxide or a derivative thereof, M1 represents at least one metal selected from Al, Ca, Si, Ti and Mg, an oxide or a derivative thereof, Zr represents zirconium, an oxide or a derivative thereof, M2 represents at least one metal selected from W, V, Mn and Mo, an oxide or a derivative thereof, and 0.2≦x / y≦2.6, 6≦x / z≦13.

[0009] In one embodiment, the step (a) may include the steps of: (a1) dissolving a Co precursor, a Zr precursor, and at least one metal precursor selected from Al, Ca, Si, Ti, and Mg in a solvent to prepare a first precursor solution; and (a2) adding at least one metal precursor selected from W, V, Mn, and Mo to the first precursor solution to prepare a second precursor solution.

[0010] In one embodiment, in step (a2), the temperature of the first precursor solution may be less than 30°C.

[0011] In an embodiment, the step (a2) may include a step of stirring the metal precursor under a nitrogen atmosphere after adding the metal precursor.

[0012] In one embodiment, the step (b) may include the steps of (b1) spraying the precursor solution into a reactor together with air at 1 to 3 bar, and (b2) pyrolyzing the sprayed precursor solution at 600 to 1,000° C.

[0013] In one embodiment, in the above formula, 0.5≦x / y≦2.0 and 8≦x / z≦9.

[0014] According to another aspect, there is provided a method for producing carbon nanotubes, comprising the steps of (1) introducing the catalyst for producing carbon nanotubes produced by the above method into a chemical vapor deposition reactor, and (2) injecting a carbon-based gas and a carrier gas to synthesize carbon nanotubes.

[0015] In one embodiment, the chemical vapor deposition reactor may be a fluidized bed chemical vapor deposition reactor.

[0016] In one embodiment, the temperature in the chemical vapor deposition reactor may be 600 to 1,000°C.

[0017] In one embodiment, the carbon-based gas may be one selected from the group consisting of saturated or unsaturated hydrocarbons having 1 to 4 carbon atoms, carbon monoxide, benzene, and a mixture of two or more thereof.

[0018] In one embodiment, the carrier gas may be one selected from the group consisting of helium, nitrogen, argon, and a mixture of two or more thereof. Effect of the Invention

[0019] The catalyst for producing carbon nanotubes according to one aspect of the present specification may be applied to the synthesis of carbon nanotubes having excellent electrical conductivity and dispersibility.

[0020] In addition, the carbon nanotubes produced according to another embodiment of the present specification have excellent physical properties including electrical conductivity and dispersibility, and when used as a conductive material for a secondary battery, the capacity and life characteristics of the secondary battery can be improved.

[0021] The effects of one embodiment of this specification are not limited to the effects described above, and should be understood to include all effects that can be inferred from the configurations described in the detailed description or claims of this specification. [Brief description of the drawings]

[0022] [Figure 1] 1 and 2 are FE-SEM images of carbon nanotubes produced using a catalyst for producing carbon nanotubes according to an embodiment of the present disclosure. [Diagram 2] 1 and 2 are FE-SEM images of carbon nanotubes produced using a catalyst for producing carbon nanotubes according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, an embodiment of the present specification will be described with reference to the accompanying drawings. However, the description of the present specification may be embodied in various forms and is not limited to the embodiments described herein. In addition, in order to clearly describe an embodiment of the present specification in the drawings, parts that are not related to the description are omitted, and similar parts are designated by similar reference numerals throughout the specification.

[0024] Throughout the specification, when a part is described as being "connected" to another part, this includes not only the case where the part is "directly connected" to another part, but also the case where the part is "indirectly connected" to another part through another member in between. Furthermore, when a part is described as "comprising" a certain component, this does not mean that the other component is excluded, but that the part may further include the other component, unless otherwise specified.

[0025] When a range of numerical values ​​is given herein, unless a specific range is specifically stated, the values ​​have the precision of the significant figures provided in accordance with standard rules in chemistry for significant figures, for example, 10 includes a range of 5.0 to 14.9, and the number 10.0 includes a range of 9.50 to 10.49.

[0026] Hereinafter, an embodiment of the present specification will be described in detail with reference to the accompanying drawings.

[0027] Method for producing catalyst for producing carbon nanotubes A method for producing a catalyst for producing carbon nanotubes according to one embodiment of the present specification includes the steps of (a) dissolving a metal precursor in a solvent to produce a precursor solution, (b) spraying the precursor solution into a reactor and pyrolyzing it, and (c) obtaining a catalyst, the catalyst including a metal component represented by the following formula 1:

[0028] <Expression 1> Co x :[M1,Zr] y:M2 z In the formula, Co may represent cobalt, an oxide or a derivative thereof. The Co may act as a main catalyst in the catalyst for synthesizing carbon nanotubes. When carbon nanotubes are synthesized using the catalyst, the carbon nanotubes may grow into a structure having relatively good dispersibility.

[0029] In the above formula, M1 is at least one metal selected from Al, Ca, Si, Ti and Mg, or an oxide or derivative thereof, and Zr can represent zirconium, an oxide or derivative thereof.

[0030] The [M1, Zr] is an inert support that can support the main catalyst and the co-catalyst components. The [M1, Zr] indicates that M1 and Zr are contained in the same or different molar amounts, and for example, M1 may be contained in an amount 1.5 times or more, 2 times or more, 2.5 times or more, or 3 times or more the molar amount of Zr, but is not limited thereto.

[0031] The crystal structure of the catalyst is formed depending on the composition and ratio of the main catalyst, co-catalyst, and inert support, and as a result, the growth form and properties of the carbon nanotubes may change. For example, when a catalyst containing M1 and Zr is used as an inert support, it is possible to realize electrical conductivity applicable as a conductive material during the synthesis of carbon nanotubes and a level of solubility and dispersibility required for application to an electrode.

[0032] In the above formula, M2 may be at least one metal selected from W, V, Mn, and Mo, or an oxide or derivative thereof. The M2 may act as a co-catalyst, which is an active component that assists the action of the main catalyst in the catalyst for producing carbon nanotubes. The synthesis efficiency can be improved while maintaining the structural characteristics of the carbon nanotubes described above.

[0033] In the formula, 0.2≦x / y≦2.6 may be used. The x / y represents the molar fraction of the main catalyst relative to the support, and may be, for example, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, or a range between two of these values. If the x / y molar fraction is lower than the above range, the activity of the catalyst and the synthesis yield of carbon nanotubes therewith may decrease, and the dispersibility of the produced carbon nanotubes may decrease, making them unsuitable as a conductive material for secondary batteries. If the x / y molar fraction is higher than the above range, the support content is relatively low, which may reduce the durability of the catalyst, and the synthesized carbon nanotubes may exhibit an entangled structure, resulting in reduced BET specific surface area and powder resistance properties, and insufficient dispersibility and electrical conductivity, making them unsuitable as a conductive material for secondary batteries.

[0034] In the formula, 6≦x / z≦13 may be satisfied. The x / z represents the molar fraction of the main catalyst relative to the cocatalyst, and may be, for example, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, or a range between two of these values. If the x / z molar fraction is lower than the range, the growth of carbon nanotubes during the reaction may be hindered due to an excess of the cocatalyst, resulting in a decrease in the production amount, and the powder resistance of the produced carbon nanotubes may decrease, making them unsuitable as a conductive material for secondary batteries. If the x / z molar fraction is higher than the range, the growth activity of carbon nanotubes during the reaction may decrease due to a shortage of the cocatalyst, resulting in a decrease in the production amount, and the powder resistance of the synthesized carbon nanotubes may decrease, making them unsuitable as a conductive material for secondary batteries.

[0035] The step (a) may include preparing a precursor solution containing a precursor of a metal component contained in a catalyst for producing carbon nanotubes, and may include adding the metal precursor to a solvent and stirring the solvent under a nitrogen atmosphere.

[0036] The metal precursor may be, but is not limited to, one selected from the group consisting of nitrates, sulfates, alkoxides, chlorides, acetates, carbonates, and mixtures of two or more of the above metals.

[0037] In step (a), the solvent may be a polar solvent, and may be water, methanol, ethanol, propanol, isopropanol, butanol, or a mixture of two or more of these, for example, deionized water, but is not limited thereto. When deionized water is used as the solvent, impurities in the precursor solution can be minimized, and thus the purity of the catalyst finally produced can be improved. The improvement in the purity of the catalyst means an improvement in the purity of the carbon nanotubes.

[0038] The step (a) may include (a1) dissolving a Co precursor, a Zr precursor, and at least one metal precursor selected from Al, Ca, Si, Ti, and Mg in a solvent to prepare a first precursor solution, and (a2) adding at least one metal precursor selected from W, V, Mn, and Mo to the first precursor solution to prepare a second precursor solution. The order of steps (a1) and (a2) is not limited.

[0039] The step (a1) is a step of dissolving a precursor of a main catalyst and a precursor of a support in a solvent, and the first precursor solution may be, but is not limited to, an acidic solution.

[0040] The step (a2) is a step of adding a precursor of a co-catalyst, and the precursor of the co-catalyst is basic, but is not limited thereto.

[0041] In step (a2), the temperature of the first precursor solution may be less than 30° C. For example, the temperature may be 29.9° C., 29.5° C., 29° C., 28.5° C., 28° C., 27.5° C., 27° C., 26.5° C., 26° C., 25.5° C., 25° C., 24.5° C., 24° C., 23.5° C., 23° C., 22.5° C., 22° C., 21.5° C., 21° C., 20.5° C., 20° C., a range between any two of these values, or less than 20° C. If the temperature of the first precursor solution is more than 30° C., a side reaction due to heat may occur, causing precipitation, which may reduce the productivity and uniformity of the catalyst.

[0042] Step (a2) may include a step of stirring the metal precursor in a nitrogen atmosphere after the metal precursor is added. If the metal precursor is stirred in an atmosphere other than nitrogen, for example, in air, a precipitation phenomenon may occur due to a reaction between the acidic first precursor solution and the basic co-catalyst precursor, which may result in a decrease in productivity and uniformity of quality of the catalyst.

[0043] The step (b) may include the steps of (b1) spraying the precursor solution into a reactor together with air at 1 to 3 bar, and (b2) pyrolyzing the sprayed precursor solution at 600 to 1,000° C.

[0044] In step (b1), the precursor solution can be sprayed into the reactor to convert it into finer droplets in order to control the particle size, apparent density, etc. of the catalyst. The pressure at which the precursor solution is sprayed can be adjusted to within a range of 1 to 3 bar. If the spray pressure is less than 1 bar, the particle size, apparent density, etc. of the catalyst cannot be adjusted within a certain range, and as a result, the purity of the synthesized carbon nanotubes may decrease. If the spray pressure exceeds 3 bar, the particle size of the droplets becomes too small, and the obtained catalyst may aggregate together.

[0045] In the step (b2), the droplets are heated to evaporate the solvent and decompose the precursor to produce a catalyst. The temperature of the reactor may be 600 to 1,000°C. For example, the temperature may be 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1,000°C, or a range between two of these values. If the temperature of the reactor is lower than the range, the drying state of the catalyst is poor, and an additional process is required, which is economically disadvantageous, and the purity and physical properties of the produced carbon nanotubes may be reduced. If the temperature of the reactor is higher than the range, not only will excessive costs be incurred in constructing the equipment and facilities, which will lead to economic losses, but the catalyst performance may be reduced due to the formation of a solid solution or deformation of the crystal structure.

[0046] In the above formula, 0.5≦x / y≦2.0 and 8≦x / z≦9 may be satisfied, but are not limited thereto. When the catalyst is a catalyst containing four-component elements, if the ratio between each component satisfies the above range, it is easier to control the process conditions for producing the desired carbon nanotubes, but are not limited thereto.

[0047] The step (c) is a step of finally obtaining a catalyst for synthesizing carbon nanotubes, and the catalyst may be obtained in a powder form, but is not limited thereto.

[0048] The catalyst for producing carbon nanotubes produced by the above method may be used in a chemical vapor deposition method for synthesizing carbon nanotubes, for example, a fluidized bed chemical vapor deposition method or a fixed bed chemical vapor deposition method, but is not limited thereto.

[0049] The catalyst for producing carbon nanotubes produced by the above method may be applied to the production of carbon nanotubes having excellent electrical conductivity and dispersibility.

[0050] Method for producing carbon nanotubes According to another aspect of the present specification, a method for producing carbon nanotubes includes (1) introducing the catalyst for producing carbon nanotubes produced by the above method into a chemical vapor deposition reactor, and (2) injecting a carbon-based gas and a carrier gas to synthesize carbon nanotubes.

[0051] The chemical vapor deposition reactor may be, but is not limited to, a fluidized bed chemical vapor deposition reactor. Unlike conventional catalysts that can only be used in fixed bed chemical vapor deposition reactors due to issues such as apparent density, catalyst morphology, and strength, the catalyst may be used in both fixed bed chemical vapor deposition reactors and fluidized bed chemical vapor deposition reactors.

[0052] A fixed-bed chemical vapor deposition reactor can use a relatively wide variety of catalysts, but the productivity and uniformity of the synthesized carbon nanotubes are insufficient. A fluidized-bed chemical vapor deposition reactor is advantageous for mass production and the production of uniform carbon nanotubes, but the types of catalysts that can be used may be limited.

[0053] The temperature in the chemical vapor deposition reactor may be 600 to 1,000°C. For example, it may be 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1,000°C, or a range between two of these values. If the temperature of the reactor is too low, the growth of carbon nanotubes may be impossible or delayed. If the temperature of the reactor is too high, the synthesized carbon nanotubes may be thermally decomposed or may be unable to maintain their shape by bonding with each other.

[0054] The carbon-based gas may be one selected from the group consisting of saturated or unsaturated hydrocarbons having 1 to 4 carbon atoms, carbon monoxide, benzene, and a mixture of two or more of these, for example, ethylene, propylene, acetylene, or methane, but is not limited thereto.

[0055] The carrier gas may be, but is not limited to, one selected from the group consisting of helium, nitrogen, argon, and a mixture of at least two of them.

[0056] In the step (2), the carbon-based gas decomposed by high temperature heat may penetrate and saturate the catalyst composition, and carbon may precipitate and grow into carbon nanotubes, but is not limited thereto.

[0057] According to the above-mentioned production method, carbon nanotubes for use as conductive materials in secondary batteries can be produced in large quantities effectively.

[0058] The carbon nanotubes manufactured by the method may be an aggregate of carbon nanotubes grown on the catalyst. The carbon nanotube aggregate can be understood as a concept including both the catalyst composition and the carbon nanotubes. The carbon nanotube aggregate includes carbon nanotubes grown from the above-mentioned catalyst seed. The growth pattern and purity of the carbon nanotubes are determined by the catalyst, and when applied as a conductive material, the electrical conductivity, dispersibility, solubility, etc. may change. Therefore, even if the diameter, length, purity, etc. of carbon nanotubes are similar, if they are manufactured using catalysts with different compositions, the properties such as dispersibility, solubility, electrical conductivity, etc. may change.

[0059] In one example, the carbon nanotubes in the carbon nanotube aggregate may be linear, curved, or a mixture thereof, and each of the carbon nanotubes may be a single-walled, double-walled, or multi-walled carbon nanotube.

[0060] In one example, the carbon nanotube aggregate may include a bundle of carbon nanotubes in which a plurality of carbon nanotubes are aggregated together. The bundle of carbon nanotubes may be linear, curved, or a mixture thereof.

[0061] In one example, the carbon nanotube aggregate may include multi-walled carbon nanotubes having an average wall number of 3 to 20. The carbon nanotube aggregate may embody properties required as a conductive material for secondary batteries while using multi-walled carbon nanotubes that are known to have relatively low conductivity compared to single-walled carbon nanotubes.

[0062] The purity of the carbon nanotubes produced by the method may be 90% or more, for example, but not limited to, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or more. If the purity is outside the above range, the electrical conductivity may be insufficient, or impurities may react inside the battery, causing a safety accident.

[0063] The BET specific surface area of ​​the carbon nanotube aggregate produced by the above method is 130 to 260 m 2 For example, 130m 2 / g, 140m 2 / g, 150m 2 / g, 160m 2 / g, 170m 2 / g, 180m 2 / g, 190m 2 / g, 200m 2 / g, 210m 2 / g, 220m 2 / g, 230m 2 / g, 240m 2 / g, 250m 2 / g, 260m 2 / g or a range between two of these values. If the BET specific surface area is smaller than the range, the electrical conductivity decreases and the conductive material becomes unsuitable for a secondary battery, and if it is larger than the range, the dispersibility may decrease.

[0064] The bulk density of the carbon nanotube aggregate produced by the method may be 0.005 to 0.10 g / ml. For example, it may be 0.005 g / ml, 0.01 g / ml, 0.02 g / ml, 0.03 g / ml, 0.04 g / ml, 0.05 g / ml, 0.06 g / ml, 0.07 g / ml, 0.08 g / ml, 0.09 g / ml, 0.10 g / ml, or a range between two of these values. The apparent density may be measured using powdered carbon nanotubes. If the apparent density is out of the above range, excessive scattering of carbon nanotubes may occur, or dispersibility and solubility may be insufficient when preparing a conductive material slurry.

[0065] The average fiber diameter of the carbon nanotubes produced by the method may be 3 to 30 nm. For example, it may be 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, 30 nm, or a range between two of these values. If the average fiber diameter is out of the above range, the synthesized carbon nanotubes have a structural problem or the desired carbon nanotube properties are not sufficiently realized.

[0066] The carbon nanotubes produced by the method may have an average powder resistivity of 0.005 to 0.045 Ω·cm, for example, 0.005 Ω·cm, 0.006 Ω·cm, 0.007 Ω·cm, 0.008 Ω·cm, 0.009 Ω·cm, 0.01 Ω·cm, 0.011 Ω·cm, 0.012 Ω·cm, 0.013 Ω·cm, 0.014 Ω·cm, 0.015 Ω·cm, 0.016 Ω·cm, 0.017 Ω·cm, 0.018 Ω·cm, 0.019 Ω·cm, 0.02 Ω·cm, 0.021 Ω·cm, 0.022 Ω·cm, 0.023 Ω·cm, 0.024 Ω·cm, 0.025 Ω·cm, 0.026 Ω·cm, 0.028 Ω·cm, 0.029 Ω·cm, 0.030 Ω·cm, 0.031 Ω·cm, 0.032 Ω·cm, 0.033 Ω·cm, 0.034 Ω·cm, 0.035 Ω·cm, 0.036 Ω·cm, 0.037 Ω·cm, 0.038 Ω·cm, 0.039 Ω·cm, 0.040 Ω·cm, 0.041 Ω·cm, 0.042 Ω·cm, 0.043 Ω·cm, 0.044 Ω·cm, 0.045 Ω·cm, 0.046 Ω·cm, 0.047 Ω·cm, 0.048 Ω·cm, 0 Ω·cm, 0.027Ω·cm, 0.028Ω·cm, 0.029Ω·cm, 0.03Ω·cm, 0.031Ω·cm, 0.032Ω·cm, 0.033Ω·cm, 0.034Ω·cm, 0.035Ω·cm, 0.036Ω·cm, 0.037Ω·cm, 0.038Ω·cm, 0.039Ω·cm, 0.04Ω·cm, 0.041Ω·cm, 0.042Ω·cm, 0.043Ω·cm, 0.044Ω·cm, 0.045Ω·cm, or a range between two of these values. If the powder resistance is higher than the range, the electrical conductivity decreases and the powder becomes unsuitable as a conductive material for a secondary battery.

[0067] Among the methods for analyzing the structure of the carbon nanotubes, Raman spectroscopy for analyzing the surface state of the carbon nanotubes may be usefully used. The term "Raman spectroscopy" as used herein refers to a spectroscopy method for determining the molecular vibration frequency in the Raman effect, which is a phenomenon in which scattered light having a difference in the number of molecular vibrations occurs when monochromatic excitation light such as laser light is irradiated, and the crystallinity of the carbon nanotubes can be quantified and measured through such Raman spectroscopy.

[0068] The Raman spectrum of the carbon nanotube has a wave number of 1580±50 cm -1 The peak in the region is called the G band, which is the sp 2 This peak indicates a bond and indicates carbon crystals without structural defects. Also, the wave number of 1360±50 cm-1 The peak in the region is called the D band, which is the sp band of carbon nanotubes. 3 The peaks indicate bonds and may indicate carbon containing structural defects.

[0069] Furthermore, the peak values ​​of the G band and the D band are respectively I G and I D The ratio between the two, the Raman spectroscopic intensity ratio (I G / I D In other words, a higher Raman spectroscopic intensity ratio means fewer structural defects in the carbon nanotube, and therefore, when a carbon nanotube having a high Raman spectroscopic intensity ratio is used, better electrical conductivity can be realized.

[0070] The Raman spectroscopic intensity ratio (I G / I D ) may be 0.5 to 2.0. For example, it may be 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, or a range between two of these values. If the Raman spectroscopic intensity ratio is out of the above range, the dispersibility of the carbon nanotubes decreases, making it difficult to realize uniform electrical conductivity when applied to an electrode.

[0071] The surface resistance of the carbon nanotubes produced by the method may be 100 to 250 Ω / sq. For example, it may be 100 Ω / sq, 110 Ω / sq, 120 Ω / sq, 130 Ω / sq, 140 Ω / sq, 150 Ω / sq, 160 Ω / sq, 170 Ω / sq, 180 Ω / sq, 190 Ω / sq, 200 Ω / sq, 210 Ω / sq, 220 Ω / sq, 230 Ω / sq, 240 Ω / sq, 250 Ω / sq, or a range between two of these values. If the surface resistance is higher than the range, the electrical conductivity decreases and the material is not suitable as a conductive material for a secondary battery.

[0072] The carbon nanotubes produced by the above method have excellent physical properties including electrical conductivity and dispersibility, and when used as a conductive material for a secondary battery, the capacity and life characteristics of the secondary battery can be improved, and thus the carbon nanotubes can be applied to the production of high-capacity secondary batteries with high energy density and low self-discharge rate.

[0073] Unlike conventional carbon nanotubes, which are difficult to use as conductive materials due to insufficient solubility during preparation of electrode material slurry, the carbon nanotube aggregates are easy to prepare into a slurry and have excellent dispersibility. The conductive material for secondary batteries can suppress safety accidents caused by localized current concentration.

[0074] The carbon nanotubes produced by the method have superior powder resistance compared to carbon black, which is used as a conventional conductive material for secondary batteries, and can increase the energy density even with a small amount of use, thereby improving the charging speed and efficiency of the secondary battery. In addition, when the conductive material for secondary batteries is used, sufficient current characteristics can be obtained even if a relatively large amount of electrode material is included.

[0075] The examples of the present specification will be described in more detail below. However, the following experimental results are only representative experimental results among the above examples, and the scope and content of the present specification should not be construed as being narrowed or limited by the examples, etc. The respective effects of some embodiments of the present specification that are not explicitly described below will be specifically described in the corresponding parts.

[0076] Examples 1 to 6 and Comparative Examples 1 to 4 Co(NO3)3·6H2O, Al(NO3)3·9H2O, ZrO(NO3)2·2H2O and deionized water were added to a reactor and stirred under nitrogen atmosphere to prepare a first precursor solution. NH4VO3 was added to the first precursor solution, which was kept at a temperature of less than 30°C, and stirred under nitrogen atmosphere to prepare a second precursor solution. At this time, each precursor was added in the required amount according to the catalyst composition in Table 1 below. The second precursor solution was sprayed into a spray pyrolysis reactor with air at a rate of 3 L / hr and pyrolyzed to obtain a catalyst composition. The air spray pressure was set to 1-3 bar, and the temperature in the spray pyrolysis reactor was set to 750°C.

[0077] [Table 1]

[0078] Comparative Example 5 A catalyst composition was prepared in the same manner and with the same composition as in Example 1, except that the temperature of the first precursor solution was maintained at 50°C.

[0079] Comparative Example 6 A catalyst composition was prepared in the same manner and by the same method as in Example 1, except that NH4VO3 was added to the first precursor solution and stirred under air.

[0080] Manufacturing Example The catalyst compositions according to the examples and comparative examples were introduced into a fluidized bed chemical vapor deposition reactor having a diameter of 350 mm, and the temperature inside the reactor was raised to and maintained at 700-800° C. under a nitrogen atmosphere. Then, a mixed gas of nitrogen and ethylene was supplied at a rate of 150 L / min, and the reaction was carried out for 50 minutes to synthesize carbon nanotubes.

[0081] Experimental Example 1 The structure, fiber diameter, and number of walls of the carbon nanotubes synthesized in the above Preparation Example were confirmed through FE-SEM images, and the BET specific surface area and powder resistivity were measured and are shown in Table 2 below. The BET specific surface area was measured using a TriStar II 3020 device (Micrometritics Co., Ltd.). For the powder resistivity, the bulk density was measured using a HPRM-FA2 device (Hantec Co., Ltd.), and the volume resistivity was calculated when the density was 0.65±0.01g / ml using the trend line of volume resistivity (Ω·cm) according to the apparent density.

[0082] 1 and 2 are FE-SEM images of carbon nanotubes synthesized according to Preparation Examples using the catalyst compositions of Example 6 and Comparative Example 1, respectively.

[0083] [Table 2]

[0084] It was confirmed that the carbon nanotubes synthesized using the catalyst compositions of Examples 1 to 6 exhibit a bundle-like structure as shown in FIG. 1, have excellent BET specific surface area and powder resistance, and are applicable as conductive materials for secondary batteries.

[0085] The carbon nanotubes synthesized using the catalyst composition of Comparative Example 1, which had a high Co / (Al+Zr) molar fraction of 3.18, exhibited an entangled structure as shown in Figure 2, and had lower BET specific surface area and powder resistivity properties than the Examples.

[0086] The carbon nanotubes synthesized using the catalyst composition of Comparative Example 2, which had a low Co / (Al+Zr) molar fraction of 0.18, had a very high BET specific surface area and excellent powder resistance, but the high BET specific surface area reduced dispersibility during dispersion production.

[0087] The carbon nanotubes synthesized using the catalyst composition of Comparative Example 3, which had a low Co / V molar fraction of 3.45, had a reduced production yield due to the excess of the active component, the cocatalyst, which hindered the growth of carbon nanotubes during the reaction, and the powder resistivity of the carbon nanotubes synthesized in the Examples was lower.

[0088] The carbon nanotubes synthesized using the catalyst composition of Comparative Example 4, which had a high Co / V molar fraction of 17.29, had a reduced production yield due to a lack of the active component, the cocatalyst, which reduced the growth activity of the carbon nanotubes during the reaction, and the powder resistivity of the carbon nanotubes synthesized in the Examples was lower.

[0089] Experimental Example 2 In order to evaluate the electrical conductivity and dispersibility of the carbon nanotubes synthesized in the above Preparation Examples, the surface resistance of the carbon nanotubes was measured and the dispersion was evaluated. The results are shown in Table 3 below.

[0090] The surface resistance of carbon nanotubes was measured using a 4-point probe after bar coating. Carbon nanotube dispersion was evaluated by adding carbon nanotubes to N-methylpyrrolidone (NMP) at 5% by weight and using a bead mill. When the viscosity did not decrease any more during preparation using a Rotating Ring Mill (RRG), the dispersion evaluation was completed and the preparation time was measured. If the carbon nanotubes did not disperse even after 48 hours of preparation, it was evaluated as not dispersible.

[0091] [Table 3]

[0092] It was confirmed that the carbon nanotubes synthesized using the catalyst composition of Example 6 had low surface resistance, excellent electrical conductivity, and high dispersibility.

[0093] The carbon nanotubes synthesized using the catalyst composition of Comparative Example 1 exhibited an intangled structure. Although the time required for producing the dispersion was short, the dispersion was not properly performed, and the electrical conductivity was lower than that of the Examples.

[0094] The carbon nanotubes synthesized using the catalyst composition of Comparative Example 2 did not disperse as the BET specific surface area became very high, and production of a 5% dispersion failed.

[0095] Experimental Example 3 In the above examples and comparative examples, the solution precipitation phenomenon according to the second precursor solution preparation method was evaluated and the results are shown in Table 4 below.

[0096] [Table 4]

[0097] Comparing Example 1 with Comparative Example 5, when the temperature of the first precursor solution was 30° C. or higher, a side reaction occurred due to heat, resulting in a precipitation phenomenon.

[0098] Comparing Example 1 and Comparative Example 6, it was confirmed that when the second precursor solution is prepared under a nitrogen atmosphere, the precipitation phenomenon that occurs during the reaction between the acidic first precursor solution and the basic NH4VO3 precursor can be suppressed.

[0099] It has been found that when solution precipitation occurs, the productivity and quality uniformity of the catalyst composition are significantly reduced.

[0100] The above description of the present specification is for illustrative purposes only, and a person having ordinary skill in the art to which one embodiment of the present specification belongs can easily understand that the present specification can be easily modified into other specific forms without changing the technical ideas and essential features described in the present specification. Therefore, it should be understood that the above-described embodiments are illustrative in all respects and are not limiting. For example, each component described as a single type may be implemented in a distributed manner, and similarly, each component described as being distributed may be implemented in a combined form.

[0101] The scope of this specification is defined by the claims set forth below, and all modifications and variations derived from the meaning and scope of the claims and their equivalent concepts should be construed as being included in the scope of this specification.

Claims

1. (a) dissolving a metal precursor in a solvent to prepare a precursor solution; (b) spraying the precursor solution into a reactor and pyrolyzing it; (c) obtaining a catalyst, The catalyst comprises a metal component represented by the following formula 1: <Formula 1> Co x :[M1, Zr] y :M2 z In the above formula, Co represents cobalt, an oxide or a derivative thereof; M1 is at least one metal selected from Al, Ca, Si, Ti, and Mg, or an oxide or derivative thereof; Zr represents zirconium, an oxide or a derivative thereof; M2 is at least one metal selected from W, V, Mn, and Mo, or an oxide or derivative thereof; 0.2≦x / y≦2.6, and 6≦x / z≦13.

2. The step (a) comprises: (a1) preparing a first precursor solution by dissolving a Co precursor, a Zr precursor, and at least one metal precursor selected from Al, Ca, Si, Ti, and Mg in a solvent; (a2) adding at least one metal precursor selected from W, V, Mn, and Mo to the first precursor solution to prepare a second precursor solution.

3. The method of claim 2, wherein in step (a2), the temperature of the first precursor solution is less than 30°C.

4. The method of claim 2, wherein in step (a2), the metal precursor is added and then stirred under a nitrogen atmosphere.

5. The step (b) comprises: (b1) spraying the precursor solution into a reactor together with 1-3 bar of air; 2. The method of claim 1, further comprising: (b2) pyrolyzing the sprayed precursor solution at 600 to 1,000° C.

6. 2. The method for producing a catalyst for producing carbon nanotubes according to claim 1, wherein, in the formula, 0.5≦x / y≦2.0 and 8≦x / z≦9.

7. (1) Putting the catalyst for producing carbon nanotubes prepared according to claim 1 into a chemical vapor deposition reactor; (2) injecting a carbon-based gas and a carrier gas to synthesize carbon nanotubes.

8. The method of claim 7, wherein the chemical vapor deposition reactor is a fluidized bed chemical vapor deposition reactor.

9. 8. The method of claim 7, wherein the temperature in the chemical vapor deposition reactor is 600 to 1,000.degree.

10. 8. The method for producing carbon nanotubes according to claim 7, wherein the carbon-based gas is one selected from the group consisting of saturated or unsaturated hydrocarbons having 1 to 4 carbon atoms, carbon monoxide, benzene, and a mixture of two or more of these.

11. 8. The method for producing carbon nanotubes according to claim 7, wherein the carrier gas is one selected from the group consisting of helium, nitrogen, argon, and a mixture of two or more thereof.

Citation Information

Patent Citations

  • Carbon nano tube array and preparation method thereof as well as application of carbon nano tube array in preparation of super capacitor

    CN102502580A

  • Catalyst for manufacturing carbon nanotubes and carbon nanotubes manufactured using the same

    JP2016502466A

  • Carbon nanotube dispersion liquid and its use

    JP2020011873A

  • Catalysts for the mass production of multiwalled carbon nanotubes

    JP2020508866A

  • Process For Preparing Catalyst Composition For The Synthesis Of Carbon Nanotube With High Yields Using The Spray Pyrolysis Method

    US20120040186A1