Pyrolysis method for waste plastics using waste resources
The use of a slag composition with calcium, iron, silicon, and magnesium oxides in the pyrolysis of waste plastics effectively converts chlorine into stable metal chlorides, addressing equipment corrosion and product deterioration issues, and achieving low impurity pyrolysis oil production.
Patent Information
- Application Number
- JP2024522577
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-20
- Filing Date
- 2022-10-19
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Waste plastic pyrolysis oil contains high levels of impurities, particularly chlorine, which leads to equipment corrosion, abnormal reactions, and product deterioration during refinery processing, necessitating costly pretreatment and frequent adsorbent replacement.
A pyrolysis process using a slag composition comprising calcium oxide, iron oxide, silicon oxide, and magnesium oxide, with specific ratios, to convert chlorine into stable metal chlorides, reducing impurity content without additional post-treatment.
Produces pyrolysis oil with low chlorine levels suitable for refinery processes, minimizing equipment corrosion and reducing the need for frequent adsorbent replacement, while enhancing process efficiency and simplifying operations.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for pyrolysis of waste plastics using waste resources. [Background technology]
[0002] Oil (waste oil) produced by the cracking and pyrolysis reactions of waste materials such as waste plastic pyrolysis oil contains a large amount of impurities originating from the waste. If it is used as fuel, there is a risk of emitting air pollutants such as SOx and NOx. In particular, there is a problem that the Cl component is converted into HCl during the high-temperature treatment process, which can cause corrosion of equipment, and is emitted.
[0003] Conventionally, Cl has been removed by converting it into HCl using a hydrotreating (HDT) process that utilizes refinery technology. However, because waste oils such as waste plastic pyrolysis oil contain high amounts of Cl, there have been reports of equipment corrosion, abnormal reactions, and deterioration of product properties due to the generation of excess HCl in the HDT process, making it difficult to introduce waste oil that has not been pretreated into the HDT process.
[0004] In addition, the technology to reduce Cl, N, etc. using adsorbents such as CaO or waste FCC catalyst (E-cat) requires feedstock oil with an extremely low impurity content, so there is a problem in that an adsorbent with a very high content (2 to 50 times the amount of the oil to be refined) must be used. In addition, since substances that have adsorbed Cl, N, etc. lose their adsorption capacity, there is a problem in that the inactivated adsorbent must be continually replaced. Therefore, a waste oil treatment technology is needed that can reduce the impurity (Cl) content to a level that allows the waste oil to be introduced into the refinery process. Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention aims to provide a technology for reducing impurities (Cl) during pyrolysis using steel slag, a waste resource, instead of CaO or E-cat, which are commonly used in the field of waste plastic pyrolysis technology.
[0006] Meanwhile, about 70% of blast furnace slag from steel slag is recycled as a high-value added cement raw material, but the entire amount of steel slag is simply landfilled for use as embankment or road aggregate. Steel slag has a chemical composition that is significantly different from that of blast furnace slag, making it impossible to apply it to cement, and the high free lime (Free-CaO) contained in steel slag limits its use as concrete aggregate. Therefore, the present invention aims to remove impurities during the thermal decomposition of waste plastics by utilizing the unreacted free lime and metal compounds in steel slag. [Means for solving the problem]
[0007] One embodiment of the present invention provides a method for producing waste plastic pyrolysis oil, which includes a pyrolysis step of feeding waste plastics and a slag composition into a pyrolysis reactor to produce pyrolysis oil, and the slag composition contains, relative to the total weight, 30 to 60 wt % calcium oxide, 5 to 30 wt % iron oxide, and 0.5 to 30 wt % of at least one selected from silicon oxide, aluminum oxide, and magnesium oxide.
[0008] In one embodiment, the slag composition may satisfy the following formulas 1 and 2:
[0009] [Formula 1] 1<Iron oxide (wt%) / Silicon oxide (wt%)<3
[0010] [Formula 2] 3<Iron oxide (wt%) / Magnesium oxide (wt%)<5
[0011] In one embodiment, the slag composition may include up to 5 wt. % aluminum oxide, based on the total weight of the slag composition. In one embodiment, the slag composition may include up to 20 wt. % silicon oxide, based on the total weight of the slag composition.
[0012] The pyrolysis step may be carried out at a temperature of 400 to 600° C. in a non-oxidizing atmosphere. The waste plastic may be household waste plastic containing 3% by weight or more of PVC (polyvinyl chloride) based on the total weight.
[0013] The slag composition is 0.5 to 10 m 2 / g. The slag composition may have a particle size of 5 to 200 μm.
[0014] The slag composition may have a compressive strength of 100 to 500 MPa. The slag composition has a content of 1.5 to 5 g / cm 2 The density may be The pyrolysis oil may contain less than 100 ppm chlorine by total weight. Effect of the Invention
[0015] The present invention can produce pyrolysis oil having a low impurity content that is applicable to refinery processes after pyrolysis of waste plastic raw materials without performing a separate post-treatment process.
[0016] In addition, impurities can be removed during the thermal decomposition process of waste plastics by utilizing the unreacted free lime (Free CaO) and metal compounds in steel slag. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Unless otherwise defined, all terms (including technical and scientific terms) used herein may be used as commonly understood by those having ordinary skill in the art to which the present invention belongs. Throughout the specification, when a part is described as "comprising" a certain component, this means that it may further include other components, not excluding other components, unless otherwise specified. In addition, the singular form includes the plural form unless otherwise specified in the text.
[0018] In this specification, "A to B" means "A or more and B or less" unless otherwise specified. In addition, "A and / or B" means at least one selected from the group consisting of A and B, unless otherwise specified.
[0019] One embodiment of the present invention provides a method for producing waste plastic pyrolysis oil. The method includes a pyrolysis step of producing pyrolysis oil by feeding waste plastic and a slag composition into a pyrolysis reactor. Thus, the present invention makes it possible to remove chlorine from the pyrolysis oil to a very high level without performing a separate post-treatment process after pyrolysis of the waste plastic raw material.
[0020] The pyrolysis process may involve feeding waste plastic into a reactor and heating it to produce a pyrolysis gas phase, a pyrolysis liquid phase containing oil and wax, and a solid phase containing pyrolysis char. Specifically, the pyrolysis process may be carried out at a temperature of 400 to 600°C in a non-oxidizing atmosphere.
[0021] The non-oxidizing atmosphere is an atmosphere in which the waste plastic does not oxidize (burn), and may be, for example, an atmosphere in which the oxygen concentration is adjusted to 1% by volume or less, an inert gas atmosphere such as nitrogen, water vapor, carbon dioxide, and argon, or a negative pressure atmosphere.
[0022] When the thermal decomposition temperature is 400°C or higher, fusion of chlorine-containing plastics can be prevented, and when the thermal decomposition temperature is 600°C or lower, the chlorine in the waste plastics can remain in the slag composition in the form of CaCl2 or the like, which is preferable.
[0023] The waste plastic may include at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), and polystyrene (PS). The waste plastic may include organic chlorine (organic Cl) and inorganic chlorine (inorganic Cl). Waste oil generated by the cracking and pyrolysis reaction of waste plastic, such as waste plastic pyrolysis oil, contains a large amount of impurities originating from the waste plastic. Therefore, when using the waste oil, there is a risk of discharging air pollutants, and in particular, there is a problem that organic chlorine and inorganic chlorine components are converted to HCl during high-temperature treatment and discharged, so it is necessary to pretreat the waste oil to remove the impurities of the chlorine components.
[0024] The waste plastics can be divided into household waste plastics and industrial waste plastics. Domestic waste plastics are plastics containing PVC, PS, PET, PBT, etc. other than PE and PP, and in the present invention, it can mean mixed waste plastics containing 3% by weight or more of PVC together with PE and PP. The chlorine content of the waste plastics may be, for example, 1,000 ppm or more, 3,000 ppm or more, or 5,000 to 15,000 ppm.
[0025] The slag composition contains, based on the total weight, 30 to 60 wt % of calcium oxide, 5 to 30 wt % of iron oxide, and 0.5 to 30 wt % of at least one selected from silicon oxide, aluminum oxide, and magnesium oxide.
[0026] The slag composition may be steel slag, which is a by-product produced when producing pig iron and steel in a steelworks, and the steel slag may include blast furnace slag and steelmaking slag, and the steel slag is preferably steelmaking slag. Blast furnace slag is widely used as an admixture for concrete, blast furnace slag cement, and the like. Steelmaking slag may include converter slag, which is a by-product of the converter process in which crude steel is produced from molten pig iron produced in a blast furnace, and electric furnace slag, which is a by-product of melting scrap in an electric furnace to produce crude steel. Steelmaking slag has a chemical composition that is significantly different from blast furnace slag, making it impossible to apply it to cement, and the use of steelmaking slag as a concrete aggregate is limited due to the high free lime contained in the steelmaking slag. Unreacted free lime (Free CaO) is a source of environmental pollution and a compound that limits the uses of slag. The present invention utilizes the unreacted free lime (Free CaO) and metal compounds in steelmaking slag to remove impurities contained in the raw materials during the thermal decomposition process of waste plastics.
[0027] Specifically, the slag composition may contain 40-60 wt%, 35-55 wt%, or 40-50 wt% calcium oxide, 5-30 wt%, 10-25 wt%, or 15-20 wt% iron oxide, 5-20 wt%, 7-18 wt%, or 10-15 wt% silicon oxide, 0-10 wt%, 0-5 wt%, or 0.5-3 wt%, aluminum oxide, and / or 0-15 wt%, 1-10 wt%, or 2-8 wt% magnesium oxide. Steelmaking slag is a by-product of the ironmaking process, and the content of each component may vary by ±5% depending on the operating conditions. When the chemical composition range of the slag composition is satisfied, the chlorine in the waste plastic and the metal oxide can react to form various metal chlorides (Fe2Cl3, CaCl2, MgCl2, SiCl4, etc.), which can improve the problem that CaCl2 and the like dissociate into chlorine again even under high temperature conditions of the pyrolysis reaction. In contrast, when conventional CaO or spent FCC catalyst is used alone, one type of chlorine reaction product such as CaCl2 is formed, which makes the chlorine dissociation reaction more likely to proceed, and a large amount of decomposed HCl is trapped in the pyrolysis oil or may be re-reacted to produce organic chlorine (organic Cl).
[0028] In one embodiment, the slag composition may satisfy the following formulas 1 and 2:
[0029] [Formula 1] 1<Iron oxide (wt%) / Silicon oxide (wt%)<3
[0030] [Formula 2] 3<Iron oxide (wt%) / Magnesium oxide (wt%)<5
[0031] In the above formulas 1 and 2, iron oxide (wt%), silicon oxide (wt%), and magnesium oxide (wt%) refer to the weight percentages of iron oxide, silicon oxide, and magnesium oxide, respectively, relative to the total weight of the slag composition.
[0032] When the slag composition satisfies the formulas 1 and 2, the effect of reacting with chlorine to form metal chlorides is significantly improved, and the chlorine in the generated waste plastic pyrolysis oil can be minimized. Specifically, the formula 1 may be 1<iron oxide (wt%) / silicon oxide (wt%)<2.7, and the formula 2 may be 3.3<iron oxide (wt%) / magnesium oxide (wt%)<4.7. More specifically, the formula 1 may be 1.5<oxide (wt%) / silicon oxide (wt%)<2.5, and the formula 2 may be 3.5<oxide (wt%) / silicon oxide (wt%)<4.5.
[0033] In one embodiment, the slag composition may contain 5 wt% or less of aluminum oxide based on the total weight of the slag composition. Specifically, the slag composition may contain 4 wt% or less of aluminum oxide, more specifically, the slag composition may contain 3 wt% or less of aluminum oxide. When the above range is satisfied, the chlorine removal effect can be further improved.
[0034] In one embodiment, the slag composition may contain 20 wt% or less of silicon oxide based on the total weight of the slag composition. Specifically, the slag composition may contain 18 wt% or less of silicon oxide, more specifically, the slag composition may contain 15 wt% or less of silicon oxide. When the above range is satisfied, the chlorine removal effect can be further improved.
[0035] The slag composition may have a particle size of 5 to 200 μm, specifically 30 to 150 μm, or 60 to 80 μm.
[0036] The slag composition is 0.5 to 10 m 2 / g, specifically, 1 to 8 m 2 / g, or 3 to 5 m 2The slag composition of the present invention may have a BET specific surface area of 100 nm to 100 nm / g. When waste plastics are pyrolyzed by adding CaO particles to a pyrolysis reactor, calcium oxide (CaO) reacts with hydrogen chloride in the reactor to generate CaCl2, which melts and causes de-fluidization. This slagging phenomenon causes the process to be stopped, resulting in a significant decrease in process efficiency. The slag composition of the present invention contains not only calcium oxide but also iron oxide, silicon oxide, aluminum oxide, and / or magnesium oxide, and thus generates less CaCl2 than CaO particles. It is also superior in chlorine removal effect compared to CaO and Spent FCC E-cat, which have a relatively high BET specific surface area. In addition, the by-products generated during chlorine removal do not melt but are fused to the pores of the slag composition, thereby suppressing the slagging and de-fluidization phenomena. This is analyzed to be due to the fact that chemical properties have a dominant effect on the removal of impurities such as chlorine from pyrolysis oil, rather than physical properties such as BET specific surface area and particle size. In particular, it was analyzed that the slag of the present invention has a better Cl reduction ability than the spent FCC catalyst (Spent FCC E-cat) with a high BET specific surface area. This result means that the slurry composition of the present invention has a very good effect of removing impurities caused by chemical reactions, and therefore can overcome the inferior physical properties.
[0037] The slag composition may have a compressive strength of 100 to 500 MPa, specifically, 200 to 400 MPa, or 250 to 350 MPa. The slag composition may have a compressive strength of 1.5 to 5 g / cm 2 and may have a density of 2 to 4 g / cm 2 , or 2.5 to 3.5 g / cm 2The steel slag has a higher iron content and a higher density than blast furnace slag. Therefore, the physical durability is improved, and even if the slag has a relatively high BET specific surface area, the shape of the slag composition particles can be maintained under high temperature and high pressure conditions in a pyrolysis reactor. Therefore, since it is not accompanied by pyrolysis gas or pyrolysis oil, it is easy to remove after the reaction, and when used as an adsorbent or neutralizer, the regeneration and replacement cycle can be increased, which is preferable in terms of process simplification.
[0038] Meanwhile, the particle size of the slag composition means D50, which means the particle diameter when the cumulative volume becomes 50% from the small particle size in particle size distribution measurement by laser scattering method. Here, D50 can be measured by taking a sample of the produced carbonaceous material according to the KS A ISO 13320-1 standard and measuring the particle size distribution using Malvern's Mastersizer 3000. Specifically, the volume density can be measured after dispersing the sample using ethanol as a solvent and, if necessary, using an ultrasonic disperser.
[0039] Meanwhile, the BET specific surface area of the slag composition can be measured by a gas adsorption method (BET) commonly used in the art, and the specific surface area of the sample surface can be analyzed by adsorbing Ar to the sample, but the present invention is not limited thereto.
[0040] Meanwhile, the compressive strength can be measured by preparing a commonly used slag sample and measuring the maximum stress until the sample breaks under compression, but the present invention is not limited thereto.
[0041] The pyrolysis reactor may be an autoclave reactor, a batch stirred reactor, a fluidized-bed reactor, a packed-bed reactor, or the like. Specifically, the present invention may be applied to any reactor capable of controlling stirring and temperature rise, and the present invention may be performed in a batch reactor.
[0042] Meanwhile, the pyrolysis step may further include a pyrolysis gas recovery step of recovering the pyrolysis gas phase and the pyrolysis liquid phase as gas, and a separation step of separating the pyrolysis solid phase (solid content) into fine particles and coarse particles.
[0043] In the gas recovery step, pyrolysis gas containing low boiling point hydrocarbon compounds such as methane (CH4), ethane (C2H6), and propane (C3H8) is recovered from the gas phase generated in the pyrolysis step. The pyrolysis gas generally contains combustible substances such as hydrogen, carbon monoxide, and low molecular weight hydrocarbon compounds. Examples of the hydrocarbon compounds include methane, ethane, ethylene, propane, propene, butane, and butene. Such pyrolysis gas can be used as fuel because it contains combustible substances.
[0044] In the separation process, the solid phase generated in the pyrolysis process, such as the carbide and the neutralizing agent and / or the copper compound, is separated into fine particles and coarse particles. Specifically, the solid phase generated in the pyrolysis reaction can be separated into fine particles and coarse particles by classifying the solid phase using a sieve that is smaller than the average particle diameter of the chlorine-containing plastic and larger than the average particle diameter of the neutralizing agent and the copper compound. In the separation process, the solid phase is preferably separated into fine particles containing a relatively large amount of the chlorine-containing neutralizing agent and the copper compound, and coarse particles containing a relatively large amount of the carbide. The fine particles and the carbide may be reprocessed as necessary, reused in the pyrolysis process, used as fuel, or discarded, but the present invention is not limited thereto.
[0045] The pyrolysis oil produced by the pyrolysis process may have a total chlorine content of less than 500 ppm, 300 ppm or less, 200 ppm or less, or 100 ppm or less by total weight, and an organic chlorine content of less than 200 ppm, 100 ppm or less, or 90 ppm or less by total weight.
[0046] In one embodiment of the present invention, a method for producing waste plastic pyrolysis oil may further include a pretreatment step of the waste plastic prior to the pyrolysis step, and the pretreatment step may further include a step of feeding the waste plastic into a screw reactor and pulverizing it at room temperature.
[0047] The waste plastic may be pulverized by a pulverization process known in the art. For example, the waste plastic may be fed into a pretreatment reactor and heated to about 300° C. to produce a pellet-shaped hydrocarbon stream precursor, but the present invention is not limited thereto. As an example, the pulverization process may involve mixing the waste plastic and a neutralizing agent and feeding the mixture into a reactor. When the waste plastic is mixed with calcium oxide or the like as the neutralizing agent and pulverized at room temperature, a mechanochemical reaction occurs to produce hydrocarbons and CaOHCl, which has the effect of stably fixing chlorine in the waste plastic raw material to CaOHCl.
[0048] The pretreatment step is characterized by subsequently feeding the pulverized waste plastic into a pretreatment reactor and heating it, and the solid waste plastic raw material may be physicochemically treated to partially remove chlorine and produce a hydrocarbon stream precursor (raw material for the pyrolysis step). The hydrocarbon stream precursor refers to a waste plastic melt, and the waste plastic melt may refer to a liquid waste plastic (melt) produced from all or a part of the pulverized or unpulverized solid waste plastic.
[0049] The heating may be performed at a temperature of 200 to 320°C under normal pressure. Specifically, it is preferably performed at a temperature of 250 to 320°C or 280 to 300°C. Generally, the pretreatment temperature for waste plastics is at least 250°C, but the above-mentioned dechlorinated hydrocarbons can be easily pretreated at a lower temperature of 200°C to generate hydrogen and methane gas. Therefore, according to the present invention, it is possible to generate flammable gases such as hydrogen and methane without generating harmful gases in the pretreatment process.
[0050] The pretreatment reactor may be an extruder, an autoclave reactor, a batch reactor, or the like, and an auger reactor may be used as an example, but the present invention is not limited thereto.
[0051] Preferred examples and comparative examples of the present invention will be described below. However, the following examples are merely preferred examples of the present invention, and the present invention is not limited to the following examples.
[0052] Working Example Example 1 Four tons of vinyl waste from daily life and 10% by weight of slag were fed into a batch pyrolysis reactor and pyrolysis was carried out up to 500℃. The pyrolysis gas produced was passed through a gas separator and a cooler, and then separated into pyrolysis oil and water in an oil-water separator. The separated pyrolysis oil was collected in a storage tank after passing through solid / liquid and liquid / liquid separation in a settling tank and a centrifuge.
[0053] In this case, the slag composition had a particle size (D50) of 70 μm and a BET specific surface area of 4 m 2 / g, and steelmaking slag having the chemical composition shown in Table 1 below was used. The household waste plastics used were a mixture of PP, PE, PVC, nylon, etc. The total Cl content in the household waste plastics was 11,000 ppm.
[0054] [Table 1]
[0055] (In Table 1, T-Fe refers to all iron (iron oxides) primarily composed of Fe2O3 and Fe3O4 that are generated during operation in the sintering plants of steelworks.)
[0056] (Examples 2 to 4) A pyrolysis oil was produced in the same manner as in Example 1, except that steelmaking slag with different D50 and BET specific surface area was used. In Example 2, a steelmaking slag composition with a particle size (D50) of 82 μm and a BET specific surface area of 4.8 m was used. 2 In Example 3, the steelmaking slag composition had a particle size (D50) of 71 μm and a BET specific surface area of 3.7 m 2 In Example 4, the steelmaking slag composition had a particle size (D50) of 93 μm and a BET specific surface area of 7.6 m 2 / g, and the chemical composition is as shown in Table 2 below.
[0057] [Table 2]
[0058] (In Table 2, T-Fe refers to all iron (iron oxides) mainly composed of Fe2O3 and Fe3O4 that are generated during operation in the sintering plants of steelworks.)
[0059] Evaluation example 1: Interpretation of impurity reduction results in pyrolysis oil Comparative Example 1 The pyrolysis oil was recovered in the same manner as in Example 1, except that the slag composition was not used.
[0060] Comparative Example 2 The pyrolysis oil was recovered in the same manner as in Example 1, except that CaO particles were used instead of the slag composition. In this case, the CaO particles had a particle size (D50) of 48.3 μm and a BET specific surface area of 5.9 m 2 / g.
[0061] Comparative Example 3 The same procedure as in Example 1 was carried out to recover pyrolysis oil, except that a waste FCC catalyst was used instead of the slag composition. In this case, the spent FCC catalyst had a particle size (D50) of 73.6 μm and a BET specific surface area of 151 m 2 / g.
[0062] Comparative Example 4 The pyrolysis oil was recovered in the same manner as in Example 1, except that blast furnace slag (see Table 1 above) was used instead of steelmaking slag.
[0063] (Evaluation method) ICP, TNS, EA-O, and XRF analyses were carried out to analyze the impurity Cl in the waste plastic pyrolysis oils produced in Examples 1 to 3 and Comparative Examples 1 to 3. The results are summarized in Table 3 below.
[0064] [Table 3]
[0065] Referring to Table 3 above, in Example 1, in which the slag composition was used as a pyrolysis additive, it was confirmed that the Cl reduction performance was far superior to that of E-cat (spent FCC catalyst) and was at a level superior to that of commonly used CaO.
[0066] In addition, by comparing the results of Example 1 and Comparative Example 4, it was confirmed that when steelmaking slag having a chemical composition satisfying the chemical composition of the slag composition of the present invention is used among steel slags, the Cl reduction effect is more excellent than that of blast furnace slag that does not satisfy the chemical composition.
[0067] Furthermore, referring to Table 4 below together with Table 3 above, it can be seen that when the chemical composition of the steelmaking slag satisfies both formula 1 and formula 2 as in Example 3, the chlorine reduction performance is significantly superior to Example 1 or Example 2 which satisfies only one of formula 1 or formula 2, and it can be seen that the chlorine reduction performance is most superior when the chemical composition of the steelmaking slag is as in Example 4.
[0068] [Table 4]
[0069] (In the above Table 4, formula 1 is 1<iron oxide (wt%) / silicon oxide (wt%)<3, and formula 2 is 3<iron oxide (wt%) / magnesium oxide (wt%)<5.)
[0070] Although the embodiments of the present invention have been described above, the present invention is not limited to the above embodiments, and may be manufactured in various different forms, and a person having ordinary skill in the art to which the present invention belongs can understand that the present invention can be embodied in other specific forms without changing the technical idea or essential features of the present invention. Therefore, it should be understood that the embodiments described above are illustrative in all respects and are not limiting.
Claims
1. The process includes a pyrolysis step of feeding waste plastic and a slag composition into a pyrolysis reactor to produce a pyrolysis oil, The slag composition contains, relative to the total weight, 30 to 60% by weight of calcium oxide, 5 to 30% by weight of iron oxide, and 0.5 to 30% by weight of at least one selected from silicon oxide, aluminum oxide, and magnesium oxide.
2. The method for producing waste plastic pyrolysis oil according to claim 1 , wherein the slag composition satisfies the following formulas 1 and 2. [Formula 1] 1<iron oxide (wt%) / silicon oxide (wt%)<3 [Formula 2] 3<Iron oxide (wt%) / Magnesium oxide (wt%)<5
3. The method for producing waste plastic pyrolysis oil according to claim 1 , wherein the slag composition contains 5% by weight or less of aluminum oxide based on the total weight of the slag composition.
4. The method for producing waste plastic pyrolysis oil according to claim 1 , wherein the slag composition contains 20% by weight or less of silicon oxide based on the total weight of the slag composition.
5. The method for producing waste plastic pyrolysis oil according to claim 1, wherein the pyrolysis step is carried out at a temperature of 400 to 600° C. in a non-oxidizing atmosphere.
6. The method for producing waste plastic pyrolysis oil according to claim 1, wherein the waste plastic is a household waste plastic containing 3% by weight or more of PVC (polyvinyl chloride) based on the total weight.
7. The slag composition has a thickness of 0.5 to 10 m 2 The method for producing waste plastic pyrolysis oil according to claim 1, wherein the oil has a BET specific surface area of 100 / g.
8. The method for producing waste plastic pyrolysis oil according to claim 1, wherein the slag composition has a particle size of 5 to 200 μm.
9. The method for producing waste plastic pyrolysis oil according to claim 1, wherein the slag composition has a compressive strength of 100 to 500 MPa.
10. The slag composition has a content of 1.5 to 5 g / cm 2 The method for producing waste plastic pyrolysis oil according to claim 1, wherein the oil has a density of about 1000 to about 10 ....
11. The method for producing waste plastic pyrolysis oil according to claim 1, wherein the pyrolysis oil contains less than 100 ppm of chlorine based on the total weight.
Citation Information
Cited By
Method for producing lower olefin
WO2026088926A1
Method for producing lower olefin
WO2026088927A1