Sealable wrapping paper
The coated paper addresses the limitations of transparent papers by providing strength, recyclability, and seal seam strength, enabling use in conventional packaging machines and being suitable for food and toy sectors, while being biodegradable and produced from renewable materials.
Patent Information
- Application Number
- JP2024518739
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-06
- Filing Date
- 2022-09-30
- Publication Date
- 2024-10-16
AI Technical Summary
Existing transparent papers lack sufficient strength, recyclability, and are not suitable for food contact, toy, and games sectors, while plastic films are not recyclable and require substantial modifications for use in conventional packaging machines.
A coated paper with a base paper containing less than 5 wt% filler and a coating layer comprising a heat-sealable material, achieving an opacity of less than 60% and suitable for direct use in existing packaging machines, with properties comparable to conventional plastics.
The coated paper provides sufficient strength, recyclability, and seal seam strength, enabling use in conventional packaging machines without modifications, and is suitable for food contact and toy sectors, while being biodegradable and produced from renewable raw materials.
Smart Images

Figure 2024537743000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a coated paper, more particularly to a translucent coated paper, to a method for producing such a coated paper, to the use of said coated paper as a packaging material, and to a packaging comprising the coated paper. [Background technology]
[0002] Packaging generally means covering or enclosing (partially or completely) an object, more specifically for its protection or better handling. Packaging materials therefore include materials that form such packages.
[0003] The packaging material can be made of, for example, paper, plastic and / or metal. The present invention provides for paper-based packaging materials.
[0004] The main requirement for packaging materials of all origins is to protect the packaged goods from external influences and to prevent leakage of the packaged goods. For this purpose, packaging materials should meet different criteria depending on the packaged goods and the packaging method: suitable packaging materials should meet mechanical and method-specific requirements, for example, they should have barrier properties against water, grease, oxygen or mineral oil for sensitive packaged goods, more particularly foodstuffs. Depending on the packaging system, the packaging material should have sufficient tear resistance, a suitable coefficient of friction and flexibility; it should be heat-sealable or compatible with cold-seal adhesives, it should also be printable from the outside and should not lose its protective action during the entire conversion and packaging process.
[0005] Transparent or at least partially transparent (semi-transparent) packaging materials are usually used whenever the object of interest should remain visible through the packaging despite being packaged, so that, for example, the object itself or printed matter on the object is visible from the outside despite the packaging, or a label or bar code on the object is readable.
[0006] Transparent or at least partially transparent packaging materials based on plastic films or transparent papers have been known for some time.
[0007] For example, a mail order catalog or promotional brochure may be shrink wrapped in plastic film or transparent paper and mailed so that the delivery address, and more particularly the bar code, can be read through the packaging.
[0008] The term transparent paper often includes the following papers: - Packing tissue: This is not actually a typical transparent paper, but it is made very thin so it appears relatively transparent. - Impregnated paper: by impregnation with drying oils, resins, waxes and / or fats, paper produced from free-beaten fibres can be made transparent. - Vegetable parchment: Paper made from pulp is usually partially dissolved in a bath of sulfuric acid. The partially dissolved cellulose fills the gaps in the paper, making it transparent. The sulfuric acid is washed away again in a final bath. - Natural tracing papers: Natural tracing papers contain wet-beaten fibres which are often further impregnated. Due to the wet-beaten nature of these papers, they are highly sensitive to fluctuations in humidity. - Glassine: The pulp is wet beaten and then very hard calendared, which removes the air between the fibres, making them more translucent.
[0009] As can be seen from the above, transparent paper has its drawbacks.
[0010] In addition, there is another drawback which generally affects all transparent papers: they cannot be fully recycled through the waste paper cycle.
[0011] Moreover, many transparent papers are also not well suited as packaging materials because they do not combine the necessary strength with low basis weight.
[0012] Transparent packaging made from plastic film also cannot be recycled through the waste paper cycle, more particularly together with the catalogues or promotional brochures which may be packaged therein. Summary of the Invention [Problem to be solved by the invention]
[0013] It is therefore an object of the present invention to provide a translucent packaging material that has a sufficiently low opacity so that, for example, the packaged item or inscriptions on the packaged item can be read through the packaging material, can be recycled through the waste paper cycle, has a sufficiently low basis weight together with sufficient strength, and / or has sufficient seal seam strength.
[0014] Also, the packaging material should preferably be suitable for the food contact and toys and games sectors; it should be biodegradable and be producible mainly from renewable raw materials; its producibility should be economical; it should be suitable for packaging foodstuffs and be usable in conventional packaging machines without the need to substantially change the machine parameters, e.g. the use of plastic-based packaging and paper-based packaging in the same packaging machine. For this reason, the packaging material should be sealable on the same side, or back-to-back or inside-to-inside and on opposite sides (front / inside). [Means for solving the problem]
[0015] Surprisingly, these objects are solved by the coated paper according to claim 1, i.e. by a coated paper comprising a base paper containing less than 5 wt.-% of filler and a coating color layer applied directly or indirectly to one side of the base paper, the coating color layer comprising or consisting of at least one heat-sealable material, the coated paper having an opacity of less than 60% in the visible range.
[0016] Preferably, the opacity in the visible range is less than 55%, particularly preferably less than 50%.
[0017] Surprisingly, it has been found that the coated paper according to the invention, despite its low basis weight, can be used directly in existing packaging machines for packaging the packaged goods in plastic packaging, without the need for significant modification of the packaging machine. More particularly, the good operating properties (mechanical properties), the required opacity and good heat sealability of the paper prove to be advantageous, as a result of which the paper can be used like conventional plastics and therefore can replace plastic packaging. The coated paper according to the invention or packaging made therefrom can be easily recycled through the waste paper cycle. [Brief description of the drawings]
[0018] [Figure 1] FIG. 13 is an explanatory diagram of a folded packaging form. [Diagram 2] FIG. 1 is an illustration of a tube bag packaging configuration. [Diagram 3] FIG. 1 is an explanatory diagram of a first form of QR code. [Figure 4] FIG. 13 is an explanatory diagram of a second form of QR code. [Diagram 5] FIG. 11 is an explanatory diagram of a third form of QR code. [Figure 6] FIG. 11 is an explanatory diagram of a fourth form of QR code. [Figure 7] FIG. 11 is an explanatory diagram of a fifth form of QR code. [Figure 8] FIG. 1 is an explanatory diagram of a jump form. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] All features of one embodiment defined in this specification and claims may be combined with features of another embodiment unless inconsistent with the features of the different embodiment.
[0020] The terminology used in the description of this disclosure is intended to describe certain embodiments only and should not be construed as limiting the subject matter. As used herein and in the claims, the singular forms "a" and "an" are to be understood to include the plural, unless the context clearly dictates otherwise. This also applies vice versa, i.e., the plural also includes the singular. The term "and / or" as used herein is also to be understood to mean and include all possible combinations of one or more of the associated listed elements. Furthermore, the terms "include", "including", "comprise", and / or "comprising" as used herein and in the claims are to be understood to specify the presence of the stated features, steps, elements, and / or components, but not to preclude the presence or addition of one or more other features, steps, elements, components, and / or groups thereof.
[0021] In this specification and claims, the terms "include", "comprise" and / or "comprising" may also mean "consisting of", i.e. excluding the presence or addition of one or more other features, steps, elements, components and / or groups.
[0022] In this specification and claims, the coated side of the paper is often referred to as the "B" side, and the uncoated side of the paper is often referred to as the "A" side.
[0023] The coated paper according to the present invention comprises a base paper and a coating color layer applied thereto, characterized in that the coated paper has an opacity of less than 60% in the visible range, where the coating color layer comprises at least one polymer.
[0024] Preferably, the opacity in the visible range is less than 55%, particularly preferably less than 50%.
[0025] Opacity is generally understood to be the opposite of transparency, ie, a lack of transparency or transmittance.
[0026] Thus, opacity in the visible range refers to the lack of light transmission in the visible range.
[0027] Opaqueness is therefore the opposite of transparency or translucency. Translucency describes semi-transparency, i.e. close to transparency but not completely transparent.
[0028] Opacity can also be expressed as the inverse of transmittance.
[0029] The opacity can be determined according to ISO 2471 (2008).
[0030] In principle, there are no restrictions on the base paper used for the coated paper according to the invention.
[0031] However, the basis weight of the coated paper is 45 g / m 2 More specifically, 40 g / m 2 It is preferable that the thickness is less than 30 g / m 2 ~40g / m 2 Coated paper basis weights in the range are particularly preferred.
[0032] Basis weight may be determined in accordance with ISO 536(2020-05).
[0033] The opacity of the coated paper can be adjusted using such basis weights without any drawbacks regarding structural integrity.
[0034] Preferably, the base paper may comprise short fibres, long fibres, recycled pulp and / or alternative fibrous materials such as grass fibre, silphium fibre and / or other mechanically or chemically processed fibrous materials, preferably materials derived from agricultural residues.
[0035] It is further preferred that the base paper comprises short fibers and long fibers, and the weight ratio of the short fibers to the long fibers is greater than 1.
[0036] More specifically, the weight ratio of short fibers to long fibers is 60:40 to 70:30.
[0037] The long fibers preferably have a fiber length of 2.6 to 4.4 mm, and the short fibers preferably have a fiber length of 0.7 to 2.2 mm.
[0038] The coated paper according to the present invention is further characterized in that the base paper contains less than 5 wt. % of a filler.
[0039] Thus, in one embodiment, the base paper may also contain no fillers at all.
[0040] Preferably, the filler is present at 0 wt% or at greater than 0 wt% up to 5 wt%.
[0041] The percentages by weight are based on the total weight of the base paper. Fillers include GCC (ground calcium carbonate), e.g. known under the trade names Hydrocarb 60 or Hydrolex 60, PCC (precipitated calcium carbonate), e.g. known under the trade name Precarb 105, natural kaolin and / or talc, as well as conventional additives such as retention and / or sizing agents.
[0042] In a preferred embodiment, the coated paper according to the invention is characterized in that the coating colour layer is heat-sealable, for this purpose the coating colour layer comprises at least one thermoplastic polymer.
[0043] The coated paper according to the invention is preferably further characterized in that at least one polymer of the coating color layer comprises a thermoplastic heat-sealable polymer.
[0044] "Heat sealing" is preferably understood to mean the joining of two layers of coated paper by exposure to localized heat.
[0045] The coated paper according to the present invention is preferably further characterized in that at least one heat-sealable material or polymer of the coating colour layer is selected from the group comprising polyolefins, vinyl acetate polymers, (modified) vinyl acetate copolymers, polyvinyl alcohol (PVOH), grafted polyvinyl alcohol, ethylene vinyl alcohol, (meth)acrylate (co)polymers, more particularly ethylene acrylic acid copolymers and styrene acrylate copolymers, acrylic acid esters, (carboxylated) styrene-butadiene copolymers, polyurethanes, carbohydrates and carbohydrate derivatives, acrylate polymers, acrylic acid esters, aqueous synthetic resin dispersions, thermoplastic ethylene copolymers, natural rubber and / or polyurethanes.
[0046] Suitable heat sealable materials or polymers are known, for example, under the trade names Hypod 2000, SealCoat MB46 HE, Cartaseal SWF, SealCoat HS 25, Rhobarr 320, EUKALIN 7238 VD, Decacode Seal, Aquasel 2330, Loctite Liofol CS22-096, Primeseal 22-096, S8128.
[0047] The at least one heat-sealable material or polymer is preferably contained in the coating color layer in an amount of 50 to 100 wt %, particularly preferably 80 to 100 wt %, based on the total weight of the coating color layer.
[0048] Preferably, waxes and / or inorganic pigments may be included as anti-blocking agents.
[0049] The coating color layer may also contain additives such as thickeners, e.g., acrylate-based thickeners; surfactants, e.g., sulfosuccinates; extensional rheological additives, e.g., acrylate-based extensional rheological aids; waxes, e.g., fatty acid or fatty acid amide-based waxes; additives that reduce abrasion sensitivity and increase slip, e.g., layered silicates, more particularly magnesium silicate hydrates or aluminosilicates; and / or crosslinkers, e.g., aldehydes and polyaldehydes, zirconates, polyepoxides, epichlorohydrin resins, and / or hydrazides.
[0050] These additives are preferably each present in an amount of from 0 or from 0 to 50 wt %, particularly preferably from 0 or from 0 to 20 wt %, based on the total weight of the coating color layer.
[0051] The coated paper according to the invention preferably further comprises a coating colour layer of 10 g / m 2 It is characterized by having a basis weight of less than 100 g.
[0052] The coating layer weight is 2~10g / m 2 , more specifically 3 to 7 g / m 2 It is particularly preferable that the range is:
[0053] Such a basis weight ensures that the coated paper has advantageous translucency without any drawbacks in terms of structural integrity.
[0054] The coated paper according to the invention is preferably further characterized in that when the coated paper seals B / B side (coated side on coated side), it has a cold seal seam strength of more than 3 N / 15 mm, measured according to DIN 55529 (2012).
[0055] The coated paper according to the present invention is preferably further characterized in that when the coated paper seals A / B side (uncoated side over coated side), it has a cold seal seam strength of greater than 1.5 N / 15 mm, measured according to DIN 55529 (2012).
[0056] The seal seam strength for coated papers can be determined as follows:
[0057] The coated paper is sealed perpendicular to the paper flow direction in the temperature range 100°C-200°C for at least 0.3 seconds at 3.3 bar and the seal seam strength is determined according to DIN 55529 (2012).
[0058] The coated paper according to the invention is preferably further characterized in that the coated paper has a burst pressure according to Mullen of more than 150 kPa, particularly preferably more than 200 kPa.
[0059] The burst pressure (Mullen) is determined, for example, according to ISO 2758 (2014-12).
[0060] Bursting pressure (Mullen) describes the strength value of paper, and such a bursting pressure is advantageous, since the paper must be characterized by high strength even at low basis weights. This is necessary in order to be able to be used without any problems during printing in the converting steps and finishing processes. For example, wrinkles must not form in the rotary printing process or in the transfer paper using a transfer calendar, and the paper, even at low basis weight, must be able to withstand the corresponding tension forces that may affect the paper during converting.
[0061] The coated paper according to the invention is preferably further characterised in that the coated paper has a longitudinal tensile strength of more than 40 N / 15 mm and / or a transverse tensile strength of more than 60 N / 15 mm, measured according to ISO 1924-2 (2009).
[0062] The coated paper according to the invention is preferably further characterised in that the coated paper has a longitudinal elongation at break of >1.5%, preferably >2%, and / or a transverse elongation at break of >4%, preferably >5%, measured according to ISO 1924-2 (2009).
[0063] The coated paper according to the invention is preferably further characterized in that the coated paper has a roughness of <5 μm, preferably <4.5 μm, on the top surface of the coating color layer. The roughness can be determined according to ISO 8791-4 (2008-05).
[0064] The coated paper according to the invention is preferably further characterized in that the base paper, preferably on the side to which the coating colour layer is applied, has a roughness of ≦7 μm, preferably ≦6 μm.
[0065] The coated paper according to the invention is preferably further characterized in that the base paper has a roughness of ≦5 μm, preferably ≦4 μm, preferably on the side to which the coating colour layer is not applied, i.e. the backside.
[0066] The coated paper according to the invention is preferably further characterized in that the coated paper has a thickness of less than 60 μm.
[0067] A thickness of 30 to 50 μm is particularly preferred.
[0068] The coated paper according to the invention is also characterized in that, in addition to visual inspection of the contents due to its translucency, it offers the possibility of identifying the contents by means of a code printed on the packaged item.
[0069] The coated paper according to the invention is further characterized in that it offers the possibility to print a code on the outer surface of the paper, for example by inkjet printing, thus marking items and reading the content of the code.
[0070] The present invention also relates to a coated paper as described above, characterized in that a precoat or surface pigmentation is present between the base paper and the coating color layer, comprising the addition of a polymeric binder, preferably starch and / or latex and / or a pigment, e.g. CaCO3.
[0071] Also possible are embodiments in which a precoat or surface coloring, including the addition of a polymeric binder, preferably starch and / or latex and / or pigment, such as CaCO3, is present on the side of the base paper where no coating color layer is present, i.e., the backside.
[0072] As already mentioned above, known translucent papers have disadvantages in the recycling process, which are often caused by a greatly increased reject fraction or sticky impurities.
[0073] Test methods exist to assess the recyclability of packaging paper with respect to these criteria on a laboratory scale. Common test methods include PTS-RH 021:2012-Category II and UNI 11743:2019. These provide information on the assessment of packaging materials for their recyclability in established paper recycling plants. They simulate the process steps on a laboratory scale and evaluate them using a specially developed evaluation system. The process steps are: disassembly - sorting (multiple times) - sheet formation.
[0074] To improve these parameters, the coated paper according to the invention preferably has a minimal content of non-paper components so as not to cause any problems in the recycling process.
[0075] The coated paper according to the invention therefore preferably meets the recycling tests according to PTS-RH 021:2012-Category II and / or UNI 11743:2019.
[0076] Coated papers according to the invention can be obtained economically using known manufacturing methods.
[0077] However, it is preferred to obtain the coated paper according to the invention by a process in which an aqueous suspension comprising the starting materials for the coating colour layer is applied to the base paper, the aqueous application suspension having a solids content of 20-60 wt.-%, preferably 30-50 wt.-%, and is applied by a curtain coating process at an operating speed of the coating system of at least 200 m / min.
[0078] This process is particularly more advantageous from an economic standpoint and for uniform coating on the paper web.
[0079] Below a value of about 30 wt.%, the economic efficiency decreases, since a large amount of water has to be removed in a short time by gentle drying, which has a detrimental effect on the coating speed, whereas above a value of 60 wt.%, the only effect is an increase in the technical efforts to ensure the stability of the coating color curtain during the coating process and drying of the applied film, since in this case the machine has to start up again very quickly.
[0080] In the curtain coating process, a free-falling curtain of coating dispersion is formed. To apply the coating dispersion to a substrate, the coating dispersion in the form of a thin film (curtain) is "poured" onto the substrate by free fall. DE10196052T1 discloses the use of the curtain coating process in the production of information recording materials, in which a multi-layer recording layer is realized by applying a curtain of several coating dispersion films to the substrate.
[0081] In a preferred embodiment of the method according to the invention, the aqueous deaerated coating suspension has a viscosity of about 100 to about 800 mPa. * s (Brookfield, 100 rpm, 20°C). * s or below 800mPa * If the viscosity exceeds 100 s, the runnability of the coating mass in the coating unit becomes insufficient. Particularly preferably, the viscosity of the aqueous deaerated coating suspension is about 200 to about 500 mPa. * It is s.
[0082] In a preferred embodiment, the surface tension of the aqueous coating suspension can be adjusted to about 25 to about 70 mN / m, preferably about 35 to about 60 mN / m (measured according to the standard for bubble pressure tensiometry (ASTM D 3825-90) as described below) to optimize the process. Better control of the entire coating process can be achieved by determining the dynamic surface tension of the coating color, selecting an appropriate surfactant, and adjusting it by determining the required amount of surfactant.
[0083] Dynamic surface tension is measured using a bubble pressure tensiometer. The maximum internal pressure of a bubble formed in a liquid via a capillary tube is measured. According to the Young-Laplace equation, the internal pressure p of a spherical bubble (Laplace pressure) depends on the radius of curvature r and the surface tension σ:
[0084]
number
[0085] When a gas bubble is created in a liquid at the tip of the capillary, the curvature first increases and then decreases again, resulting in a pressure maximum. The maximum curvature, and therefore the maximum pressure, occurs when the radius of curvature corresponds to the capillary radius.
[0086] Pressure characteristics for bag pressure measurement, position of maximum pressure:
[0087] The radius of the capillary is determined using a standard measurement made on a liquid of known surface tension, usually water. Once the radius is known, the surface tension can be calculated from the maximum pressure pmax. Since the capillary is immersed in the liquid, the hydrostatic pressure p0 resulting from the immersion depth and the density of the liquid must be subtracted from the measured pressure (this is done automatically in modern instruments). This results in the following equation for the bubble pressure process:
[0088]
number
[0089] The measured value corresponds to the surface tension at a certain surface age, the time from the beginning of bubble formation to the appearance of a pressure maximum. By varying the rate at which the bubbles form, the dependence of the surface tension on the surface age can be obtained, resulting in a curve in which the surface tension is plotted against time.
[0090] This dependence plays an important role in the use of surfactants, since the equilibrium value of the interfacial tension is not even reached in many processes due to the sometimes low diffusion and adsorption rates of the surfactants.
[0091] The individual coatings can be applied on-line on a paper machine equipped with a coating unit, or off-line on a coating machine in separate coating processes.
[0092] In other embodiments, the individual layers can also be applied to the base paper using the following process:
[0093] The coating color layer can be applied to the base paper and / or the existing precoat using a printing process.
[0094] The coating color layer can be applied to the base paper and / or to an existing precoat by extrusion.
[0095] This technique has the advantage that significantly more material can be applied, but this is only of interest if the entire product does not need to be recyclable as paper. The disadvantages are the lower application speed, higher energy consumption and higher minimum application weight.
[0096] The coating color layer can be applied by lapping or backing the paper, for example in the form of a plastic film, onto the base paper and / or an existing precoat.
[0097] The coating color layers and precoats can also be applied one after the other over several application steps.
[0098] The uncoated surface may be smoothed by the application of heat and / or pressure.
[0099] The present invention further relates to a coated paper obtainable by the above described process.
[0100] The present invention also relates to the use of the coated paper or of a coated paper obtainable by the process described above as packaging material and in combination with cardboard and / or paperboard.
[0101] In particular, the coated paper or the coated paper obtainable by the above-mentioned process is suitable as packaging material for: - Mail order catalogs, because the shipping address remains visible through the packaging, plus the lower basis weight results in lower material costs and lower postage charges. - A packaging type of playing card packaging in which the A / B sides are sealed and serves as a direct substitute for, for example, cellophane film, since the playing cards remain visible through the packaging, allowing quality control. - Packaging for transport of fabrics / clothing, e.g. shirts, trousers, T-shirts, sweaters, underwear. - Packaging of playing cards in a packaging type where the B / B side is sealed, for example in the form of a tubular bag, and serves as a direct substitute for conventional foil packaging, since the playing cards remain visible through the packaging, allowing quality control. - Hygiene products like toilet paper. - Primary or secondary packaging.
[0102] The present invention also relates to packaging comprising said coated paper, and to packaging comprising said coated paper in combination with cardboard and / or paperboard.
[0103] The packaging can also be a heat sealed packaging.
[0104] The package can also be a cold sealed package.
[0105] Preferably, the packaging has a cold seam sealing strength of at least 3N / 15mm when sealed with the sealing layer coated side on the sealing layer coated side (B / B).
[0106] Preferably the packaging has a cold seam seal strength of 1.5N / 15mm or greater when sealed with a side coated with the sealing layer onto a side not coated with the sealing layer (B / A).
[0107] The paper can be coated on one or both sides, over the entire surface or partially with a paint of the material classes mentioned above, to further improve the (B / A) seal in demanding applications requiring high sealing forces (times < 1 sec, pressures ≦ 3.3 bar; increased temperatures, e.g. 140°C cold seam seal strength > 2N / 15mm).
[0108] The paper can be partially coated on the coated or printed side with a coating from the material classes mentioned above to improve the robustness of the package, more particularly the triple point (ply jump from 2 to 4 plies; see Figure 8) package.
[0109] In certain embodiments, the selection of sealing medium / coating material is also determined by the grease tightness (KIT > / = 3; PKOT KAT 1; HVTR < 100 g / m 2 / d or WVTR<100g / m 2 Further properties such as (at 23° C. / 50% rh) can also be achieved.
[0110] The present invention will now be described in more detail with reference to the following non-limiting examples. EXAMPLES
[0111] EXAMPLES
[0112] The coating is 60% long fibre and 40% short fibre base paper 35g / m 2 The base paper additionally contains 2 wt% of filler.
[0113] Precoat / Primer: The precoat contains 100wt% starch. The basis weight of the precoat is 1g / m 2 It is.
[0114] Coating color layer: The coating color layer has the following composition:
[0115] [Table 1]
[0116] Coating color layer is 5g / m 2 The sheet has a basis weight of 1.0 g.
[0117] For this, a film press was used to apply the precoat, and a curtain coater was used to apply the coating color layer.
[0118] The resulting coated paper was examined and the results are shown in the following table:
[0119] [Table 2] EXAMPLES
[0120] Packaging of playing cards (folded packaging): A deck of playing cards is wrapped in a wrapping machine designed for folding wrapping such as that shown in FIG.
[0121] Seal using heat seal bars vertically and horizontally. Seal with the inner surface coated with the sealing layer onto the uncoated top surface (A / B seal).
[0122] A cold seal seam strength of 1.5N / 15mm has proven sufficient for this type of packaging.
[0123] The wrapped deck of cards is then packed into a separate box or placed in the appropriate compartment of a game box. EXAMPLES
[0124] Tubular bag packaging (Flowpack): A few playing cards are packaged in a packaging machine designed for tubular bag packaging such as that shown in FIG.
[0125] The heat seal bar is used vertically and horizontally to seal. An inner surface coated with a sealing layer is sealed on an inner surface coated with a sealing layer (B / B seal).
[0126] A cold seal seam strength of 3N / 15mm has proven sufficient for this type of packaging.
[0127] The wrapped playing cards are then packed into a separate box or placed into the appropriate compartment of the game box. EXAMPLES
[0128] Coding Various tests were carried out with QR codes to test the possibility of labeling both the uncoated side of the paper according to the invention and flat filling good (e.g. playing cardboard) by direct printing and reading them through the translucent paper.
[0129] The printer used was a standard HP Office Jet Pro 8210 with the corresponding HP ink 957. A "REA VeriCube" code reader and tester was used as the reader.
[0130] The software used was "TransWin32 V.1.2.0.0 / 15701r".
[0131] The following results were achieved:
[0132] 1. QR Code with little to no content printed on the uncoated outer surface of paper: Code content: Readable
[0133] The QR code is shown in Figure 3.
[0134] [Table 3]
[0135] [Table 4]
[0136] Symbol Characteristics
[0137] [Table 5]
[0138] 2. QR Code with more extensive content printed on the uncoated outer surface of paper: Code content: Readable
[0139] The QR code is shown in Figure 4.
[0140] [Table 6]
[0141] [Table 7]
[0142] Symbol Characteristics
[0143] [Table 8]
[0144] 3. QR code with little content, tight fitting paper on flat filling item, read through translucent paper. Code content: Readable
[0145] The QR code is shown in Figure 5.
[0146] [Table 9]
[0147] [Table 10]
[0148] Symbol Characteristics
[0149] [Table 11]
[0150] 4. QR code with little content, loose fitting paper on flat filling item, read through translucent paper. Code content: Readable.
[0151] The QR code is shown in Figure 6.
[0152] [Table 12]
[0153] [Table 13]
[0154] Symbol Characteristics
[0155] [Table 14]
[0156] 5. QR code with extensive content that can be read through translucent paper on a tightly fitted paper on flat filling items. Code content: Readable
[0157] The QR code is shown in Figure 7.
[0158] [Table 15]
[0159] [Table 16]
[0160] Symbol Characteristics [Table 17] EXAMPLES
[0161] The coating is 40% long fiber and 60% short fiber base paper 35g / m 2 The base paper additionally contains 2 wt% of filler.
[0162] Precoat / Primer: The precoat contains 100wt% starch. The basis weight of the precoat is 1g / m 2 It is.
[0163] Coating color layer: The coating color layer has the following composition:
[0164] [Table 18]
[0165] Coating color layer is 5g / m 2 The sheet has a basis weight of 1.0 g.
[0166] The precoat was applied using a film press. The coating color layer was applied using a curtain coater.
[0167] The resulting coated paper was examined and the results are shown in the following table:
[0168] [Table 19] EXAMPLES
[0169] The coating is 25g / m2 with 40% long fibre and 60% short fibre content 2 The base paper additionally contains 2 wt% of filler.
[0170] Precoat / Primer: The precoat contains 100wt% starch. The basis weight of the precoat is 1g / m 2 It is.
[0171] Coating color layer: The coating color layer has the following composition:
[0172] [Table 20]
[0173] Coating color layer is 4g / m 2 The sheet has a basis weight of 1.0 g.
[0174] The precoat was applied using a film press. The coating color layer was applied using a curtain coater.
[0175] The resulting coated paper was examined and the results are shown in the following table:
[0176] [Table 21] EXAMPLES
[0177] The coating is 25g / m2 with 40% long fibre and 60% short fibre content 2 The base paper additionally contains 2 wt% of filler.
[0178] Precoat / Primer: The precoat contains 100wt% starch. The basis weight of the precoat is 1g / m 2 It is.
[0179] Coating color layer: The coating color layer has the following composition:
[0180] [Table 22]
[0181] Coating color layer is 3g / m 2 The sheet has a basis weight of 1.0 g.
[0182] The precoat was applied using a film press. The coating color layer was applied using a curtain coater.
[0183] The resulting coated paper was examined and the results are shown in the following table:
[0184] [Table 23] EXAMPLES
[0185] The coating is 40% long fiber and 60% short fiber base paper 30g / m 2 The base paper additionally contains 2 wt% of filler.
[0186] Precoat / Primer: The precoat contains 100wt% starch. The basis weight of the precoat is 1g / m 2 It is.
[0187] Coating color layer: The coating color layer has the following composition:
[0188] [Table 24]
[0189] Coating color layer is 4g / m 2 The sheet has a basis weight of 1.0 g.
[0190] The precoat was applied using a film press. The coating color layer was applied using a curtain coater.
[0191] The resulting coated paper was examined and the results are shown in the following table:
[0192] [Table 25] EXAMPLES
[0193] The coating is 40% long fiber and 60% short fiber base paper 30g / m 2 The base paper additionally contains 2 wt% of filler.
[0194] Precoat / Primer: The precoat contains 100wt% starch. The basis weight of the precoat is 1g / m 2 It is.
[0195] Coating color layer: The coating color layer has the following composition:
[0196] [Table 26]
[0197] Coating color layer is 3g / m 2 The sheet has a basis weight of 1.0 g.
[0198] The precoat was applied using a film press. The coating color layer was applied using a curtain coater.
[0199] The resulting coated paper was examined and the results are shown in the following table:
[0200] [Table 27] EXAMPLES
[0201] The coating is 40% long fiber and 60% short fiber base paper 40g / m 2The base paper additionally contains 2 wt% of filler.
[0202] Precoat / Primer: The precoat contains 100wt% starch. The basis weight of the precoat is 1g / m 2 It is.
[0203] Coating color layer: The coating color layer has the following composition:
[0204] [Table 28]
[0205] Coating color layer is 4g / m 2 The sheet has a basis weight of 1.0 g.
[0206] The precoat was applied using a film press. The coating color layer was applied using a curtain coater.
[0207] The resulting coated paper was examined and the results are shown in the following table:
[0208] [Table 29]
[0209] All examples were made and tested using Hypod 2000 or SealCoat MB 46 HE as the sealing media. The sealing media can be substituted with other sealing media of comparable value to that of this application.
Claims
1. 1. A coated paper comprising a base paper containing less than 5 wt. % of a filler and a coating color layer applied directly or indirectly to one side of the base paper, the coating color layer comprising or consisting of at least one heat-sealable material, the coated paper having an opacity of less than 60% in the visible range.
2. The basis weight of the base paper is 45 g / m 2 2. The coated paper according to claim 1, characterized in that:
3. 3. Coated paper according to claim 1 or 2, characterized in that the base paper comprises short fibres, long fibres, recycled pulp and / or alternative fibre materials, such as grass fibres, silphium fibres and / or other mechanically or chemically processed fibre materials, preferably materials derived from agricultural residues.
4. 4. The coated paper according to claim 1, wherein the base paper comprises short and long fibers, the weight ratio of short to long fibers being greater than 1.
5. 5. The coated paper according to claim 1, characterized in that when a seal is formed by a side coated with a sealing layer on a side coated with a sealing layer (B / B), the coated paper has a cold seam seal strength of 3 N / 15 mm or more.
6. 6. The coated paper according to claim 1, characterized in that when a seal is formed by a side coated with a sealing layer onto a side not coated with a sealing layer (B / A), the coated paper has a cold seam seal strength of 1.5 N / 15 mm or more.
7. The coating color layer is 10 g / m 2 7. Coated paper according to claim 1, characterized in that it has a basis weight of less than 1000 g / m.
8. 8. Coated paper according to any one of claims 1 to 7, characterized in that the heat-sealable material is selected from the group of thermoplastic polymers, more particularly polyolefins, vinyl acetate polymers, vinyl acetate copolymers, polyvinyl alcohol, grafted polyvinyl alcohol, ethylene vinyl alcohol, (meth)acrylate (co)polymers, more particularly ethylene acrylic acid copolymers and styrene acrylate copolymers, acrylic acid esters, (carboxylated) styrene-butadiene copolymers, polyurethanes, carbohydrates and carbohydrate derivatives, aqueous synthetic resin dispersions, thermoplastic ethylene copolymers, and / or natural rubber.
9. 9. Coated paper according to any one of the preceding claims, characterized in that it has a Mullen burst pressure of more than 150 kPa.
10. 10. Coated paper according to any one of the preceding claims, characterized in that it has a longitudinal tensile strength of more than 40 N / 15 mm and / or a transverse tensile strength of more than 60 N / 15 mm, measured according to ISO 1924-2 (2009).
11. 11. Coated paper according to claim 1, characterized in that it has a longitudinal elongation at break of > 1.5% and / or a transverse elongation at break of > 4%, measured according to ISO 1924-2 (2009).
12. Coated paper according to any one of the preceding claims, characterized in that it has a thickness of less than 60 μm.
13. A precoat comprising a polymeric binder, preferably starch, or a surface colorant and / or pigment comprising a polymeric binder, preferably starch and / or latex, e.g., CaCO 3 13. Coated paper according to claim 1, characterized in that the addition of is present between the base paper and the coating colour.
14. 14. A method for producing coated paper according to any one of the preceding claims, characterized in that an aqueous suspension comprising starting materials for the coating colour layer is applied to the base paper, said aqueous coating suspension having a solids content of 5-50 wt.-%, preferably 10-30 wt.-%, and is applied by a curtain coating process, preferably a double curtain coating process, at a working speed of the coating plant of at least 200 m / min.
15. Use of the coated paper according to any one of claims 1 to 13 or obtainable by the method according to claim 14 as a packaging material or as a component of a packaging material.
16. Packaging comprising the coated paper according to any one of claims 1 to 13 or obtainable by the method according to claim 14.
17. 17. The package of claim 16, having a cold seam seal strength of 3N / 15mm or more when sealed with a side coated with a sealing layer (B / B) on a side coated with a sealing layer.
18. 18. The package of claim 16 or 17, having a cold seam seal strength of 1.5 N / 15 mm or more when sealed with a side coated with a sealing layer onto a side not coated with a sealing layer (B / A).
Citation Information
Patent Citations
Recyclable transparent barrier laminate
JP2003154609A
Transparent paper and method of production for the same
JP2003201694A
Transparent memo pad
JP2004360087A
Paper for preventing forgery and method for producing the same
JP2005273110A
Base paper for cosmetic coating materials
JP2011506794A