Silicon and zinc-containing coupling agents for cellulosic-polymer composites
Coupling agent formulations with organic peroxides and zinc/silicon reagents improve the compatibility and mechanical properties of cellulosic-polymer composites, addressing issues of moisture uptake and creep, enhancing their durability for outdoor use.
Patent Information
- Application Number
- JP2024521211
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-06
- Filing Date
- 2022-10-04
- Publication Date
- 2024-10-16
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing cellulosic-polymer composites used in outdoor applications like decks, fences, and siding suffer from poor compatibility, leading to issues such as excessive moisture uptake, creep, and inadequate mechanical properties, which are not effectively addressed by current polymeric coupling agents like maleic anhydride graft polymers, resulting in deterioration and reduced durability.
The use of coupling agent formulations containing organic peroxides and zinc-containing or silicon-containing reagents, or combinations thereof, to enhance the compatibility and mechanical properties of cellulosic-polymer composites, providing improved water resistance and stiffness.
The proposed formulations result in cellulosic-polymer composites with enhanced modulus of rupture, reduced water absorption, and improved resistance to creep, making them suitable for outdoor applications.
Smart Images

Figure 2024537877000001 
Figure 2024537877000002 
Figure 2024537877000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Patent Application No. 17 / 495,051, filed October 6, 2021, the entire contents of which are incorporated herein by reference for all purposes.
[0002] FIELD OF THEINVENTION The present disclosure relates to coupling agent formulations for improving the properties of cellulosic-polymer composites. The technology is applicable to a variety of cellulosic materials, such as wood or wood products, as fillers in such polymer matrix composites. [Background technology]
[0003] 2. Background of the Invention Melt blending a combination of cellulosic materials (such as wood flour) and polymers in an extruder to form boards that resemble wood is a commercial process for producing cellulosic-polymer composite decks, fences, and siding. Cellulosic materials and polymers tend to be incompatible with one another. For example, cellulosic-polymer composite decks, fences, and sidings can deteriorate over time, often due to excessive moisture uptake from the environment. These composites also tend to suffer from creep, a slow buckling of the material over a period of time. Creep is exacerbated in vertical applications such as fences and siding. The current approach to solving this incompatibility problem is to incorporate commercially available maleic anhydride grafted polymers into the cellulosic-polymer matrix blend. Maleic anhydride grafted polyethylene (MAH-g-PE) or maleic anhydride grafted polypropylene (MAH-g-PP) polymers are called polymeric compatibilizers or polymeric coupling agents and can be expensive. Commercially known maleated polyolefins include the Polybond series from Chemtura, the Fusabond series from DuPont, the Exxelor series from ExxonMobil, and the Orevac series from Arkema. These additives may not provide a composite with sufficient stiffness for fences and siding. Additionally, the physical properties of current technology for compatibilizers may not provide sufficient resistance to rupture as measured by modulus of rupture (MOR) or stiffness as measured by a modulus related to resistance to creep.
[0004] Poor compatibility of cellulosic materials with polyethylene, polypropylene, and other non-polar polymers, or blends thereof, leads to cracking of the composite board, poor board physical properties, and high water absorption. Water absorption reduces the aging characteristics of the composite, i.e., retention of physical properties over time. There is a need for coupling additives that increase mechanical strength and reduce water absorption, especially for cellulosic-polymer composites, such as wood-polymer composite boards intended for load-bearing applications, and more particularly for such load-bearing applications exposed to the exterior environment, e.g., for exterior decking, fencing, or siding.
[0005] US Patent Application Publication No. 2020 / 0056020 describes a capstock resin for wood polymer composites. The building material can be composed of a capstock with a wood-polymer composite core, which is additively processed, i.e., ethylene propylene diamine monomer (EPDM), wood filler, PE, clay, and t-butyl peroxybenzoate, with a stand oil intermediate, mixed, pressed into a sheet, and cured at 140°C.
[0006] No. 7,850,771 describes the preparation of an aqueous emulsion of polyethylene wax, wood preservative, and optional agents such as tung oil, linseed oil, acrylic acid, and organic acids, which constitute a wood preservative composition, using azobisisobutyronitrile (AIBN) and hydrogen peroxide as free radical initiators. This US patent describes the use of alkyl acrylates that can be cured with AIBN, hydrogen peroxide, or potassium persulfate. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] US Patent Application Publication No. 2020 / 0056020 [Patent Document 2] U.S. Patent No. 7,850,771 Summary of the Invention [Problem to be solved by the invention]
[0008] There remains a need for cost-effective, easy-to-use coupling agents for cellulosic-polymer composites that have aging resistance and physical properties suitable for use in place of traditional wood, particularly in outdoor applications such as decks, fences, siding, and the like. [Means for solving the problem]
[0009] Summary of the Invention The present inventors have discovered that a specific formulation comprising an organic peroxide and a combination of at least one of a zinc-containing agent and / or a silicon-containing agent provides a coupling agent for polymer matrix composites with cellulosic materials (such as wood) as fillers that is cost effective and provides improved water uptake, modulus of rupture and stiffness (high modulus) to cellulosic-polymer composites.
[0010] A coupling agent formulation for cellulosic-polymer composites is provided, the formulation comprising, consisting of, or consisting essentially of the following components: (a) at least one organic peroxide having a half-life of at least 1 hour at 98° C.; and (b) (i) at least one zinc-containing reagent; and / or (ii) at least one silicon-containing reagent having the following structure (I): SiR 1 R 2 R 3 R 4 (I).
[0011] In structure (I), R 1 , R 2 , R 3 , or R 4 at least one of R comprises, consists of, or consists essentially of at least one unsaturation, and the remaining R 1 , R2 , R 3 , or R 4 are hydrogen or alkyl or alkoxy groups and may be the same or different.
[0012] Also provided are coupling agent masterbatches for wood and / or other cellulosic filled polymer matrix composites. The masterbatches comprise, consist of, or consist essentially of the coupling agent formulations described above and a suitable carrier. Typically, the masterbatches are provided as a powder or pelletized solid. Methods for making the masterbatches are also disclosed, as well as methods for making the cellulosic-polymer composites.
[0013] In summary, a coupling agent formulation is disclosed that can be added to cellulosic materials and polymers, either separately or as a masterbatch, and then the final composition is melt blended and extruded to form, for example, cellulosic-polymer composite deck boards, fences, or siding.
[0014] In one embodiment, the coupling agent can completely replace the traditional polymeric grafted MAH compatibilizer in the cellulosic-polymer composite formulation, while in another embodiment, the coupling agent formulation can partially replace the traditional polymeric MAH coupling agent in the cellulosic-polymer composite. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Detailed Description The following description is merely exemplary in nature and is in no way intended to limit the disclosure or its application or uses.
[0016] Unless otherwise noted, all percentages herein are by weight.
[0017] As used herein, "polymer" is meant to include organic molecules having a weight average molecular weight greater than 20,000 g / mol, preferably greater than 50,000 g / mol, as measured by gel permeation chromatography.
[0018] As used herein with respect to cellulosic fillers for cellulosic-polymer composites, the term "dry" means 0% to 1% to 2% by weight moisture, but not more than 5% by weight moisture, measured as weight loss by thermogravimetric analysis when the cellulosic filler is heated at 103°C until a constant mass is achieved. This method is described in Philipp Dietsch et al., "Methods to determine wood moisture and their applicability in monitoring concepts," Journal of Civil Structural Health Monitoring; Vol 5, p. 115-127 (2015). Additionally, an instrument called "Sawdust Moisture Meter TK100W" from KJ Industry has a moisture measurement range of 0% to 84% by weight. This instrument can be used to measure the moisture content of various cellulosic materials, such as wood flour, sawdust, palustre, and bamboo flour.
[0019] As used herein, "coupling agent" means a substance or combination of substances capable of reacting with both a cellulosic material and a polymeric matrix, or a substance or combination of substances that facilitates the formation of a blend or composite of a polymeric matrix and a cellulosic material, such that the blend or composite has improved properties compared to a similar blend or composite without the coupling agent.
[0020] As used herein, "masterbatch" means a formulation in which a high concentration of an additive is present that is used to precisely separate the additive into a larger bulk of the composition.
[0021] One-hour half-life information for various organic peroxides is provided in the Luperox® Organic Peroxides / High Polymers catalog from Arkema (Colombes Cedex), which is incorporated herein in its entirety for all purposes. Organic peroxides with a one-hour half-life below 98°C are acceptable for use as disclosed herein only if the peroxide does not exhibit significant loss of peroxide assay at the same temperature for at least one month. The half-life time is the time at which 50% of the peroxide decomposes at a given temperature, and the half-life temperature is the temperature at which 50% of the peroxide decomposes at a given time, and are described in "SAFETY AND HANDLING OF ORGANIC PEROXIDES: A Guide Prepared by the Organic Peroxide Producers Safety Division of Plastics Industry Association," Plastics Industry Association, Inc., OPPSD Bulletin AS-109 (August 2018), which is incorporated herein in its entirety for all purposes.
[0022] It is important to reduce the moisture content of wood flour or sawdust or other cellulosic materials used as fillers in these composites. Certain cellulosic materials, such as wood flour, may have a moisture content (moisture) of 4% to 6% or more by weight. Preferably, the moisture content of the cellulosic material after drying is less than 4% by weight, preferably about 3% by weight, more preferably about 2% by weight, even more preferably about 1% by weight, and even more preferably about 0.5% by weight or less.
[0023] When wood flour is used as the cellulosic material, the particle size is typically 80-40 mesh (180-425 μm). Particle sizes outside this typical range are contemplated, for example up to 20 mesh (850 μm or 0.85 mm diameter). If used, the type of wood flour and / or sawdust used in the practice of the invention can be sourced from a variety of hardwood wood harvested from broad-leafed deciduous trees, and softwood wood harvested from coniferous or coniferous trees.
[0024] Disclosed herein are coupling agent formulations and masterbatches that comprise, consist of, or consist essentially of at least one zinc-containing agent and / or at least one silicon-containing agent.In particular, the inventors have found coupling agent compositions for cellulosic-polymer composites that combine at least one zinc-containing agent and / or at least one silicon-containing agent with at least one room temperature organic peroxide, which may or may not be functionalized, or an organic peroxide formulation that includes at least one or more room temperature organic peroxides, which may or may not be functionalized, or a combination thereof.
[0025] Importantly, the coupling agent formulation disclosed herein may comprise, consist of, or consist essentially of at least one zinc-containing reagent and at least one organic peroxide. The coupling agent formulation may comprise, consist of, or consist essentially of at least one silicon-containing reagent and at least one organic peroxide. The coupling agent formulation disclosed herein may comprise, consist of, or consist essentially of at least one zinc-containing reagent, at least one silicon-containing reagent, and at least one organic peroxide. Combinations of zinc-containing reagents, combinations of silicon-containing reagents, and combinations of organic peroxides are also contemplated.
[0026] Zinc-containing reagents: Surprisingly, these zinc-containing reagents are effective when used with organic peroxides as coupling agents, with or without silicon-containing reagents. Zinc-containing reagents used in the practice of the present invention can include zinc acrylates and zinc methacrylates; zinc species with Zn-O functionality; zinc alkoxides; zinc carboxylates; zinc (acetylacetonates); zinc formates; or zinc oxide. Also suitable are zinc-containing reagents having at least one substituent that contains at least one carbon-carbon double bond reactive to free radicals, such as zinc acrylates and zinc methacrylates. Other zinc-containing reagents suitable for use in embodiments of the present invention include zinc halides, zinc dithiodicarbamates, zinc sulfonates, zinc hydrates, zinc tetrahydrofuran adducts, or zinc N,N,N',N'-tetramethylethylenediamine adducts; or combinations thereof. Specific examples of suitable zinc-containing reagents include zinc diacrylate, zinc dimethacrylate, zinc monoacrylate, zinc monomethacrylate, zinc methoxide, zinc ethoxide, zinc isopropoxide, zinc methoxyethoxide, zinc bis(acetate), zinc bis(2-ethylhexanoate), zinc bis(neodecanoate), zinc bis(cyclohexanebutyrate), zinc naphthenate, zinc undecylenate, oxo[hexa(trifluoroacetato)]tetrazinc, zinc bis(2,2,6,6-tetrazinc ... zinc bis(hexafluoroacetylacetonate); zinc formate; zinc oxide; zinc dimethyldithiocarbamate; zinc diethyldithiocarbamate; zinc dibutyldithiocarbamate; zinc chloride, zinc bromide, zinc fluoride, zinc iodide; zinc sulfonate; zinc carbonate; zinc nitrate; zinc hydrate; zinc tetrahydrofuran adduct; zinc N,N,N',N'-tetramethylethylenediamine adduct; or combinations thereof.
[0027] Zinc diacrylate, zinc dimethacrylate, zinc monoacrylate, zinc monomethacrylate, zinc methoxide, zinc ethoxide, zinc isopropoxide, zinc methoxyethoxide, zinc bis(acetate), zinc bis(2-ethylhexanoate), zinc bis(neodecanoate), zinc bis(cyclohexanebutyrate), zinc naphthenate, zinc undecylenate, oxo[hexa(trifluoroacetato)]tetrazinc, zinc bis(2,2,6,6-tetramethyl-3,5-heptanedionato), zinc bis(hexafluoroacetylacetonate), zinc formate, zinc oxide, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate, or combinations thereof are preferred. Zinc diacrylate, zinc dimethacrylate, zinc monoacrylate, zinc monomethacrylate, or combinations thereof are more preferred. More preferred are zinc diacrylate; zinc dimethacrylate; or a combination thereof.
[0028] Silicon-containing reagents: Surprisingly, it has been found that silicon-containing agents, when used with organic peroxides in the presence or absence of a zinc-containing agent, provide improved cellulosic-polymer composites. At least one silicon-containing agent has the following structure (I): SiR 1 R 2 R 3 R 4 (I).
[0029] R 1 , R 2 , R 3 , or R 4 at least one of R comprises, consists of, or consists essentially of at least one unsaturation, and the remaining R 1 , R 2 , R 3 , or R 4 are hydrogen or alkyl or alkoxy groups and may be the same or different.
[0030] Examples of silicon-containing agents include, but are not limited to, unsaturated silicon-containing species; vinyl(alkoxy)silanes; vinyl(alkyl)silanes; poly(vinyl)silanes; (vinyl)(alkyl)(alkoxy)silanes; vinyl-terminated polydimethylsiloxanes; allylsilanes; vinylsilanes. Specific compounds include vinyltriethoxysilane; vinyltrimethoxysilane, vinyltriisopropoxysilane, vinyltri-t-butoxysilane; vinyltris(2-methoxyethoxy)silane; vinyltriacetoxysilane; trivinylmethoxysilane; trivinylethoxysilane; trivinylisopropoxysilane; divinyldimethoxysilane; divinyldiethoxysilane; vinyltrimethylsilane; vinyltriethylsilane; vinyltriisopropyl ... Nyltributylsilane;Divinyldimethylsilane;Divinylsilane;Trivinylsilane;Tetravinylsilane;Vinyldimethylethoxysilane;Vinylmethyldiethoxysilane;1,3-Divinyltetramethyldisiloxane;1,3,5-Trivinyl-1,3,5-trimethylcyclotrisiloxane;1,3,5,7-Tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane;Vinylmethylbis(trimethylsiloxy)silane;1,1,3,3-Tetravinyldimethylsilane 1,4-Divinyl-1,1,4,4-tetramethyl-1,4-disilabutane;Methylbis(trimethylsilyloxy)vinylsilane;2-(Dimethylvinylsilyl)pyridine;Tris(2-methoxyethoxy)(vinyl)silane;Triacetoxy(vinyl)silane;Tris(trimethylsiloxy)(vinyl)silane;1-Cyclopenten-1-yl(trimethyl)silane;Trimethyl[(1Z)-1-propyl-1-butane Thenyl]silane;(5,5-dimethyl-1-cyclopenten-1-yl)(trimethyl)silane;Trimethyl(6-methyl-1-cyclohexen-1-yl)silane;(4-methoxy-1-cyclohexen-1-yl)(trimethyl)silane;Trimethyl(4-methyl-1,5-cyclohexadien-1-yl)silane;Trimethyl(5-methyl-1,5-cyclohexadien-1-yl)silane;(6,6-dimethyl-1-cyclohexen-1-yl)(trimethyl)silane;Allyl(methyl)1-naphthyl(phenyl)silane;Trimethyl(1-phenyl-2-propenyl)silane;2-Cycloocten-1-yl(trimethyl)silane;Trimethyl[(2E)-3-phenyl-2-propenyl]silane;Trimethyl[2-[(trimethylsilyl)methyl]-2-propenyl]silane;Trimethyl(3-phenyl-2-cyclohexen-1-yl)silane;t-Butyldimethyl(2-propynyloxy)silane;Dimethyldi(methacryloyloxy-1-ethoxy)silane;Trimethoxy(7-octen-1-yl)silane;Trimethyl(2,3,4,5-tetramethyl-2,4-cyclo pentadien-1-yl)silane; (2-methylallyl)triphenylsilane; (1-hydroxyallyl)trimethylsilane; (3-methyl-3-butenyl)(triphenyl)silane; 1-cyclododecen-1-yl(methyl)silane; 1-cyclohepten-1-yl(trimethyl)silane; [2-(cyclohexylmethyl)-2-propenyl](trimethyl)silane; 2-cyclohexen-1-yl(trimethyl)silane; bis(pentafluorophenyl)methyl(α-styryl)silane; t-butyl(dimethyl)[(2E)-2,4-pentadienyloxy]silane; or combinations thereof.
[0031] Preferred compounds are vinyltriethoxysilane, vinyltrimethoxysilane, vinyltriisopropoxysilane, vinyltri-t-butoxysilane, vinyltris(2-methoxyethoxy)silane, vinyltriacetoxysilane, trivinylmethoxysilane, trivinylethoxysilane, trivinylisopropoxysilane, divinyldimethoxysilane, divinyldiethoxysilane, vinyltrimethylsilane, vinyltriethylsilane, vinyltriisopropylsilane, vinyltributylsilane, divinyldimethylsilane, or a combination thereof. More preferred are vinyltriethoxysilane, vinyltrimethoxysilane, vinyltriisopropoxysilane, vinyltri-t-butoxysilane, or a combination thereof. Even more preferred are vinyltriethoxysilane, vinyltrimethoxysilane, or a combination thereof.
[0032] Two or more of these unsaturated silane reagents can also be used in combination.
[0033] Optionally, at least one saturated silane compound may be used in combination with these saturated silane species. In less preferred embodiments, in those embodiments that do not include unsaturated silanes having structure (I) above, saturated silane compounds may be included with the zinc-containing reagent. These saturated silanes may have the following structure (II): SiR 5 R 6 R 7 R 8 (II). In structure (II), R 5 , R 6 , R 7 , or R 8 are free of unsaturation, consisting of unsaturation, or consisting essentially of unsaturation, are hydrogen or alkyl or alkoxy groups, and may be the same or different from each other; R 1 , R 2 , R 3 , or R 4 The groups may be the same or different.
[0034] Examples of saturated silane reagents of structure (II) include, but are not limited to, tetra(alkoxy)silanes and (alkyl)(alkoxy)silanes.Specific examples of compounds include, but are not limited to, tetramethoxysilane, tetraethoxysilane, tetraisopropoxysilane, and tetrabutoxysilane; methyltris(methoxy)silane; methyltris(ethoxy)silane; methyltris(isopropoxy)silane; ethyltris(methoxy)silane; ethyltris(ethoxysilane); ethyltris(isopropoxy)silane; propyltris(methoxy)silane; propyltris(ethoxysilane); propyltris(isopropoxy)silane; or combinations thereof. When present, preferred are tetramethoxysilane, tetraethoxysilane, methyltris(methoxy)silane, methyltris(ethoxy)silane, methyltris(isopropoxy)silane, ethyltris(methoxy)silane, ethyltris(ethoxysilane), ethyltris(isopropoxy)silane, or combinations thereof. More preferred are tetramethoxysilane, tetraethoxysilane, methyltris(methoxy)silane, methyltris(ethoxy)silane, ethyltris(methoxy)silane, ethyltris(ethoxysilane), ethyltris(isopropoxy)silane, or combinations thereof. Even more preferred are tetramethoxysilane, tetraethoxysilane, methyltris(methoxy)silane, methyltris(ethoxy)silane, ethyltris(isopropoxy)silane, or combinations thereof.
[0035] Combination of a boron compound with a silicon-containing reagent of formula (I): Optionally, when the coupling agent formulation comprises, consists of, or consists essentially of at least one silicon-containing reagent of formula (I), it can advantageously further comprise, further consist of, or consist essentially of at least one borate or borate salt or boric acid reagent.
[0036] Examples include, but are not limited to, boric acid, sodium tetraborate decahydrate, sodium tetraborate pentahydrate, anhydrous sodium tetraborate, disodium octaborate tetrahydrate, anhydrous disodium octaborate, sodium metaborate, calcium borate, zinc borate, ammonium borate, or combinations thereof. Boric acid is preferred.
[0037] When present, the weight ratio of boric acid or borate to the silicon-based reagent of structure (I) is from 10:1 to 1:10, or from 2:1 to 1:8, or from 1:1 to 1:6, or from 1:3 to 1:5, or from 1:3.5 to 1:4.5.
[0038] Organic peroxide: The organic peroxide may contain a high boiling non-aromatic compound such as mineral spirits or mineral oil, which acts as a safety diluent. The organic peroxide formulation may also contain sorbitan monooleate, sorbitan dioleate, polysorbate 80, polypropylene glycol, or mixtures thereof.
[0039] The organic peroxide may be a liquid or solid organic peroxide, but must be stable (retain potency) at 20°C for at least one month, preferably at least three months. Both t-amylperoxy and t-butylperoxy type peroxides may be useful in certain embodiments of the present disclosure. In particular, preferred organic peroxides have a half-life of at least one hour at above 98°C. One-hour half-life information for various organic peroxides is provided in the Luperox® Organic Peroxides / High Polymers catalog published by Arkema (Colombes Cedex), the entire contents of which are incorporated herein by reference for all purposes. The half-life of organic peroxides at 98°C can be determined from dilute solution kinetics or by direct peroxide analysis by gas or liquid chromatography, as appropriate for the class or type of peroxide. The solid organic peroxides and solid functionalized organic peroxides can exhibit ambient 20° C. stability with no significant % assay loss for at least one month, preferably three months, as determined directly by either titration, gas chromatography, or liquid chromatography depending on the class of peroxide.
[0040] In some embodiments, the organic peroxide formulation may contain at least one stabilizer, such as, but not limited to, at least one quinone type compound or at least one nitroxide type compound, or a combination thereof. In some embodiments, the peroxide formulation containing at least one quinone compound or at least one nitroxide compound, or a combination thereof, may also contain at least one allyl compound, more preferably a diallyl compound, and even more preferably a triallyl compound, to function as an allyl coagent.
[0041] In some embodiments, the functionalized organic peroxide can be selected from room temperature stable peroxides (i.e., those with a half-life of at least 1 hour at 98°C having a carboxylic acid, one or more double bonds capable of reacting with free radicals, methoxy or hydroxyl functional groups). An example of a suitable functionalized peroxide includes, but is not limited to, t-butyl peroxymaleic acid available from Arkema under the trade name Luperox® PNP-25. This carboxylic acid functionalized organic peroxide can be blended with various additives disclosed herein, including acids such as itaconic acid, its anhydrides and / or its allyl esters. The coupling agent formulation may further include a carrier, such as, but not limited to, particulate cellulosic materials, particulate organic or inorganic materials, such as particulate polymers, silica, clay, dried wood flour, dried sawdust, cellulose acetate butyrate powder, to create a novel coupling agent masterbatch. These carriers are described in more detail below.
[0042] The organic peroxide suitable for use in the practice of some embodiments of the present invention can be selected from organic peroxides that are stable at room temperature. The organic peroxide can be in liquid form, solid form, solid flakes, solid powder form spread on inert filler, meltable solid form, or castable paste form. These various peroxide forms can be used in the coupling agent composition disclosed herein. Suitable organic peroxides may be capable of decomposing to form reactive free radicals when exposed to a heat source, for example, in an extruder.
[0043] The organic peroxide suitable for use in certain embodiments of the zinc-containing and / or silicon-containing reagent coupling agent composition for cellulosic-polymer composites can be selected from room temperature stable peroxides having carboxylic acid, methoxy or hydroxyl functional groups. In the present invention, "room temperature stable" means an organic peroxide that has not decomposed, i.e., retains its assay, after at least 3 months at 20°C. In the present invention, a room temperature stable organic peroxide can be defined as having a half-life of at least 1 hour at 98°C. An exception to this rule applies to diacyl solid peroxides: non-limiting examples such as dibenzoyl peroxide; 2,4-dichlorobenzoyl peroxide; or p-methyldibenzoyl peroxide are thermally stable at an ambient temperature of 20°C, but have a half-life of less than 1 hour at 98°C.
[0044] Examples of suitable organic peroxide classes include, but are not limited to, the diacyl peroxide, peroxyester, monoperoxycarbonate, peroxyketal, hemiperoxyketal, peroxydicarbonate solid at ambient temperature (20° C.), and dialkyl peroxide classes, as well as t-butylperoxy and t-amylperoxy classes. In addition, cyclic organic peroxides, such as Trigonox® 301 and Trigonox® 311 peroxides from Nouryon, are contemplated. Suitable peroxides are described in "Organic Peroxides" by Jose Sanchez and Terry N. Myers; Kirk Othmer Encyclopedia of Chemical Technology, Fourth Edition, Volume 18, (1996), the disclosure of which is incorporated herein by reference in its entirety for all purposes. Thermally stable functionalized peroxides having carboxylic acid, hydroxyl, and / or free radical reactive unsaturated groups are also suitable. The organic peroxide may contain mineral spirits, mineral oil, or food grade white mineral oil to function as a safe diluent.
[0045] The organic peroxide may also be extended onto inert fillers (e.g., wood flour, sawdust, bamboo flour, straw, straw powder, rice husk, wheat straw, hemp, flax, peanut shell powder, waste paper, waste cardboard, Burgess clay, kaolin clay, calcium carbonate, silica, fumed silica, precipitated silica, gypsum, calcium silicate, cellulose acetate butyrate) or used in powder or pellet form as a peroxide masterbatch on EPDM (ethylene propylene diene monomer rubber), EPM (ethylene propylene rubber), PE (polyethylene), HDPE (high density polyethylene), PP (polypropylene), microcrystalline wax, polycaprolactone, where the peroxide concentration may vary from 1% to 80% by weight, preferably 0.1% to 60% by weight, more preferably 0.1% to 40% by weight.
[0046] Examples of suitable organic peroxides include di-t-butyl peroxide; t-butylcumyl peroxide; t-amyl cumyl peroxide; dicumyl peroxide; 2,5-di(cumylperoxy)-2,5-dimethylhexane; 2,5-di(cumylperoxy)-2,5-dimethylhexyne-3; 4-methyl-4-(t-butylperoxy)-2-pentanol; 4-methyl-4-(t-amylperoxy)-2-pentanol; 4-methyl-4-(cumylperoxy)-2-pentanol; 4-methyl-4-(t-butylperoxy)-2-pentanone. 4-Methyl-4-(t-amylperoxy)-2-pentanone;4-Methyl-4-(cumylperoxy)-2-pentanone;2,5-Dimethyl-2,5-di(t-butylperoxy)hexane;2,5-Dimethyl-2,5-di(t-amylperoxy)hexane;2,5-Dimethyl-2,5-di(t-butylperoxy)hexyne-3;2,5-Dimethyl-2,5-di(t-amylperoxy)hexyne-3;2,5-Dimethyl-2-t-butylperoxy-5-hydroperoxyhexane;2,5-Dimethyl-2-cumylperoxy-5-hydroperoxyhexane Peroxyhexane;2,5-Dimethyl-2-t-amylperoxy-5-hydroperoxyhexane;m / p-α,α-Di(t-butylperoxy)diisopropylbenzene;m-Di(t-butylperoxy)diisopropylbenzene;p-Di(t-butylperoxy)diisopropylbenzene;1,3,5-Tris(t-butylperoxyisopropyl)benzene;1,3,5-Tris(t-amylperoxyisopropyl)benzene;1,3,5-Tris(cumylperoxyisopropyl)benzene;Di[1,3-dimethyl-3-(t-butyl Peroxy)butyl]carbonate;Di[1,3-dimethyl-3-(t-amylperoxy)butyl]carbonate;Di[1,3-dimethyl-3-(cumylperoxy)butyl]carbonate;Di-t-amyl peroxide;t-Amyl peroxide;t-Butylperoxy-isopropenylcumyl peroxide;t-Amylperoxy-isopropenylcumyl peroxide;2,4-Diallyloxy-6-t-butylperoxide-1,3,5-triazine;2,4-Diallyloxy-6-t-amylperoxide-1,3,5-triazine;Exemplary solid room temperature stable peroxydicarbonates include, but are not limited to, di(2-phenoxyethyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, dimyristylperoxydicarbonate, dibenzylperoxydicarbonate, and di(isobornyl)peroxydicarbonate. Exemplary solid room temperature stable peroxydicarbonates include, but are not limited to, di(2-phenoxyethyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, dimyristylperoxydicarbonate, dibenzylperoxydicarbonate, and di(isobornyl)peroxydicarbonate. Solid diacyl peroxides include dibenzoyl peroxide; 2,4-dichlorobenzoyl peroxide; and di(methylbenzoyl) peroxide.
[0047] Other dialkyl-type organic peroxides that can be used alone or in combination with other organic peroxides contemplated by this disclosure are those selected from the group represented by the following formula: [ka] In the formula, R 4 and R 5 are independently located at the meta or para position, may be the same or different, and are selected from hydrogen or linear or branched alkyl of 1 to 6 carbon atoms. Examples include dicumyl peroxide and isopropylcumyl peroxide.
[0048] Other dialkyl peroxides include, but are not limited to, 3-cumylperoxy-1,3-dimethylbutyl methacrylate; 3-t-butylperoxy-1,3-dimethylbutyl methacrylate; 3-t-amylperoxy-1,3-dimethylbutyl methacrylate; tri(1,3-dimethyl-3-t-butylperoxybutyloxy)vinylsilane; 1,3-dimethyl-3-(t-butylperoxy)butyl N-[1-{3-(1-methylethenyl)phenyl}-1-methylethyl]carbamate; 1,3-dimethyl-3-(t-amylperoxy)butyl N-[1-{3-(1-methylethenyl)phenyl}-1-methylethyl]carbamate; 1,3-dimethyl-3-(cumylperoxy))butyl N-[1-{3-(1-methylethenyl)phenyl}-1-methylethyl]carbamate.
[0049] Other variations of dialkyl-type peroxides containing two different peroxide groups with different chemical and / or thermal reactivities can be included in the present invention, including, but not limited to, 2,5-dimethyl(2-hydroperoxy-5-t-butylperoxy)hexane and 2,5-dimethyl(2-hydroperoxy-5-t-amylperoxy)hexane.
[0050] In the group of diperoxyketal type organic peroxides, suitable compounds include, but are not limited to, 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane; 1,1-di(t-amylperoxy)-3,3,5-trimethylcyclohexane; 1,1-di(t-butylperoxy)cyclohexane; 1,1-di(t-amylperoxy)cyclohexane; n-butyl 4,4-di(t-amylperoxy)valerate; ethyl 3,3-di(t-butylperoxy)butyrate; 2,2-di(t-amylperoxy)propane; 3,6,6,9,9-pentamethyl-3-ethoxycarbonylmethyl-1,2,4,5-tetraoxacyclononane; n-butyl-4,4-bis(t-butylperoxy)valerate; ethyl-3,3-di(t-amylperoxy)butyrate; and mixtures thereof.
[0051] Other organic peroxides that can be used in accordance with at least one embodiment of the present disclosure include benzoyl peroxide, OO-t-butyl-O-hydrogen-monoperoxy-succinate, and OO-t-amyl-O-hydrogen-monoperoxy-succinate.
[0052] Exemplary cyclic ketone peroxides are compounds having the general formulas (I), (II) and / or (III). [ka] (I) [ka] (II) [ka] (III) In the formula, R 1 ~R 10 is independently selected from the group consisting of hydrogen, C1-C20 alkyl, C3-C20 cycloalkyl, C6-C20 aryl, C7-C20 aralkyl, and C7-C20 alkaryl, which groups may include linear or branched alkyl character; R 1 ~R 10 Each of may be substituted with one or more groups selected from hydroxy, C1 to C20 alkoxy, linear or branched C1 to C20 alkyl, C6 to C20 aryloxy, halogen, ester, carboxy, nitride, and amido.
[0053] Examples of suitable cyclic ketone peroxides include, but are not limited to, 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane (or methyl ethyl ketone peroxide cyclic trimer), methyl ethyl ketone peroxide cyclic dimer, and 3,3,6,6,9,9-hexamethyl-1,2,4,5-tetraoxacyclononane.
[0054] Examples of peroxyesters include 2,5-dimethyl-2,5-di(benzoylperoxy)hexane; t-butyl perbenzoate; t-butyl peroxyacetate; t-butyl peroxy-2-ethylhexanoate; t-amyl perbenzoate; t-amyl peroxyacetate; t-butyl peroxyisobutyrate; 3-hydroxy-1,1-dimethyl t-butylperoxy-2-ethylhexanoate; OO-t-amyl-O-hydrogen-monoperoxysuccinate. t-butylperoxy-3,5,5-trimethylhexanoate; t-butyl-peroxy-(cis-3-carboxy)propionate; and allyl 3-methyl-3-t-butylperoxybutyrate. Exemplary monoperoxycarbonates include OO-t-butyl-O-isopropyl monoperoxycarbonate; OO-t-amyl-O-isopropyl monoperoxycarbonate; OO-t-butyl-O-(2-ethylhexyl) monoperoxycarbonate; OO-t-amyl-O-(2-ethylhexyl) monoperoxycarbonate; 1,1,1-tris[2-(t-butylperoxy-carbonyloxy)ethoxymethyl]propane; 1,1,1-tris[2-(t-amylperoxy-carbonyloxy)ethoxymethyl]propane; 1,1,1-tris[2-(cumylperoxy-carbonyloxy)ethoxymethyl]propane; OO-t-amyl-O-isopropyl monoperoxycarbonate.
[0055] Other peroxides that may be used in accordance with at least one embodiment of the present disclosure include functionalized peroxyester type peroxides: OO-t-butyl-O-hydrogen-monoperoxy-succinate; OO-t-amyl-O-hydrogen-monoperoxysuccinate; OO-t-amylperoxymaleic acid and OO-t-butylperoxymaleic acid.
[0056] Also suitable in the practice of this invention are organic peroxide branched oligomers containing at least three peroxide groups, including compounds represented by the structure: [ka] where the sum of W, X, Y and Z is 6 or 7. An example of this type of uniquely branched organic peroxide is the tetrafunctional polyether tetrakis(t-butylperoxycarbonate). An example of this type of peroxide is Luperox® JWEB50 (Arkema).
[0057] Exemplary hemiperoxyketal class organic peroxides include 1-methoxy-1-t-amylperoxycyclohexane; 1-methoxy-1-t-butylperoxycyclohexane; 1-methoxy-1-t-amylperoxy-3,3,5-trimethylcyclohexane; 1-methoxy-1-t-butylperoxy-3,3,5-trimethylcyclohexane. An example of this type of peroxide is Luperox® V10 (Arkema), which is 93% assay 1-methoxy-1,1-dimethylpropylperoxycyclohexane.
[0058] Exemplary diacyl peroxides include, but are not limited to, di(4-methylbenzoyl) peroxide; di(3-methylbenzoyl) peroxide; di(2-methylbenzoyl) peroxide; didecanoyl peroxide; dilauroyl peroxide; 2,4-dibromobenzoyl peroxide; succinic acid peroxide; dibenzoyl peroxide; di(2,4-dichloro-benzoyl) peroxide.Imide peroxides of the type described in PCT Publication No. 97 / 03961 are also suitable for use, and are incorporated herein by reference for all purposes.
[0059] The functionalized organic peroxides are suitable for use in zinc-containing and / or silicon-containing agent coupling agent formulations for cellulosic-polymer composites. An example of a functionalized organic peroxide is, but is not limited to, t-butylperoxymaleic acid. Examples of functionalized peroxides include, but are not limited to, t-butylperoxymaleic acid; t-amylperoxymaleic acid; t-butylperoxy-isopropenylcumyl peroxide; t-amylperoxy-isopropenylcumyl peroxide; 4-methyl-4-(t-butylperoxy)-2-pentanol; 4-methyl-4-(t-amylperoxy)-2-pentanol; 4-methyl-4-(cumylperoxy)-2-pentanol; 2,5-dimethyl-(2-hydroperoxy-5-t-butylperoxy)hexane and 2,5-dimethyl-(2-hydroperoxy-5-t-amylperoxy)hexane; 2,4-diallyloxy-6-t-butylperoxy-1,3,5-triazine; 2,4-diallyloxy-6-t-amylperoxy-1,3,5-triazine; and mixtures thereof.Preferred organic peroxides include t-butylperoxymaleic acid; 1-methoxy-1-t-amylperoxycyclohexane; dilauryl peroxide; t-butylperoxy-2-ethylhexanoate; 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane; 1,1-di(t-amylperoxy)cyclohexane; 1,1-di(t-butylperoxy)cyclohexane; t-butylperoxy-3,5 ,5-Trimethylhexanoate;t-Amyl peroxyacetate;t-Butyl peroxyacetate;t-Amyl perbenzoate;t-Butyl perbenzoate;OO-t-Butyl-O-isopropyl monoperoxycarbonate;OO-t-Amyl-O-isopropyl monoperoxycarbonate;OO-t-Butyl-O-(2-ethylhexyl) monoperoxycarbonate;OO-t-Amyl-O-(2-ethylhexyl) monoperoxycarbonate Peroxycarbonate; dicumyl peroxide; Luperox® JWEB-50, polyether poly-t-butyl peroxycarbonate (Arkema); Luperox® 313, a complex mixture of peroxides containing <15% by weight of t-butylcumyl peroxide (Arkema); Luperox® D-68, a complex mixture of dicumyl peroxide, di-t-butylperoxydiisopropylbenzene and t-butylcumyl peroxide (Arkema); Luperox® D-446-B, a complex mixture of di-t-butylperoxydiisopropylbenzene and t-butylcumyl peroxide (Arkema); t-butylcumyl peroxide; t-butylperoxy-isopropenylcumyl peroxide; m / p-di-t-butylperoxydiisopropylbenzene and mixtures thereof.
[0060] More preferred peroxides are t-butylperoxymaleic acid; 1-methoxy-1-t-amylperoxycyclohexane; dilauryl peroxide; t-butylperoxy-2-ethylhexanoate; 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane; 1,1-di(t-amylperoxy)cyclohexane; 1,1-di(t-butylperoxy)cyclohexane; t-butylperoxy-3,5,5-trimethylhexanoate; t-amylperoxyacetate; t-butylperoxyacetate; t-amylperbenzoate; t-butylperbenzoate; OO-t-butyl-O-isopropyl monoperoxycarbonate; OO-t-amyl-O-isopropyl Pyl monoperoxycarbonate; OO-t-butyl-O-(2-ethylhexyl) monoperoxycarbonate; OO-t-amyl-O-(2-ethylhexyl) monoperoxycarbonate; dicumyl peroxide; Luperox® 313, a complex mixture of peroxides containing <15% by weight of t-butylcumyl peroxide (Arkema); Luperox® D-68, a complex mixture of dicumyl peroxide, di-t-butylperoxydiisopropylbenzene and t-butylcumyl peroxide (Arkema); t-butylperoxy-isopropenylcumyl peroxide; m / p-di-t-butylperoxydiisopropylbenzene and mixtures thereof.
[0061] More preferably, t-butylperoxymaleic acid; t-butylperoxy-2-ethylhexanoate; 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane; 1,1-di(t-amylperoxy)cyclohexane; 1,1-di(t-butylperoxy)cyclohexane; t-butylperoxy-3,5,5-trimethylhexanoate; t-amylperbenzoate; t-butylperbenzoate; OO-t-butyl-O-isopropyl monoperoxycarbonate; OO-t-amyl-O-isopropyl monoperoxycarbonate; OO-t-butyl-O-(2-ethyl Luperox® 313, a complex mixture of peroxides containing <15% by weight of t-butylcumyl peroxide (Arkema); Luperox® D-68, a complex mixture of dicumyl peroxide, di-t-butylperoxydiisopropylbenzene and t-butylcumyl peroxide (Arkema); t-butylperoxy-isopropenylcumyl peroxide; m / p-di-t-butylperoxydiisopropylbenzene, bis(t-butyldioxyisopropyl)benzene (VulCup®) and mixtures thereof.
[0062] Amount of zinc-containing reagent and / or silicon-containing reagent and organic peroxide in the coupling agent formulation for cellulosic-polymer composites: In some embodiments, the cellulosic-polymer composite coupling agent formulation can include 1% to 99% by weight of an organic peroxide and 99% to 1% by weight of a zinc-containing agent and / or a silicon-containing agent, based on the total weight of the formulation.
[0063] According to certain embodiments, the at least one organic peroxide is present in an amount of 1% to 95% by weight, or 5% to 95% by weight, or 10% to 90% by weight, or 20% to 99% by weight, or 30% to 90% by weight, or 40% to 75% by weight, or 40% to 70% by weight, or 40% to 65% by weight, or 45% to 80% by weight, or 45% to 75% by weight, based on the total formulation. %, or 45% to 70% by weight, or 45% to 65% by weight, or 50% to 98% by weight, or 50% to 75% by weight, or 50% to 70% by weight, or 50% to 65% by weight, or 50% to 60% by weight, 1% to 50% by weight; or 1% to 40% by weight; or 1% to 25% by weight.
[0064] According to certain embodiments, the zinc-containing agent and / or silicon-containing agent may be included in the cellulosic-polymer composite coupling agent formulation in an amount of 95% to 5% by weight, or 90% to 10% by weight, or 99% to 20% by weight, or 90% to 30% by weight, or 75% to 40% by weight, or 70% to 40% by weight, or 65% to 40% by weight, or 80% to 45% by weight, or 75% to 45% by weight, or 70% to 40% by weight, or 65% to 45% by weight, or 98% to 50% by weight, or 75% to 50% by weight, or 70% to 50% by weight, or 65% to 50% by weight, or 60% to 50% by weight, based on the total weight of the cellulosic-polymer composite coupling agent formulation.
[0065] The weight ratio of organic peroxide to zinc-containing reagent and / or silicon-containing reagent may be 1:1000-1000:1, or 1:100-100:1, or 1:9-9:1, or 4:5-5:4, or 1:5-5:1, or 1:1-1:2, or 2:1-3:1, or 1:9-1:1, or 1:1-9:1, or 2:1-1:1. The ratio of organic peroxide to zinc-containing reagent and / or silicon-containing reagent may be 1:40-1:1, 1:20-1:1, 1:10-1:1, 1:5-1:1, or 1:3-1:1.
[0066] The weight ratio of zinc-containing reagent and / or silicon-containing reagent to organic peroxide may be 2:0.4. A typical cellulosic-polymer composite may comprise, consist of, or consist essentially of 40-85 wt% cellulosic material; 60-15 wt% polymer, and 1-5 wt% coupling agent formulation. The composite may comprise 45-75 wt%, 40-65 wt%, or 45-60 wt% cellulosic material. The composite may comprise 50-25 wt%, 45-30 wt%, or 40-30 wt% polymer. The composite may comprise 1-4 wt%, or 2-4 wt% coupling agent formulation.
[0067] Polymer matrix materials for cellulosic-polymer composites: Suitable polymer matrix materials for cellulosic-polymer composites include, but are not limited to, LLDPE (linear low density polyethylene), HDPE (high density polyethylene), MDPE (medium density polyethylene) and / or LDPE (low density polyethylene). Recycled polymers are also suitable. All preferably have a high melt flow index (MFI) of <40g / 10min; preferably <20g / 10min; more preferably <10g / 10min; more preferably <5g / 10min; even more preferably <1g / 10min, and most preferably <0.5g / 10min at 190°C and 2.15kg load, as described in test method ASTM 01238. The polyethylene used in the present invention is preferably of high molecular weight, with molecular weights of polyethylene grades starting from approximately 50,000g / mol to 200,000, up to about 250,000g / mol for PE types including LDPE, LLDPE, MDPE (medium density polyethylene) and HDPE or blends thereof from virgin or recycled sources. Ultra-high molecular weight polyethylene (UHWMPE) may have a molecular weight of 3,000,000 g / mol to 7,500,000 g / mol. Other polymers, such as polypropylene, acrylic, polyvinyl chloride, and polystyrene, are also suitable and are used in combination with polyethylenes.
[0068] Also contemplated are recycled polymers such as polyolefins, particularly polyethylene (e.g., HDPE, LLDPE, MDPE, and LDPE). However, low-cost ground solid polymer particles from mixed recycled polymer waste streams can be considered for some embodiments where cost is a concern. As is known in the art, polyethylene obtained from plastic waste streams can contain other polymers in addition to polyethylene, such as, for example, polystyrene, polyethylene terephthalate, polypropylene, scrap paper / cardboard, etc.
[0069] Cellulosic materials: Wood and wood products are commonly used as the cellulosic component in cellulosic-polymer composites. Wood flour is a common cellulosic filler used in cellulosic composite deck boards, fences, and siding. Wood flour is finely ground wood with a density similar to sand or sawdust, but with particle sizes ranging from fine powder to the size of rice. Most wood flour manufacturers can produce wood flour with the same overall density. All high quality wood flours are made from hardwoods for durability and strength. Very low grade wood flours are sometimes made from non-sap producing softwoods such as pine and fir. However, better and / or more economical and lower cost fillers to replace wood flour are constantly being sought. Other natural fillers that can be considered in the practice of the present invention include rice husk flour, straw flour or fiber, such as wheat straw; bamboo fiber, flax, jute, hemp, cellulose, ground wood, sawdust, palm fiber, bagasse, peanut shells, chitin, kenaf fiber. Waste paper and cardboard, alone or in combination with wood flour or sawdust, may also be used in embodiments of the present disclosure. Wood flour can be made from softwood, hardwood, or a mixture thereof. Typically, lignin is removed from the wood flour, although this is optional.
[0070] Sawdust or shavings may also be suitable for use as a filler in the cellulosic-polymer composites of certain embodiments of the present disclosure. Sawdust (or shavings) may be a by-product or waste product and is composed of fine particles of wood.
[0071] Another relatively low cost filler contemplated in the practice of the present invention is ground up retread truck tires and / or passenger tires. Worn tires may be ground into a powder useful in the present invention. The amount of ground tires may be 50% to 1% by weight of the composite.
[0072] One embodiment of the present invention is to use the regrind rubber tire filler with wood flour or other cellulosic filler, polyethylene, and at least one coupling agent and at least one organic peroxide. Other fillers that can be used in some embodiments with wood flour / sawdust (or other cellulosic materials) include chlorinated polyethylene powder and chlorosulfonated polyethylene powder. Cellulose acetate butyrate (CAB) can be used as a filler in certain embodiments. Preferred CAB grades have an upper melting point of 160° C. or less, preferably 150° C. or less, more preferably 145° C. or less, and most preferably 143° C. or less. The most preferred grade of CAB that can be included as a filler has a butyryl content of about 52%. Examples include, but are not limited to, Eastman Chemical Company's cellulose acetate butyrate (CAB-551-0.2) and (CAB-551-0.01).
[0073] Improved properties: Properties of cellulosic-polymer composites that can be improved or modified by including the zinc-containing and / or silicon-containing agent coupling agent formulation for cellulosic-polymer composites include, but are not limited to, improved compatibility of the polymer matrix with the cellulosic filler, reduced water absorption, improved stiffness, improved impact resistance, improved compatibility with other polymers, improved compatibility with fillers, and allowing for increased use of low-cost regrind materials such as, for example, paper, cardboard, waste rugs, tires, polyethylene plastic bags / bottles, and recycled PET containers. The use of recycled materials results in useful products while reducing waste streams.
[0074] For example, cellulosic-polymer composites containing the coupling agent formulations disclosed herein may improve the compatibility of polymer blends where the polymer matrix includes polyethylene and other polymers. Examples of such other polymers include, but are not limited to, polyacrylates and copolymers of polyacrylates. Elium® resins (Arkema) are contemplated. Fluoropolymers such as polyvinylidene fluoride (PVDF, e.g., Kynar® (Arkema)) and polytetrafluoroethylene (PTFE) are also contemplated in small amounts (<2% to <1% by weight of the total formulation). The coupling agents for cellulosic-polymer composites disclosed herein may be more compatible with fillers or extenders or reinforcing agents or impact modifiers than such composites that do not include the zinc-containing and / or silicon-containing agent coupling agent formulations for cellulosic-polymer composites. Cellulose acetate butyrate (CAB) may be used as a filler.
[0075] The cellulosic-polymer composite coupling agent formulation can be in solid or liquid form depending on the form of the organic peroxide and the form of the zinc-containing and / or silicon-containing reagent. The cellulosic-polymer composite zinc-containing and / or silicon-containing coupling agent formulation can also be in the form of a masterbatch formulation.
[0076] Masterbatch: A coupling agent masterbatch for a cellulosic-polymer composite is provided that can comprise, consist of, or consist essentially of (a) at least one organic peroxide; (b) at least one of (i) at least one zinc-containing agent; and / or (ii) at least one silicon-containing agent; and (c) at least one carrier for the coupling agent masterbatch.
[0077] (ii) at least one silicon-containing agent has the following structure (I): SiR 1 R 2 R 3 R 4 (I). In structure (I), R 1 , R 2 , R 3 , or R 4 at least one of R comprises, consists of, or consists essentially of at least one unsaturation, and the remaining R 1 , R 2 , R 3 , or R 4 are hydrogen or alkyl or alkoxy groups and may be the same or different.
[0078] The at least one organic peroxide, the at least one zinc-containing reagent, and the at least one silicon-containing reagent are as described above.
[0079] As known in the art, a masterbatch is a concentrated combination of cellulosic-polymer composite coupling agent formulation that is added to a polymer matrix and cellulosic filler that is processed (compounded) into a finished product such as deck boards, siding, fences, etc.
[0080] Carrier for coupling agent masterbatch: These coupling agent formulations can be spread onto fillers or blends of fillers to obtain free-flowing powder products or masterbatches. Examples of such fillers include calcium carbonate, Burgess clay, fumed silica, kaolin clay, precipitated silica, microcellulose, cellulose acetate butyrate (CAB), calcium silicate, silica, fly ash, perlite, talc, magnesium hydroxide, gypsum, silica, dry wood flour, dry sawdust, dry straw particles / flour, or mixtures thereof. Burgess clay, precipitated calcium carbonate, precipitated silica, calcium silicate, microcellulose, dry wood flour, dry sawdust, cellulose acetate butyrate, and mixtures thereof are preferred. Burgess clay, precipitated silica, calcium silicate, dry wood flour, dry sawdust, and mixtures thereof are more preferred.
[0081] The carrier for the coupling agent masterbatch for cellulosic-polymer composites can comprise, consist of, or consist essentially of one or more of the polymer and / or cellulosic filler components of the final cellulosic-polymer composite. For example, the coupling agent formulation comprising the organic peroxide and the zinc-containing and / or silane reagents of formula (I) can be mixed with wood flour, sawdust, polyethylene, calcium carbonate, synthetic calcium silicate, Burgess clay, kaolin clay, fumed silica, precipitated silica, fine cellulose, fly ash, talc, magnesium hydroxide, gypsum, dry wood flour, dry sawdust, dry straw particles, perlite, calcium silicate, and combinations thereof. In some embodiments, particulate materials may be preferred as carriers since the masterbatch can be produced by blending the organic peroxide and zinc and / or silane reagent formulation with the particulate material to form a flowable, non-caking particulate masterbatch.
[0082] Other examples of particulate carrier materials suitable for the masterbatch include, but are not limited to, dry sawdust, dry wood flour, bamboo flour, hemp flour, waste paper, waste cardboard, cellulose acetate butyrate, and combinations thereof. Also suitable are inert carriers such as silica, fumed silica, precipitated silica, talc, calcium carbonate, clay, Burgess clay, kaolin, and fly ash.
[0083] In another embodiment, the carrier material can, for example, comprise, consist of, or consist essentially of low melting waxes. The organic peroxide and zinc and / or silicon-containing agent can be melt blended with the wax, and the resulting masterbatch can then be pelletized. These waxes are considered in small amounts, so that the final cellulosic-polymer composite contains less than 5% by weight of low melting wax. Suitable waxes include, but are not limited to, biologically based waxes, such as beeswax, soy wax, bayberry wax, candelilla wax, carnauba wax, castor wax, vegetable wax, cucumber wax, rice bran wax, lanolin, and the like. Other known non-biologically based petroleum waxes can also be included.
[0084] According to one embodiment, the coupling agent formulation as disclosed herein can be melt blended with a polymeric carrier and formed into granules or pellets. Examples of suitable polymers include those suitable for use as the matrix of cellulosic-polymer composites, such as polyolefins and their copolymers, polyethylene, polypropylene, acrylic, polyvinyl chloride, polystyrene, or combinations thereof.
[0085] The combined weight percent concentration of the organic peroxide, zinc reagent of formula (I) and / or silicon-containing reagent, and optionally other additives disclosed herein, in the masterbatch can be varied depending on the desired concentration of the letdown and final cellulosic-polymer composite coupling agent formulation. Examples of suitable concentrations in the masterbatch can range from 40 to 65 weight percent, or 30 to 75 weight percent, or 50 to 70 weight percent, or 40 to 50 weight percent of the organic peroxide of structure (I) and the zinc reagent and / or silicon-containing reagent, although the range can be 1 weight percent to 80 weight percent, or 2 weight percent to 60 weight percent, or 5 weight percent to 50 weight percent, or 10 weight percent to 40 weight percent depending on the peroxide, zinc reagent, silicon-containing reagent, and other additives selected for the masterbatch blend.
[0086] Stabilizers for organic peroxides: The cellulosic-polymer composite coupling agent formulation can comprise, consist of, or consist essentially of a stabilizer for organic peroxide, such as at least one quinone type compound. In certain embodiments, when at least one quinone compound is used as a stabilizer for organic peroxide, at least one allyl compound, preferably a triallyl compound, can also be included with the organic peroxide. Examples of allyl compounds include, but are not limited to, TAC (triallyl cyanurate), TAIC (triallyl isocyanurate), triallyl trimellitate, diallyl maleate, diallyl tartrate, diallyl phthalate, diallyl carbonate, allyl phenyl ether, allyl methacrylate, and high molecular weight allyl methacrylate oligomers available from Sartomer.
[0087] In some embodiments, at least one stabilizer or free radical trap can be selected from the group consisting of nitroxides (e.g., 4-hydroxy-TEMPO) and quinones, e.g., mono-t-butylhydroquinone (MTBHQ). These stabilizers can be referred to as free radical traps (i.e., any agent that interacts with free radicals and inactivates them), and any such agent known to those skilled in the art can be employed in the practice of the present invention. Many of the hindered phenols as stabilizers can also be considered, such as olive leaf oil (oleuropein), or Irganox® 1076 or Irganox® 1010. Vitamins K1, K2, and K3 are also part of this group. As used herein, the term "quinone" encompasses both quinones and hydroquinones. Examples of quinones that can be used in the formulations of the present invention include, but are not limited to, mono-t-butylhydroquinone (MTBHQ), hydroquinone, hydroquinone monomethyl ether (HQMME) (also known as 4-methoxyphenol), mono-t-amylhydroquinone, hydroquinone bis(2-hydroxyethyl)ether, 4-ethoxyphenol, 4-phenoxyphenol, 4-(benzyloxy)phenol, 2,5-bis(morpholinomethyl)hydroquinone, and benzoquinone.
[0088] Coupling agent masterbatch production method: A method for making a coupling agent masterbatch for a cellulosic-polymer composite is provided, which can comprise, consist of, or consist essentially of steps (A) and (B).
[0089] Step (A) comprises reacting (a) at least one organic peroxide with (b) at least one of (i) at least one zinc-containing reagent; and / or (ii) at least one silicon-containing reagent having the following structure (I): SiR 1 R 2 R 3 R 4 (I) (where R 1 , R2 , R 3 , or R 4 At least one of R contains at least one unsaturation, and the remaining R 1 , R 2 , R 3 , or R 4 are hydrogen or alkyl or alkoxy groups, which may be the same or different; (c) optionally, at least one silicon-containing reagent having the following structure (II): SiR 5 R 6 R 7 R 8 (II) (where R 5 , R 6 , R 7 , or R 8 are free of unsaturation and are hydrogen or alkyl or alkoxy groups, which may be the same or different from each other, and R 1 , R 2 , R 3 , or R 4 may be the same as or different from the group. to form a cellulosic-polymer composite coupling agent blend.
[0090] (a) The organic peroxide has a half-life of at least 1 hour at 98°C.
[0091] The optional additives can be selected from the group consisting of coagulants; sulfur-containing compounds and / or elemental sulfur; and mixtures thereof. Another optional additive is boric acid or a borate salt. Other additives commonly known and used in the art include, but are not limited to, polymer stabilizers and peroxide stabilizers.
[0092] Step (B) can comprise, consist of, or consist essentially of combining the cellulosic-polymer composite coupling agent formulation with (c) at least one carrier to form a cellulosic-polymer composite coupling agent masterbatch.
[0093] According to certain embodiments of the present disclosure, the coupling agent formulation for cellulosic-polymer composites may be in the form of a liquid and at least one carrier may be in the form of a solid particulate. Suitable solid particulates that can be used in certain embodiments are calcium carbonate, Burgess clay, precipitated silica, fine cellulose, fly ash, dry wood flour, dry sawdust, dry straw particles, recycled ground wastepaper, recycled ground / shredded cardboard waste, recycled ground carpet fiber waste, recycled ground passenger / truck tires, and combinations thereof. The solid particulates may be as described above. In certain embodiments of the present invention, step (B) may include mixing the liquid coupling agent formulation with at least one carrier in the form of solid particulates to form a coupling agent masterbatch such that the coupling agent masterbatch can be in the form of solid particulates at 25° C. Thus, the coupling agent masterbatch may be in the form of a free-flowing solid particulate.
[0094] According to another embodiment, steps (A) and (B) can be carried out simultaneously, i.e., at least one organic peroxide, at least one zinc-containing agent and / or at least one silicon-containing agent, and at least one carrier material can be mixed simultaneously.For example, steps (A) and (B) can be carried out in a low shear ribbon blender, such as a Marion® ribbon blender, to form a coupling agent master batch containing the above-mentioned fine particles to form a master batch.Also, the mixing of various components can be carried out in a high shear Henschel® blender to make a free-flowing powder master batch.
[0095] The at least one organic peroxide can be selected from those described above or mixtures thereof. The at least one zinc-containing reagent and / or the at least one silicon-containing reagent can be selected from those described above or combinations thereof.
[0096] The mixing step (B) can include melt blending various components into a polymer. The melt blending can be carried out, for example, in a single screw extruder, a twin screw extruder, a ZSK mixer, a Banbury mixer, a Buss kneader, a two-roll mill, or an impeller mixer, or other types of suitable polymer melt blending equipment for producing a coupling agent masterbatch. The blending time and temperature conditions of the mixing step (B) can be selected so that the organic peroxide used decomposes by less than 4% by weight, preferably less than 2% by weight, and more preferably less than 1% by weight.
[0097] Method for producing cellulosic-polymer composites: A method for making a cellulosic-polymer composite is provided. The method comprises, consists of, or consists essentially of a step (I) of mixing components (A), (B), and (C) to form a component mixture, where components (A), (B), and (C) comprise, consist of, or consist essentially of: (A) comprises, consists of, or consists essentially of a cellulosic-polymer composite coupling agent as disclosed herein; (B) comprises, consists of, or consists essentially of a polymer matrix for a cellulosic-polymer composite as described above; and (C) comprises, consists of, or consists essentially of at least one cellulosic filler selected from those described above. The method also comprises, consists of, or consists essentially of a step (II) of forming the component mixture into a composite.
[0098] Another method for making a cellulosic-polymer composite is also provided. This method is similar to the first method, except that the other method includes, consists of, or consists essentially of using a coupling agent masterbatch. In particular, the other method is a step (I) of mixing components (A), (B) and (C) to form a component mixture. Components (A), (B) and (C) include, consist of, or consist essentially of: (A) comprises, consists of, or consists essentially of a cellulosic-polymer composite coupling agent masterbatch disclosed herein; (B) comprises, consists of, or consists essentially of a cellulosic-polymer composite polymer matrix as described above; and (C) comprises, consists of, or consists essentially of at least one cellulosic filler selected from those described above. The other method also includes, consists of, or consists essentially of a step (II) of forming the component mixture into a composite.
[0099] In both of these methods of forming cellulosic-polymer composites, the mixing step (I) may be, for example, feeding and mixing the components (A) polymer matrix, (C) cellulosic filler, and (B) either the zinc-containing and / or silicon-containing agent coupling agent formulation or coupling agent masterbatch into an extruder. For example, these components may be metered into the hopper of the extruder such that the feed of the extruder provides the majority of the mixing step. The mixing step may include dry mixing the components in a drum tumbler, ribbon blender, high shear blender, or the like, and then feeding the dry mix into the hopper of the extruder. If the coupling agent formulation or coupling agent masterbatch is in liquid form, the liquid may be metered separately into the feed throat of the extruder and the polymer matrix and filler may be mixed directly in the hopper of the extruder or dry mixed separately. Other such methods as known in the art may be used in some embodiments. For example, melt blending can be used to mix the components in a single screw extruder, twin screw extruder, ZSK mixer, Banbury mixer, Buss kneader, two roll mill, or impeller mixer, or other type of suitable polymer melt blending equipment to produce a reaction mixture. The mixing step can be part of a process to produce a finished product, such as extrusion through a die to form a solid cellulosic-polymer composite board, using a roll mill to make a sheet for use in a thermoforming process, using a blown film process, or using a compression molding process to make various parts. In some embodiments, other processes known in the art, such as injection molding, injection blow molding, thermoforming, or vacuum forming, can be performed to make a finished product.
[0100] The forming step (II) in any method of forming the composite may be, for example, extruding the mixture of components through a die attached to an extruder. The forming step may be, for example, a step of thermoforming using a set of heated dies. Other possible forming methods include injection molding, calendar molding, blow molding, foam molding, injection blow molding, vacuum molding, compression molding, thermoforming, and the like. The composite may be, for example, a polymeric lumber such as a deck board intended for use in an outdoor environment. Other useful manufactured articles include, but are not limited to, cladding, siding, outdoor furniture, exterior decks, interior flooring, indoor furniture, pallets, floors, railings, fences, siding, moldings, trim, window frames, door frames, landscape lumber, industrial cribbing, marine walls and pilings, boat slips, wall panels, and the like.
[0101] Other Additives: Fillers and / or stabilizers for the peroxide may also be included in the cellulosic-polymer composite coupling agent formulation. For example, calcium carbonate, talc, silica, fumed silica, precipitated silica, calcium carbonate, calcium silicate, diatomaceous earth, clay, Burgess clay, kaolin, fly ash, powdered polyethylene, or ground / powdered recycled passenger or truck tires, ground / powdered recycled carpet fiber, ground / powdered recycled mixed polymer streams that may contain small amounts of various polymers including polypropylene, poly(ethylene propylene) copolymers, poly(ethylene octene) copolymers, LDPE, HDPE, LLDPE; chopped glass fiber, ground paper, ground cardboard, and / or ground particle board waste may be used.
[0102] The cellulosic-polymer composite formulation may include other additives known to those skilled in the art, such as colorants, mildewcides, biocides, fillers other than wood flour, antioxidants, light / UV stabilizers, blowing or foaming agents, polymer flow aids, extrusion slip aids such as erucamide, non-metallic lubricants such as ethylene bis-stearic acid imide; Glycolube™ WP2200 from Lonza; Struktol® TPW113 and Struktol® TPW617 are non-limiting examples; mildewcides (such as Folpet® and Bethoxazin® from Zeneca Ag Products); process aids, release agents, antioxidants, antiblocking agents, and the like. Suitable release agents known in the art include fatty acids, zinc, calcium, and magnesium salts of fatty acids. Release and slip agents may be added in amounts of less than about 5% by weight based on the total weight of the final cellulosic-polymer composite.
[0103] The zinc-containing and / or silicon-containing coupling agent formulation may further include at least one sulfur-containing compound that functions as a co-curing agent. Examples of these co-curing agents include, but are not limited to, disulfides, elemental sulfur, and sulfur-containing amino acids. The Vanderbilt Rubber Handbook, 13th Edition, 1990, RT Vanderbilt Company, Inc. (the entire disclosure of which is incorporated herein by reference for all purposes) lists many types of sulfur-containing compounds used in curing rubber. Examples include, but are not limited to, monosulfides, 2-mercaptobenzothiazole (MBT), 2,2'-dithiobis(benzothiazole) (MBTS), disulfides, diallyl disulfides, polysulfides, and aryl polysulfide compounds such as amylphenol polysulfides, e.g., VULTAC® (Arkema). Specific examples include Vultac® 5, Vultac® 3, Vultac® 7, mercaptobenzothiazole disulfide (MBTS), zinc dialkyldithiophosphate (ZDDP), etc. Also included as co-curing agents are sulfur-containing amino acid compounds such as cysteine, methionine, homocysteine, taurine, n-formylmethionine, s-adenosylhomocysteine. The organic peroxide formulation may contain at least one sulfur-containing compound, particularly at least one disulfide-containing compound or elemental sulfur, or a combination thereof, as a co-curing agent.
[0104] The zinc-containing and / or silicon-containing agent coupling agent formulation may also include co-agents capable of cooperating with at least one organic peroxide. Importantly, these co-agents are different from the zinc-containing and silicon-containing agents that are part of the coupling agent formulation. Cross-linking co-agents have a different function than peroxides. Without wishing to be limited by theory, the co-agents can be activated with the aid of free radical initiators such as organic peroxides. When activated in this manner during the decomposition of the peroxide, the co-agent forms cross-linked bridges with the polymer, and thus is incorporated into the cross-linked polymer chains, unlike the peroxides. Examples of suitable co-agents include, but are not limited to, allyl, acrylic, methacrylic and styrene-containing compounds that are different from the zinc-containing reagents disclosed herein. Monoallyl, diallyl and triallyl compounds are contemplated. Examples include, but are not limited to, allyl phenyl ether, epoxidized allyl phenyl ether, allyl methacrylate monomer and oligomer (sold by Sartomer), diallyl maleate, diallyl disulfide, diallyl itaconate, diallyl tartrate, diallyl phthalate, trimethylolpropane diallyl ether triallyl trimellitate, triallyl cyanurate, partially epoxidized triallyl cyanurate, triallyl isocyanurate, partially epoxidized triallyl cyanurate, and trimethylolpropane triallyl ether. Other examples of such coagents include, but are not limited to, alpha-methylstyrene dimer, or poly(methyl methacrylate) dissolved in methyl methacrylate monomer (available from Arkema under the name Elium®). The present disclosure contemplates the use of Elium® resin in combination with at least one organic peroxide formulation. Elium® can also be used in combination with other components disclosed herein.
[0105] Mixtures of any or all of these additives are contemplated.
[0106] Excluded from certain embodiments of the present invention are "stand oils" made by polymerization of natural or bio-based oils. Made with polyester resins and various acids as listed in the disclosure herein. Also excluded from certain embodiments is water added as a separate component to the formulation in amounts of about 5%, about 4%, about 3%, about 2%, about 1%, about 0.5% weight percent or about 1000 ppm by weight. Inorganic peroxides are excluded. Intentional inclusion of water or use of additives diluted with significant amounts of water is undesirable in the practice of the present invention. AIBN (azobisisobutyronitrile) or azo initiators are excluded. Any or all of these compounds may be present in the cellulosic-polymer composite coupling agent formulation at levels of 5%, 4%, 3%, 2%, 1% or less by weight based on the total weight of the organic peroxide and zinc-containing and / or silicon-containing reagents. Preferably, none of these compounds are present in the formulation.
[0107] Reference test method and equipment used in the practice of this invention: Standard Guide for Evaluation of Mechanical and Physical Properties of Wood-Plastic Composite Products ASTM D7031-11(2019). This ASTM standard guide discloses test methods suitable for evaluating a wide range of performance properties of cellulosic-polymer composites, such as wood-polymer composite (WPC) products.
[0108] The following test methods are used: ASTM D6109-19(2019) Test Method for Flexural Properties of Unreinforced and Reinforced Plastic Lumber and Related Products; ASTM D6341-98(1998) Test Method for Determination of the Coefficient of Linear Thermal Expansion of Plastic Lumber and Plastic Lumber Articles at 30°F to 140°F (34.4°C to 60°C); ASTM D4442-16(2016) Test Method for Direct Determination of Moisture Content of Wood and Wood-Based Materials; ASTM D4761-19(2019) Test Method for Mechanical Properties (e.g., Modulus of Rupture: MOR) of Lumber and Wood-Based Structural Materials; ASTM D1238-13(2013) Standard Test Method for Melt Flow Rate of Thermoplastics by Extrusion Plastometer (used to measure the Melt Flow Index (MFI) of polyethylene); ASTM D5289-19a(2019) Standard Test Method for Rubber Properties-Vulcanization Using a Rotorless Curing Meter (can be used for polyethylene); and ASTM D4440-15(2015) Standard test methods for plastics: Dynamic mechanical properties-Melt rheology.
[0109] Non-limiting aspects of the disclosure are summarized below. EXAMPLES
[0110] Sample Mixing Procedure Wood flour (40M1 hardwood 40 mesh wood flour, American Wood Fibers) was placed in a stainless steel pan in a ventilated oven and heated at 110 °C for 22-24 hours. The dried wood flour, high density polyethylene, talc, zinc stearate, N,N'-ethylene bisstearamide, and other ingredients (including peroxide and additives) were weighed on a balance and loaded into a 1 gallon polyethylene bag (total mass of mixing material = ~230 grams), the bag was sealed, and initial mixing was performed by shaking the bag by hand (~30 seconds). The contents of the bag were then transferred to an internal mixer (Brabender Intelli Torque Plasticorder, 3 pieces, 350cc prep mixer bowl, Banbury blade, WinMix software) and mixed at 150 °C, 50 RPM until a stable torque reading was reached. The materials were removed from the mixing bowl and then added back to the mixing bowl and mixed (50 RPM, 150 °C) for a total of 3 minutes. The material was then removed from the bowl and final compounding was performed using a press (Carver 15 ton Model 3893; 10 ksi, 10 seconds at 150°C).
[0111] Plaque manufacturing procedure A thin metal sheet (8" x 8" x 0.035") was placed on top of an 8" x 8" x 0.108" stainless steel plate, and then an 8" x 8" x 0.016mm aluminum foil was placed on top of it. An 8" x 8" x 0.125" stainless steel plaque frame was placed on top of the aluminum foil with an inner cavity dimension of 6" x 6". Approximately 90 grams of compounded wood plastic composite was placed in the plaque frame cavity and then covered with layers of aluminum foil, thin metal sheet, and stainless steel plate. The entire plaque assembly was subjected to 15 kpsi pressure (Wabash Genesis 30 ton G30H press) at 185°C for 13 minutes. The plaque frame and samples were removed from the press and allowed to cool to below 35°C. After cooling, rectangular (4" x 0.5") pressed material strips were cut from the plaques (using a band saw) for bend testing.
[0112] Physical Property Testing Procedures Three-point bend tests were performed using an Instron 33R4204 incorporating a 2-inch span, a 500N static load cell, and a bend rate of 0.5 in / min in accordance with ASTM D790. Reported values for modulus of rupture (MOR) and modulus of elasticity (MOE) are average values obtained from measurements of three to five samples cut from each test plaque, with outliers (defined as showing a deviation of 5% or more from the average of the remaining measurements) excluded from the calculations.
[0113] The results are shown below.
[0114] [Table 1] **Maleic anhydride (MAH) grafted high density polyethylene (HPDE) polymer in powder form. *These are the means and standard deviations of data from triplicate runs of the same composition.
[0115] [Table 2]
[0116] Examples 5-6 show that the additives of the present invention work in conjunction with bio-based additives, including but not limited to magnesium sulfate, magnesium oxide, borax, and boric acid.
[0117] The extruded wood polymer board samples of Examples 1 and 2 made with the coupling agent of the present invention were tested using the methods described in the detailed description. All boards showed improved physical properties compared to wood polymer composite boards without coupling agent and compared to comparative samples made with maleic anhydride. The improved modulus of the samples made from the coupling agent formulation of the present invention is particularly important in reducing the effects of creep in fencing and siding, as well as other creep sensitive applications.
[0118] Hypothetical Example 1: Improvement of creep by the coupling agent of the present invention: Compound wood-plastic composites made with the additive of the present invention, prepared as described above, are subjected to creep tests as described in ASTM D2990-17 and ASTM D6112-18. The creep of composites made with the additive of the present invention is significantly less than composites made without a coupling agent or compatibilizing additive. The creep of composites made with the additive of the present invention is significantly less than composites made incorporating maleic anhydride grafted polymers as coupling agents.
[0119] Scenario 2: Extrusion of cellulosic-polymer composite: Dry wood flour, high density polyethylene, talc, zinc stearate, N,N'-ethylene bisstearamide, and other components of the present invention (including peroxide and additives) are dry mixed in a ribbon blender and then charged into a gravity hopper connected to a co-rotating twin screw extruder. In the twin screw extruder, the ingredients are heated and mixed and then passed through a heated profile die. After extrusion from the die, the profiles are cooled in a cooling tank and cut to lengths suitable for various applications (such as decking, siding, or physical property testing). Profiles made with the coupling agent formulation of the present invention have significantly improved physical properties compared to those made without coupling agent or those formulated with maleic anhydride grafted polymer as coupling agent. Physical properties include mechanical strength (break resistance and stiffness), water absorption, impact resistance, and creep. Similar results are obtained when coupling agent is formulated into the composite using a masterbatch of coupling agent.
[0120] The above description of various embodiments of the present invention has been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed. Numerous modifications or variations are possible in light of the above teachings. The forms discussed were chosen and described in order to best illustrate the principles of the invention and its practical application, so that those skilled in the art can utilize the invention with various modifications in various forms suited to the particular uses intended. All such modifications and variations are within the scope of the present invention, as determined by the appended claims, when interpreted in accordance with the breadth to which they are fairly, legally, and equitably entitled.
Claims
1. 1. A coupling agent formulation for a cellulosic-polymer composite comprising: (a) at least one organic peroxide; (b) at least one of (i) at least one zinc-containing reagent; and / or (ii) at least one silicon-containing reagent having the following structure (I): SiR 1 R 2 R 3 R 4 (I) (In the formula, R 1 , R 2 , R 3 , or R 4 At least one of R contains at least one unsaturation, and the remaining R 1 , R 2 , R 3 , or R 4 are hydrogen or alkyl or alkoxy groups, and may be the same or different. A coupling agent formulation comprising:
2. (c) at least one silicon-containing reagent having the following structure (II): SiR 5 R 6 R 7 R 8 (II) (In the formula, R 5 , R 6 , R 7 , or R 8 R is free of unsaturation and is hydrogen or an alkyl or alkoxy group, and may be the same or different from each other. R is free of unsaturation. 1 , R 2 , R 3 , or R 4 may be the same as or different from the group.) 2. The coupling agent formulation of claim 1 further comprising:
3. 2. The coupling agent formulation of claim 1 comprising at least one silicon-containing agent of formula (I) and further comprising at least one of boric acid, sodium tetraborate decahydrate, sodium tetraborate pentahydrate, sodium tetraborate anhydrous, disodium octaborate tetrahydrate, disodium octaborate anhydrous, sodium metaborate, calcium borate, zinc borate, ammonium borate, or combinations thereof.
4. The at least one zinc-containing reagent - organozinc compounds containing Zn-O functional groups, organozinc compounds containing a Zn-O functional group and at least one polymerizable substituent; organozinc compounds containing a Zn-O functional group and at least one unsaturation; - non-organic zinc oxide or its hydrates, zinc halide; or ・Combinations of these The coupling agent formulation of claim 1 comprising at least one of:
5. The at least one silicon-containing agent having structure (I) is selected from the group consisting of vinyl(alkoxy)silanes; vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, vinyltri-t-butoxysilane; vinyltris(2-methoxyethoxy)silane; vinyltriacetoxysilane; trivinylmethoxysilane; trivinylethoxysilane; trivinylisopropoxysilane, divinyldimethoxysilane; divinyldiethoxysilane; vinyl(alkyl)silanes; vinyltrimethylsilane; vinyltriethylsilane; vinyltriisopropylsilane; vinyltributylsilane; divinyldimethylsilane; poly(vinyl)silane; divinylsilane; trivinylsilane; tetravinylsilane; (vinyl)(alkyl)(alkoxy)silanes; vinyldimethylethoxysilane; vinylmethyldiethoxysilane; 1,3-divinyltetramethyldisiloxane; 1,3,5-trivinyl-1,3,5-trimethylcyclotrisiloxane; 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane; vinylmethylbis(trimethylsiloxy)silane; 1,1,3,3-Tetravinyldimethyldisiloxane; Vinyl-terminated polydimethylsiloxane; 1,4-divinyl-1,1,4,4-tetramethyl-1,4-disilabutane; Methylbis(trimethylsilyloxy)vinylsilane; 2-(dimethylvinylsilyl)pyridine; Tris(2-methoxyethoxy)(vinyl)silane; Triacetoxy(vinyl)silane; Tris(trimethylsiloxy)(vinyl)silane; 1-cyclopentasiloxane (5,5-dimethyl-1-cyclopenten-1-yl)(trimethyl)silane; Trimethyl(6-methyl-1-cyclohexen-1-yl)silane; (4-methoxy-1-cyclohexen-1-yl)(trimethyl)silane; Trimethyl(4-methyl-1,5-cyclohexadien-1-yl)silane; Trimethyl(5-methyl-1,5-cyclohexadiene (6,6-dimethyl-1-cyclohexen-1-yl)(trimethyl)silane; allyl(methyl)1-naphthyl(phenyl)silane; trimethyl(1-phenyl-2-propenyl)silane; 2-cycloocten-1-yl(trimethyl)silane; trimethyl[(2E)-3-phenyl-2-propenyl]silane; trimethyl[2-[(trimethylsilyl)methyl]-2-propenyl]silane; trimethyl(3-phenyl-2-cyclohexen-1-yl)silane dimethyl-di(methacryloyloxy-1-ethoxy)silane; trimethoxy(7-octen-1-yl)silane; trimethyl(2,3,4,5-tetramethyl-2,4-cyclopentadiene-1-yl)silane; (2-methyl-allyl)-triphenyl-silane; (1-hydroxy-allyl)-tri-methyl-silane; (3-methyl-3-butenyl)(triphenyl)silane; 2. The coupling agent formulation of claim 1 comprising at least one of 1-cyclododecen-1-yl(methyl)silane; 1-cyclohepten-1-yl(trimethyl)silane; [2-(cyclohexylmethyl)-2-propenyl](trimethyl)silane; 2-cyclohexen-1-yl(trimethyl)silane; bis(pentafluorophenyl)methyl(α-styryl)silane; t-butyl(dimethyl)[(2E)-2,4-pentadienyloxy]silane; or combinations thereof.
6. 3. The coupling agent formulation of claim 2, wherein the at least one silicon-containing agent having structure (II) comprises at least one of tetra(alkoxy)silane; tetramethoxysilane; tetraethoxysilane; tetraisopropoxysilane; tetrabutoxysilane; (alkyl)(alkoxy)silane; methyltris(methoxy)silane; methyltris(ethoxy)silane; methyltris(isopropoxy)silane; ethyltris(methoxy)silane; ethyltris(ethoxysilane); ethyltris(isopropoxy)silane; propyltris(methoxy)silane; propyltris(ethoxysilane); propyltris(isopropoxy)silane; or combinations thereof.
7. 2. The coupling agent formulation of claim 1, wherein said at least one organic peroxide has a half-life of at least 1 hour at 98°C.
8. 2. The coupling agent formulation of claim 1, wherein said at least one organic peroxide comprises at least one functionalized organic peroxide.
9. 2. The coupling agent formulation of claim 1, wherein the at least one organic peroxide comprises at least one of a diacyl peroxide; a peroxyester; a monoperoxycarbonate; a peroxyketal; a dialkyl peroxide; a t-butyl peroxide; a t-amyl peroxide; a carboxylic acid functionalized peroxide, a hydroxyl functionalized peroxide, a functionalized peroxide having a free radical reactive unsaturated group; 3,6,9-triethyl-3,6,9-trimethyl-1,2,4,5,7,8-hexoxonane, 3,3,5,7,7-pentamethyl-1,2,4-trioxepane, t-butylperoxymaleate, or a combination thereof.
10. The at least one zinc-containing reagent may be selected from the group consisting of zinc diacrylate, zinc di(meth)acrylate, zinc monoacrylate, zinc monomethacrylate, zinc alkoxide, zinc methoxide, zinc ethoxide, zinc isopropoxide, zinc methoxyethoxide, zinc carboxylate, zinc bis(acetate), zinc bis(2-ethylhexanoate), zinc bis(neodecanoate), zinc bis(cyclohexanebutyrate), zinc naphthenate, zinc undecylenate, oxo[hexa(trifluoroacetato)]tetrazinc, zinc(acetylacetonate), zinc bis(2,2,6,6-tetrazinc oxo[hexa(trifluoroacetato)]tetrazinc, 2. The coupling agent formulation of claim 1, comprising at least one of the following: zinc bis(hexafluoroacetylacetonate); zinc formate; zinc oxide; zinc dithiodicarbamate; zinc dimethyldithiocarbamate; zinc diethyldithiocarbamate; zinc dibutyldithiocarbamate; zinc halide; zinc chloride, zinc bromide, zinc fluoride, zinc iodide; zinc sulfonate; zinc carbonate; zinc nitrate; zinc hydrate; zinc tetrahydrofuran adduct; N,N,N',N'-tetramethylethylenediamine adduct; or combinations thereof.
11. 1. A coupling agent masterbatch for a cellulosic-polymer composite comprising: (a) at least one organic peroxide; (b) at least one of: (i) at least one zinc-containing reagent; and / or (ii) at least one silicon-containing reagent having the following structure (I): SiR 1 R 2 R 3 R 4 (I) (In the formula, R 1 , R 2 , R 3 , or R 4 At least one of R contains at least one unsaturation, and the remaining R 1 , R 2 , R 3 , or R 4 are hydrogen or alkyl or alkoxy groups, and may be the same or different; (c) at least one carrier for the coupling agent masterbatch; A coupling agent masterbatch comprising:
12. (d) at least one silicon-containing reagent having the following structure (II): SiR 5 R 6 R 7 R 8 (II) (In the formula, R 5 , R 6 , R 7 , or R 8 R is free of unsaturation and is hydrogen or an alkyl or alkoxy group, and may be the same or different from each other. R is free of unsaturation. 1 , R 2 , R 3 , or R 4 may be the same as or different from the group.) 12. The coupling agent masterbatch of claim 11, further comprising:
13. 12. The coupling agent masterbatch of claim 11, wherein the at least one carrier for the coupling agent masterbatch comprises at least one of polyethylene, polypropylene, acrylic, polyvinyl chloride, polystyrene, fumed silica, perlite, calcium carbonate, Burgess clay, clay, kaolin clay, talc, magnesium hydroxide, gypsum, precipitated silica, cellulose acetate butyrate (CAB), fine cellulose, fly ash, dried wood flour, dried sawdust, dried straw particles, calcium silicate, silica, or combinations thereof.
14. The (i) at least one zinc-containing reagent or combination thereof - organozinc compounds containing Zn-O functional groups, organozinc compounds containing a Zn-O functional group and at least one polymerizable substituent; organozinc compounds containing a Zn-O functional group and at least one unsaturation; - non-organic zinc oxide or its hydrates, zinc halide; or ・Combinations of these 12. The coupling agent masterbatch of claim 11, comprising at least one of:
15. 12. The coupling agent masterbatch of claim 11, wherein said at least one organic peroxide has a half-life of at least 1 hour at 98°C.
16. 12. The coupling agent masterbatch of claim 11, wherein said at least one organic peroxide comprises at least one functionalized organic peroxide.
17. 12. The coupling agent master batch of claim 11, wherein the at least one organic peroxide comprises at least one of a diacyl peroxide; a peroxyester; a monoperoxycarbonate; a peroxyketal; a dialkyl peroxide; a t-butyl peroxide; a t-amyl peroxide; a carboxylic acid functionalized peroxide, a hydroxyl functionalized peroxide, a functionalized peroxide having a free radical reactive unsaturated group; 3,6,9-triethyl-3,6,9-trimethyl-1,2,4,5,7,8-hexoxonane, 3,3,5,7,7-pentamethyl-1,2,4-trioxepane, t-butylperoxymaleic acid, bis(t-butyldioxyisopropyl)benzene, or a combination thereof.
18. The at least one zinc-containing reagent is selected from the group consisting of zinc diacrylate, zinc di(meth)acrylate, zinc monoacrylate, zinc monomethacrylate, zinc alkoxide, zinc methoxide, zinc ethoxide, zinc isopropoxide, zinc methoxyethoxide, zinc carboxylate, zinc bis(acetate), zinc bis(2-ethylhexanoate), zinc bis(neodecanoate), zinc bis(cyclohexanebutyrate), zinc naphthenate, zinc undecylenate, oxo[hexa(trifluoroacetato)]tetrazinc, zinc(acetylacetonate), zinc bis(2,2,6,6-tetramethylphenyl)acetate, ...
12. The coupling agent master batch of claim 11, comprising at least one of the following: zinc bis(hexafluoroacetylacetonate); zinc formate; zinc oxide; zinc dithiodicarbamate; zinc dimethyldithiocarbamate; zinc diethyldithiocarbamate; zinc dibutyldithiocarbamate; zinc halide; zinc chloride, zinc bromide, zinc fluoride, zinc iodide; zinc sulfonate; zinc carbonate; zinc nitrate; zinc hydrate; zinc tetrahydrofuran adduct; N,N,N',N'-tetramethylethylenediamine adduct; or combinations thereof.
19. The at least one silicon-containing agent having structure (I) is selected from the group consisting of vinyl(alkoxy)silanes; vinyltrimethoxysilane, vinyltriisopropoxysilane, vinyltri-t-butoxysilane; vinyltris(2-methoxyethoxy)silane; vinyltriacetoxysilane; trivinylmethoxysilane; trivinylethoxysilane; trivinylisopropoxysilane divinyldimethoxysilane; divinyldiethoxysilane; vinyl(alkyl)silanes; vinyltrimethylsilane; vinyltriethylsilane; vinyltriisopropylsilane; vinyltributylsilane; divinyldimethylsilane; poly(vinyl)silane; divinylsilane; trivinylsilane; tetravinylsilane; (vinyl)(alkyl)(alkoxy)silanes; vinyldimethylethoxysilane; vinylmethyldiethoxysilane; 1,3-divinyltetramethyldisiloxane; 1,3,5-trivinyl-1,3,5-trimethylcyclotrisiloxane; 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane; vinylmethylbis(trimethylsiloxy)silane; 1,1,3,3-Tetravinyldimethyldisiloxane; Vinyl-terminated polydimethylsiloxane; 1,4-divinyl-1,1,4,4-tetramethyl-1,4-disilabutane; Methylbis(trimethylsilyloxy)vinylsilane; 2-(dimethylvinylsilyl)pyridine; Tris(2-methoxyethoxy)(vinyl)silane; Triacetoxy(vinyl)silane; Tris(trimethylsiloxy)(vinyl)silane; 1-cyclopentasiloxane (5,5-dimethyl-1-cyclopenten-1-yl)(trimethyl)silane; Trimethyl(6-methyl-1-cyclohexen-1-yl)silane; (4-methoxy-1-cyclohexen-1-yl)(trimethyl)silane; Trimethyl(4-methyl-1,5-cyclohexadien-1-yl)silane; Trimethyl(5-methyl-1,5-cyclohexadiene (6,6-dimethyl-1-cyclohexen-1-yl)(trimethyl)silane; allyl(methyl)1-naphthyl(phenyl)silane; trimethyl(1-phenyl-2-propenyl)silane; 2-cycloocten-1-yl(trimethyl)silane; trimethyl[(2E)-3-phenyl-2-propenyl]silane; trimethyl[2-[(trimethylsilyl)methyl]-2-propenyl]silane; trimethyl(3-phenyl-2-cyclohexen-1-yl)silane dimethyl-di(methacryloyloxy-1-ethoxy)silane; trimethoxy(7-octen-1-yl)silane; trimethyl(2,3,4,5-tetramethyl-2,4-cyclopentadiene-1-yl)silane; (2-methyl-allyl)-triphenyl-silane; (1-hydroxy-allyl)-tri-methyl-silane; (3-methyl-3-butenyl)(triphenyl)silane; 12. The coupling agent master batch of claim 11 comprising at least one of 1-cyclododecen-1-yl(methyl)silane; 1-cyclohepten-1-yl(trimethyl)silane; [2-(cyclohexylmethyl)-2-propenyl](trimethyl)silane; 2-cyclohexen-1-yl(trimethyl)silane; bis(pentafluorophenyl)methyl(α-styryl)silane; t-butyl(dimethyl)[(2E)-2,4-pentadienyloxy]silane; or combinations thereof.
20. 12. The coupling agent master batch of claim 11, wherein the at least one silicon-containing agent having structure (II) comprises at least one of tetra(alkoxy)silane; tetramethoxysilane; tetraethoxysilane; tetraisopropoxysilane; tetrabutoxysilane; (alkyl)(alkoxy)silane; methyltris(methoxy)silane; methyltris(ethoxy)silane; methyltris(isopropoxy)silane; ethyltris(methoxy)silane; ethyltris(ethoxysilane); ethyltris(isopropoxy)silane; propyltris(methoxy)silane; propyltris(ethoxysilane); propyltris(isopropoxy)silane; and combinations thereof.
21. 1. A composition comprising: (a) at least one organic peroxide or a decomposition product or residue thereof, said at least one organic peroxide having a half-life of at least 1 hour at 98° C.; (b) at least one of (i) at least one zinc-containing reagent or a residue thereof or a reaction product thereof; and / or (ii) at least one silicon-containing reagent or a residue thereof or a reaction product thereof having the following structure (I): SiR 1 R 2 R 3 R 4 (I) (In the formula, R 1 , R 2 , R 3 , or R 4 At least one of R contains at least one unsaturation, and the remaining R 1 , R 2 , R 3 , or R 4 are hydrogen or alkyl or alkoxy groups, and may be the same or different; (c) optionally, at least one silicon-containing reagent having the following structure (II): SiR 5 R 6 R 7 R 8 (II) (In the formula, R 5 , R 6 , R 7 , or R 8 R is free of unsaturation and is hydrogen or an alkyl or alkoxy group, and may be the same or different from each other. R 1 , R 2 , R 3 , or R 4 group may be the same as or different from (d) at least one polymer matrix; (e) at least one filler comprising at least one of wood particles, wood product particles, wood flour, sawdust, rice husk flour, straw flour, straw fiber, wheat straw, bamboo fiber, flax, jute, hemp, cellulose, ground wood, palm fiber, bagasse, peanut shells, chitin, kenaf fiber, waste paper, cardboard, or combinations thereof; A composition comprising:
22. 1. A method for producing a coupling agent masterbatch for a cellulosic-polymer composite, comprising the steps of: (A) The following: (a) at least one organic peroxide; (b) at least one of (i) at least one zinc-containing reagent; and / or (ii) at least one silicon-containing reagent having the following structure (I): SiR 1 R 2 R 3 R 4 (I) (In the formula, R 1 , R 2 , R 3 , or R 4 At least one of R contains at least one unsaturation, and the remaining R 1 , R 2 , R 3 , or R 4 are hydrogen or alkyl or alkoxy groups, which may be the same or different; and (c) optionally, at least one silicon-containing reagent having the following structure (II): SiR 5 R 6 R 7 R 8 (II) (In the formula, R 5 , R 6 , R 7 , or R 8 R is free of unsaturation and is hydrogen or an alkyl or alkoxy group, and may be the same or different from each other. R 1 , R 2 , R 3 , or R 4 may be the same as or different from the group.) to form a coupling agent formulation for a cellulosic-polymer composite; (B) mixing the coupling agent formulation for the cellulosic material-polymer composite with (e) at least one carrier for the coupling agent masterbatch to form a coupling agent masterbatch for the cellulosic material-polymer composite. The method includes:
23. 1. A method for producing a cellulosic-polymer composite comprising the steps of: (I) The following: (A) a coupling agent for cellulosic material-polymer composites according to claim 1; (B) a polymer matrix; and (C) Filler mixing the ingredients to form a component mixture; and (II) forming the mixture of components into a composite material; A method for producing a cellulosic-polymer composite, comprising:
24. 24. The method of claim 23, wherein step (I) further comprises feeding components (A), (B) and (C) to an extruder, and step (II) comprises extruding through a die.
25. 1. A method for producing a cellulosic-polymer composite comprising the steps of: (I) The following: (A) the coupling agent masterbatch for cellulosic material-polymer composites according to claim 11; (B) a polymer matrix; and (C) Filler mixing the ingredients to form a component mixture; and (II) forming the mixture of components into a composite material; A method for producing a cellulosic-polymer composite, comprising:
26. 26. The method of claim 25, wherein step (I) further comprises feeding components (A), (B) and (C) to an extruder, and step (II) comprises extruding through a die.
Citation Information
Patent Citations
Wood plastic composite
US20200056020A1
Emulsion compositions for wood protection
US7850771B2
Cited By
Crosslinkable resin composition, crosslinked resin composition, resin molded body, and resin composition kit
WO2026105826A1