Ferritic stainless steel material with excellent workability for clad plate material and its manufacturing method

Optimized alloy components and manufacturing process for ferritic stainless steel improve workability and reduce cracks and bending in clad plate materials by controlling alloy composition and processing parameters.

JP2024537909AInactive Publication Date: 2024-10-16POHANG IRON & STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024523511
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-25
Filing Date
2022-10-19
Publication Date
2024-10-16
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Ferritic stainless steel materials used in clad plate materials for cooking utensils suffer from processing cracks and bending due to differences in physical properties, limiting their workability and material quality.

Method used

A ferritic stainless steel material with optimized alloy components (C: 0.0005-0.02%, N: 0.005-0.02%, Si: 0.01-1.0%, Mn: 0.01-1.0%, P: 0.001-0.05%, Cr: 10.0-25.0%, Nb: 0.01-0.5%, Ti: 0.01-0.5%, Fe balance) and a manufacturing process involving hot rolling, hot rolling annealing, and final cold rolling annealing at specific temperature ranges to achieve an average R-bar value of 1.5 or more and controlled hardness differences.

Benefits of technology

The solution results in a clad plate material with excellent workability, minimizing processing cracks and bending to 25 μm or less, enhancing material quality and workability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537909000001_ABST
    Figure 2024537909000001_ABST
Patent Text Reader

Abstract

Optimizing the composition of ferritic stainless steel improves the material properties and workability of clad plate materials. [Solution] The ferritic stainless steel material of the present invention, which has excellent workability as a clad plate material, contains, by weight, C: 0.0005-0.02%, N: 0.005-0.02%, Si: 0.01-1.0%, Mn: 0.01-1.0%, P: 0.001-0.05%, Cr: 10.0-25.0%, Nb: 0.01-0.5%, Ti: 0.01-0.5%, with the balance being Fe and unavoidable impurities, has an average R-bar value of 1.5 or more for the directional R values, and has a bending height of 25 μm or less after processing into a clad plate material. The present invention also provides a method for producing a ferritic stainless steel material having excellent workability as a clad plate material, the method comprising the steps of: producing a slab containing, by weight, 0.0005-0.02% C, 0.005-0.02% N, 0.01-1.0% Si, 0.01-1.0% Mn, 0.001-0.05% P, 10.0-25.0% Cr, 0.01-0.5% Nb, 0.01-0.5% Ti, with the remainder being Fe and unavoidable impurities, in a continuous casting process; hot rolling the produced slab in a range of 800-1250°C; hot rolling annealing in a temperature range of 900-1050°C, followed by cold rolling at a reduction rate of 70% or more; and final cold rolling annealing in a temperature range of 800-950°C for less than 1 hour.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ferritic stainless steel material having excellent workability as a clad plate material and a manufacturing method thereof, and more particularly to a ferritic stainless steel material having excellent workability as a clad plate material in which the material properties and workability are improved by controlling the alloy components of the steel, and a manufacturing method thereof. [Background technology]

[0002] Ferritic stainless steel is widely used in home appliances such as washing machines and refrigerators, and kitchenware such as pots and rice cookers, due to its low cost and beautiful surface quality compared to austenitic stainless steel. In particular, ferritic stainless steel is widely used in pots and rice cookers due to the harmful effects of conventional aluminum, and the demand for high-performance surfaces and induction heaters. However, when using only ferritic stainless steel, it is heavier and has lower thermal conductivity than conventional aluminum, which is disadvantageous for cooking food. Therefore, in order to improve these points, there are an increasing number of cases where stainless steel is clad with aluminum or copper to produce pots and rice cookers. When processing clad plate materials, there is a problem that processing cracks and bending occur due to the difference in physical properties of the materials. Therefore, it is necessary to develop a ferritic stainless steel material with excellent workability for clad plate materials. Summary of the Invention [Problem to be solved by the invention]

[0003] The present invention is intended to solve the above-mentioned problems, and has an object to improve the material properties and workability of clad plate materials by optimizing the components of ferritic stainless steel materials. [Means for solving the problem]

[0004] The ferritic stainless steel material of the present invention contains, by weight, C: 0.0005-0.02%, N: 0.005-0.02%, Si: 0.01-1.0%, Mn: 0.01-1.0%, P: 0.001-0.05%, Cr: 10.0-25.0%, Nb: 0.01-0.5%, Ti: 0.01-0.5%, with the balance being Fe and unavoidable impurities, and has an average R-bar value of 1.5 or more (wherein the average R-bar value is (R0+2R 45 +R 90 ) / 4), and is characterized in that the bending height after processing of the clad plate material is 25 μm or less.

[0005] The method for producing a ferritic stainless steel material of the present invention is characterized by comprising the steps of: producing a slab containing, by weight, 0.0005-0.02% C, 0.005-0.02% N, 0.01-1.0% Si, 0.01-1.0% Mn, 0.001-0.05% P, 10.0-25.0% Cr, 0.01-0.5% Nb, 0.01-0.5% Ti, with the balance being Fe and unavoidable impurities, in a continuous casting process; hot rolling the produced slab in a range of 800-1250°C; hot rolling annealing in a temperature range of 900-1050°C, followed by cold rolling at a reduction rate of 70% or more; and final cold rolling annealing in a temperature range of 800-950°C for less than 1 hour. Effect of the Invention

[0006] According to the present invention, a ferritic stainless steel material having excellent workability as a clad plate material can be produced. [Brief description of the drawings]

[0007] [Figure 1] 1 is a photograph showing the occurrence of bending and the cross-sectional structure of a clad plate material after ladle forming. [Diagram 2] 1 is a graph showing the bending height depending on the hardness difference between ferritic stainless steel and Al. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The ferritic stainless steel material of the present invention contains, by weight, C: 0.0005-0.02%, N: 0.005-0.02%, Si: 0.01-1.0%, Mn: 0.01-1.0%, P: 0.001-0.05%, Cr: 10.0-25.0%, Nb: 0.01-0.5%, Ti: 0.01-0.5%, with the balance being Fe and unavoidable impurities, and has an average R-bar value of 1.5 or more (wherein the average R-bar value is (R0+2R 45 +R 90 ) / 4), and is characterized in that the bending height after processing of the clad plate material is 25 μm or less.

[0009] Hereinafter, unless otherwise specified, the unit is % by weight. Furthermore, when any part is said to "contain" a certain component, this does not mean that other components are excluded, but that other components may be further contained, unless otherwise specified to the contrary. The reasons for limiting the range of each alloy element will be explained below.

[0010] Carbon (C): 0.0005~0.02% The amount of carbon (C) is 0.0005% or more and 0.02% or less. If the amount of carbon (C) is less than 0.0005%, the refining costs for producing a high-purity product will be high, and if it exceeds 0.02%, there will be problems with the increase in impurities in the material, which will reduce the elongation rate and corrosion resistance.

[0011] Nitrogen (N): 0.005-0.02% The amount of nitrogen (N) is 0.005% or more and 0.02% or less. If the amount of nitrogen (N) is less than 0.005%, the amount of TiN crystallization is low and the equiaxed crystal ratio of the slab is low, while if the amount of nitrogen (N) is more than 0.02%, there is a problem that the amount of impurities in the material increases and the elongation rate and corrosion resistance decrease.

[0012] Silicon (Si): 0.01 to 1.0% The amount of silicon (Si) is between 0.01% and 1.0%. If the amount of silicon (Si) is less than 0.01%, the refining cost to produce a high-purity product will be high, and if it exceeds 1.0%, the hardness of the material will increase excessively, reducing workability and causing bending problems.

[0013] Chromium (Cr): 10.0~25.0% The amount of chromium (Cr) is 10.0% or more and 25.0% or less. If the amount of chromium (Cr) is less than 10.0%, there is a problem of reduced corrosion resistance and strength, and if it exceeds 25.0%, there is a problem of increased costs.

[0014] Manganese (Mn): 0.01 to 1.0% The amount of manganese (Mn) is between 0.01% and 1.0%. If the amount of manganese (Mn) is less than 0.01%, there is a problem of increased refining costs, and if it exceeds 1.0%, the amount of impurities in the material increases and the elongation rate decreases.

[0015] Phosphorus (P): 0.001 to 0.05% The amount of phosphorus (P) is 0.001% or more and 0.05% or less. Phosphorus (P) is an impurity inevitably contained in ferritic stainless steel materials, and is an element that is a major cause of grain boundary corrosion during pickling and of impairing hot workability, so it is preferable to control the content as low as possible. However, if it is controlled to less than 0.001%, refining costs increase, and if it exceeds 0.05%, the increase in impurities reduces the elongation and work hardening index.

[0016] Niobium (Nb): 0.01-0.5% The amount of niobium (Nb) is 0.01% or more and 0.5% or less. If the amount of niobium (Nb) is less than 0.01%, as in Comparative Examples 1 to 4 below, there is a problem that the crystal grains become very large and the R value decreases, and if it exceeds 0.5%, there is a problem that the workability decreases and it is expensive.

[0017] Titanium (Ti): 0.01-0.5% The amount of titanium (Ti) is 0.01% or more and 0.5% or less. If the amount of titanium (Ti) is less than 0.01%, as in Comparative Examples 1 to 4 below, there is a problem that the crystal grains become very large and the R value decreases, and if the amount of titanium (Ti) exceeds 0.5%, there is a problem that defects due to Ti-based inclusions increase.

[0018] (characteristic) The average R value for each direction is R-bar = (R0 + 2R 45 +R 90 If the R-bar value is less than 1.5, processing cracks occur frequently in the clad plate material, and the bend height after forming of the clad plate material becomes large. In addition, in the present invention, after joining with Al, the cross-sectional hardness difference between the two materials may be 50 to 150 Hv. If the hardness difference is less than 50 Hv, there is a problem of frequent occurrence of cracks during processing of the clad plate material, and if the hardness difference exceeds 150 Hv, even if the R-bar value is 1.5 or more, local necking occurs periodically in the ferritic stainless steel material due to non-uniform deformation of Al during processing of the clad plate material, forming a bend on the surface.

[0019] [Method of manufacturing stainless steel materials] A method for producing a stainless steel material of the present invention includes the steps of producing a slab containing, by weight%, 0.0005-0.02% C, 0.005-0.02% N, 0.01-1.0% Si, 0.01-1.0% Mn, 0.001-0.05% P, 10.0-25.0% Cr, 0.01-0.5% Nb, 0.01-0.5% Ti, with the balance being Fe and unavoidable impurities, by a continuous casting process; hot rolling the produced slab at a temperature range of 800 to 1250 ° C; A step of performing hot rolling annealing at a temperature range of 900 to 1050 ° C., followed by cold rolling at a rolling reduction of 70% or more; The method includes a final cold roll annealing step in a temperature range of 800 to 950°C for less than 1 hour.

[0020] The present invention will now be described more specifically with reference to examples. The following examples are presented to fully convey the concept of the present invention to those skilled in the art to which the present invention pertains, and the present invention is not limited to the examples presented herein and may be embodied in other forms. (Example) The steel having the composition shown in Table 1 was produced into a slab through continuous casting, hot-rolled at 800 to 1250°C, hot-rolled and annealed at 900 to 1050°C, cold-rolled at a rolling reduction of 70% or more, and then cold-rolled and annealed at 800 to 950°C for less than 1 hour to produce stainless steels according to Examples 1 to 3 and Comparative Examples 1 to 7 shown in Table 2. The R-bar, hardness difference and bending height were measured and shown in Table 2. The R-bar value was measured by processing tensile test pieces in the 0°, 45°, and 90° directions relative to the rolling direction and measuring the R value (Lankford value) after a 15% tensile test. The average value (R-bar value = (R0 + 2R 45 +R 90 ) / 4) was calculated. The hardness difference was measured by finding the difference in Vickers hardness of the cross section of the two materials after joining with Al, and the Vickers hardness was measured using a Mitutoyo HV-114 Vickers hardness tester. The bending height was measured using a Mitutoyo surface roughness meter under the conditions of λc=8 and n=2.

[0021] [Table 1]

[0022] [Table 2]

[0023] In Examples 1 to 3, by satisfying the alloy composition range and manufacturing conditions of the present invention, it was possible to produce clad plate materials with excellent workability, in which the R-bar value was ensured to be 1.5 or more, the hardness difference was controlled to be 50 to 150 Hv, and the occurrence of bending was reduced to 25 μm or less. On the other hand, it was confirmed that in Comparative Examples 1 to 4, the R-bar value was less than 1.5, processing cracks occurred frequently in the clad plate material, and the bending height after forming of the clad plate material was increased to 25 μm or more. In addition, in Comparative Examples 5 to 7, in which the hardness difference exceeds 150 Hv, even if the R-bar value is 1.5 or more, it was confirmed that localized necking occurs periodically in the ferritic stainless steel material due to the non-uniform deformation of Al during processing of the clad plate material, forming bends on the surface (Figure 1). [Industrial Applicability]

[0024] According to the present invention, it is possible to produce a ferritic stainless steel material having excellent workability as a clad plate material capable of reducing the occurrence of processing cracks and bending, and the industrial applicability is recognized.

Claims

1. The alloy contains, by weight, C: 0.0005-0.02%, N: 0.005-0.02%, Si: 0.01-1.0%, Mn: 0.01-1.0%, P: 0.001-0.05%, Cr: 10.0-25.0%, Nb: 0.01-0.5%, Ti: 0.01-0.5%, and the balance being Fe and unavoidable impurities. The average R-bar value of the directional R-values ​​is 1.5 or more (wherein the average R-bar value is (R 0 +2R 45 +R 90 ) / 4), a bending height after processing into a clad plate material is 25 μm or less.

2. 2. The ferritic stainless steel material with excellent workability as a clad plate material according to claim 1, characterized in that after said clad plate material processing, the difference in hardness from Al is 50 to 150 Hv.

3. a step of producing a slab comprising, by weight percent, 0.0005-0.02% C, 0.005-0.02% N, 0.01-1.0% Si, 0.01-1.0% Mn, 0.001-0.05% P, 10.0-25.0% Cr, 0.01-0.5% Nb, 0.01-0.5% Ti, with the balance being Fe and unavoidable impurities, by a continuous casting process; hot rolling the produced slab at a temperature in the range of 800 to 1250°C; A step of performing hot rolling annealing at a temperature range of 900 to 1050 ° C., followed by cold rolling at a rolling reduction of 70% or more; A method for producing a ferritic stainless steel material having excellent workability as a clad plate material, comprising a step of performing final cold rolling annealing at a temperature range of 800 to 950°C for less than one hour.

Citation Information

Patent Citations

  • Cold rolled ferritic stainless steel sheet excellent in surface distortion resistance and surface property

    JP2007254763A

  • Ferritic stainless steel sheet and manufacturing method therefor

    JP2020164956A

  • Ferritic stainless steel with improved heat dissipation and workability and method for producing the same

    JP2020532651A