High hardness low alloy hot rolled steel and its manufacturing method

A high hardness, low alloy hot rolled steel with controlled cooling rates and specific composition enhances martensite formation, addressing wear resistance and toughness challenges, achieving improved performance in mining and civil engineering applications.

JP2024537914APending Publication Date: 2024-10-16TATA STEEL LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024523937
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-20
Filing Date
2022-10-20
Publication Date
2024-10-16

AI Technical Summary

Technical Problem

Existing high carbon steels with martensitic microstructures face challenges in producing sufficient martensite, leading to inadequate wear resistance and impact toughness, especially in low alloy steels, which are difficult to produce and often not economically viable alternatives.

Method used

A high hardness, low alloy hot rolled steel with a composition of C: 0.10~0.25, Mn: 1.05~1.5, Si: 0.25~0.35, Cr: 0.15~0.25, Mo: 0.05~0.15, Ni: 0.45~0.55, Al: 0.15~0.25, and the balance being iron, featuring a microstructure of ferrite, austenite, pearlite, bainite, and martensite, produced through a thermomechanical process and heat treatment, with controlled cooling rates after finish rolling to enhance martensite formation.

Benefits of technology

The steel achieves a hardness of 200-460 Hv, tensile strength ≥600 MPa, yield strength ≥500 MPa, and 10-20% elongation, with improved wear resistance, impact toughness, and weldability, suitable for structural and wear-resistant applications in mining and civil engineering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537914000001_ABST
    Figure 2024537914000001_ABST
Patent Text Reader

Abstract

A high-hardness low-alloy hot-rolled steel with improved wear resistance, impact toughness, hardness, and weldability is provided. The high-hardness low-alloy hot-rolled steel has the following composition expressed in weight percent: C: 0.10-0.25, Mn: 1.05-1.5, Si: 0.25-0.35, Cr: 0.15-0.25, Mo: 0.05-0.15, Ni: 0.45-0.55, Al: 0.15-0.25, carbon equivalent: 0.34-0.69, and the balance being iron (Fe) and unavoidable impurities. The high-hardness low-alloy hot-rolled steel has a microstructure of up to 10% ferrite, up to 10% austenite, up to 20% pearlite, up to 20% bainite, and 60-100% martensite. The high hardness low alloy hot rolled steel exhibits a tensile strength of ≧600 MPa, a total elongation of 10-20%, a hardness of ≧200 Hv, and a yield strength of ≧500 MPa. A method (100) for producing high hardness low alloy hot rolled steel strip of the above composition is also provided.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THEINVENTION The present invention relates to a high hardness, low alloy hot rolled steel, more specifically to a high hardness, wear resistant hot rolled steel having improved wear resistance and impact toughness, and to a method for producing the high hardness, low alloy hot rolled steel. [Background technology]

[0002] background

[0002] Wear involves the gradual breakdown of material from any surface due to the relative motion between an active and an opposing object type. This can occur either by mechanical action or chemical reaction. In certain engineering applications, such as the L&E or mining sector, abrasive wear-resistant materials are in high demand. Surprisingly, as much as 63% of the total wear losses are caused by abrasive wear alone, which is undesirable. By better design or by choosing some alternative materials, this can be significantly reduced. However, new designs of parts often have other associated risks and do not always result in economically viable alternatives. Conversely, a better material choice may be considered to be the better option.

[0003]

[0003] In recent years, medium to high carbon steels containing martensite or tempered martensitic microstructures are used for the majority of wear-resistant applications. The wear resistance of steels is greatly improved by the surface hardness, which is directly proportional to the amount of martensite that can be produced in the steel matrix. In other words, the higher the amount of martensite in the microstructure, the higher the hardness of the steel. This is why there is a unidirectional effort worldwide to produce martensitic steels for wear-resistant applications. However, producing martensite is a difficult task, especially in low alloy steels.

[0004] The present disclosure is directed to overcoming one or more of the limitations set forth above or any other limitations associated with the prior art. Summary of the Invention [Problem to be solved by the invention]

[0005] Object of the invention

[0005] The object of the present invention is to solve the problems of the prior art and to develop a high hardness low alloy hot rolled wear resistant steel for L&E and mining applications.

[0006]

[0006] Another object of the present invention is to provide a high hardness, low alloy hot rolled steel sheet having the following composition by weight: C: 0.10-0.25, Mn: 1.05-1.5, Si: 0.25-0.35, Cr: 0.15-0.25, Mo: 0.05-0.15, Ni: 0.45-0.55, Al: 0.15-0.25, carbon equivalent: 0.34-0.69, the balance being iron (Fe) and unavoidable impurities, and having a microstructure consisting of ferrite, austenite, pearlite, bainite and martensite.

[0007]

[0007] Another object of the present invention is to provide a method for producing high hardness low alloy hot rolled steel having a sufficient amount of martensite by controlling the cooling rate after finish rolling in the run out table (ROT) during hot rolling operation.

[0008]

[0008] Another object of the present invention is to estimate the saturation cooling rate for obtaining the maximum possible hardness within the composition range.

[0009]

[0009] Yet another object of the present invention is to provide a new and easier manufacturing method that combines thermomechanical and heat treatment processes for a proposed chemical composition to produce high hardness low alloy hot rolled steel with improved wear resistance, impact toughness, hardness and weldability. [Means for solving the problem]

[0010] Summary of the Invention

[0010] This Summary is provided to introduce concepts related to high hardness, low alloy, hot rolled steels with improved wear resistance, impact toughness, hardness, and weldability, and methods for manufacturing high hardness, low alloy, hot rolled steel sheets. The concepts are further described in the Detailed Description below. This Summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter.

[0011]

[0011] In one embodiment of the present invention, there is provided a high-hardness low-alloy hot-rolled steel, which has the following composition expressed in weight percent: carbon (C): 0.10% to 0.25%, manganese (Mn): 1.05% to 1.5%, chromium (Cr): 0.15 to 0.25%, silicon (Si): 0.25% to 0.35%, nickel (Ni): 0.45% to 0.55%, aluminum (Al): 0.15 to 0.25%, molybdenum (Mo): 0.05% to 0.15%, vanadium: 0.03% maximum, carbon equivalent: 0.34 to 0.69, and the balance being substantially iron and incidental impurities. High hardness low alloy hot rolled steel contains a microstructure of up to 10% ferrite, up to 10% austenite, up to 20% pearlite, up to 20% bainite and 60-100% martensite.

[0012]

[0012] In an embodiment, the high hardness low alloy hot rolled steel has a hardness (HV 1kg) ≧ 200Hv. In an embodiment, the high hardness low alloy hot rolled steel has a hardness (HV 1kg) in the range of 200 to 460Hv.

[0013]

[0013] In an embodiment, the high hardness low alloy hot rolled steel has a tensile strength of ≧600 MPa. In an embodiment, the high hardness low alloy hot rolled steel has a yield strength of ≧500 MPa. In an embodiment, the high hardness low alloy hot rolled steel has a total elongation in the range of 10-20%.

[0014]

[0014] In an embodiment, the Mn content of the high hardness low alloy hot rolled steel is kept below 1.8 wt.% to avoid centerline segregation. In an embodiment, the C content of the high hardness low alloy hot rolled steel helps to stabilize austenite at room temperature. In an embodiment, the Si content of the high hardness low alloy hot rolled steel is kept in the range between 0.25-0.35 wt.% to partially delay the formation of cementite.

[0015]

[0015] In an embodiment, the high hardness low alloy hot rolled steel has a composition expressed in weight percent: C-0.15, Mn-1.1, Si-0.3, Cr-0.2, V-0.03, Ni-0.5, Al-0.2, Mo-0.1, carbon equivalent 0.43, and the balance being iron (Fe) and unavoidable impurities.

[0016]

[0016] In an embodiment, the high hardness low alloy hot rolled steel has a composition expressed in weight percent: C-0.21, Mn-1.47, Si-0.3, Cr-0.2, Ni-0.5, Mo-0.1, carbon equivalent 0.55, and the balance being iron (Fe) and unavoidable impurities.

[0017]

[0017] In an embodiment, the high hardness low alloy hot rolled steel has a hardness (HV 1kg) in the range of 220 to 380 Hv.

[0018]

[0018] In an embodiment, the high hardness low alloy hot rolled steel has a hardness (HV 1kg) in the range of 300 to 460 Hv.

[0019]

[0019] In another aspect of the present invention, there is provided a method for producing high hardness low alloy hot rolled steel sheet. The method comprises casting a steel slab having the following composition, expressed in weight percent: C: 0.10-0.25, Mn: 1.05-1.5, Si: 0.25-0.35, Cr: 0.15-0.25, Mo: 0.05-0.15, Ni: 0.45-0.55, Al: 0.15-0.25, carbon equivalent: 0.34-0.69, balance being iron (Fe) and unavoidable impurities. The method also comprises reheating the steel slab to a temperature above 1150°C. The method further comprises finish rolling at a temperature (TFRT ) to hot roll the steel slab to about 70% deformation to produce a steel sheet. FRT varies in the range of 830°C to 890°C. The method includes cooling at a cooling rate in the range of 5°C / s to 60°C / s until room temperature is reached to obtain a high hardness low alloy hot rolled steel sheet.

[0020]

[0020] In an embodiment, the high hardness low alloy hot rolled steel comprises a microstructure of up to 10% ferrite, up to 10% austenite, up to 20% pearlite, up to 20% bainite and 60-100% martensite.

[0021]

[0021] In an embodiment, the high hardness low alloy hot rolled steel has a tensile strength of ≧600 MPa and a yield strength of ≧500 MPa, and a total elongation in the range of 10 to 20%. FRT is 870°C.

[0022]

[0022] In an embodiment, the high hardness low alloy hot rolled steel has a composition expressed in weight percent: C-0.15, Mn-1.1, Si-0.3, Cr-0.2, V-0.03, Ni-0.5, Al-0.2, Mo-0.1, carbon equivalent 0.43, and the balance being iron (Fe) and unavoidable impurities.

[0023]

[0023] In an embodiment, the high hardness low alloy hot rolled steel has a composition expressed in weight percent: C-0.21, Mn-1.47, Si-0.3, Cr-0.2, Ni-0.5, Mo-0.1, carbon equivalent 0.55, and the balance being iron (Fe) and unavoidable impurities.

[0024]

[0024] In an embodiment, the high hardness low alloy hot rolled steel has a hardness (HV 1 kg) in the range of 220 to 380 Hv.

[0025]

[0025] In an embodiment, the high hardness low alloy hot rolled steel has a hardness (HV 1kg) in the range of 300 to 460 Hv.

[0026]

[0026] In an embodiment, the saturation cooling rate for high hardness low alloy hot rolled steel is in the range of 20 to 30°C / s.

[0027]

[0027] In an embodiment, the maximum hardness (HV 1kg) of the high hardness low alloy hot rolled steel is in the range of 360 to 380 Hv.

[0028]

[0028] In an embodiment, the maximum hardness (HV 1kg) of the high hardness low alloy hot rolled steel is in the range of 450 to 460 Hv.

[0029] In an embodiment, the steel slab is reheated to a temperature between 1150° C. and 1250° C. for a period of time between 20 minutes and 2 hours depending on the thickness of the slab.

[0030]

[0030] In an embodiment, the thickness of the steel sheet is in the range of 4 mm to 8 mm.

[0031] In an embodiment, a component manufactured from high hardness low alloy hot rolled steel, in an embodiment, the component is used in structural and wear resistant applications in L&E equipment, particularly in mining and civil engineering applications.

[0032]

[0032] Other features and aspects of the present disclosure will become apparent from the following description and the accompanying drawings. [Brief description of the drawings]

[0033] [Figure 1]

[0033] A flow chart of a method for manufacturing high hardness low alloy hot rolled steel sheet according to an embodiment of the present invention is shown. [Diagram 2]

[0034] FIG. 2 shows a schematic diagram of a cooling technique performed after rolling (at the run-out table of a hot strip mill) during the production of high hardness low alloy hot rolled steel sheet according to an embodiment of the present invention. [Diagram 3]

[0035] 1 shows a graphical representation of the change in hardness versus cooling rate for example high hardness low alloy hot rolled steels (Steel 1 and Steel 2) in accordance with an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034]

[0036] The drawings referred to in this description should not be understood as being drawn to scale, unless specifically noted, and such drawings are merely illustrative in nature.

[0035] Detailed Description

[0037] Detailed descriptions of various exemplary embodiments of the present disclosure are described herein with reference to the accompanying drawings. It should be noted that the embodiments are described in detail herein to clearly convey the present disclosure. However, the amount of detail provided herein is not intended to limit the anticipated variations of the embodiments, but rather to cover all modifications, equivalents, and alternatives that are included within the spirit and scope of the present disclosure as defined by the claims.

[0036]

[0038] It should also be understood that various arrangements can be devised that embody the principles of the present disclosure, although not explicitly described or shown herein. Moreover, all statements herein reciting principles, aspects, and embodiments of the present disclosure, as well as specific examples, are intended to encompass equivalents thereof.

[0037]

[0039] The terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the exemplary embodiments. As used herein, the singular forms "a", "an" and "the" are intended to include the plural forms unless the context clearly indicates otherwise. Furthermore, it will be understood that the terms "comprises", "comprising", "includes" and / or "including" as used herein specify the presence of stated features, integers, steps, operations, elements and / or components, but do not preclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof.

[0038]

[0040] It should also be noted that in some alternative implementations, the functions / acts noted may occur in an order different from that noted in the figures. For example, two figures shown in succession may, in fact, be executed concurrently or the functions / acts may sometimes be executed in the reverse order, depending on the functions / acts involved.

[0039]

[0041] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the exemplary embodiments belong. Furthermore, terms, such as those defined in commonly used dictionaries, should be interpreted to have a meaning consistent with their meaning in the context of the relevant art, and will not be interpreted in an idealized or overly formal sense unless expressly so defined herein.

[0040]

[0042] The high hardness low alloy hot rolled steel having a minimum tensile strength of 600 MPa according to the present invention has the following composition expressed in weight percent: C: 0.10-0.25, Mn: 1.05-1.5, Si: 0.25-0.35, Cr: 0.15-0.25, Mo: 0.05-0.15, Ni: 0.45-0.55, Al: 0.15-0.25, carbon equivalent: 0.34-0.69, and the balance being iron (Fe) and unavoidable impurities. The high hardness low alloy hot rolled steel has a microstructure of up to 10% ferrite, up to 10% austenite, up to 20% pearlite, up to 20% bainite, and 60-100% martensite.

[0041]

[0043] The high hardness low alloy hot rolled steel has a hardness ≧200Hv. In the described example, the high hardness low alloy hot rolled steel has a hardness in the range of 200-460Hv. The high hardness low alloy hot rolled steel has a yield strength ≧500MPa and a total elongation in the range between 10-20%. The high hardness low alloy hot rolled steel has improved wear resistance, impact toughness, hardness, and weldability.

[0042]

[0044] In one illustrated example (Steel 1), the high hardness low alloy hot rolled steel has the composition expressed in weight percent: C-0.15, Mn-1.1, Si-0.3, Cr-0.2, V-0.03, Ni-0.5, Al-0.2, Mo-0.1, carbon equivalent 0.43, balance iron (Fe) and unavoidable impurities. The high hardness low alloy hot rolled steel has a hardness in the range of 220-380 Hv (HV 1 kg).

[0043]

[0045] In another illustrative example (Steel 2), a high hardness low alloy hot rolled steel has the composition expressed in weight percent: C-0.21, Mn-1.47, Si-0.3, Cr-0.2, Ni-0.5, Mo-0.1, carbon equivalent 0.55, the balance being iron (Fe) and unavoidable impurities. The high hardness low alloy hot rolled steel has a hardness in the range of 300-460 Hv (HV 1kg).

[0044]

[0046] High hardness low alloy hot rolled steel sheet with tensile strength of minimum 600MPa consists of ferrite + pearlite + austenite + bainite + martensite. The martensite in the microstructure provides excellent resistance to abrasive wear and improves impact toughness. High hardness low alloy hot rolled steel is suitable for manufacturing parts used in structural and wear-resistant applications of lift & drilling equipment, especially parts used in mining and civil engineering applications.

[0045]

[0047] With reference to Figures 1 and 2, a method (100) for producing high hardness low alloy hot rolled steel sheet of a desired composition is shown. In step (102), the method (100) comprises casting molten steel having the composition expressed in weight percent: C: 0.10-0.25, Mn: 1.05-1.5, Si: 0.25-0.35, Cr: 0.15-0.25, Mo: 0.05-0.15, Ni: 0.45-0.55, Al: 0.15-0.25, carbon equivalent: 0.34-0.69, with the balance being iron (Fe) and unavoidable impurities. The molten steel is cast in a casting apparatus to obtain a steel slab (cast ingot). In the illustrated example, the steel is cast in either a conventional continuous caster or a thin slab caster.

[0046]

[0048] In step (104), the method (100) includes reheating the steel slab (steel casting) to a temperature above 1150° C. In the illustrated example, the slab is reheated to a temperature ranging between 1150-1250° C. for a time period between 20 minutes and 2 hours depending on the thickness of the slab. Also, reheat temperatures above 1250° C. are undesirable as they may cause excessive austenite coarsening and / or scale loss.

[0047]

[0049] In step (106), the method (100) comprises: FRT ) to produce a steel sheet by hot rolling a steel slab to a deformation of about 70%. FRT The T varies in the range of 830°C to 890°C, more preferably 870°C. Steel slabs are cast with the specified composition, reheated and then hot rolled. Slabs of larger thickness are rough rolled in roughing stands of a conventional hot rolling mill. Rough rolling is performed above the recrystallization temperature. Finish rolling is then carried out in a 6 or 7 stand tandem rolling mill. Rolling is performed at 830≦T FRT Finish rolling temperature T given to be ≦890℃ FRT The finishing temperature (T FRT The above ranges of T are selected to finish hot rolling in the austenitic range. FRT To take advantage of thermomechanically controlled rolling, nr is kept below

[0048]

[0050] In step (108), the method (100) includes cooling at a cooling rate in the range of 5° C. / s to 60° C. / s until room temperature is reached to obtain a high hardness low alloy hot rolled steel sheet. The cooling rate is kept between 5° C. / s to 60° C. / s to ensure sufficient amount of martensite formation in the microstructure.

[0049]

[0051] The steel may be cooled to allow the development of a larger amount of martensite in the final microstructure resulting in improved wear resistance, impact toughness, hardness and weldability. The resulting high hardness low alloy hot rolled steel sheet has a microstructure represented by area percentages of up to 10% ferrite, up to 10% austenite, up to 20% pearlite, up to 20% bainite and 60-100% martensite. In the described example, the high hardness low alloy hot rolled steel has a hardness of ≧200Hv. More specifically, in the range of 200-460Hv. The high hardness low alloy hot rolled steel sheet exhibits a tensile strength of more than 600MPa, a total elongation in the range of 10-20%, and a yield strength of more than 500MPa. In the described example, the thickness of the steel sheet is in the range of 4mm-8mm.

[0050]

[0052] According to the disclosed method (100) of the present invention, it is possible to produce high hardness hot rolled steel sheets with ferrite + pearlite + bainite + austenite + martensite microstructure and tensile strength of at least 600 MPa with improved wear resistance, impact toughness, hardness and weldability. Such steel sheets are suitable for producing parts used in structural and wear-resistant applications of L&E equipment, especially in mining and civil engineering applications where high hardness together with good abrasive wear resistance and impact toughness are essential requirements.

[0051]

[0053] In the following parts of this disclosure, details are provided about the percentage of each element in the composition of high hardness low alloy hot rolled steel sheet and its role in enhancing properties.

[0052]

[0054] C: 0.10-0.25%: The presence of carbon is inevitable in any commercial steel. Carbon is added to control the strength of the steel. Depending on the final requirements, the weight percentage of carbon addition varies. After quenching from the austenitic region to the partitioning temperature, the microstructure is mainly composed of austenite and martensite. Depending on the partitioning temperature and composition of the base steel, carbon is rejected from the supersaturated martensite. This carbon migrates from martensite to austenite. As a result of the carbon enrichment of austenite, the stability of this phase increases. Then, at room temperature, the presence of austenite in the microstructure may be visible. This austenite improves the mechanical properties of the steel. Thus, in other words, the presence of carbon in the steel helps to stabilize the austenite at room temperature. However, carbon cannot be significantly increased in the steel, as it impairs the weldability of the steel. Therefore, in the steel of the present invention, the carbon content is limited to between 0.10-0.25 wt.%.

[0053]

[0055] Si: 0.25-0.35%: Si is added as an effective deoxidizer during the steel manufacturing process. Moreover, Si is a very efficient solid solution strengthener. Moreover, cementite precipitation can be significantly delayed by Si. This is due to the accumulation of Si at the front of the advancing cementite / matrix interface. As Si has little solubility in cementite, it is rejected by the growing cementite grains, resulting in the enrichment of Si at the interface. Here in case of continuous precipitation, Si should diffuse away from the interface. This does not happen. As a result, this creates a favorable situation for carbon partitioning to occur instead of carbide precipitation. However, the higher the amount of Si in the steel, the more operational problems arise regarding the appearance of the steel surface. Therefore, the Si content in this study is limited between 0.25-0.35 wt.%.

[0054]

[0056] Al: 0.15-0.25%: Al is also added to molten steel as a deoxidizer. The presence of nitrogen in steel creates an environment for the formation of AlN precipitates. These precipitates limit the grain growth during reheating of the steel slab before hot rolling. Furthermore, Al, like Si, also exhibits inhibition of carbide precipitation in steel. However, it does not cause any operational interference during hot rolling. Therefore, in the context of the present invention, Al is added between 0.15-0.25 wt.%.

[0055]

[0057] Mn: 1.05-1.50%: Mn is a moderate solid solution strengthener. It reduces the ductile to brittle transition temperature. More importantly, Mn is an austenite stabilizer. Mn delays the decomposition of austenite during accelerated cooling. As a result, finish rolling can be performed more effectively in the austenite region, giving larger deformations. This results in finer ferrite grain size, which in turn increases the strength of the steel. However, at higher Mn contents, there is always a possibility that centerline segregation may occur in the steel due to the low diffusivity of Mn. Therefore, in the context of the present invention, the Mn content is limited between 1.05-1.50 wt.%.

[0056]

[0058] Cr: 0.15-0.25%: Cr significantly improves the hardenability of steel. During continuous cooling from the austenite region, Cr retards the formation of pearlite. Thus, it helps in the formation of martensite events at the nominal cooling rate. Hence, the Cr content is restricted between 0.15-0.25wt.%.

[0057]

[0059] Mo: 0.05~0.15%: Mo is also added mainly to improve the hardenability of steel. Mo reduces the formation of bainite to some extent, but significantly delays the formation of pearlite. Taking this into consideration, Mo is added in the range of 0.05~0.15wt.%.

[0058]

[0060] Ni: 0.45-0.55%: Ni is added to steel primarily to improve fracture toughness. Ni causes grain refinement by lowering the transformation temperature. This in turn increases the number of grain boundaries which is responsible for better fracture toughness properties. With this in mind, Ni is added in the range of 0.45-0.55wt.% in the context of the present invention.

[0059]

[0061] V: 0.03% or less: V forms VN / VC in the ferrite region, thereby increasing the strength of the material, which is the reason why V is added to the steel of the present invention.

[0060]

[0062] Microstructure: The final set of properties desired in high hardness low alloy hot rolled steel is achieved by the presence of ferrite, bainite, pearlite, austenite and martensite. Hot rolling, controlled cooling and coiling conditions are all important in achieving the final microstructure and properties. The contribution of each of the phases, namely ferrite, pearlite, austenite, bainite and martensite, is described below.

[0061]

[0063] Ferrite: The final hot rolled microstructure contains a small amount of 10% ferrite, which is strengthened by contributions from the alloying elements mentioned above.

[0062]

[0064] Pearlite: Small amounts of fine pearlite (up to 20%) are observed in the final microstructure. Small amounts of fine pearlite impart strength to the final microstructure.

[0063]

[0065] Austenite: A small amount of austenite (up to 10%) is observed in the final microstructure. This is essential to impart toughness to the final product.

[0064]

[0066] Bainite: A small amount of bainite (up to 20%) is observed in the final microstructure. It contributes to the final strength and toughness of the product.

[0065]

[0067] Martensite: The final hot rolled microstructure contains 60-100% martensite. The martensite in the microstructure ensures that a hardness of 200-460Hv is achieved in the final hot rolled steel sheet. EXAMPLES

[0066]

[0068] Further embodiments of the present disclosure will now be described using examples of compositions of high hardness low alloy hot rolled steels shown in Table 1. Various experiments and tests were carried out on a laboratory scale to evaluate different conditions.

[0067]

[0069] The two alloys were designed taking into account the following factors: Higher Ms temperature. Low carbon equivalent to eliminate weldability issues, and low carbon content to improve impact toughness. Higher hardenability to eliminate the formation of bainite or pearlite during quenching.

[0068]

[0070] The chemical compositions of the proposed alloys, their carbon equivalent (CE) values, and Ms temperatures calculated empirically and through dilatometry experiments are shown in Table 1.

[0069] [Table 1]

[0070]

[0071] Two different alloys were designed and cast in 40 kg scale and subsequently hot forged. To ensure complete homogenization, the forged steel plate was first austenitized at 1200°C for 2 hours. The plate was then hot rolled by 70%. The finish rolling temperature (FRT) was maintained at about 870°C. After this, the hot rolled plate was cooled to room temperature at different cooling rates ranging from 5°C / s to 60°C / s. In a real industrial setting, this is achieved in the ROT section. The detailed hot rolling scheme is shown in Figure 2.

[0071]

[0072] After cooling to room temperature, samples were prepared for hardness measurement according to standard metallographic techniques. They were characterized in a Vickers hardness tester with a 1 kg scale and a dwell time of 10 seconds. The measured hardness values ​​for both steels are shown in Table 2.

[0072] [Table 2]

[0073] This variation of hardness values ​​with cooling rate is shown pictorially in FIG. 3 for both steels. From the figure, it appears that the hardness values ​​increase with increasing cooling rate. However, there exists a saturation cooling rate after a certain range, beyond which the hardness does not change. This is also shown in FIG. 3. The saturation cooling rate exists in the range of 20-30° C. / s for the high hardness low alloy hot rolled steels. From the figure, it appears that beyond a cooling rate of 30° C. / s, the hardness values ​​do not change. Furthermore, the maximum hardness (HV 1 kg) of Steel 1 ranges from 360-380 Hv. The maximum hardness (HV 1 kg) of Steel 2 ranges from 450-460 Hv. By controlling the cooling rate experienced by the two alloys, it is possible to exploit the maximum achievable hardness values ​​of these steels, which is an essential property for wear resistant plates used in L&E and mining applications.

[0074]

[0074] The present invention provides high hardness low alloy hot rolled steel with improved wear resistance, impact toughness, hardness and weldability. The martensite present in the microstructure provides higher hardness to the produced steel. The disclosed steel is suitable for producing parts used in structural and wear-resistant applications of L&E equipment, especially parts used in mining and civil engineering applications. The present invention also provides a method for producing high hardness low alloy hot rolled steel with a large amount of martensite by controlling the cooling rate after finish rolling in the run-out table (ROT) during hot rolling operations. High hardness low alloy hot rolled steel is a significant contribution towards durable, cost-effective, futuristic and strategic steel applications with a larger safety factor. Furthermore, steel with high hardness and good wear resistance can be used in sectors such as engineering, mining, construction, agriculture, ports, power and metallurgy.

[0075] It should be understood that the experiments were performed for a specific composition of high hardness low alloy hot rolled steel sheet and the results obtained in the previous paragraph are for the composition shown in Table 1. However, this composition should not be construed as a limitation on the present disclosure as it may be extended to other compositions of high hardness low alloy hot rolled steel strip.

[0076]

[0076] Furthermore, the terms used in this specification are only for describing the embodiments and are not intended to limit the present disclosure. It will be recognized that some of the features and functions disclosed above and other features and functions, or alternatives thereof, can be combined into other systems or applications. Various presently unforeseen or unanticipated alternatives, modifications, variations, or improvements may be made thereto by those skilled in the art without departing from the scope of the present disclosure, which is encompassed by the following claims.

[0077]

[0077] The claims encompass variations, substitutions, modifications, improvements, equivalents, and substantial equivalents of the embodiments and teachings disclosed herein as originally presented and as they may be amended, including those that are presently unforeseen or unappreciated and those that may arise, for example, from the applicant / patentee, etc.

[0078]

[0078] While various embodiments of the present invention have been described above, other and further embodiments of the present invention may be devised without departing from the basic scope thereof. The scope of the present invention is determined by the claims that follow. The present invention is not limited to the described embodiments, versions or examples, which, when combined with information and knowledge available to the skilled artisan, are included to enable the skilled artisan to make and use the invention.

Claims

1. The following composition expressed in weight percent: Carbon (C): 0.10% to 0.25%, Manganese (Mn): 1.05% to 1.5%, Chromium (Cr): 0.15-0.25%, Silicon (Si): 0.25% to 0.35%, Nickel (Ni): 0.45% to 0.55%, Aluminum (Al): 0.15-0.25%, 1. A high hardness, low alloy, hot rolled steel comprising 0.05% to 0.15% molybdenum (Mo), 0.03% max vanadium, 0.34 to 0.69 carbon equivalent, the balance being essentially iron and incidental impurities, the high hardness, low alloy, hot rolled steel comprising a microstructure of 10% max ferrite, 10% max austenite, 20% max pearlite, 20% max bainite and 60 to 100% martensite.

2. 2. The high hardness low alloy hot rolled steel according to claim 1, wherein the high hardness low alloy hot rolled steel has a hardness (HV 1 kg) ≥ 200 Hv.

3. The high hardness low alloy hot rolled steel according to claim 2, wherein the high hardness low alloy hot rolled steel has a hardness (HV 1 kg) in the range of 200 to 460 Hv.

4. 2. The high hardness, low alloy, hot rolled steel according to claim 1, wherein the high hardness, low alloy, hot rolled steel has a tensile strength of > 600 MPa.

5. 2. The high hardness, low alloy, hot rolled steel of claim 1, wherein the high hardness, low alloy, hot rolled steel has a yield strength of > 500 MPa.

6. 2. The high hardness, low alloy, hot rolled steel of claim 1, wherein the high hardness, low alloy, hot rolled steel has a total elongation in the range of 10 to 20%.

7. 2. The high hardness, low alloy, hot rolled steel of claim 1, wherein the Mn content of said high hardness, low alloy, hot rolled steel is kept below 1.8 wt.% to avoid centerline segregation.

8. 2. The high hardness, low alloy, hot rolled steel of claim 1, wherein the C content of the high hardness, low alloy, hot rolled steel helps to stabilize the austenite at room temperature.

9. 2. The high hardness, low alloy, hot rolled steel of claim 1, wherein the Si content of the high hardness, low alloy, hot rolled steel is maintained in the range between 0.25 and 0.35 wt.% to partially delay the formation of cementite.

10. The high hardness, low alloy hot rolled steel according to claim 1, comprising a composition expressed in weight percent: C-0.15, Mn-1.1, Si-0.3, Cr-0.2, V-0.03, Ni-0.5, Al-0.2, Mo-0.1, a carbon equivalent of 0.43, and the balance being iron (Fe) and unavoidable impurities.

11. The high hardness low alloy hot rolled steel has a composition expressed in weight percent: C-0.21, Mn-1.47, Si-0.3, Cr-0.2, Ni-0.5, Mo-0.1, carbon equivalent 0.55, and the balance being iron (Fe) and unavoidable impurities. The high hardness low alloy hot rolled steel according to claim 1.

12. The high hardness low alloy hot rolled steel according to claim 10, wherein the high hardness low alloy hot rolled steel has a hardness (HV 1 kg) in the range of 220 to 380 Hv.

13. The high hardness low alloy hot rolled steel according to claim 11, wherein the high hardness low alloy hot rolled steel has a hardness (HV 1 kg) in the range of 300 to 460 Hv.

14. A method (100) for producing high hardness low alloy hot rolled steel sheet, comprising the steps of: casting a steel slab having a composition expressed in weight percent of: C: 0.10-0.25, Mn: 1.05-1.5, Si: 0.25-0.35, Cr: 0.15-0.25, Mo: 0.05-0.15, Ni: 0.45-0.55, Al: 0.15-0.25, carbon equivalent: 0.34-0.69, with the remainder being iron (Fe) and unavoidable impurities; reheating the steel slab to a temperature above 1150°C; The finishing rolling is performed at a temperature (T FRT ) hot rolling the steel slab to a deformation of about 70% to produce a steel sheet, FRT varies in the range of 830°C to 890°C; and cooling the steel at a cooling rate in the range of 5° C. / s to 60° C. / s until room temperature is reached to obtain the high hardness low alloy hot rolled steel sheet. A method (100) comprising:

15. 15. The method (100) for producing high hardness low alloy hot rolled steel sheet according to claim 14, wherein said high hardness low alloy hot rolled steel comprises a microstructure of up to 10% ferrite, up to 10% austenite, up to 20% pearlite, up to 20% bainite and 60-100% martensite.

16. 16. The method (100) for manufacturing high hardness low alloy hot rolled steel sheet according to claim 14 or 15, wherein said high hardness low alloy hot rolled steel has a tensile strength ≧600 MPa and a yield strength ≧500 MPa, a total elongation in the range of 10-20%.

17. T FRT The method (100) for producing high hardness low alloy hot rolled steel sheet according to claim 14, wherein the hardness temperature is 870°C.

18. The method (100) for producing a high hardness low alloy hot rolled steel sheet according to claim 14, wherein the high hardness low alloy hot rolled steel has a composition expressed in weight percent: C-0.15, Mn-1.1, Si-0.3, Cr-0.2, V-0.03, Ni-0.5, Al-0.2, Mo-0.1, carbon equivalent 0.43, and the balance being iron (Fe) and unavoidable impurities.

19. The method (100) for producing a high hardness low alloy hot rolled steel sheet according to claim 14, wherein the high hardness low alloy hot rolled steel has a composition expressed in weight percent: C-0.21, Mn-1.47, Si-0.3, Cr-0.2, Ni-0.5, Mo-0.1, carbon equivalent 0.55, and the balance being iron (Fe) and unavoidable impurities.

20. The method (100) for manufacturing high hardness low alloy hot rolled steel sheet according to claim 18, wherein said high hardness low alloy hot rolled steel has a hardness in the range of 220 to 380 Hv (HV 1 kg).

21. The method (100) for manufacturing high hardness low alloy hot rolled steel sheet according to claim 19, wherein said high hardness low alloy hot rolled steel has a hardness in the range of 300 to 460 Hv (HV 1 kg).

22. The method (100) for manufacturing high hardness low alloy hot rolled steel sheet according to claim 18 or 19, wherein the saturation cooling rate for the high hardness low alloy hot rolled steel is in the range of 20-30 °C / s.

23. The method (100) for manufacturing high hardness low alloy hot rolled steel sheet according to claim 18 or 22, wherein the maximum hardness (HV 1 kg) of said high hardness low alloy hot rolled steel is in the range of 360-380 Hv.

24. The method (100) for manufacturing high hardness low alloy hot rolled steel sheet according to claim 19 or 22, wherein the maximum hardness (HV 1 kg) of said high hardness low alloy hot rolled steel is in the range of 450-460 Hv.

25. 15. The method (100) for producing high hardness low alloy hot rolled steel sheet according to claim 14, wherein the steel slab is reheated to a temperature between 1150°C and 1250°C for a time between 20 minutes and 2 hours depending on the thickness of the slab.

26. Method (100) for manufacturing high hardness low alloy hot rolled steel sheet according to any one of claims 15 to 20, wherein the thickness of said steel sheet is in the range of 4 mm to 8 mm.

27. A component manufactured from the high hardness, low alloy, hot rolled steel according to any one of the preceding claims.

28. 28. The part of claim 27, wherein the part is used in structural and wear applications for L&E equipment, particularly in mining and civil engineering applications.

Citation Information

Patent Citations

  • Manufacturing method of low yield ratio high-strength steel plate

    JP2021155823A

  • Steel material and method for producing the same

    JP2021161507A

  • Steel sheet having excellent weldability, hardness uniformity in the thickness direction and low temperature toughness, and method for manufacturing the same