Iridium catalyst, preparation method thereof, and hydroformylation method
The iridium-based catalyst addresses the inefficiencies of rhodium-based hydroformylation by enhancing selectivity and reducing costs through controlled reaction conditions, achieving superior n-butyraldehyde/isobutyraldehyde ratios.
Patent Information
- Application Number
- JP2024523907
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-27
- Filing Date
- 2021-11-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-11-16
AI Technical Summary
Existing hydroformylation processes using rhodium-based catalysts face issues with high costs due to rising metal prices, slow deactivation, and low n-butyraldehyde/isobutyraldehyde selectivity, leading to inefficient production.
Development of an iridium-based catalyst, specifically POP(R)-Ir-X, prepared by mixing 4,5-bis(diphenylphosphino)-9,9-dialkyloxanthene with an iridium compound in a solvent, followed by heating and stirring, and used in a hydroformylation process with controlled reaction conditions.
The iridium catalyst achieves improved selectivity and reduced production costs by maintaining high n-butyraldehyde/isobutyraldehyde ratios under mild reaction conditions, outperforming traditional rhodium catalysts in efficiency and cost-effectiveness.
Smart Images

Figure 2024538219000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of formylation reaction, in particular to an iridium catalyst and its preparation method, It relates to a formylation process. [Background technology]
[0002] Butyraldehyde and octanol are bulk chemical industrial raw materials with a wide range of uses. At present, butanol is industrially synthesized mainly through the hydroformylation reaction of olefins. n-Butyl aldehyde and isobutyraldehyde were prepared and then used as raw materials. The hydroformylation of olefins is used in the synthesis of butanol. This is an important process in the process.
[0003] n-Butyraldehyde and isobutyraldehyde from the hydroformylation of olefins Numerous patents have been disclosed regarding the synthesis of In commercial processes, catalysts based on rhodium metal are generally employed. In the documents 1, 2 and 3, triphenylphosphine-rhodium is used as a catalyst. Patent Document 4 uses cyclooctadiene acetic acid-rhodium as a catalyst. Reference 5 uses 6,6'-((3,3'-di-tert-butyl-5,5'-dimeth- yl) as a catalyst. 2,3-Dibenzo[d,f][1,3, 2] Dioxaphosphepine-rhodium is used. Patent Document 6 uses acetyl molybdenum as a catalyst. Patent Document 7 uses acetate-rhodium as a catalyst. Patent Document 8 discloses a catalyst containing tris(2,4-di-tert-butylphenyl)-phosphite. Patent Document 9 uses a long-chain carboxylic acid-rhodium catalyst. Patent Document 10 uses acetylacetonatocarbonyl-rhodium as a catalyst. Patent Document 11 discloses a catalyst containing hydridocarbonyl-tris(triphenylphosphine)-ro Patent Document 12 uses rhodium(II) acetate + tris(3-sodium) as a catalyst. (phenyl)sodium phosphine salt hydrate is used.
[0004] In addition to the above patents, rhodium metal-based catalysts are commonly used in published literature. For example, Non-Patent Document 1 uses a heterocyclic phosphorus ligand-rhodium as a catalyst. The maximum n-butyraldehyde / isobutyraldehyde ratio was 2.6. Patent Document 2 uses N-Triphos ligand-rhodium as a catalyst, and achieves a maximum of 2. The n-butyraldehyde / isobutyraldehyde ratio of 3 was obtained. The hydridocarbonyl-tris(triphenylphosphine)-rhodium is used. The maximum n-butyraldehyde / isobutyraldehyde ratio obtained is 12.7. In reference 4, a porphyrin-modified triphenylphosphine ligand-rhodium was used as a catalyst. The maximum n-butyraldehyde / isobutyraldehyde ratio obtained was 2.3.
[0005] Rhodium metal can be recycled many times in the hydroformylation of olefins. However, slow loss and deactivation during the reaction is inevitable. Prices are rising rapidly and, accordingly, catalyst costs for the production process are also rising rapidly. In addition, the n-butyraldehyde / isobutyraldehyde ratio is low, which is valuable in the production process. A large amount of low-value isobutyraldehyde was produced.
[0006] The present invention has been made in view of this. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] WO 02 / 00583 [Patent Document 2] European Patent Application Publication No. 3712126 [Patent Document 3] China Patent Application Publication No. 102826967 [Patent Document 4] JP 2002-047294 A [Patent Document 5] China Patent Application Publication No. 110156580 [Patent Document 6] China Patent Publication No. 103896748 [Patent Document 7] European Patent Application Publication No. 3770144 [Patent Document 8] China Patent Publication No. 111348995 [Patent Document 9] U.S. Patent No. 9,550,179 [Patent Document 10] China Patent Application Publication No. 102826973 [Patent Document 11] European Patent No. 2417094 [Patent Document 12] European Patent No. 2417093 [Non-patent literature]
[0008] [Non-Patent Document 1] Angew.Chem.Int.Ed. 2019, 58, 2120-2124 [Non-Patent Document 2] ACS Catal. 2018, 8, 5799-5809 [Non-Patent Document 3] Journal of Molecular Catalysis A:Chemical, 2009, 300, 116-120 [Non-Patent Document 4] Chem. Eur. J. 2017, 23, 14769-14777 Summary of the Invention [Problem to be solved by the invention]
[0009] The first object of the present invention is to provide an iridium-based catalyst. Lithium-based catalysts are cheaper than conventional iridium-based catalysts, significantly reducing production costs. will be done.
[0010] A second object of the present invention is to provide a method for preparing an iridium-based catalyst, The method has mild reaction conditions, significantly reduces energy consumption, and is easy to prepare. The catalytic action of the catalyst is superior to that of conventional catalysts.
[0011] The third object of the present invention is to carry out the hydroformylation of olefins using an iridium catalyst. The present invention provides a method for hydroformylating olefins, comprising the steps of: By using a catalyst, the reaction temperature is low and the reaction conditions are mild, The selectivity of the target product is significantly improved. [Means for solving the problem]
[0012] In order to achieve the above object of the present invention, the following technical solutions are used.
[0013] The present invention provides an iridium catalyst, the chemical structure of which is as follows: do.
[0014] [ka]
[0015] In the formula, Ph is a phenyl group, R is a methyl group or an ethyl group, and X is CH3CO2, NO 3, Cl, BF4, PF6, SbF6 or more. China's Iridium-based Catalyst The name is 4,5-bis(diphenylphosphino)-9,9-dialkyloxanthene-i It is a lithium catalyst and its abbreviation is POP(R)-Ir-X.
[0016] The present invention further provides a method for preparing an iridium-based catalyst, which includes the steps of:
[0017] 4,5-Bis(diphenylphosphino)-9,9-dialkyloxanthene, solvent and The iridium compounds are mixed and stirred, and then heated and stirred to obtain an iridium catalyst. The solvent used was tetrahydrofuran, and the iridium compound was cyclooctadiene iridium. 4,5-bis(diphenylphosphino)diamine was selected as the dibasic phosphinodiamine in tetrahydrofuran. -9,9-Dialkyloxanthene and cyclooctadiene iridium chloride in a ratio of 2:1 The iridium catalyst POP(R)-Ir-X was obtained by reacting in a ratio of 1:1.
[0018] The mixing and stirring time is preferably 1.5 to 3 hours, and more preferably 2 hours.
[0019] Preferably, the temperature is raised to 40 to 60°C during heating and stirring, but preferably to 50°C. Then, the mixture is stirred for 1.5 to 3 hours, preferably for 2 hours.
[0020] Preferably, X in the iridium-based catalyst is CH3CO2, NO3, BF4, PF6, SbF In the case of 6, first heat and stir to obtain the target substance for substitution, and then add the compound containing the X group to the target substance for substitution. To add to something and make a substitution.
[0021] The present invention further provides a method for the hydroformylation of olefins using an iridium catalyst. It includes the following steps:
[0022] In the presence of the above catalyst, olefin, carbon monoxide, and hydrogen are used as raw materials, and the catalyst is Before the reaction, the catalyst is added to n-butyraldehyde, isobutyraldehyde, and toluene. The compound must be dissolved in toluene or tetrahydrofuran.
[0023] Preferably, the reaction temperature of the catalytic reaction is 70 to 120°C, more preferably 80 to 110°C. be.
[0024] Preferably, the catalytic reaction time is 6 to 9 hours, preferably 8 hours. The reaction time is not too long. A relatively short reaction time is not required, and a relatively high yield of the desired product is obtained.
[0025] Preferably, the reaction pressure of the catalytic reaction is 0.5 MPa to 3.0 MPa, preferably 1.0 MPa~2.0MPa.
[0026] Preferably, the partial pressure ratio of olefin to carbon monoxide is 10:1 to 1:10, more preferably 5:1 to 1:10. :1~1:5.
[0027] Preferably, the partial pressure ratio of olefin to hydrogen is 10:1 to 1:10, more preferably 5:1 to The ratio is 1:5.
[0028] Preferably, the catalyst dosage is 0.005 wt% to 2.0 wt% of the solvent amount, preferably 0. 05wt%~1.0%. Effect of the Invention
[0029] The iridium catalyst used in the present invention is a catalyst that uses propylene, carbon monoxide, and hydrogen as raw materials and Formylation is carried out to prepare n-butyraldehyde and isobutyraldehyde. Compared to conventional rhodium-based catalysts, rhodium metal exhibits a slower flow rate in the reaction. This inevitably affects the conversion rate and selectivity of the reaction, and also affects the The price of iridium metal is also rising rapidly, but the iridium catalyst used in the present invention is The cost is low, the preparation conditions and hydroformylation reaction conditions are mild, and n-butyraldehyde and the effect of preparing isobutyraldehyde is better. [Brief description of the drawings]
[0030] Those skilled in the art will recognize numerous other advantages of the present invention upon reading the detailed description of the preferred embodiments below. The drawings are only for the purpose of illustrating the preferred embodiment, and the advantages thereof will be clearly understood. In the drawings, like reference numerals refer to like elements throughout. The combinations are used.
[0031] [Figure 1] 1 is a chromatogram of the reaction product in Example 6 of the present invention. [Diagram 2] 1 is a chromatogram of the reaction product in Example 10 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] Hereinafter, the embodiments of the present invention will be described in detail based on examples. The following is merely illustrative of the invention and should not be construed as limiting the scope of the invention. It will be understood that the above conditions are not necessarily specified in the examples. The tests were carried out according to conventional conditions or those recommended by the manufacturer. Any drugs or devices for which the manufacturer is not specified are generic products available on the market. be. EXAMPLES
[0033] The method for preparing the iridium catalyst is as follows.
[0034] Synthesis of POP(CH3)-Ir-Cl: Place the 250 ml reaction flask under nitrogen. 100 ml of tetrahydrofuran, 5.0 g of cyclooctadiene iridium chloride, 4,5- Add 8.6 g of bis(diphenylphosphino)-9,9-dialkyloxanthene and heat at room temperature. The mixture was stirred at 40° C. for 2 hours and then heated to 50° C. and stirred for 2 hours. The solid was evaporated to dryness, washed twice with 20 ml of n-hexane, and weighed 11.9 g after drying. of POP(CH3)-Ir-Cl was obtained. EXAMPLES
[0035] The specific operation steps are the same as in Example 1, except that the mixing and stirring time is 1.5 The temperature during heating and stirring was 40°C, and the stirring time was 1.5 hours. 1.4 g of POP(CH3)-Ir-Cl was obtained. EXAMPLES
[0036] The specific operation steps are the same as in Example 1, except that the mixing and stirring time was 3 hours. The temperature was raised and the stirring time was set to 60°C and the stirring time was set to 3 hours. Finally, 11.5 g of of POP(CH3)-Ir-Cl was obtained. EXAMPLES
[0037] Synthesis of POP(CH3)-Ir-NO3: Add tetrahydrofuran to a 250 ml reaction flask. 150 ml of orchid, 5.0 g of POP(CH3)-Ir-Cl obtained in Examples 1 to 3, and silver nitrate Add 0.92 g of ethyl acetate and 20 ml of water, and react with stirring at room temperature for 6 hours in the dark. Filter out the insoluble matter. The solvent was evaporated to dryness, and the resulting solid was washed twice with 20 ml of n-hexane and dried. 4.5 g of POP(CH3)-Ir-NO3 was obtained. EXAMPLES
[0038] Synthesis of POP(CH3)-Ir-CH3CO2: Add tetrahydrofuran to a 250 mL reaction flask. 150 ml of Dorofuran, 5.0 g of POP(CH3)-Ir-Cl obtained in Examples 1 to 3, Add 0.90 g of silver nitrate and 20 ml of water, and react with stirring at room temperature for 6 hours in the dark. The solvent was evaporated to dryness, and the resulting solid was washed twice with 20 ml of n-hexane and dried. After drying, 4.6 g of POP(CH3)-Ir-CH3CO2 was obtained. EXAMPLES
[0039] The operation steps of the hydroformylation reaction are as follows:
[0040] In a 50 ml high-pressure reactor, POP(CH3)-Ir-CH3CO281m g, 12 ml of toluene was added, and the mixture was replaced with hydrogen three times. Then, propylene at 3 bar, 8 bar Carbon monoxide and 8 bar of hydrogen were then introduced, and the temperature was raised to 90° C. with stirring. The reaction was allowed to proceed at room temperature for 8 hours with stirring, and the reaction solution was then cooled to 0°C. The pressure was slowly reduced, and the reaction mixture was cooled to 0°C. Based on the results of the gas chromatography, The catalyst turnover number TON is 78.8, and the selectivity for n-butyraldehyde and isobutyraldehyde is 99.8% (n-butyraldehyde / isobutyraldehyde = 29.1:1) was able to calculate. [Examples 7 to 11]
[0041] The propylene hydroformylation reaction method of Example 6 was used, and the reaction temperature was changed to different values. The results are shown in Table 1.
[0042] Table 1. Effect of temperature on the hydroformylation reaction of propylene TIFF2024538219000003.tif60142 [Examples 12 to 17]
[0043] Using the propylene hydroformylation reaction method of Example 6, different gas pressures were used. The reaction was carried out using the above reaction mixture, and the results are shown in Table 2.
[0044] Table 2. Effect of pressure on the hydroformylation reaction of propylene TIFF2024538219000004.tif70147 Comparative example 1
[0045] The other operation steps were the same as in Example 6, except that the catalyst used was CN111. Tris(2,4-di-tert-butylphenyl) phosphite disclosed in US Pat. No. 3,48995A -Rhodium. The results are shown below.
[0046] Table 3. Effects of different catalysts on hydroformylation reaction TIFF2024538219000005.tif39141
[0047] As can be seen from the above table, the process of hydroformylation reaction using iridium catalysts In the process, the temperature is 80°C and the propylene gas pressure is 3 bar, The present invention achieves the highest n-butyraldehyde / isobutyraldehyde ratio of 29.1:1. This is because the present invention allows for good reaction selection even under low temperature and pressure conditions. The selectivity and conversion rate of the reaction are also shown in Comparative Example 1. Comparison with conventional catalysts shows that the new catalyst of the present invention not only reduces costs, but also has a catalytic effect that is superior to conventional catalysts. It can also be seen that the new iridium catalyst used in the present invention is superior to the conventional catalyst. By carrying out catalytic reactions and exploring the reaction conditions, we were able to carry out reactions under conditions of low energy consumption. Not only was it possible to carry out the reaction, but the reaction efficiency was also good.
[0048] Finally, the above-described embodiments are merely exemplary embodiments used to explain the principles of the present invention. It should be understood that the present invention is not limited thereto. Various modifications and improvements can be made without departing from the principles and essence of the present invention. are also considered to fall within the scope of protection of the present invention.
Claims
1. A process for the hydroformylation of olefins using an iridium-based catalyst, The process is as follows: In the presence of an iridium catalyst, olefins, carbon monoxide, and hydrogen are used as raw materials. and carrying out a catalytic reaction. Dissolving the iridium catalyst in a solvent prior to the reaction; The solvent is n-butyraldehyde, isobutyraldehyde, toluene or tetrahydrofuran. It is one of the flan, The iridium catalyst has the following chemical structure: 【Chemistry 1】 And, In the formula, Ph is a phenyl group, R is a methyl group or an ethyl group, and X is CH 3 CO 2 , NO 3 , B.F. 4 , P.F. 6 , SbF 6 and A method for preparing the iridium-based catalyst, comprising the steps of: 4,5-bis(diphenylphosphino)-9,9-dialkyloxanthene, a solvent and A step of mixing and stirring the iridium compounds, and further increasing the temperature and stirring to obtain the iridium catalyst. Including, The mixing and stirring time is 2 hours. In the heating and stirring, the temperature is raised to 50° C. and then stirring is continued for 2 hours. X in the iridium catalyst is CH 3 CO 2 , NO 3 , B.F. 4 , P.F. 6 , SbF 6 Yes In this case, the temperature is raised and the mixture is stirred to obtain a substance to be substituted, and then the compound containing the X group is added to the substance to be substituted. and performing a substitution. A method for hydroformylating olefins using an iridium catalyst, comprising: 。
2. The method according to claim 1, wherein the reaction temperature of the catalytic reaction is 70 to 120° C. Law.
3. The method according to claim 1, wherein the reaction temperature of the catalytic reaction is 80 to 110° C. Law.
4. The reaction pressure of the catalytic reaction is 0.5 MPa to 3.0 MPa.
2. The method according to claim 1.
5. The reaction pressure of the catalytic reaction is 1.0 MPa to 2.0 MPa.
2. The method according to claim 1.
6. The partial pressure ratio of the olefin to the carbon monoxide is 10:1 to 1:
10. The method according to claim 1 .
7. The partial pressure ratio of the olefin to the carbon monoxide is 5:1 to 1:
5. The method according to claim 1.
8. The partial pressure ratio of the olefin to the hydrogen is 10:1 to 1:
10. Item 1. The method according to item 1.
9. 2. The method according to claim 1, wherein the partial pressure ratio of the olefin to the hydrogen is 5:1 to 1:
5. The method according to
10. The mass of the iridium catalyst is 0.005 wt % to 2.0 wt % of the mass of the solvent.
2. The method of claim 1 ,
11. The mass of the iridium catalyst is 0.05 wt % to 1.0 wt % of the mass of the solvent.
2. The method of claim 1 .
Citation Information
Patent Citations
Phosphine-containing organic mixed polymer-metal multi-phase catalyst and method and application thereof
CN106140302A
Method for preparing aldehyde by olefin hydroformylation
CN111348995A
Carbonylation process using metal tridentate ligand catalysts
JP2006528960A
Method for hydroformylating unsaturated compounds
JP2014501709A
Method for controlling a hydroformylation process
JP2021525231A