ZSM-5 molecular sieve, its manufacturing method and use, hydrotreating catalyst, hydrodewaxing catalyst and use thereof
The modified ZSM-5 molecular sieve addresses pore and acidity issues by controlling acid content and mesopore distribution, enhancing hydrodewaxing efficiency and diesel quality through selective hydrogenation and reduced secondary cracking.
Patent Information
- Application Number
- JP2024524613
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-29
- Filing Date
- 2022-10-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-10-28
AI Technical Summary
Existing ZSM-5 molecular sieves suffer from side reactions due to pore openings and outer surface acidity, leading to reduced catalytic performance and efficiency in hydrodewaxing processes, necessitating frequent impregnation to remove acidity and causing waste of ester sil and pore channel clogging.
A modified ZSM-5 molecular sieve with controlled acid content and mesopore distribution is produced through hydrothermal treatment, aluminum removal, and silicon replenishment, followed by filtration, washing, and roasting, to enhance catalytic performance and stability.
The modified ZSM-5 molecular sieve improves the quality and yield of low freezing point diesel by selectively hydrogenating polycyclic aromatic hydrocarbons and preventing secondary cracking, resulting in higher diesel product yield and reduced acid center exposure.
Smart Images

Figure 2024538239000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of Chinese patent application No. 202111269100.0, filed on October 29, 2021, the contents of which are incorporated herein by reference.
[0002] [Technical field] The present invention relates to the field of molecular sieves and their preparation, in particular to ZSM-5 molecular sieves, their preparation and use, as well as hydrotreating catalysts, hydrodewaxing catalysts and their use. [Background technology]
[0003] In 1972, Mobile succeeded in synthesizing the first molecular sieve belonging to the "Pentasil" family using tetraethylammonium hydroxide as a template agent, and named this molecular sieve ZSM-5. The emergence of this molecular sieve was a milestone in the development of molecular sieves. In 1978, Kokotailo et al. analyzed the structure of ZSM-5 molecular sieve and confirmed that it has a three-dimensional double 10-membered ring pore channel structure with linear pore channels and sinusoidal pore channels, respectively. The two types of 10-ring pore channels are orthogonal to each other. The linear 10-ring pore channel is parallel to the b axis, with a pore size of 0.53×0.56 nm, and the sinusoidal 10-ring pore channel is parallel to the a axis, with a pore size of 0.51×0.55 nm, with cell parameters of a=2.017 nm, b=1.996 nm, and c=1.343 nm, respectively. These pore structure features provide shape-selective catalytic properties. Hydrodewaxing reaction enables selective cracking of chain hydrocarbons with poor low-temperature fluidity because the molecular dynamic size of most cyclic hydrocarbons and isoparaffinic hydrocarbons is larger than that of the 10-ring pore channel of ZSM-5 molecular sieve and they cannot enter the inside of the pore channel to react. In ZSM-5 molecular sieve raw powder, side reactions occur due to the acidity of the pore openings and outer surface, which affects the catalytic performance.
[0004] To obtain a catalyst with higher paraselectivity and reaction stability, it is necessary to modify ZSM-5 molecular sieves. Among them, silanization of molecular sieves is a frequently used and effective method to modify the acidity of the outer surface. Current silanization can be classified into (1) vacuum chemical vapor deposition, (2) flow chemical vapor deposition, (3) liquid-phase chemical impregnation, (4) reflux liquid-phase deposition, and (5) chemical reaction deposition. Although these methods have different processes, the main purpose is to remove the acidic center on the outer surface by supporting amorphous silica on the outer surface of the molecular sieve by deposition. However, the traditional silanization method needs to be repeatedly and periodically impregnated many times to achieve the purpose of removing the acidity of the outer surface, which results in a large amount of estersil being wasted and the efficiency of the modification process is greatly reduced. Although the improved chemical reaction deposition method improves the modification efficiency and the utilization rate of estersil, it requires special operations, which makes the process complicated and inevitably clogs the pore channels. Summary of the Invention [Problem to be solved by the invention]
[0005] In view of the shortcomings of the prior art, the present invention provides a ZSM-5 molecular sieve, its preparation method and use, as well as a hydrotreating catalyst, a hydrodewaxing catalyst and its use. The ZSM-5 molecular sieve can be widely used as a carrier or active component, for example, the catalyst prepared by using the ZSM-5 molecular sieve as a carrier can be used in the process of partially mixing catalytic diesel and / or coked diesel with straight-run diesel by hydrodewaxing to improve both the quality and yield of low-freezing point diesel. [Means for solving the problem]
[0006] A first aspect of the present invention provides a ZSM-5 molecular sieve, in which the total acid amount of pyridine measured by infrared ray is 0.03 to 0.40 mmol / g, the total acid amount of di-tert-butylpyridine measured by infrared ray is 0.002 to 0.02 mmol / g, the mesopore volume accounts for 10% to 20% of the total pore volume, and / or the volume of mesopores having a size of 2 to 10 nm accounts for 70% to 95% of the total mesopore volume.
[0007] A second aspect of the present invention is (1) hydrothermally treating a raw ZSM-5 molecular sieve; (2) removing non-framework aluminum from the molecular sieve obtained in (1); (3) impregnating the material obtained in step (2) with a pore channel protection liquid; a step (4) of treating the material obtained in step (3) with an organic acid; Step (5) of mixing the material obtained in step (4) with an aluminum removal silicon replenishment reagent to perform aluminum removal silicon replenishment; and (6) subjecting the material obtained in step (5) to filtering, washing, drying and roasting.
[0008] A third aspect of the present invention provides the use of said molecular sieve as a support and / or catalytically active component, preferably as a hydrogenation catalyst support.
[0009] A fourth aspect of the present invention provides a hydrotreating catalyst comprising the ZSM-5 molecular sieve of the present invention and a hydrogenation active component.
[0010] A fifth aspect of the present invention provides a hydrodewaxing catalyst containing the ZSM-5 molecular sieve of the present invention, preferably the ZSM-5 molecular sieve and a Group VIII metal component, the content of the ZSM-5 molecular sieve being 30% to 90% and the content of the Group VIII metal component being 5% to 40% calculated as an oxide, based on the weight of the catalyst.
[0011] A sixth aspect of the present invention provides the use of the hydrodewaxing catalyst of the present invention in the hydrodewaxing of an oil product, preferably wherein the oil product is a blend of straight run diesel and catalytic diesel and / or coked diesel. Effect of the Invention
[0012] Compared with the prior art, the present invention has the following advantages: 1. The ZSM-5 molecular sieve of the present invention has a low total acid content as measured by infrared spectroscopy using di-tert-butylpyridine, can remove mesopore acid and outer surface acid, and has a suitable mesopore distribution. The ZSM-5 molecular sieve can be widely used as a carrier or active component, for example, the catalyst prepared by using the ZSM-5 molecular sieve as a carrier can be used in the process of partially mixing catalytic diesel and / or coked diesel with straight-run diesel by hydrodewaxing to refine the diesel, thereby improving both the quality and yield of low-freezing point diesel. 2. In the preparation method of ZSM-5 molecular sieve of the present invention, first, obtain a certain amount of mesopores by hydrothermal treatment, then remove non-framework aluminum to smooth the pore channel, and then selectively remove the acid center of the non-"zigzag" pore channel by pore channel protection. Most of the aluminum sites in the non-zigzag pore channel are replaced by non-acidic silicon atoms through the action of aluminum removal silicon supplement, and the structure of the molecular sieve is kept intact. In a preferred embodiment of the present invention, the molecular sieve has better performance advantages because a small amount of acid centers can be retained on the outer surface and in the mesopores of the molecular sieve as needed. For example, when used in hydrodewaxing, a small amount of polycyclic aromatic hydrocarbons that are easily adsorbed in the feedstock are hydrogenated and ring-opened in the mesopores and on the weak acid sites on the outer surface, thereby improving the quality of diesel. Monocyclic and isomeric chain hydrocarbons with high quality and low freezing point are retained in the product because they have low competitive adsorption capacity and are difficult to enter the micropore channels of the ZSM-5 molecular sieve. Since the adsorption capacity of n-alkanes is weaker than that of aromatic hydrocarbons, they are not dominant in the competitive adsorption outside the pore channels, and therefore enter the micropore channels and undergo shape-selective cracking reactions, resulting in primary cracking products with reduced freezing points. The reduction of acid centers on the outer surface prevents the cracking products from continuing to crack into smaller non-diesel components. The smooth pore channels allow the primary cracking products to diffuse out of the pore channels in a timely manner, reducing secondary cracking, and ultimately significantly increasing the yield of low-freezing point diesel. [Brief description of the drawings]
[0013] [Figure 1] 1 shows XRD patterns of a commercially available ZSM-5 molecular sieve, the ZSM-5 molecular sieve Z-T4 obtained in Example 4 of the present invention, and the molecular sieve ZB obtained in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The functions and effects of the technical solution of the present invention will be further illustrated below with reference to examples and comparative examples, but the following examples do not limit the protection scope of the present invention.
[0015] The present invention provides a ZSM-5 molecular sieve, wherein the total acid amount of pyridine in the ZSM-5 molecular sieve as measured by infrared ray is 0.03 to 0.40 mmol / g, for example, 0.03 mmol / g, 0.04 mmol / g, 0.05 mmol / g, 0.06 mmol / g, 0.07 mmol / g, 0.08 mmol / g, 0.09 mmol / g, 0.10 mmol / g, 0.11 mmol / g, 0.12 mmol / g, 0.13 mmol / g, 0.14mmol / g, 0.15mmol / g, 0.16mmol / g, 0.17mmol / g, 0.18mmol / g, 0.19mmol / g, 0.20mmol / g, 0.21mmol / g, 0.22mm ol / g, 0.23mmol / g, 0.24mmol / g, 0.25mmol / g, 0.26mmol / g, 0.27mmol / g, 0.28mmol / g, 0.29mmol / g, 0.30mmol / g, 0. 31mmol / g, 0.32mmol / g, 0.33mmol / g, 0.34mmol / g, 0.35mmol / g, 0.36mmol / g, 0.37mmol / g, 0.38mmol / g, 0.39mmol / g, 0.40mmol / g, and the total acid amount by infrared measurement of di-tert-butylpyridine is 0.002 to 0.02mmol / g, for example, 0.002mmol / g, 0.003mmol / g, 0.004mmol / g, 0.005mmol / g, 0.006mmol / g, 0.007mmol / g, 0.008mmol / g, 0.009mmol / g, 0.010mmol / g, 0.011mmol / g, 0.012mmol / g, 0.013mmol / g, 0.014mmol / g, 0.015mmol / g, 0.016mmol / g, 0.017mmol / g, 0.018mmol / g, 0.019mmol / g, 0.020mmol / g, 0.021mmol / g, 0.022mmol / g, 0.023mmol / g, 0.024mmol / g, 0.025mmol / g, 0.026mmol / g, 0.027mmol / g, 0.028mmol / g, 0.029mmol / g, 0.030mmol / g, 0.031mmol / g, 0.32mmol / g, 0.33mmol / g, 0.34mmol / g, 0.35mmol / g, 0.3 mmol / g, 0.005mmol / g, 0.006mmol / g, 0.007mmol / g, 0.008mmol / g, 0.009mmol / g, 0.010mmol / g, 0.011mmol / g, 0.0 12mmol / g, 0.013mmol / g, 0.014mmol / g, 0.015mmol / g, 0.016mmol / g, 0.017mmol / g, 0.018mmol / g, 0.019mmol / g, 0.020mmol / g, the mesopore volume of the ZSM-5 molecular sieve accounts for 10%-20%, e.g., 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20% of the total pore volume, and / or the mesopore volume of 2-10 nm in the ZSM-5 molecular sieve accounts for 70%-95%, e.g., 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95% of the total mesopore volume.
[0016] According to a preferred embodiment of the present invention, the total acid amount of pyridine in the ZSM-5 molecular sieve measured by infrared ray is 0.10 to 0.20 mmol / g, for example, 0.10 mmol / g, 0.11 mmol / g, 0.12 mmol / g, 0.13 mmol / g, 0.14 mmol / g, 0.15 mmol / g, 0.16 mmol / g, 0.17 mmol / g, 0.18 mmol / g, 0.19 mmol / g, or 0.20 mmol / g, and the total acid amount of di-tert-butylpyridine measured by infrared ray is 0.005 to 0.01 mmol / g, for example, 0.005 mmol / g, 0.006 mmol / g, 0.007 mmol / g, 0.008 mmol / g, 0.009 mmol / g, or 0.010 mmol / g.
[0017] According to one preferred embodiment of the present invention, the ratio of the SiO2 / Al2O3 molar ratio of the outer surface of the ZSM-5 molecular sieve to the total SiO2 / Al2O3 molar ratio of the ZSM-5 molecular sieve is 2-100:1, preferably 5-30:1, for example, 5:1, 6:1, 7:1, 8:1, 8:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, 21:1, 22:1, 23:1, 24:1, 25:1, 26:1, 27:1, 28:1, 29:1, 30:1.
[0018] According to a preferred embodiment of the present invention, the SiO2 / Al2O3 molar ratio on the outer surface of said ZSM-5 molecular sieve is 200-1000, preferably 500-1000.
[0019] According to a preferred embodiment of the present invention, the total SiO2 / Al2O3 molar ratio of said ZSM-5 molecular sieve is 30-100, preferably 40-70.
[0020] According to a preferred embodiment of the present invention, the mesopore volume of the ZSM-5 molecular sieve accounts for 10%-20% of the total pore volume.
[0021] According to a preferred embodiment of the present invention, in the ZSM-5 molecular sieve, the volume of mesopores having a size of 2 to 10 nm accounts for 70% to 95% of the total mesopore volume.
[0022] As long as the molecular sieve has the above-mentioned characteristics of the present invention, the object of the present invention can be achieved, and there is no particular requirement for its preparation method. According to one preferred embodiment of the present invention, the present invention provides: (1) hydrothermally treating a raw ZSM-5 molecular sieve; (2) removing non-framework aluminum from the molecular sieve obtained in (1); (3) impregnating the material obtained in step (2) with a pore channel protection liquid; a step (4) of treating the material obtained in step (3) with an organic acid; Step (5) of mixing the material obtained in step (4) with an aluminum removal silicon replenishment reagent to perform aluminum removal silicon replenishment; and (6) subjecting the material obtained in step (5) to filtering, washing, drying and roasting.
[0023] In the present invention, the ZSM-5 molecular sieve raw material may be a commercially available product or a macroporous hydrogen type ZSM-5 molecular sieve produced by a conventional technique. Preferably, the ZSM-5 molecular sieve raw material has the following characteristics: SiO2 / Al2O3 molar ratio of 30 to 100, specific surface area of 300 to 450 m 2 / g, pore volume 0.15-0.20 cm 3 / g.
[0024] According to a preferred embodiment of the present invention, in step (1), the temperature of the hydrothermal treatment is 400 to 700°C, preferably 500 to 600°C.
[0025] According to the present invention, the time of the hydrothermal treatment is adjusted depending on the temperature, and in the present invention, preferably, the time of the hydrothermal treatment is 0.5 to 5 h, preferably 1 to 2 h.
[0026] According to the present invention, the pressure of the hydrothermal treatment is adjusted depending on the temperature, and in the present invention, the pressure of the hydrothermal treatment is 0.05 to 0.5 MPa, preferably 0.1 to 0.3 MPa.
[0027] In the present invention, there are several methods for removing non-skeletal aluminum, including, but not limited to, removing non-skeletal aluminum using a buffer solution. The buffer solution refers to a mixed solution consisting of a weak acid and its salt, or a weak base and its corresponding salt, which can to some extent eliminate or reduce the effect of an externally added strong acid or strong base on the acidity / alkalinity of the solution, thereby maintaining the pH value of the solution relatively stable.
[0028] In the present invention, unless otherwise specified, a solution refers to an aqueous solution.
[0029] In the present invention, the weak acid is preferably an inorganic acid and / or an organic acid having a molecular size of less than 0.5 nm and capable of being removed without damaging the structure of the molecular sieve by, for example, roasting.
[0030] According to one preferred embodiment of the invention, the inorganic acid is one or more of phosphoric acid, carbonic acid, and boric acid.
[0031] According to one preferred embodiment of the invention, the inorganic acid salts are ammonium salts of phosphoric acid, carbonic acid and boric acid.
[0032] According to one preferred embodiment of the present invention, the organic acid is selected from C2 to C6 monobasic or polybasic acids, preferably one or more of citric acid, formic acid, acetic acid, oxalic acid, propionic acid, malonic acid, butyric acid, and succinic acid.
[0033] According to one preferred embodiment of the present invention, the organic acid salt is selected from C2 to C6 monobasic or polybasic acid salts, preferably one or more of ammonium salts of citric acid, formic acid, acetic acid, oxalic acid, propionic acid, malonic acid, butyric acid, and succinic acid.
[0034] According to one preferred embodiment of the present invention, more preferably, the buffer solution is one or more of an oxalic acid-ammonium oxalate solution, and an acetic acid-ammonium acetate solution.
[0035] According to one preferred embodiment of the present invention, the buffer solution is acidic, and preferably has a pH value in the range of 4.5 to 6.5.
[0036] According to a preferred embodiment of the present invention, in the buffer solution, the molar concentration of the organic acid is 0.1 to 1.0 mol / L.
[0037] In the present invention, the range of the amount of the buffer solution used is wide, and according to one preferred embodiment of the present invention, the liquid / solid volume ratio of the buffer solution to the molecular sieve obtained in step (1) is 3:1 to 10:1.
[0038] According to one preferred embodiment of the present invention, the process of step (2) includes mixing and stirring the molecular sieve obtained in step (1) with a buffer solution, followed by solid-liquid separation, and optionally repeating the above operation 2 to 4 times. According to the present invention, the treatment temperature is preferably 40 to 80°C, and the treatment time is adjusted according to the temperature, but is preferably 0.5 to 3 h.
[0039] In the present invention, the pore channel protecting agent of the pore channel protecting solution is one or more of inorganic alkali or organic alkali, which has a molecular size of less than 0.5 nm and is easily removed by means such as roasting without damaging the structure of the molecular sieve, such as ammonia water, ethylenediamine, propylamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetramethylammonium bromide, and tetraethylammonium bromide.
[0040] According to one preferred embodiment of the present invention, in step (3), the pore channel protecting agent of the pore channel protecting solution is one or more of isopropylamine solution, tetramethylammonium hydroxide, tetraethylammonium hydroxide solution, and tetrapropylammonium hydroxide.
[0041] According to one preferred embodiment of the present invention, the pore channel protection liquid is preferably an aqueous solution of a pore channel protection agent, preferably one or more of an isopropylamine solution, a tetraethylammonium hydroxide solution, and a tetrapropylammonium hydroxide solution.
[0042] According to one preferred embodiment of the present invention, the concentration of the pore channel protecting solution is preferably 0.8 to 2.0 mol / L.
[0043] In the present invention, there is no particular requirement for the impregnation method, and in the present invention, the impregnation is preferably equal volume impregnation.
[0044] According to a preferred embodiment of the present invention, the impregnation temperature is 20 to 25°C.
[0045] In the present invention, in step (4), the organic acid is preferably an organic acid having a molecular size of 0.55 nm to 2 nm and being easily removable by a means such as roasting that does not damage the structure of the molecular sieve, for example, one or more of C7 to C10 organic acids.
[0046] According to a preferred embodiment of the invention, the organic acid is one or more of 2-methylbenzoic acid, 2-methylbenzenesulfonic acid, 2,4-xylenesulfonic acid, 2,4-dimethylbenzoic acid, 1,2,5-trimethylbenzenesulfonic acid, and 1,2,5-trimethylbenzoic acid.
[0047] According to a preferred embodiment of the present invention, in step (4), the organic acid is preferably one or more of 2,4-xylenesulfonic acid and 2,4-dimethylbenzoic acid.
[0048] According to a preferred embodiment of the present invention, the treatment process in step (4) preferably includes firstly mixing the material obtained in step (3) with water, such that the liquid / solid volume ratio between the water and the material obtained in step (3) is 2:1-6:1, and then adding an organic acid until the pH value of the solution is reduced to below 8, preferably 6.5-7.5.
[0049] In the present invention, in step (5), the type of aluminum-removing silicon supplement agent has a wide range of scope. According to a preferred embodiment of the present invention, the aluminum-removing silicon supplement agent of the aluminum-removing silicon supplement reagent is one or more of fluorosilicic acid, fluorosilicic acid salts (including but not limited to ammonium hexafluorosilicate, fluorosilicic acid, sodium fluorosilicate), silicon halide (including but not limited to silicon tetrachloride, silicon tetrafluoride), silicate (including but not limited to ethyl orthosilicate), preferably one or more of ammonium hexafluorosilicate, fluorosilicic acid, sodium fluorosilicate, silicon tetrachloride, silicon tetrafluoride, and ethyl orthosilicate; more preferably, the aluminum-removing silicon supplement reagent is at least one of ammonium hexafluorosilicate solution and ethyl orthosilicate solution.
[0050] According to a preferred embodiment of the present invention, the molar concentration of the aluminum-removing silicon-replenishing reagent is 0.3 to 1.0 mol / L.
[0051] In the present invention, the range of the amount of aluminum-removing silicon replenishment reagent used is wide, and according to a preferred embodiment of the present invention, the mass ratio of the material obtained in step (4) to the aluminum-removing silicon replenishment reagent is 1:1 to 1:5.
[0052] According to a preferred embodiment of the present invention, in step (5), the mixing temperature is 60 to 100°C.
[0053] According to a preferred embodiment of the present invention, the operation process of step (5) includes heating the material obtained in step (4) to 60-100°C, continuously stirring, dripping the aluminum removing silicon replenishment reagent, and continuing to stir for 60-120 minutes after the dripping is completed.
[0054] According to one preferred embodiment of the present invention, preferably, in step (6), the filtration and washing may be performed by a common method in the art, the drying temperature is 100°C to 150°C, the drying time is 2 to 4 hours, the roasting temperature is 400°C to 600°C, and the roasting time is 3 to 5 hours.
[0055] According to the present invention, there is provided the use of the molecular sieve of the present invention as a support and / or catalytically active component, preferably as a hydrogenation catalyst support.
[0056] According to the present invention, there is provided a hydrotreating catalyst comprising the ZSM-5 molecular sieve of the present invention and a hydrogenation active component, wherein the hydrogenation active component is preferably one or more selected from group VIB, VIIB and VIII metals, preferably one or more selected from Pt, Pd, Ni, W, Mo and Co.
[0057] According to the present invention, there is provided a hydrodewaxing catalyst containing the ZSM-5 molecular sieve of the present invention.
[0058] According to a preferred embodiment of the present invention, the hydrodewaxing catalyst preferably comprises the ZSM-5 molecular sieve and a Group VIII metal component, and the content of the ZSM-5 molecular sieve is 30% to 90%, and the content of the Group VIII metal component, calculated as an oxide, is 5% to 40%, based on the weight of the catalyst.
[0059] The present invention provides a use of the hydrodewaxing catalyst of the present invention in the hydrodewaxing of an oil product, preferably the oil product is a mixed oil product of straight run diesel and catalytic diesel and / or coked diesel.
[0060] According to a preferred embodiment of the present invention, the SiO2 / Al2O3 molar ratio of the outer surface of the ZSM-5 molecular sieve is 200-1000, the total SiO2 / Al2O3 molar ratio is 30-100, the total acid amount of pyridine is 0.03-0.40 mmol / g by infrared measurement, the total acid amount of di-tert-butylpyridine is 0.002-0.02 mmol / g by infrared measurement, and the mesopore volume of the ZSM-5 molecular sieve accounts for 10%-20% of the total pore volume.
[0061] According to a preferred embodiment of the present invention, preferably, the SiO2 / Al2O3 molar ratio of the outer surface of said ZSM-5 molecular sieve is 500-1000, and the total SiO2 / Al2O3 molar ratio is 40-70.
[0062] According to a preferred embodiment of the present invention, the ZSM-5 molecular sieve preferably has a total acid amount of pyridine measured by infrared ray of 0.10-0.20 mmol / g, and a total acid amount of di-tert-butylpyridine measured by infrared ray of 0.005-0.01 mmol / g.
[0063] According to a preferred embodiment of the present invention, the mesopores in the ZSM-5 molecular sieve are preferably concentrated in the range of 2 to 10 nm, and the volume of the mesopores in the range of 2 to 10 nm accounts for 70% to 95% of the total mesopore volume. In the present invention, the mesopores are pores having a pore diameter of 2 to 50 nm.
[0064] According to one preferred embodiment of the present invention, the present invention comprises: (1) hydrothermally treating a ZSM-5 molecular sieve; (2) removing non-framework aluminum from the molecular sieve obtained in (1); (3) impregnating the material obtained in step (2) with a pore channel protection liquid; a step (4) of treating the material obtained in step (3) with an organic acid; Step (5) of mixing the material obtained in step (4) with an aluminum removal silicon replenishment reagent to perform aluminum removal silicon replenishment; and (6) filtering, washing, drying and roasting the material obtained in step (5) to obtain ZSM-5 molecular sieve.
[0065] According to one preferred embodiment of the present invention, preferably in step (1), the temperature of the hydrothermal treatment is 400 to 700°C, preferably 500 to 600°C, the time is 0.5 to 5 h, preferably 1 to 2 h, and the pressure is 0.05 to 0.5 MPa, preferably 0.1 to 0.3 MPa.
[0066] According to one preferred embodiment of the present invention, preferably, in step (2), the method for removing non-framework aluminum may be a method of removing non-framework aluminum using a buffer solution. The buffer solution used is one or more of an oxalic acid-ammonium oxalate solution and an acetic acid-ammonium acetate solution. The pH value of the buffer solution is in the range of 4.5-6.5, preferably 5.0-6.0. In the buffer solution, the molar concentration of the organic acid is 0.1-1.0 mol / L. The liquid / solid volume ratio of the buffer solution to the molecular sieve obtained in step (1) is 3:1-10:1.
[0067] According to one preferred embodiment of the present invention, preferably, in step (2), the specific treatment process is as follows: the molecular sieve obtained in step (1) is mixed with a buffer solution and stirred, the treatment temperature is 40-80°C, the treatment time is 0.5-3h, and then solid-liquid separation (for example, suction filtration) is performed, and the above operation is repeated 2-4 times.
[0068] According to a preferred embodiment of the present invention, in step (3), the pore channel protection solution is preferably one or more of isopropylamine solution, tetraethylammonium hydroxide solution, tetrapropylammonium hydroxide solution, etc. The concentration of the pore channel protection solution is 0.8-2.0 mol / L, preferably 1.1-1.5 mol / L.
[0069] According to one preferred embodiment of the present invention, preferably in step (3), the impregnation is preferably equal volume impregnation. The temperature of the impregnation treatment is room temperature, generally 20 to 25°C.
[0070] According to one preferred embodiment of the present invention, in step (4), the organic acid is preferably one or more of 2,4-xylenesulfonic acid and 2,5-dimethylbenzoic acid.
[0071] According to one preferred embodiment of the present invention, the specific operation is preferably as follows: first, mix the material obtained in step (3) with water, so that the liquid / solid volume ratio between the water and the material obtained in step (3) is 2:1-6:1, and then add organic acid until the pH value of the solution is reduced to below 8, preferably 6.5-7.5.
[0072] According to one preferred embodiment of the present invention, in step (5), the aluminum-removed silicon replenishment reagent is at least one of an ammonium hexafluorosilicate solution, an ethyl orthosilicate solution, etc. The molar concentration of the aluminum-removed silicon replenishment reagent is 0.3-1.0 mol / L. The mass ratio of the material obtained in step (4) to the aluminum-removed silicon replenishment reagent is 1:1-1:5. The mixing temperature is 60-100°C.
[0073] According to one preferred embodiment of the present invention, the specific operation process of step (5) is preferably as follows: the material obtained in step (4) is rapidly heated to 60-100°C, stirred continuously, and the aluminum removing silicon replenishment reagent is dripped in, and after the dripping is completed, stirring is continued for 60-120 min. The dripping speed is 0.5 mL / min g (material obtained in step (4)), preferably 0.2-0.4 mL / min g (material obtained in step (4)).
[0074] According to one preferred embodiment of the present invention, preferably, in step (6), the filtration and washing may be performed by a common method in the art, the drying temperature is 100°C to 150°C, the drying time is 2 to 4 hours, the roasting temperature is 400°C to 600°C, and the roasting time is 3 to 5 hours.
[0075] According to one preferred embodiment of the present invention, there is provided a hydrodewaxing catalyst comprising the above-described ZSM-5 molecular sieve.
[0076] According to one preferred embodiment of the present invention, the hydrodewaxing catalyst preferably contains the above-mentioned ZSM-5 molecular sieve and a Group VIII metal component, and the content of the ZSM-5 molecular sieve is 30% to 90%, preferably 40% to 70%, and the content of the Group VIII metal component, calculated as an oxide, is 5% to 40%, preferably 10% to 30%, based on the weight of the catalyst.
[0077] According to one preferred embodiment of the present invention, the hydrodewaxing catalyst preferably comprises the ZSM-5 molecular sieve, alumina, and a Group VIII metal component, and the content of the ZSM-5 molecular sieve is 30% to 50%, the content of alumina is 40% to 70%, and the content of the Group VIII metal component, calculated as an oxide, is 5% to 40%, based on the weight of the catalyst.
[0078] According to one preferred embodiment of the present invention, preferably said Group VIII metal is cobalt and / or nickel.
[0079] According to one preferred embodiment of the present invention, the present invention provides the use of the above-described hydrodewaxing catalyst in the hydrodewaxing of a feedstock.
[0080] According to one preferred embodiment of the present invention, preferably said use comprises reacting a feedstock with the action of said hydrodewaxing catalyst in the presence of hydrogen to obtain a low freezing point diesel.
[0081] According to one preferred embodiment of the present invention, the reaction conditions for hydrodewaxing in the above-mentioned use are preferably a reaction pressure of 5.0 to 8.0 MPa, a hydrogen / oil volume ratio of 400:1 to 600:1, and a liquid hourly space velocity of 0.5 to 2 h -1 The reaction temperature is 280 to 400°C.
[0082] According to one preferred embodiment of the present invention, the feedstock oil is preferably a mixture of straight-run diesel and catalytic diesel and / or coked diesel. In the feedstock oil, the total mixture amount of catalytic diesel and / or coked diesel is 20% to 40%, the content of wax (n-alkane having more than 20 carbon atoms) is 5% to 15% by mass, and the content of polycyclic aromatic hydrocarbons is 10% to 30% by mass. The distillation range of the feedstock oil is usually 150 to 400°C. EXAMPLES
[0083] In the present invention, % in the examples and comparative examples means mass fraction unless otherwise specified.
[0084] In the present invention, the molar ratio of SiO2 / Al2O3 on the outer surface is measured by X-ray photoelectron spectroscopy (XPS), and the elemental composition and state of the catalyst surface are measured by a Multilab2000 electron energy spectrometer from Thermo Fisher Scientific, USA, with the excitation source being MgKα, the cathode voltage and current being 13 kV and 20 mA, respectively. The electron binding energy is calibrated using C1s (284.6 eV).
[0085] In the present invention, the total SiO2 / Al2O3 molar ratio is obtained by X-ray fluorescence spectroscopy (XRF) analysis, using a ZSX100e X-ray fluorescence spectrometer, the spectral line is Kα, the crystal is LiF1, the target material is Rh, the detector is a SC scintillation counter, the timing is 20 seconds, and the atmosphere of the optical path is vacuum.
[0086] In the present invention, the specific surface area, pore volume, and pore distribution are measured as follows: A low-temperature liquid nitrogen physical adsorption apparatus ASAP 2420 manufactured by Micromeritics, Inc., USA is used, the pretreatment temperature is 300° C., and the pretreatment time is 4 hours.
[0087] In the present invention, the infrared measurement method for pyridine is as follows: Powdered ZSM-5 molecular sieve is pressed into a sheet, vacuum-suctioned, and then degassed at 450°C for 2h. When the temperature is lowered to room temperature, the infrared spectrum of chemical desorption is measured using pyridine molecules as probe molecules, and the amount of adsorption is calculated.
[0088] In the present invention, the total acid amount of di-tert-butylpyridine measured by infrared measurement refers to the protonic acid that can be contacted by 2,6-di-tert-butylpyridine molecules with a dynamic diameter of 10.5 Å. The infrared measurement method for 2,6-di-tert-butylpyridine is as follows. Powdered ZSM-5 molecular sieve is pressed into a sheet, vacuum-suctioned, and degassed at 450°C for 2 hours. When the temperature is lowered to room temperature, the infrared spectrum of chemical desorption is measured using 2,6-di-tert-butylpyridine molecules as probe molecules, and the adsorption amount is calculated.
[0089] The ZSM-5 raw powder according to the examples and comparative examples of the present invention is a commercially available product, which is a microporous hydrogen-type ZSM-5 molecular sieve. The characteristics of the ZSM-5 are a specific surface area of 405 m 2 / g, pore volume 0.182 cm 3 / g, water absorption is 55%, and SiO2 / Al2O3 ratio (mol) is 31.2.
[0090] Example 1 30 g of commercially available ZSM-5 raw powder was placed in a hydrothermal treatment furnace and treated at 500 °C and 0.1 MPa pressure for 2 h. The resulting material was placed in 300 mL of oxalic acid-ammonium oxalate solution with a pH value of 6.0 and a molar concentration of oxalic acid of 0.3 mol / L, stirred and heated to 60 °C, and suction filtered for 30 min. This process was repeated three times. Then, an equal volume of impregnation was performed using 16.5 mL of isopropylamine solution with a concentration of 1.1 mol / L and allowed to stand for 10 min. 170 mL of water was added, 2,5-xylenesulfonic acid was dripped in until the pH value reached 6.5, stirred and heated to 60 °C, and 90 mL of ammonium hexafluorosilicate solution with a concentration of 0.3 mol / L was dripped in at a rate of 0.2 mL / min g by a peristaltic pump, and the temperature was maintained at 60 °C and stirred for 90 min. The mixture was filtered under suction while still hot, and 300 mL of water was added to the filter cake obtained, which was then heated to 60°C and kept warm for 20 min. The mixture was filtered under suction while still hot, and the filter cake was dried at 120°C for 24 h, and then roasted at 500°C for 3 h to obtain a molecular sieve, which was named Z-T1.
[0091] Example 2 30 g of commercial ZSM-5 raw powder was placed in a hydrothermal treatment furnace and treated at 530 °C and 0.1 MPa pressure for 2 h. The resulting material was placed in 300 mL of acetic acid-ammonium acetate solution with a pH value of 6.0 and a molar concentration of acetic acid of 0.2 mol / L, stirred and heated to 60 °C, and suction filtered for 30 min. This process was repeated three times. Then, an equal volume impregnation was performed using 16.5 mL of tetraethylammonium hydroxide solution with a concentration of 1.2 mol / L, and the mixture was left to stand for 10 min. 170 mL of water was added, 2,5-dimethylbenzoic acid was added dropwise until the pH value reached 7.0, stirred and heated to 65 °C. 90 mL of ammonium hexafluorosilicate solution with a concentration of 0.5 mol / L was added dropwise at a rate of 0.2 mL / min·g by a peristaltic pump, and the mixture was stirred for 90 min while maintaining the temperature at 65 °C. The mixture was filtered under suction while still hot, and 300 mL of water was added to the filter cake obtained, which was then heated to 60°C and kept warm for 20 min. The mixture was filtered under suction while still hot, and the filter cake was dried at 120°C for 24 h, and then roasted at 500°C for 3 h to obtain a molecular sieve, which was named Z-T2.
[0092] Example 3 30 g of commercially available ZSM-5 raw powder was placed in a hydrothermal treatment furnace and treated at 550 °C and 0.1 MPa for 2 h. The resulting material was placed in 300 mL of oxalic acid-ammonium oxalate solution with a pH value of 5.5 and a molar concentration of oxalic acid of 0.4 mol / L, stirred and heated to 70 °C, and suction filtered for 30 min. This process was repeated three times. The resulting material was impregnated with 16.5 mL of tetrapropylammonium hydroxide solution with a concentration of 1.2 mol / L at an equal volume, left to stand for 10 min, 170 mL of water was added, 2,4-xylenesulfonic acid was dripped until the pH value reached 6.5, stirred and heated to 65 °C, and 90 mL of ethyl orthosilicate solution with a concentration of 0.6 mol / L was dripped at a rate of 0.3 mL / min·g by a peristaltic pump, and the temperature was maintained at 65 °C and stirred for 90 min. The mixture was filtered under suction while still hot, 300 mL of water was added to the filter cake obtained, and the mixture was heated to 60°C and kept warm for 20 min. The mixture was filtered under suction while still hot, and the filter cake was dried at 120°C for 24 h and then roasted at 500°C for 3 h to obtain a molecular sieve, which was named Z-T3.
[0093] Example 4 30 g of commercially available ZSM-5 raw powder was placed in a hydrothermal treatment furnace and treated at 550 °C and 0.15 MPa for 2 h. The resulting material was placed in 300 mL of oxalic acid-ammonium oxalate solution with a pH value of 5.5 and an oxalic acid concentration of 0.4 mol / L, stirred and heated to 80 °C, and suction filtered for 30 min. This process was repeated three times. The resulting material was impregnated with 16.5 mL of isopropylamine solution with a concentration of 1.2 mol / L in equal volume, left to stand for 10 min, 170 mL of water was added, 2,4-xylenesulfonic acid was dripped until the pH value reached 7.0, stirred and heated to 65 °C, and 90 g of ammonium hexafluorosilicate solution with a concentration of 0.6 mol / L was dripped at a rate of 0.3 mL / min·g by a peristaltic pump, and the temperature was maintained at 65 °C and stirred for 90 min. The mixture was filtered under suction while still hot, and 300 mL of water was added to the filter cake obtained, which was then heated to 60°C and kept warm for 20 min. The mixture was filtered under suction while still hot, and the filter cake was dried at 120°C for 24 h, and then roasted at 500°C for 3 h to obtain a molecular sieve, which was named Z-T4.
[0094] Example 5 30 g of commercially available ZSM-5 raw powder was placed in a hydrothermal treatment furnace and treated at 550 °C and 0.15 MPa for 2 h. The resulting material was placed in 300 mL of oxalic acid-ammonium oxalate solution with a pH value of 5.0 and an oxalic acid concentration of 0.3 mol / L, stirred and heated to 60 °C, and suction filtered for 30 min. This process was repeated three times. The resulting material was impregnated with 16.5 mL of isopropylamine solution with a concentration of 1.2 mol / L in equal volume, left to stand for 10 min, 170 mL of water was added, 2,4-dimethylbenzoic acid was dripped until the pH value reached 7.0, stirred and heated to 65 °C, and 90 mL of ammonium hexafluorosilicate solution with a concentration of 0.6 mol / L was dripped at a rate of 0.3 mL / min g by a peristaltic pump, and the temperature was maintained at 65 °C and stirred for 90 min. The mixture was filtered under suction while still hot, and 300 mL of water was added to the filter cake obtained, which was then heated to 60°C and kept warm for 20 min. The mixture was filtered under suction while still hot, and the filter cake was dried at 120°C for 24 h, and then roasted at 500°C for 3 h to obtain a molecular sieve, which was named Z-T5.
[0095] Example 6 30 g of commercially available ZSM-5 raw powder was placed in a hydrothermal treatment furnace and treated at 550 °C and 0.15 MPa for 2 h. The resulting material was placed in 300 mL of acetic acid-ammonium acetate solution with a pH value of 5.0 and an acetic acid concentration of 0.3 mol / L, stirred and heated to 60 °C, and suction filtered for 30 min. This process was repeated three times. The resulting material was impregnated with 16.5 mL of tetraethylammonium hydroxide solution with a concentration of 1.3 mol / L in equal volume, left to stand for 10 min, added with 170 mL of water, dropped with 2,4-xylenesulfonic acid until the pH value reached 7.5, stirred and heated to 65 °C, and 90 mL of ammonium hexafluorosilicate solution with a 0.6 mol / L was added dropwise at a rate of 0.3 mL / min·g by a peristaltic pump, and stirred for 90 min while maintaining the temperature at 65 °C. The mixture was filtered under suction while still hot, and 300 mL of water was added to the filter cake obtained, which was then heated to 60°C and kept warm for 20 min. The mixture was filtered under suction while still hot, and the filter cake was dried at 120°C for 24 h, and then roasted at 500°C for 3 h to obtain a molecular sieve, which was named Z-T6.
[0096] Example 7 30 g of commercially available ZSM-5 raw powder was placed in a hydrothermal treatment furnace and treated at 570 °C and 0.15 MPa for 2 h. The resulting material was placed in 300 mL of acetic acid-ammonium acetate solution with a pH value of 5.0 and an acetic acid concentration of 0.5 mol / L, stirred and heated to 60 °C, and suction filtered for 30 min. This process was repeated three times. The resulting material was impregnated with 16.5 mL of isopropylamine solution with a concentration of 1.5 mol / L in equal volume, left to stand for 10 min, 170 mL of water was added, 2,4-dimethylbenzoic acid was dripped until the pH value reached 7.5, stirred and heated to 65 °C, and 90 mL of ethyl orthosilicate solution with a concentration of 0.8 mol / L was dripped at a rate of 0.4 mL / min g by a peristaltic pump, and the temperature was maintained at 65 °C and stirred for 90 min. The mixture was filtered under suction while still hot, and 300 mL of water was added to the filter cake obtained, which was then heated to 60°C and kept warm for 20 min. The mixture was filtered under suction while still hot, and the filter cake was dried at 120°C for 24 h, and then roasted at 500°C for 3 h to obtain a molecular sieve, which was named Z-T7.
[0097] Example 8 30 g of commercially available ZSM-5 raw powder was placed in a hydrothermal treatment furnace and treated at 570 °C and 0.2 MPa for 2 h. The resulting material was placed in 300 mL of oxalic acid-ammonium oxalate solution with a pH value of 5.0 and an oxalic acid concentration of 0.5 mol / L, stirred and heated to 60 °C, and suction filtered for 30 min. This process was repeated three times. The resulting material was impregnated with 16.5 mL of isopropylamine solution with a concentration of 1.5 mol / L by equal volume, left to stand for 10 min, 170 mL of water was added, 2,4-dimethylbenzoic acid was dripped until the pH value reached 7.5, stirred and heated to 65 °C, and 90 mL of 1.0 mol / L ammonium hexafluorosilicate solution was dripped at a rate of 0.4 mL / min g by a peristaltic pump, and the temperature was maintained at 65 °C and stirred for 90 min. The mixture was filtered under suction while still hot, and 300 mL of water was added to the filter cake obtained, which was then heated to 60°C and kept warm for 20 min. The mixture was filtered under suction while still hot, and the filter cake was dried at 120°C for 24 h, and then roasted at 500°C for 3 h to obtain a molecular sieve, which was named Z-T8.
[0098] Comparative Example 1 30g of commercial ZSM-5 raw powder was placed in a hydrothermal treatment furnace and treated at 550℃ and 0.15MPa pressure for 2h, the resulting material was placed in 300mL of oxalic acid-ammonium oxalate solution with pH value of 5.0 and molar concentration of oxalic acid of 0.3mol / L, stirred and heated to 60℃, and suction filtered for 30min, this process was repeated three times, the filter cake was dried at 120℃ for 24h, and then roasted at 500℃ for 3h to obtain a molecular sieve, which was named ZB.
[0099] Comparative Example 2 30 g of commercially available ZSM-5 raw powder was placed in a hydrothermal treatment furnace and treated at 550 °C and 0.15 MPa for 2 h. The resulting material was placed in 300 mL of oxalic acid-ammonium oxalate solution with a pH value of 5.0 and an oxalic acid concentration of 0.3 mol / L, stirred and heated to 60 °C, and suction filtered for 30 min. This process was repeated three times. 90 mL of 0.6 mol / L ammonium hexafluorosilicate solution was dripped into the resulting material at a constant rate of 0.3 mL / min g by a peristaltic pump, and the temperature was maintained at 65 °C and stirred for 90 min. The mixture was suction filtered while hot, and the filter cake was dried at 120 °C for 24 h, and then roasted at 500 °C for 3 h to obtain a molecular sieve, which was named ZC.
[0100] Comparative Example 3 30 g of commercially available ZSM-5 raw powder was placed in a hydrothermal treatment furnace and treated at 550°C and 0.15 MPa for 2 h. The resulting material was impregnated with 16.5 mL of 0.6 mol / L isopropylamine solution at an equal volume, left to stand for 10 min, 170 mL of water was added, 2,4-dimethylbenzoic acid was added dropwise until the pH value reached 7.0, the mixture was stirred and heated to 65°C, and 90 mL of 0.6 mol / L ammonium hexafluorosilicate solution was added dropwise at a rate of 0.3 mL / min g using a peristaltic pump. The mixture was stirred for 90 min while maintaining the temperature at 65°C. The mixture was filtered under suction while still hot, 300 mL of water was added to the filter cake obtained, and the mixture was heated to 60°C and kept warm for 20 min. The mixture was filtered under suction while still hot, and the filter cake was dried at 120°C for 24 h and then roasted at 500°C for 3 h to obtain a molecular sieve, which was named ZD.
[0101] Comparative Example 4 30 g of commercially available ZSM-5 raw powder was heated to 65°C with stirring, and 180 mL of 1.0 mol / L ammonium hexafluorosilicate solution was added dropwise at a rate of 0.4 mL / min g using a peristaltic pump. The temperature was maintained at 65°C and stirring was continued for 90 min. The mixture was filtered under suction while still hot, and the filter cake was dried at 120°C for 24 h and then roasted at 500°C for 3 h to obtain a molecular sieve, which was named ZE.
[0102] [Table 1]
[0103] Example 9 The method was the same as that in Example 5, except that the buffer solution used was a citric acid-ammonium citrate solution with a pH value of 5.0. The obtained molecular sieve was named Z-T9.
[0104] Example 10 The pore channel protection solution was ammonia water with a concentration of 1.2 mol / L, but the same as the method of Example 5. The obtained molecular sieve was named Z-T10.
[0105] Example 11 The organic acid in step (4) was 2-methylbenzenesulfonic acid, and the procedure was the same as in Example 5. The resulting molecular sieve was named Z-T11.
[0106] Example 12 Except that the aluminum removing silicon supplementing reagent was 0.6 mol / L fluorosilicic acid solution, the method was the same as that in Example 5. The obtained molecular sieve was named Z-T12.
[0107] Example 13 Catalysts were produced using the molecular sieves Z-T1 to Z-T12 obtained in Examples 1 to 12, respectively. In the production, the roasted molecular sieves and macroporous alumina (specific surface area: 302 m 2 / g, pore volume is 0.96 cm 3The carrier was obtained by kneading the molecular sieve (wt%) with alumina sol as a binder, extruding the extruded material into a strand shape, forming the material, and then drying and roasting the material. The carrier was impregnated with an impregnation solution of nickel nitrate, and then drying and roasting the material to obtain catalysts, which were named C1 to C12. The mass fraction of the molecular sieve was 30 wt%, the mass fraction of the macroporous alumina was 50 wt%, the mass fraction of NiO was 10 wt%, and the remainder was the binder. 10 g of each of catalysts C1 to C12 was placed in a fixed-bed reactor, and the reaction pressure was 6.0 MPa, hydrogen / oil volume ratio was 500:1, and liquid hourly space velocity was 10 h -1 The hydrodewaxing reaction was carried out at a reaction temperature of 320° C. The characteristics of the raw material are shown in Table 2, and the product distribution and characteristics of the product are shown in Table 3.
[0108] [Table 2]
[0109] [Table 3]
[0110] Comparative Example 4 Commercially available ZSM-5 molecular sieves and macroporous alumina (specific surface area is 302 m 2 / g, pore volume is 0.96 cm 3 The catalyst DC1 was obtained by kneading ZSM-5 (ZSM-5 mass percentage: 30 wt%), macroporous alumina mass percentage: 50 wt%, NiO mass percentage: 10 wt%, and the remainder was binder. 10 g of catalyst DC1 was placed in a fixed-bed reactor, and the reaction pressure was 6.0 MPa, hydrogen / oil volume ratio was 500:1, and the liquid hourly space velocity was 10 h -1 The hydrodewaxing reaction was carried out under hydrodewaxing conditions of 1000 g / l and a reaction temperature of 340° C. The characteristics of the raw materials are shown in Table 2, and the product distribution and characteristics of the products are shown in Table 4.
[0111] [Table 4]
[0112] Comparative Example 5 Molecular sieve ZB and macroporous alumina (specific surface area is 302 m 2 / g, pore volume is 0.96 cm 3 The catalyst DC2 was obtained by kneading ZSM-5 (ZSM-5 mass percentage: 30 wt%) with alumina sol as a binder, extruding the mixture into a strand shape, forming the mixture, and then drying and roasting the mixture to obtain a carrier. The carrier was impregnated with an impregnation solution of nickel nitrate, and then drying and roasting the mixture to obtain catalyst DC2. The mass percentage of ZSM-5 was 30 wt%, the mass percentage of macroporous alumina was 50 wt%, the mass percentage of NiO was 10 wt%, and the remainder was the binder. 10 g of catalyst DC2 was placed in a fixed-bed reactor, and the reaction pressure was 6.0 MPa, hydrogen / oil volume ratio was 500:1, and liquid hourly space velocity was 10 h -1 The hydrodewaxing reaction was carried out under hydrodewaxing conditions of 1000 g / l and a reaction temperature of 340° C. The characteristics of the raw materials are shown in Table 2, and the product distribution and characteristics of the products are shown in Table 5.
[0113] [Table 5]
[0114] Comparative Example 6 Molecular sieve ZC and macroporous alumina (specific surface area is 302 m 2 / g, pore volume is 0.96 cm 3 The catalyst DC3 was obtained by kneading ZSM-5 (ZSM-5 mass percentage: 30 wt%) with alumina sol as a binder, extruding the mixture into a strand shape, forming the mixture, and then drying and roasting the mixture to obtain a carrier. The carrier was impregnated with an impregnation solution of nickel nitrate, and then drying and roasting the mixture to obtain a catalyst DC3. The mass percentage of ZSM-5 was 30 wt%, the mass percentage of macroporous alumina was 50 wt%, the mass percentage of NiO was 10 wt%, and the remainder was the binder. 10g of catalyst DC3 was placed in a fixed-bed reactor, the reaction pressure was 6.0MPa, the hydrogen / oil volume ratio was 500:1, and the liquid hourly space velocity was 10h -1 The hydrodewaxing reaction was carried out under hydrodewaxing conditions of 1000 g / l and a reaction temperature of 340° C. The characteristics of the raw materials are shown in Table 2, and the product distribution and characteristics of the products are shown in Table 6.
[0115] [Table 6]
[0116] Comparative Example 7 Molecular sieve ZD and macroporous alumina (specific surface area is 302 m 2 / g, pore volume is 0.96 cm 3 The catalyst DC4 was obtained by kneading ZSM-5 (ZSM-5 mass percentage: 30 wt%) with alumina sol as a binder, extruding the mixture into a strand shape, forming the mixture, and then drying and roasting the mixture to obtain a carrier. The carrier was impregnated with an impregnation solution of nickel nitrate, and then drying and roasting the mixture to obtain a catalyst DC4. The mass percentage of ZSM-5 was 30 wt%, the mass percentage of macroporous alumina was 50 wt%, the mass percentage of NiO was 10 wt%, and the remainder was the binder. 10 g of catalyst DC4 was placed in a fixed-bed reactor, and the reaction pressure was 6.0 MPa, hydrogen / oil volume ratio was 500:1, and the liquid hourly space velocity was 10 h -1 The hydrodewaxing reaction was carried out under hydrodewaxing conditions of 1000 g / l and a reaction temperature of 340° C. The characteristics of the raw materials are shown in Table 2, and the product distribution and characteristics of the products are shown in Table 7.
[0117] [Table 7]
[0118] Comparative Example 8 Molecular sieve ZE and macroporous alumina (specific surface area is 302 m 2 / g, pore volume is 0.96 cm 3 The catalyst DC5 was obtained by kneading ZSM-5 (ZSM-5 mass percentage: 30 wt%) with alumina sol as a binder, extruding the mixture into a strand shape, forming the mixture, and then drying and roasting the mixture to obtain a carrier. The carrier was impregnated with an impregnation solution of nickel nitrate, and then drying and roasting the mixture to obtain a catalyst DC5. The mass percentage of ZSM-5 was 30 wt%, the mass percentage of macroporous alumina was 50 wt%, the mass percentage of NiO was 10 wt%, and the remainder was the binder. 10 g of catalyst DC5 was placed in a fixed-bed reactor, and the reaction pressure was 6.0 MPa, hydrogen / oil volume ratio was 500:1, and liquid hourly space velocity was 10 h -1The hydrodewaxing reaction was carried out under hydrodewaxing conditions of 100% and a reaction temperature of 340° C. The characteristics of the raw materials are shown in Table 2, and the product distribution and characteristics of the products are shown in Table 8.
[0119] [Table 8]
Claims
1. A ZSM-5 molecular sieve, characterized in that the total acid amount of pyridine measured by infrared ray is 0.03 to 0.40 mmol / g, the total acid amount of di-tert-butylpyridine measured by infrared ray is 0.002 to 0.02 mmol / g, the mesopore volume accounts for 10% to 20% of the total pore volume, and / or the mesopore volume of 2 to 10 nm accounts for 70% to 95% of the total mesopore volume.
2. The total acid amount of pyridine measured by infrared measurement is 0.10 to 0.20 mmol / g, and the total acid amount of di-tert-butylpyridine measured by infrared measurement is 0.005 to 0.01 mmol / g, and / or Outer SiO 2 / Al 2 O 3 Molar ratio and total SiO 2 / Al 2 O 3 The molecular sieve of claim 1, wherein the molar ratio is 2-100:1, preferably 5-30:
1.
3. Outer SiO 2 / Al 2 O 3 the molar ratio is between 200 and 1000, preferably between 500 and 1000, and / or Total SiO 2 / Al 2 O 3 The molecular sieve according to claim 1 or 2, wherein the molar ratio is from 30 to 100, preferably from 40 to 70.
4. (1) hydrothermally treating a raw ZSM-5 molecular sieve; (2) removing non-framework aluminum in the molecular sieve obtained in (1); Step (3) of impregnating the material obtained in step (2) with a pore channel protection liquid; a step (4) of treating the material obtained in step (3) with an organic acid; Step (5) of mixing the material obtained in step (4) with an aluminum removal silicon replenishment reagent to perform aluminum removal silicon replenishment; and (6) filtering, washing, drying and roasting the material obtained in step (5).
5. In step (1), The temperature of the hydrothermal treatment is 400 to 700° C., preferably 500 to 600° C. Preferably, The duration of the hydrothermal treatment is between 0.5 and 5 h, preferably between 1 and 2 h; and / or The method according to claim 4, wherein the pressure of the hydrothermal treatment is 0.05-0.5 MPa, preferably 0.1-0.3 MPa.
6. In step (2), removing non-framework aluminum using a buffer solution that is a mixture of a weak acid and / or a weak base and their corresponding salts; Preferably, The weak acid is an inorganic acid and / or an organic acid having a molecular size of less than 0.5 nm and capable of being removed without damaging the structure of the molecular sieve; Preferably, the inorganic acid is one or more of phosphoric acid, carbonic acid, and boric acid; The inorganic acid salt is one or more of an ammonium phosphate salt, an ammonium carbonate salt, and an ammonium borate salt; The organic acid is selected from C2-C6 mono- or polybasic acids, preferably one or more of citric acid, formic acid, acetic acid, oxalic acid, propionic acid, malonic acid, butyric acid, and succinic acid; The organic acid salt is selected from C2 to C6 monobasic or polybasic acid salts, and is preferably one or more of the following ammonium salts: ammonium citrate, ammonium formate, ammonium acetate, ammonium oxalate, ammonium propionate, ammonium malonate, ammonium butyrate, and ammonium succinate; More preferably, the buffer solution is one or more of an oxalic acid-ammonium oxalate solution, and an acetic acid-ammonium acetate solution.
7. the pH value of said buffer solution is in the range of 4.5 to 6.5; and / or The molar concentration of the acid in the buffer solution is 0.1 to 1.0 mol / L; and / or 7. The method of claim 6, wherein the liquid / solid volume ratio of the buffer solution to the molecular sieve obtained in step (1) is 3:1 to 10:
1.
8. The process of step (2) is as follows: The method according to any one of claims 4 to 7, comprising mixing and stirring the molecular sieve obtained in step (1) with a buffer solution, followed by solid-liquid separation, and optionally repeating the above operation 2 to 4 times, preferably, the treatment temperature is 40 to 80°C, and the treatment time is 0.5 to 3h.
9. In step (3), The pore channel protecting agent of the pore channel protecting solution is an inorganic alkali and / or an organic alkali having a molecular size of less than 0.5 nm and removable by roasting without damaging the structure of the molecular sieve; Preferably, the pore channel protecting agent is one or more of ammonia water, ethylenediamine, propylamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetramethylammonium bromide, and tetraethylammonium bromide; Preferably, the pore channel protection liquid is one or more of an isopropylamine solution, a tetraethylammonium hydroxide solution, and a tetrapropylammonium hydroxide solution; and / or The method according to any one of claims 4 to 8, wherein the concentration of the pore channel protection solution is 0.8 to 2.0 mol / L.
10. In step (3), the impregnation is an isovolumetric impregnation, and / or The method according to any one of claims 4 to 9, wherein the impregnation temperature is from 20 to 25°C.
11. In step (4), The organic acid has a molecular size of 0.55 nm to 2 nm and is an organic acid that can be removed by roasting without damaging the structure of the molecular sieve; Preferably, the organic acid is one or more of a C7 to C10 organic acid; More preferably, the organic acid is one or more of 2-methylbenzoic acid, 2-methylbenzenesulfonic acid, 2,4-xylenesulfonic acid, 2,4-dimethylbenzoic acid, 1,2,5-trimethylbenzenesulfonic acid, and 1,2,5-trimethylbenzoic acid; More preferably, the organic acid is one or more of 2,4-xylenesulfonic acid and 2,4-dimethylbenzoic acid.
12. 12. The method according to any one of claims 4 to 11, wherein the process of treating in step (4) comprises firstly mixing the material obtained in step (3) with water, preferably such that the liquid / solid volume ratio between the water and the material obtained in step (3) is between 2:1 and 6:1, and then adding an organic acid until the pH value of the solution is reduced to below 8, preferably between 6.5 and 7.
5.
13. In step (5), The aluminum-removing silicon supplementing material of the aluminum-removing silicon supplementing reagent is one or more of fluorosilicic acid, fluorosilicic acid salts, silicon halides, and silicates, preferably one or more of ammonium hexafluorosilicate, fluorosilicic acid, sodium fluorosilicate, silicon tetrachloride, silicon tetrafluoride, and ethyl orthosilicate; More preferably, the aluminum-removing silicon replenishment reagent is at least one of an ammonium hexafluorosilicate solution and an ethyl orthosilicate solution; and / or The molar concentration of the aluminum-removing silicon-replenishing reagent is 0.3 to 1.0 mol / L; and / or The mass ratio of the material obtained in step (4) to the aluminum-removing silicon-replenishing reagent is 1:1 to 1:5; and / or The method according to any one of claims 4 to 12, wherein the mixing temperature is from 60 to 100°C.
14. The method according to any one of claims 4 to 13, wherein the operation process of step (5) includes: heating the material obtained in step (4) to 60-100°C, continuously stirring, dropping the aluminum removing silicon replenishment reagent, and continuing to stir for 60-120 min after the dropping is completed.
15. Use of the molecular sieve according to any one of claims 1 to 3 as a support and / or catalytically active component, preferably as a hydrogenation catalyst support.
16. A hydrotreating catalyst comprising the ZSM-5 molecular sieve according to any one of claims 1 to 3 and a hydrogenation active component, wherein the hydrogenation active component is preferably one or more selected from group VIB, VIIB and VIII metals, preferably one or more selected from Pt, Pd, Ni, W, Mo and Co.
17. The ZSM-5 molecular sieve according to any one of claims 1 to 3 is contained, Preferably, the catalyst comprises the ZSM-5 molecular sieve and a Group VIII metal component, and the content of the ZSM-5 molecular sieve is 30% to 90% based on the weight of the catalyst, and the content of the Group VIII metal component is 5% to 40% in terms of oxide, Preferably, the hydrodewaxing catalyst comprises the ZSM-5 molecular sieve, alumina, and a Group VIII metal component, the content of the ZSM-5 molecular sieve being 30% to 50%, the content of the alumina being 40% to 70%, and the content of the Group VIII metal component being 5% to 40% in terms of oxide, based on the weight of the catalyst.
18. Use of the hydrodewaxing catalyst according to claim 17 in the hydrodewaxing of oil products, preferably comprising: The oil product is a blend of straight-run diesel and catalytic diesel and / or coked diesel.
Citation Information
Patent Citations
Mesoporous-microporous molecular sieve hydrocracking catalyst
CN104624227A
Zeolite for cleaning exhaust gas and manufacturing thereof
JP1999226391A
Novel zeolite, and catalyst comprising the same for producing aromatic hydrocarbon
JP2021014371A