Process for recovering dialkyl terephthalates from tetramethylcyclobutanediol (TMCD)-containing polymers

The method addresses the inefficiencies of conventional recycling processes by depolymerizing TMCD-containing polyesters with ethylene glycol or methanol and alcoholysis at reduced temperatures, achieving high yields and purity of dialkyl terephthalates while reducing energy and resource use.

JP2024538242APending Publication Date: 2024-10-18EASTMAN CHEM CO
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024524624
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-25
Filing Date
2022-10-25
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Conventional glycolysis and methanolysis processes for recycling TMCD-containing polymers require substantial amounts of resources and energy, leading to inefficiencies and high energy consumption.

Method used

A method involving depolymerization of TMCD-containing polyesters with ethylene glycol or methanol under controlled conditions, followed by alcoholysis at reduced temperatures to recover dialkyl terephthalates, with optional pretreatment to remove foreign substances and subsequent separation of components to enhance efficiency and reduce resource usage.

Benefits of technology

The method achieves high yields and high purity of dialkyl terephthalates with reduced energy and resource consumption by minimizing side reactions and allowing for the reuse of glycols, thereby improving the recycling process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538242000005
    Figure 2024538242000005
  • Figure 2024538242000001
    Figure 2024538242000001
  • Figure 2024538242000002
    Figure 2024538242000002
Patent Text Reader

Abstract

A method for recovering dialkyl terephthalates. The method may include exposing a feedstock composition comprising one or more tetramethylcyclobutanediol (TMCD)-containing polyesters to ethylene glycol, methanol, or both under depolymerization conditions, thereby providing one or more depolymerization products. The one or more depolymerization products may be exposed to an alcoholysis process to recover dialkyl terephthalates.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This disclosure relates to methods for recycling TMCD-containing polymers, and more particularly, to recovering dialkyl terephthalates from feedstocks that include TMCD-containing polyesters. [Background technology]

[0002] Certain conventional systems may utilize glycolysis and / or methanolysis processes in an attempt to recycle polyesters, however, certain conventional glycolysis and / or methanolysis processes may require substantial amounts of resources and energy to arrive at a product suitable for use in a subsequent production process, such as a production process to make recycled polyester or other compositions. Summary of the Invention

[0003] In one aspect, a method for recovering one or more dialkyl terephthalates from a feedstock is provided. The method may include exposing a feedstock composition comprising one or more tetramethylcyclobutanediol (TMCD)-containing polyesters to i) ethylene glycol (EG), methanol, or both; and ii) a depolymerization catalyst in a first reaction vessel under depolymerization conditions to provide a first mixture having a first solid component and a first liquid component. The first liquid component may include one or more depolymerization products. The depolymerization conditions may include a temperature between 150° C. and 260° C., and a pressure between 1 atm (14.7 psig) and 102 atm (1500 psig), and a time period between 0.5 hours and 10 hours. The method may also include cooling at least a portion of the first mixture to a temperature below 150° C. The method may also include exposing at least a portion of the first liquid component to an alcohol composition and an alcoholysis catalyst under conditions including a temperature of 23° C. to 70° C. and a pressure of 1 atm to 2 atm for a period of 0.5 hours to 5 hours to provide a second mixture. The second mixture may include one or more dialkyl terephthalates. The method may also include separating at least a portion of the one or more dialkyl terephthalates by solid-liquid separation. [Brief description of the drawings]

[0004] [Figure 1] 1 is an exemplary system for recovering one or more dialkyl terephthalates from a feedstock composition according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0005] overview The present disclosure may be more readily understood by reference to the following detailed description of certain aspects and examples of the disclosure. In accordance with the purposes of this disclosure, certain aspects of the disclosure are described in the Summary of the Invention and further described herein below. Other aspects of the disclosure are also described herein.

[0006] Embodiments herein relate to methods for recovering one or more dialkyl terephthalates from a feedstock composition comprising a TMCD-containing polyester. As described herein, in certain embodiments, an exemplary method may include exposing a feedstock composition comprising a TMCD-containing polyester to ethylene glycol (EG), methanol, or both under depolymerization conditions to produce one or more depolymerization products which are then exposed to an alcoholysis process to recover the dialkyl terephthalates.

[0007] As discussed above, certain conventional glycolysis and / or methanolysis processes may require substantial amounts of resources and energy to arrive at a product suitable for use in a downstream production process, such as a production process for making recycled polyester or other compositions.

[0008] The methods and systems disclosed herein can alleviate one or more of the above problems. For example, in certain embodiments, the methods disclosed herein can include exposing a feedstock composition comprising a TMCD-containing polyester to depolymerization conditions with one or more glycols and / or methanol to provide one or more depolymerized products. In various embodiments, the one or more depolymerized products can include monomers, oligomers, or combinations thereof. In embodiments, the one or more depolymerized products can be exposed to alcoholysis conditions to obtain high yields and high purity dialkyl terephthalate products. As discussed herein, the alcoholysis conditions include reduced temperatures compared to certain conventional systems, which reduces the overall energy and resources required. In embodiments, as discussed herein, the depolymerization and alcoholysis conditions described herein are substantially milder than certain conventional processes, resulting in less ethylene glycol yield loss, for example, due to fewer side reactions or decomposition reactions that convert ethylene glycol to various impurities. Additionally, in certain embodiments discussed further below, the glycols present in the resulting alcoholysis liquid component can be separated from at least a portion of the alcohol composition utilized in the alcoholysis, and these recycled glycols may be reused in subsequent dialkyl terephthalate recovery chains, again reducing resource consumption.

[0009] Feedstock Composition As discussed above, the methods described herein relate to recovering one or more dialkyl terephthalates from a feedstock composition. In certain embodiments, the feedstock composition may include one or more polyesters. In various embodiments, the feedstock composition may include a 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD)-containing polyester. In certain embodiments, the feedstock composition may include a TMCD-containing polyester, and optionally a polyethylene terephthalate (PET). In one or more embodiments, the feedstock composition may include a TMCD-containing polyester and a polyethylene terephthalate (PET). In various embodiments, the feedstock composition may also include or optionally include additional components, such as contaminants, as discussed herein.

[0010] The term "polyester" may refer to a synthetic polymer prepared by the reaction of one or more difunctional carboxylic acids and / or polyfunctional carboxylic acids with one or more difunctional hydroxyl compounds and / or polyfunctional hydroxyl compounds. The difunctional carboxylic acids may be dicarboxylic acids and the difunctional hydroxyl compounds may be dihydric alcohols such as glycols. Additionally, as used herein, the term "diacid" or "dicarboxylic acid" includes polyfunctional acids such as branching agents. As used herein, the term "glycol" or "diol" includes but is not limited to diols, glycols, and / or polyfunctional hydroxyl compounds. The dicarboxylic acid residue may be derived from a dicarboxylic acid monomer or its associated acid halide, ester, salt, anhydride, or mixtures thereof. Thus, as used herein, the term dicarboxylic acid is intended to include dicarboxylic acids and any derivatives of dicarboxylic acids including their associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides, or mixtures thereof that are useful in the reaction process with diols to create polyesters. As used herein, the term "polyester" should be understood to also refer to copolyesters.

[0011] As used herein, the term "residue" refers to a monomeric or repeating unit in a polymer, oligomer, or dimer. As an illustrative, non-limiting example, a polymer may be made from the condensation of the following monomers: terephthalic acid ("TPA") and cyclohexyl-1,4-dimethanol ("CHDM"). The condensation reaction results in the loss of a water molecule. The residue in the resulting polymer is derived from either terephthalic acid or cyclohexyl-1,4-dimethanol. A non-limiting example of a polyester is shown below in formula (I):

[0012] [ka]

[0013] The polyesters used in the methods disclosed herein may typically be prepared from dicarboxylic acids and diols that react in substantially equal proportions and are incorporated into the polyester polymer as their corresponding residues. Thus, the polyesters of the present invention may contain substantially equal molar proportions of acid residues (100 mol%) and diol (and / or multifunctional hydroxyl compound) residues (100 mol%), such that the total moles of repeat units equal 100 mol%. Thus, the mole percentages provided in this disclosure may be based on the total moles of acid residues, the total moles of diol residues, or the total moles of repeat units. For example, a polyester that contains 10 mol% isophthalic acid based on the total acid residues means that the polyester contains 10 mol% isophthalic acid residues out of a total of 100 mol% acid residues. Thus, there are 10 moles of isophthalic acid residues out of every 100 moles of acid residues. In another example, a polyester that contains 30 mol% TMCD based on the total diol residues means that the polyester contains 30 mol% TMCD residues out of a total of 100 mol% diol residues. Thus, in such an example, there are 30 moles of TMCD residues for every 100 moles of diol residues.

[0014] In embodiments, the one or more polyesters exhibit an intrinsic viscosity of from about 0.1 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, from about 0.2 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, from about 0.3 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, or from about 0.4 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70.

[0015] In certain aspects, terephthalic acid may be used as a starting material. In other embodiments, dimethyl terephthalate may be used as a starting material. In yet other embodiments, a mixture of terephthalic acid and dimethyl terephthalate may be used as a starting material and / or intermediate material. In one or more aspects, the dicarboxylic acid component of the polyester may include one or more modified aromatic dicarboxylic acids, such as, for example, isophthalic acid.

[0016] As discussed above, in embodiments, the feedstock composition may include one or more 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD)-containing polyesters. In certain embodiments, any polyester containing TMCD is contemplated for use in the methods disclosed herein. In certain embodiments, the TMCD-containing polyester may be composed of 1 mol% to 60 mol% TMCD, 1 mol% to 55 mol% TMCD, 1 mol% to 50 mol% TMCD, 1 mol% to 40 mol% TMCD, 1 mol% to 35 mol% TMCD, 1 mol% to 30 mol% TMCD, 1 mol% to 25 mol% TMCD, 1 mol% to 20 mol% TMCD, or 20 mol% to 40 mol% TMCD. In the same or alternative embodiments, the TMCD-containing polyester may contain 1 mol% to 60 mol% TMCD, 1 mol% to 55 mol% TMCD, 1 mol% to 50 mol% TMCD, 1 mol% to 40 mol% TMCD, 1 mol% to 35 mol% TMCD, 1 mol% to 30 mol% TMCD, 1 mol% to 25 mol% TMCD, 1 mol% to 20 mol% TMCD, or 20 mol% to 40 mol% TMCD, with the remainder of the diol component being ethylene glycol (EG), CHDM, or both. In certain embodiments, the TMCD-containing polyester comprises 1 mol% to 60 mol% TMCD, 1 mol% to 55 mol% TMCD, 1 mol% to 50 mol% TMCD, 1 mol% to 40 mol% TMCD, 1 mol% to 35 mol% TMCD, 1 mol% to 30 mol% TMCD, 1 mol% to 25 mol% TMCD, 1 mol% to 20 mol% TMCD, or 20 mol% to 40 mol% TMCD; 0 mol% to 99 mol% EG, It may contain 1 mol% to 99 mol% EG, 0 mol% to 85 mol% EG, 1 mol% to 85 mol% EG, 40 mol% to 90 mol% EG, or 60 mol% to 80 mol% EG; 0 mol% to 99 mol% CHDM, 1 mol% to 99 mol% CHDM, 0 mol% to 85 mol% CHDM, 1 mol% to 85 mol% CHDM, 40 mol% to 90 mol% CHDM, or 60 mol% to 80 mol% CHDM.In one embodiment, the TMCD-containing polyester may comprise 20 mol% to 40 mol% TMCD and 60 mol% to 80 mol% EG. In a particular embodiment, the TMCD-containing polyester may comprise 20 mol% to 40 mol% TMCD and 60 mol% to 80 mol% CHDM. In a particular embodiment, the TMCD-containing polyester may comprise 1 mol% to 60 mol% TMCD, 1 mol% to 55 mol% TMCD, 1 mol% to 50 mol% TMCD, 1 mol% to 40 mol% TMCD, 1 mol% to 35 mol% TMCD, 1 mol% to 30 mol% TMCD, 1 mol% to 25 mol% TMCD, 1 mol% to 20 mol% TMCD, or 20 mol% to 40 mol% TMCD, with the remainder of the diol component being ethylene glycol (EG), CHDM, trimethylolpropane (TMP), monopropylene glycol (MPG), or a combination thereof.

[0017] In various embodiments, the feedstock composition may include or may optionally include polyethylene terephthalate (PET), glycol-modified PET, or both. Examples of glycol-modified PET include 1,4-cyclohexanedimethanol (CHDM)-modified PET, isophthalic acid (IPA)-modified PET, diethylene glycol (DEG)-modified PET, glycol-modified PET, neopentyl glycol (NPG)-modified PET, propanediol (PDO)-modified PET, butanediol (BDO)-modified PET, heaxanediol (HDO)-modified PET, 2-methyl-2,4-pentanediol (MP-diol)-modified PET, isosorbide-modified PET, poly(tetramethylene ether) glycol (PTMG)-modified PET, poly(ethylene) glycol (PEG)-modified PET, polycyclohexylene dimethylene terephthalate (PCT), cyclohexanedimethanol (CHDM)-containing copolyesters, isosorbide-containing copolyesters, or combinations thereof. In the same or alternative embodiments, polyethylene terephthalate (PET) may include CHDM, IPA, DEG, NPG, PDO, BDO, HDO, MP diol, isosorbide, PTMG, PEG, or combinations thereof.

[0018] In various embodiments, PET may include CHDM. In one embodiment, PET may include about 0 mol% to about 100 mol% CHDM, about 1 mol% to about 100 mol% CHDM, about 1 mol% to about 90 mol% CHDM, about 1 mol% to about 80 mol% CHDM, about 1 mol% to about 70% CHDM, about 1 mol% to about 60 mol% CHDM, about 1 mol% to about 50 mol% CHDM, about 1 mol% to about 40 mol% CHDM, about 1 mol% to about 35 mol% CHDM, about 1 mol% to about 30 mol% CHDM, about 1 mol% to about 25 mol% CHDM, about 1 mol% to about 20 mol% CHDM, about 1 mol% to about 10 mol% CHDM, or about 1 mol% to about 5 mol% CHDM. In an embodiment, the mol% of CHDM refers to the mol% of CHDM relative to all diol equivalents in PET. In various embodiments, PET may include DEG. In embodiments, PET may include about 0 mol% to about 100 mol% DEG, about 1 mol% to about 100 mol% DEG, about 1 mol% to about 90 mol% DEG, about 1 mol% to about 80 mol% DEG, about 1 mol% to about 70 mol% DEG, about 1 mol% to about 60 mol% DEG, about 1 mol% to about 50 mol% DEG, about 1 mol% to about 40 mol% DEG, about 1 mol% to about 35 mol% DEG, about 1 mol% to about 30 mol% DEG, about 1 mol% to about 20 mol% DEG, about 1 mol% to about 10 mol% DEG, about 1 mol% to about 5 mol% DEG, or about 1 mol% to about 3 mol% DEG. In embodiments, the mol% of DEG refers to the mol% of DEG relative to all diol equivalents in PET. In an embodiment, the PET may include isophthalic acid. In an embodiment, the PET may include about 0 mol% to about 30 mol% isophthalic acid, about 1 mol% to about 30 mol% isophthalic acid, about 1 mol% to about 25 mol% isophthalic acid, about 1 mol% to about 20 mol% isophthalic acid, about 1 mol% to about 15 mol% isophthalic acid, about 1 mol% to about 10 mol% isophthalic acid, about 1 mol% to about 7.5 mol% isophthalic acid, about 1 mol% to about 5 mol% isophthalic acid, about 1 mol% to about 3 mol% isophthalic acid, about 10 mol% or less isophthalic acid, about 7.5 mol% or less isophthalic acid, about 5 mol% or less isophthalic acid, or about 3 mol% or less isophthalic acid. In an embodiment, the mol% of isophthalic acid refers to the mol% of isophthalic acid relative to the total diacid equivalents in the PET.In certain embodiments, PET may include about 0 mol% to about 100 mol% CHDM, about 0 mol% to about 100 mol% DEG, about 0 mol% to about 30 mol% isophthalic acid, or a combination thereof. In certain embodiments, PET may include about 1 mol% to about 100 mol% CHDM, about 1 mol% to about 100 mol% DEG, about 1 mol% to about 30 mol% isophthalic acid, or a combination thereof. In various embodiments, PET may include other glycols, such as those listed above. For example, in embodiments, PET may include, but is not limited to, neopentyl glycol (NPG), 2-methyl-2,4-pentanediol (MP diol), butanediol (BDO), propanediol (PDO), hexanediol (HDO), isosorbide, poly(tetramethylene ether) glycol (PTMG), poly(ethylene) glycol (PEG), or a combination thereof. In certain embodiments, each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG and PEG may be present in PET in an amount of 0 mol % to about 100 mol %, about 1 mol % to about 100 mol %, about 1 mol % to about 90 mol %, about 1 mol % to about 80 mol %, about 1 mol % to about 70 mol %, about 1 mol % to about 60 mol %, about 1 mol % to about 50 mol %, about 1 mol % to about 40 mol %, about 1 mol % to about 35 mol %, about 1 mol % to about 30 mol %, about 1 mol % to about 25 mol %, about 1 mol % to about 20 mol %, about 1 mol % to about 10 mol %, or about 1 mol % to about 5 mol %. In embodiments, the mole % of each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, and PEG refers to the mole % of each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, and PEG, respectively, relative to the total diol equivalents in PET. In various embodiments, the PET may include CHDM, DEG, NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, PEG, isophthalic acid, or combinations thereof, each component being present in any of the amounts for such components described in this paragraph.

[0019] In various embodiments, when PET is present in the feedstock composition, the weight ratio of PET to TMCD-containing polyester in the feedstock composition can be 10:1 to 1:10, 9:1 to 1:9, 8:1 to 1:8, 7:1 to 1:7, 6:1 to 1:6, 5:1 to 1:5, 4:1 to 1:4, 3:1 to 1:3, or 2:1 to 1:2. In embodiments, when glycol-modified PET is present in the feedstock composition, it can be present in the same relative amounts as described in this paragraph.

[0020] In embodiments, the feedstock composition may include recycled polyester, e.g., recycled TMCD-containing polyester, recycled PET, or both. In various embodiments, the recycled polyester may include materials recovered as manufacturing scrap, post-industrial waste, post-consumer waste, or combinations thereof. In embodiments, the recycled polyester may be a post-consumer product that has been used and / or discarded. In embodiments, the feedstock composition and / or recycled polyester may be obtained from various sources and / or in various forms, including, but not limited to, textiles, carpets, thermoforming materials, bottles, pellets, and films. In one or more embodiments, the feedstock composition may include recycled polyester, e.g., recycled TMCD-containing polyester, recycled PET, or both, formed from DMT recovered from a prior DMT recovery process, such as the processes described herein.

[0021] In various embodiments, the feedstock composition may include one or more foreign materials. In embodiments, the one or more foreign materials may include, but are not limited to, polyesters other than TMCD-containing polyesters and polyethylene terephthalate (PET), polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum and iron, or combinations thereof. In various embodiments, the one or more contaminants may be present in the feedstock composition in an amount of from about 0.01 wt.% to about 50 wt.%, from about 0.01 wt.% to about 40 wt.%, from about 0.01 wt.% to about 30 wt.%, from about 0.01 wt.% to about 20 wt.%, from about 0.01 wt.% to about 15 wt.%, from about 0.01 wt.% to about 10 wt.%, from about 0.01 wt.% to about 7.5 wt.%, from about 0.01 wt.% to about 5 wt.%, from about 0.01 wt.% to about 2.5 wt.%, or from about 0.01 wt.% to about 1.0 wt.%, based on the weight of the one or more TMCD-containing polyesters in the feedstock composition and / or based on the weight of the TMCD-containing polyesters and PET in the feedstock composition.

[0022] In embodiments, the feedstock composition may be in a solid form, liquid form, molten form, or in solution. In certain embodiments, the solution may include the feedstock composition pre-dissolved in a solvent, such as DMT, EG, DEG, TEG, or combinations thereof.

[0023] Optional Pretreatment of the Polyester Composition In certain embodiments, optional pretreatment of the feedstock composition may be performed prior to depolymerization and / or methanolysis. In various embodiments, the optional pretreatment may include any type of treatment that aids in removing a portion of any contaminants from the feedstock composition and / or aids in recovering one or more polyesters from a mixed feedstock, e.g., a feedstock containing the contaminants discussed above. For example, in one embodiment, the optional pretreatment may include exposing the feedstock composition to one or more solvents to selectively dissolve one or more polyesters in the feedstock composition (or at least a portion of the contaminants in the feedstock composition) to allow separation between at least a portion of the contaminants and the TMCD-containing polyester and / or PET in the feedstock composition. In one example embodiment, the optional pretreatment may include exposing the feedstock composition to one or more solvents, e.g., one or more solvents that can cause dissolution of one or more polyesters in the feedstock composition. For example, the one or more solvents may include, but are not limited to, 4-methylcyclohexanemethanol (MCHM), ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), dibutyl terephthalate (DBT), dioctyl terephthalate (DOTP), ethylene carbonate (EC), dimethyl carbonate (DMC), dimethyl sulfoxide (DMSO), dimethylformamide (DMF), or combinations thereof. In the same or alternative embodiment, the feedstock composition may be exposed to one or more solvents at a particular temperature to effect dissolution of one or more components.In various embodiments, the pretreatment process may include one or more dissolution and separation steps using various solvents and / or temperatures to achieve a desired level of contaminant removal and / or purity level of the TMCD-containing polyester and / or PET. For example, in one embodiment, dissolution and separation may be utilized using one solvent at a particular temperature, e.g., to remove one or more contaminants, followed by subsequent dissolution and separation of the polyester fraction using another solvent at a particular temperature, e.g., to remove one or more other contaminants. The dissolution and / or separation in this optional pretreatment step may utilize any suitable system, reactor, vessel, and / or separation technique to achieve the desired pretreated feedstock composition.

[0024] Depolymerization of Feedstock Compositions As discussed above, in various embodiments, the methods disclosed herein may include exposing a feedstock composition to depolymerization conditions to depolymerize at least a portion of one or more polyesters, e.g., TMCD-containing polyesters and / or PET, into one or more depolymerized products. In various embodiments, the one or more depolymerized products may include monomers, oligomers, or combinations thereof. In certain embodiments, the oligomers may exhibit a degree of polymerization of 2-10, 2-8, 2-6, or 2-4. In embodiments, the one or more polyesters may be depolymerized into one or more depolymerized products that may include monomers and oligomers having a degree of polymerization of 2-10, 2-8, 2-6, or 2-4. In embodiments, liquid chromatography may be performed to identify the degree of polymerization of the oligomers, and / or gel permeation chromatography may be utilized to identify the molecular weight of the oligomers.

[0025] In an embodiment, the term degree of polymerization (DP) may refer to the number of residues in an oligomer. As used herein, degree of polymerization (DP) refers to the number of difunctional carboxylic acid residues and / or polyfunctional carboxylic acid residues in an oligomer. For example, in one exemplary embodiment, a DP of 1 refers to a residue that contains one terephthalic acid residue or one isophthalic acid residue. In such an exemplary embodiment, a DP of 1 may also be referred to as a monomer. A non-limiting example of a DP of 1 is provided below in formula (II), where R may be a glycol, such as any of the glycols described herein in the embodiments. For example, for the TMCD-containing polyesters described herein, R may be a TMCD.

[0026] [ka]

[0027] The following formulas (III)-(V) show non-limiting examples of oligomers having DPs of 2, 3, and n, respectively, in embodiments. In formulas (III), (IV), and (V), R can be a glycol, such as any of the glycols described herein in embodiments. For example, in the case of the TMCD-containing polyesters described herein, R can be a TMCD.

[0028] [ka]

[0029] In one or more embodiments, the depolymerization process may be carried out via a glycolysis process. In general, in embodiments, the glycolysis process may include exposing the feedstock composition to one or more glycols, which react with the polyester, optionally in the presence of a transesterification catalyst, to form a mixture of bis(hydroxyethyl) terephthalate (BHET) and low molecular weight terephthalate oligomers. Some representative examples of the glycolysis process are disclosed in U.S. Patent Nos. 3,257,335; 3,907,868; 6,706,843; and 7,462,649, which are incorporated herein by reference. In certain embodiments, the depolymerization process may include exposing the feedstock composition to one or more glycols, methanol, or both under depolymerization conditions.

[0030] In one embodiment of the depolymerization process, one or more polyesters, such as one or more TMCD-containing polyesters, and one or more glycols and / or methanol can be fed to a depolymerization reactor where the TMCD-containing polyesters are dissolved and depolymerized under depolymerization conditions.

[0031] In embodiments, any amount of one or more glycols and methanol suitable for use in the depolymerization process can be utilized. In various embodiments, the weight ratio of one or more glycols, methanol, or both to the TMCD-containing polyester in the feedstock composition can range from 10:1 to 2:1, 9:1 to 2:1, 8:1 to 2:1, 7:1 to 2:1, 6:1 to 2:1, 5:1 to 2:1, or 4:1 to 2:1.

[0032] In certain aspects, the one or more glycols may include any glycol suitable for use in the glycolysis process. In aspects, the term glycol may refer to aliphatic, cycloaliphatic, and aralkyl glycols. Exemplary glycols include ethylene glycol, 1,2-propanediol (also known as propylene glycol), 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,2-dimethyl-1,3-propanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, p-xylylenediol, and the like. These glycols may also include ether linkages, such as in the case of diethylene glycol, triethylene glycol, and tetraethylene glycol. Additional embodiments of glycols include the higher molecular weight homologs known as polyethylene glycols, such as those produced by Dow Chemical Company under the trade name Carbowax™. In one embodiment, the polyethylene glycol has a molecular weight of from greater than 200 to about 10,000 daltons (M n ) These glycols also include higher alkyl analogs such as dipropylene glycol, dibutylene glycol, etc. Similarly, additional glycols have molecular weights of about 200 to about 10,000 Daltons (M n) (also referred to as g / mol) range, and higher polyalkylene ether diols such as polypropylene glycol and polytetramethylene glycol. In one aspect, the glycol can be selected from aliphatic, cycloaliphatic and aralkyl glycols. In the same or alternative aspect, the glycol can be selected from polyalkylene ether diols selected from ethylene glycol; 1,2-propanediol; 1,3-propanediol; 1,4-butanediol; 1,5-pentanediol; 1,6-hexanediol; 2,2-dimethyl-1,3-propanediol; 1,2-cyclohexanedimethanol; 1,3-cyclohexanedimethanol; 1,4-cyclohexanedimethanol; 2,2,4,4-tetramethyl-1,3-cyclobutanediol; isosorbide; p-xylylenediol; diethylene glycol; triethylene glycol; tetraethylene glycol; polyethylene glycol; dipropylene glycol; dibutylene glycol; polypropylene glycol and polytetramethylene glycol.

[0033] In various embodiments, the one or more glycols may include ethylene glycol (EG). In certain embodiments, EG and methanol may be utilized in the depolymerization process. In certain embodiments, as discussed in detail below, the one or more glycols may be recycled glycols recovered from prior glycolysis and methanolysis processes to recover one or more dialkyl terephthalates, as disclosed herein. In the same or alternative embodiments, methanol, if present in the depolymerization process, may be recycled from the glycolysis process, the methanolysis process, or both.

[0034] In various embodiments, as discussed above, the depolymerization process may include one or more catalysts, such as a transesterification catalyst. In certain embodiments, the catalyst may be present in an amount of 0.1 wt.% to 10 wt.% based on the weight of the feedstock composition or based on the weight of the TMCD-containing polyester and / or PET in the feedstock composition. In embodiments, any suitable catalyst may be utilized. In one embodiment, the catalyst may include a carbonate catalyst, such as, but not limited to, Li2CO3, Na2CO3, Cs2CO3, ZrCO3, or combinations thereof. In one embodiment, the catalyst may include a hydroxide catalyst, such as, but not limited to, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), or combinations thereof. In one embodiment, the catalyst may include an alkoxide catalyst, such as, but not limited to, sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide, potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In one embodiment, the catalyst may include tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac)2), zinc acetate (Zn(OAc)2), and manganese(II) acetate (Mn(OAc)2)), or combinations thereof. In certain embodiments, the catalyst may include LiOH, NaOH, KOH, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), ZrCO3, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), sodium methoxide (NaOMe), lithium methoxide (LiOMe), and zinc acetylacetonate hydrate (Zn(acac)2), or combinations thereof. In one embodiment, the catalyst may include LiOH, NaOH, KOH, sodium methoxide (NaOMe), and lithium methoxide (LiOMe).In certain embodiments, the catalyst may include Li2CO3, CaCO3, Na2CO3, Cs2CO3, ZrCO3, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide (Mg(OMe)2, potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac)2), zinc acetate (Zn(OAc)2), manganese(II) acetate (Mn(OAc)2), hydrotalcite, zeolite, lithium chloride, or combinations thereof.

[0035] Depolymerization conditions may include temperatures of 150° C. to 260° C. for 0.5 to 10 hours in an agitated reactor, and absolute pressures of 1 atm (14.7 psig) to 102 atm (1500 psig), 1 atm (14.7 psig) to 50 atm (734 psig), 1 atm (14.7 psig) to 30 atm (440 psig), 1 atmosphere (atm) (14.7 psig) to 15 atm (220 psig), or 1 atm (14.7 psig) to 2 atm (30 psig). Higher temperatures may be used to increase the rate of depolymerization, but a reactor system capable of withstanding high pressures may be required. One or more reactors may be used for the reaction of the polyester with one or more glycols and / or methanol. For example, the reaction mixture may be continuously withdrawn from a first stage and introduced into a second stage maintained under pressure, along with additional glycol and / or methanol, with the depolymerization continuing to the desired degree of completion. In various embodiments, any type of vessel, reactor, and / or reactor system may be utilized for the depolymerization or glycolysis of polyesters. In one embodiment, a continuous stirred tank reactor or vessel, a fixed bed reactor, or a melt extruder. In the same or alternative embodiments, the depolymerization or glycolysis of the feedstock composition may be a batch or continuous process.

[0036] After exposure to the depolymerization conditions detailed above, the resulting mixture can be optionally cooled to a temperature of about 150° C. or less, or from about 50° C. to about 150° C. In embodiments, the resulting mixture can be cooled to a desired temperature in the depolymerization reactor or transferred to a different vessel to reduce the temperature. The resulting mixture can include a solid component and a liquid component. In embodiments, the liquid component can include one or more depolymerization products, e.g., monomers and / or oligomers having a degree of polymerization of 2 to 10, along with one or more glycols and / or methanol, and can further include any additional soluble components from the polyester composition, one or more glycols, catalyst, or combinations thereof. In various embodiments, the solid component can be residual foreign matter and any other insoluble components of the polyester composition and can be considered waste to be disposed of.

[0037] As further discussed below, the liquid component is further subjected to at least a methanolysis process to recover one or more dialkyl terephthalates. In various embodiments, the liquid component can be separated from the solid component prior to the methanolysis process. In embodiments, the liquid component may be separated from the solid component using any system. In one embodiment, the liquid component can be separated from the solid component while the resulting mixture is at a temperature of about 50° C. to about 150° C. In such an embodiment, separating the liquid component from the solid component at a temperature of about 150° C. or less, e.g., about 50° C. to about 150° C., can provide a more efficient and / or less resource intensive process than current conventional processes. In the same or alternative embodiment, separating the liquid component from the solid component at a temperature of about 150° C. or less, e.g., about 50° C. to about 150° C., can be beneficial because some impurities may be unstable at higher temperatures, e.g., temperatures above 150° C., thereby adversely affecting the process described herein, product yield, and / or product purity.

[0038] In various embodiments, the separation of the liquid component from the solid component may include a filtration process. In such embodiments, any suitable filtration process capable of withstanding elevated filtration temperatures of about 50° C. to about 150° C. may be utilized. In certain embodiments, the solid components may be removed by centrifugation. In certain embodiments, the solids may be removed by settling or sedimentation. In certain embodiments, the solid components may settle to the bottom of the vessel, and the liquid components may be removed through vessel conduits or valves appropriately positioned within the vessel. In one embodiment, such conduits and / or valves may include filtration devices to minimize inclusion of the solid components in downstream processes.

[0039] In one or more embodiments, the contaminants and / or one or more solid components resulting from the depolymerization process may not be separated from the depolymerization product prior to methanolysis, but instead may be separated during isolation of the dialkyl terephthalate resulting from the methanolysis process.

[0040] Alcoholysis of one or more of the depolymerization products As discussed above, in embodiments, one or more depolymerized products produced in the depolymerization processes described above may be subjected to an alcoholysis process.

[0041] Generally, in a typical alcoholysis process, a polyester is reacted with an alcohol, such as methanol, to produce a depolymerized mixture that includes oligomers, terephthalate monomers, such as dimethyl terephthalate (DMT), and one or more glycols. In other embodiments, depending on the composition of the polyester, other monomers may also be produced, such as, for example, CHDM, DEG, and dimethyl isophthalate (DMI). In one embodiment, during the alcoholysis process, terephthalate oligomers are reacted with methanol to produce a depolymerized polyester mixture that includes polyester oligomers, DMT, CHDM, and / or EG.

[0042] Some representative examples of the methanolysis of PET are described in U.S. Patent Nos. 3,321,510; 3,776,945; 5,051,528; 5,298,530; 5,414,022; 5,432,203; 5,576,456; and 6,262,294, which are incorporated herein by reference.

[0043] In an embodiment, the alcoholysis process may include exposing the liquid component and / or one or more depolymerized products resulting from the depolymerization process to an alcohol composition under conditions that result in one or more dialkyl terephthalates. As discussed above, in an embodiment, the one or more depolymerized products may be present in the liquid component resulting from the depolymerization process. In various embodiments, as discussed above, the liquid component may be separated from the resulting mixture and / or from the resulting solid component of the glycolysis process before subjecting the one or more depolymerized products and / or liquid component resulting from the depolymerization process to the alcoholysis process. In certain embodiments, after separating the liquid component from the solid component of the depolymerization process, the liquid component may be directly utilized in the alcoholysis process. In the same or alternative embodiments, after separating the liquid component from the solid component of the glycolysis process, the liquid component is not subjected to further processing, such as distillation and / or other separation processes, before being utilized in the alcoholysis process.

[0044] The alcohol composition may comprise any suitable alcohol known in the art for use in an alcoholysis process to obtain a particular dialkyl terephthalate. In one embodiment, the alcohol composition may be methanol. In an embodiment, when methanol is utilized as the alcohol composition, it may be the methanolysis product that results in DMT.

[0045] In certain embodiments, the amount of the alcohol composition may be any amount that is in excess, by weight, relative to the amount or weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition. In certain embodiments, the weight ratio of the amount of the alcohol composition to the amount of the TMCD-containing polyester in the feedstock composition and / or the feedstock composition may be from about 2:1 to about 10:1. In such embodiments, the feedstock composition and / or the amount of the TMCD-containing polyester in the feedstock composition refers to the amount or weight of the TMCD-containing polyester in the feedstock composition and / or the feedstock composition that is utilized in the depolymerization process.

[0046] In embodiments, the alcoholysis reaction may be carried out at a temperature of about 90° C. or less, about 80° C. or less, about 70° C. or less, about 60° C. or less, about 50° C. or less, about 40° C. or less, or about 30° C. or less. In the same or alternative embodiments, the alcoholysis reaction may be carried out at a temperature of about 20° C. to about 90° C., about 20° C. to about 80° C., about 20° C. to about 70° C., about 20° C. to about 60° C., about 20° C. to about 50° C., about 20° C. to about 40° C., about 20° C. to about 30° C., or about 23° C. to about 70° C. In various embodiments, without being bound by any particular theory, it is believed that in the methods disclosed herein, because the TMCD-containing polyester and / or PET in the feedstock composition has already undergone at least a partial depolymerization process, e.g., in the depolymerization step discussed above, the methanolysis process can be carried out at a relatively reduced temperature as compared to certain other conventional processes. Additionally or alternatively, without being bound to any particular theory, it is believed that in certain embodiments the alcoholysis process can be carried out at the reduced temperatures described above, since one or more depolymerization products produced in the depolymerization process can be separated from waste or insoluble materials prior to the alcoholysis process.

[0047] In embodiments, the alcoholysis process may be carried out in any suitable reactor and / or vessel. In embodiments, the alcoholysis reactor may be in fluid communication with the reactor utilized in the depolymerization process described above. In certain embodiments, the alcoholysis reactor is a different reactor than the vessel used for depolymerization. Alternatively, in various embodiments, the alcoholysis process may be carried out in the same vessel as the depolymerization process and / or filtration process described above. In certain embodiments, the alcoholysis process may be carried out at ambient pressure, e.g., about 1 atm, or from about 1 atm to about 5 atm, from about 1 atm to about 3 atm, or from about 1 atm to about 2 atm. In various embodiments, the alcoholysis reaction may be carried out at pressures above ambient pressure, e.g., greater than 1 atm, or less than about 5 atm, less than about 3 atm, or less than about 2 atm, when the alcoholysis reaction temperature is high for the process conditions disclosed herein, e.g., greater than about 50° C., greater than about 60° C., greater than about 70° C., greater than about 80° C., or greater than about 90° C.

[0048] In various embodiments, an alcoholysis catalyst can be utilized in the alcoholysis process. In embodiments, the alcoholysis catalyst can be present in an amount of from about 0.1 wt.% to about 20 wt.% based on the weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition, or from about 0.1 wt.% to about 10 wt.% based on the weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition, or from about 0.1 wt.% to about 5 wt.% based on the weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition, or from about 0.1 wt.% to about 2 wt.% based on the weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition, or from about 0.1 wt.% to about 1 wt.% based on the weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition, or from about 0.1 wt.% to about 0.5 wt.% based on the weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition. In such embodiments, the feedstock composition and / or the amount of TMCD-containing polyester in the feedstock composition refers to the amount or weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition utilized in the depolymerization process. In various embodiments, the amount of alcoholysis catalyst disclosed in this paragraph refers to the amount of alcoholysis catalyst present in the alcoholysis reaction. In various embodiments, the amount of alcoholysis catalyst disclosed in this paragraph refers to the amount of alcoholysis catalyst added to one or more depolymerization products and one or more alcohols to facilitate the alcoholysis reaction.In certain embodiments, a reduced or lesser amount of an alcoholysis catalyst can be added to the one or more depolymerized products and one or more alcohols to facilitate the alcoholysis reaction, for example, in an amount of from about 0.1 wt.% to about 10 wt.% based on the weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition, or from about 0.1 wt.% to about 5 wt.% based on the weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition, or from about 0.1 wt.% to about 2 wt.% based on the weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition, or from about 0.1 wt.% to about 1 wt.% based on the weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition, or from about 0.1 wt.% to about 0.5 wt.% based on the weight of the feedstock composition and / or the TMCD-containing polyester in the feedstock composition. In embodiments, such lesser amounts of alcoholysis catalyst can be added, at least in part, because the alcoholysis catalyst is already present in the one or more depolymerization products and / or one or more alcohols. In such embodiments, as discussed below, the alcohols and / or glycols may be recycled and reused in subsequent depolymerization and alcoholysis processes disclosed herein, which may include at least a portion of the alcoholysis catalyst from a prior alcoholysis and / or glycolysis process.

[0049] In various embodiments, the alcoholysis catalyst may include carbonate catalysts, such as, but not limited to, K2CO3, Na2CO3, Li2CO3, Cs2CO3; hydroxide catalysts, such as, but not limited to, KOH, LiOH, NaOH; alkoxide catalysts, such as, but not limited to, NaOMe, Mg(OMe)2, KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In certain embodiments, the alcoholysis catalyst may include KOH, NaOH, LiOH, or combinations thereof. In certain embodiments, the alcoholysis catalyst may include NaOMe, KOMe, Mg(OMe)2, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In various embodiments, the alcoholysis catalyst may be in solid form, in solution form in water, methanol, or ethylene glycol, or combinations thereof. In certain embodiments, an alcoholysis catalyst may be added to the one or more depolymerization products and the alcohol composition once the alcohol composition and the one or more depolymerization products reach the desired reaction temperature or temperature range disclosed above.

[0050] The one or more depolymerization products may be exposed to the alcohol composition and optionally the alcoholysis catalyst under the above-mentioned temperature and pressure conditions for a time to achieve a desired yield of the resulting dialkyl terephthalate. In certain embodiments, the one or more depolymerization products may be exposed to the alcohol composition and optionally the alcoholysis catalyst under the above-mentioned temperature and pressure conditions for a time of about 0.5 hours to about 5 hours.

[0051] In an embodiment, the alcoholysis process results in a mixture comprising one or more dialkyl terephthalates. In various embodiments, the alcoholysis process results in a mixture in which the dialkyl terephthalates are insoluble and / or solid components. In an embodiment, the liquid component of the mixture may comprise a glycol, an alcohol composition, DEG, CHDM, or a combination thereof. In an embodiment, the glycol may be a glycol utilized in the depolymerization process that was present with the one or more depolymerization products at the start of the alcoholysis process. In various embodiments, the dialkyl terephthalates may be isolated from the mixture using any known separation technique, such as filtration, centrifugation, precipitation, sedimentation, or a combination of one or more separation techniques. In an embodiment, the filtration may include washing the solid component with additional alcohol composition or other solvent. The resulting liquid component may include a filtrate and a wash. The resulting solid component may comprise about 90 wt.% or more of a dialkyl terephthalate, e.g., DMT, about 93 wt.% or more of a dialkyl terephthalate, e.g., DMT, or about 95 wt.% or more of a dialkyl terephthalate, e.g., DMT, based on the weight of the solid component. In the same or alternative embodiments, the dialkyl terephthalate, e.g., DMT, in the resulting solid component may be about 90% or more pure, about 93% or more pure, or about 95% or more pure. In various embodiments, the solid component may also comprise dimethyl isophthalate (DMI). In such embodiments, the DMI may be present in an amount of about 1000 ppm or less, or about 500 ppm or less, or about 1 ppm to about 1000 ppm, or about 1 ppm to about 500 ppm. In one or more embodiments, the solid component may also comprise bisphenol A (BPA). In such embodiments, BPA may be present in an amount of about 1000 ppm or less, or about 500 ppm or less, or from about 1 ppm to about 1000 ppm, or from about 1 ppm to about 500 ppm.

[0052] The processes described herein, e.g., depolymerization and / or alcoholysis processes, are substantially milder than certain conventional processes, e.g., high temperature one-step glycolysis or methanolysis processes. For example, certain conventional one-step processes may utilize a glycolysis process at temperatures of 240° C. or higher in the presence of a Lewis acid catalyst, e.g., Zn(OAc) 2 or KOAc. Such harsh conditions may result in reduced EG yields from depolymerization due to EG being converted in various side reactions to various impurity compounds, including, but not limited to, diethylene glycol (DEG), triethylene glycol (TEG), acetaldehyde, 1,1-dimethoxyethane, 1,2-dimethoxyethane, dioxane, 2-methoxyethanol, 1-methoxyethanol, and dimethyl ether. In an embodiment, the processes described herein are substantially milder than such conventional processes, and further result in less EG yield loss, e.g., due to fewer side reactions that convert EG to various impurities. In one embodiment, the process described herein results in a yield loss of about 5% or less of EG, a yield loss of about 2% or less of EG, or a yield loss of about 1% or less of EG, or a yield loss of about 0.5% or less of EG. In such an embodiment, the yield loss of EG is the percentage of EG formed into impurities, e.g., DEG, relative to the combined amount of EG from the polyester composition feed and EG added in the glycolysis process. In the same or alternative embodiment, the process described herein produces minimal glycol impurities. For example, in one aspect, the processes described herein can result in a net generation of about 5 wt.% or less DEG, about 2 wt.% or less DEG, or about 1 wt.% or less DEG, or about 0.5 wt.% or less DEG, or about 0.01 wt.% to about 5 wt.% DEG, about 0.01 wt.% to about 2 wt.% DEG, or about 0.01 wt.% to about 1 wt.% DEG, or about 0.01 wt.% to about 0.5 wt.% DEG, or about 0.01 wt.% to about 0.2 wt.% DEG when EG is used as one or more glycols in the glycolysis process.In an embodiment, the processes described herein can result in a net generation of about 5 wt.% or less DEG and / or other impurities, about 2 wt.% or less DEG and / or other impurities, or about 1 wt.% or less DEG and / or other impurities, or about 0.5 wt.% or less DEG and / or other impurities, or about 0.01 wt.% to about 5 wt.% DEG and / or other impurities, about 0.01 wt.% to about 2 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 1 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.5 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.2 wt.% DEG and / or other impurities when EG is used as one or more glycols in the glycolysis process. In an embodiment, the net generation of DEG (or other impurities) is the weight percent of the amount of DEG or other impurities present relative to the amount of DEG or other impurities present in the polyester composition feed. In an embodiment, the DEG produced may be produced in a glycolysis process described herein and / or an alcoholysis process described herein. In certain embodiments, when EG is used as one or more glycols in the glycolysis process, EG such as DEG and / or any glycol impurities may be present in the liquid component resulting from the alcoholysis step. In certain embodiments, the utilization of a Lewis base catalyst, e.g., a hydroxide-based or carbonate-based catalyst, in the glycolysis process may also facilitate or contribute to the reduction of EG decomposition and / or the reduction of glycol impurities. In certain embodiments, the processes described herein additionally or alternatively result in a reduction in TMCD yield loss. For example, in various embodiments, the processes described herein result in a yield loss of about 30% or less of TMCD, a yield loss of about 25% or less of TMCD, a yield loss of about 20% or less of TMCD, a yield loss of about 15% or less of TMCD, a yield loss of about 10% or less of TMCD, or a yield loss of about 5% or less of TMCD. In the same or alternative embodiments, the processes described herein additionally or alternatively result in reduced yield loss of CHDM.For example, in various embodiments, the processes described herein result in a yield loss of about 15% or less of CHDM, a yield loss of about 10% or less of CHDM, a yield loss of about 5% or less of CHDM, or a yield loss of about 1% or less of CHDM.

[0053] Glycol Recycling As discussed above, in various embodiments, the glycol utilized in the glycolysis process can be reused in a subsequent process sequence to recover one or more dialkyl terephthalates disclosed herein. In embodiments, at a high level, the liquid components resulting from the alcoholysis process can be processed for reuse, for example, in a subsequent glycolysis sequence of a subsequent polyester composition to recover one or more dialkyl terephthalates.

[0054] In embodiments, as discussed above, the liquid component resulting from the alcoholysis process may include glycols, alcohol compositions, DEG, CHDM, TMCD, or combinations thereof. In certain embodiments, the glycols in the liquid component may be glycols utilized in the depolymerization process and present with one or more depolymerization products at the start of the alcoholysis process. In various embodiments, the liquid component may be subjected to a separation process, for example, to remove or separate at least a portion of the alcohol composition, for example, methanol, or a mixture of methanol and ethylene glycol. In certain embodiments, the liquid component may be exposed to distillation or short path distillation to remove at least a portion of the alcohol composition. In such embodiments, the distillation conditions may include exposing the liquid component to a temperature of about 220° C. or less, about 200° C. or less, about 180° C. or less, about 160° C. or less, about 150° C. or less, about 130° C. or less, about 60° C. or more, about 70° C. or more, about 60° C. to about 220° C., about 70° C. to about 220° C., about 60° C. to about 180° C., or about 60° C. to about 160° C. In the same or alternative embodiments, the distillation conditions may include a pressure of about 1 Torr (133.3 Pa) to about 800 Torr (106,657 Pa), or about 30 Torr (3999 Pa) to about 500 Torr (66,661 Pa). In embodiments, the liquid component may be exposed to the distillation conditions until all or a substantial portion of the alcoholic composition is removed from the liquid component, e.g., vaporized. In certain embodiments, at least a portion of the alcohol composition, if present with the recycle glycol, may be removed during the subsequent glycolysis process, e.g., removed or vaporized by the glycolysis conditions.

[0055] In embodiments, distillation of the liquid components may be carried out in any vessel or distillation system suitable for use in the methods and systems described herein. In one embodiment, the distillation vessel can be in fluid communication with the alcoholysis reaction vessel and / or any component of the filtration process utilized subsequent to alcoholysis, for example, to isolate the dialkyl terephthalate solid or insoluble components. In the same or alternative embodiments, the distillation vessel can be in fluid communication with the glycolysis vessel.

[0056] In various embodiments, distillation of the liquid component can vaporize the alcohol composition and leave a pot residue. In embodiments, the pot residue includes glycol and any other heavies, such as non-vaporizable compounds, present in the liquid component. In embodiments, the glycol in the pot residue may be referred to as recycled glycol and / or the glycol from the non-vaporizable portion of the continuous distillation process using the distillation conditions described herein may be referred to as recycled glycol.

[0057] In an embodiment, as discussed above, the recycled glycol may be utilized in a subsequent process sequence described herein to recover one or more dialkyl terephthalates from the polyester composition. Furthermore, in an embodiment, the recycled glycol may be recycled again using the process described herein after this subsequent dialkyl terephthalate recovery sequence. In an embodiment, the recycled glycol may be recovered and reused at least two times, at least three times, at least four times, or at least five times. In certain embodiments, when the recycled glycol is used in a subsequent dialkyl terephthalate recovery sequence, the addition of a catalyst in the subsequent glycolysis step may be omitted since the recycled glycol may contain a used catalyst.

[0058] In embodiments, when recycled glycol is recovered and reused, the resulting recovered dialkyl terephthalate exhibits a purity comparable to that of dialkyl terephthalate recovered using glycol that was not recovered and reused. In embodiments, this comparable purity of dialkyl terephthalate exists after reusing recycled glycol at least two, at least three, at least four, or at least five times, resulting in a recovered dialkyl terephthalate having a purity of at least about 90%, at least about 93%, or at least about 95%.

[0059] As discussed above, in embodiments, the processes described herein are substantially milder than certain conventional processes and result in less EG yield loss, for example, due to fewer side reactions that convert EG to various impurities. In one example with three EG recycle runs, the yield loss of EG to DEG is about 5% or less, about 2% or less, about 1% or less, or about 0.5% or less. In one example with four EG recycle runs, the yield loss of EG to DEG is about 5% or less, about 2% or less, about 1% or less, or about 0.5% or less. In the same or alternative embodiments, the processes described herein produce minimal glycol impurities. In certain embodiments, when EG is used as one or more glycols in the glycolysis process, any glycol impurities, such as EG and / or DEG, may be present in the liquid component resulting from the alcoholysis process discussed above. In such embodiments, DEG or any glycol impurities may be recovered and / or may be present in the recycled glycol described herein. In such embodiments, the recycled glycol may contain about 5 wt.% or less DEG and / or other impurities, about 2 wt.% or less DEG and / or other impurities, or about 1 wt.% or less DEG and / or other impurities, or about 0.5 wt.% or less DEG and / or other impurities, or about 0.01 wt.% to about 5 wt.% DEG and / or other impurities, about 0.01 wt.% to about 2 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 1 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.5 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.2 wt.% DEG and / or other impurities when EG is used as one or more glycols in the glycolysis process.

[0060] Use of Recovered Dialkyl Terephthalates to Form Polyesters or Other Products As discussed above, the methods disclosed herein can result in high purity dialkyl terephthalates such as DMT. In certain embodiments, the recovered DMT may be utilized to form one or more polyesters, including but not limited to PET and TMCD-containing polyesters. In certain embodiments, the polyesters formed using the recovered DMT may be referred to as recycled polyesters. In various embodiments, the products formed using the recovered DMT may be indistinguishable from similar products formed from virgin DMT. In such embodiments, any suitable process for forming PET and TMCD-containing polyesters may be utilized, as the DMT is of sufficient purity.

[0061] In the same or alternative embodiments, the recovered DMT may be utilized to form CHDM. In various embodiments, the CHDM formed using the recovered DMT may be indistinguishable from CHDM formed from virgin DMT due to the high purity of the recovered DMT. In such embodiments, the CHDM may be formed from the recovered DMT using any suitable process.

[0062] In various embodiments, the recovered DMT may be utilized to form one or more plasticizers. In certain embodiments, the plasticizers formed using the recovered DMT may include dibutyl terephthalate (DBT) and / or dioctyl terephthalate (DOTP). In various embodiments, the DBT and / or DOTP formed using the recovered DMT may be indistinguishable from the DBT and / or DOTP, respectively, formed from virgin DMT due to the high purity of the recovered DMT. In such embodiments, the DBT and / or DOTP may be formed from the recovered DMT using any suitable process.

[0063] Exemplary System FIG. 1 illustrates generally one exemplary system and / or method for recovering one or more dialkyl terephthalates from a feedstock composition. As discussed above, the feedstock composition comprises one or more TMCD-containing polyesters. System 100 includes a source 110 of a feedstock composition, such as the feedstock composition described above. Optionally, as discussed above, the feedstock composition may be subjected to a pretreatment step to remove at least a portion of the contaminants before entering the depolymerization and alcoholysis process. Vessel 120 represents a depolymerization vessel, in which the feedstock composition is received and exposed to one or more glycols and / or methanol under depolymerization conditions, as discussed in detail above. In embodiments, vessel 120 can be in fluid communication with source 110. In various embodiments, as discussed above, the feedstock composition is converted to one or more depolymerization products after being exposed to depolymerization conditions in vessel 120. In various embodiments, as discussed above, the one or more depolymerization products may include monomers and / or oligomers having a degree of polymerization of 2-10, 2-8, 2-6, or 2-4. In embodiments, the one or more depolymerization products are present in a mixture including a liquid component and a solid component, with the one or more depolymerization products in the liquid component. In embodiments, as discussed above, the mixture may be exposed to a solid-liquid separation device 130, such as a filtration system, where the liquid component including the one or more depolymerization products is separated from the solid component. In various embodiments, the solid-liquid separation device 130 may be in fluid communication with vessel 120 and / or vessel 140, as discussed herein. In the embodiment shown in FIG. 1, the one or more depolymerization products and / or liquid components may be exposed to alcoholysis conditions in vessel 140. In embodiments, the one or more depolymerization products and / or liquid components may be directly utilized in the alcoholysis process. In such embodiments, the one or more depolymerization products and / or liquid components may not be subjected to any further processing, such as distillation and / or other separation processes, before being utilized in the alcoholysis process. Alcohololysis conditions are discussed in detail above.In embodiments, as discussed above, alcoholysis of one or more depolymerization products and / or liquid components may result in a mixture including an insoluble or solid component including dialkyl terephthalate, and a liquid component including alcohol composition, glycol, methanol, and / or potentially other soluble components as described herein. As discussed above, the resulting alcoholysis reaction mixture may be exposed to a solid-liquid separation device 150, e.g., a filtration system, to separate the solid component including recovered dialkyl terephthalate 160. In embodiments, solid-liquid separation device 150 may be in fluid communication with vessel 140. In certain embodiments, the methods described herein related to system 100 may be carried out as continuous, batch, or semi-continuous methods. It is understood that system 100 is merely an example system and other configurations of system components are contemplated by the disclosure herein. For example, one or more components of system 100 may not be physically separated or distinct from one or more other components of system 100. It is further understood that system 100 is depicted merely diagrammatically to highlight aspects of the methods disclosed herein.

[0064] The present disclosure can be further illustrated by the following examples of its aspects, although it will be understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the disclosure unless specifically indicated otherwise. EXAMPLES

[0065] material The TMCD-containing polymers used in these examples are commercially available Tritan™ TX1000 copolyester (TX1000), and copolyester GMX200 (GMX200), both available from Eastman Chemical, Kingsport, Tennessee.

[0066] FDST-5 contains 100 mol % TPA, 93.0 mol % EG, 4.1 mol % CHDM, and 2.9 mol % DEG and is available from Eastman. IV: 0.751 dL / g.

[0067] All other chemicals and reagents were obtained from Aldrich and used as received unless otherwise stated.

[0068] Analytical procedures Gas Chromatography (GC) Analysis. GC analysis was performed on an Agilent Model 7890B Gas Chromatograph equipped with a 7693A autosampler and two G4513A towers. The GC was equipped with two columns, a 60m x 0.32mm x 1.0 micron DB-1701™ (J&W123-0763) and a 60m x 0.32 x 1 micron DB-1™ (J&W123-1063), and samples were injected simultaneously onto both columns. A common oven temperature program was used and sample components were detected by flame ionization detection (FID). A five-point calibration was performed for components of interest. The gas chromatograph was interfaced to an EZChrom Elite Chromatography Data System.

[0069] Methanolysis product samples were prepared by adding a known volume of pyridine-based internal standard solution to a known mass of sample, followed by derivatization with N,O-bis(trimethylsilyl)trifluoroacetamide (BSTFA).

[0070] The % DMT yield was calculated as follows: (weight of final DMT) / (weight of theoretical DMT). * 100%. DMT GC purity % was calculated as follows: (wt.% DMT in final product by GC) / (total wt.% by GC). * 100%. Major impurities as shown by GC include MeOH, water, and EG. DMT purity in almost all examples is greater than 99% excluding MeOH, water, and EG.

[0071] Examples 1A-1G: Changes in depolymerization catalyst and EG / methanol in the two-step process of TX1000 The TX1000 was subjected to a two-step process for the recovery of DMT, which includes an initial depolymerization step followed by a low-temperature methanolysis step. In particular, in Examples 1A-1C and 1E-1G, different catalysts and varying amounts of EG / methanol were tested in the initial depolymerization step and then exposed to low-temperature methanolysis. In Example 1D, a catalyst was tested in the initial depolymerization step. The results are summarized in Table 1 below.

[0072] Example 1A A three-necked, 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. TX1000 (70.04 g), butyltin tris(2-ethylhexanoate) (2.1858 g), and ethylene glycol (141.41 g) were charged to the flask. The resulting mixture was heated to 195° C. under a nitrogen atmosphere. The reaction was held at 195° C. for 3 hours until no pellets remained. The resulting mixture was a hazy white solution and a sample was taken (1.54 g). The heating mantle was removed and the solution was cooled to ambient temperature. Methanol (197.00 g) was charged to the mixture. The resulting mixture was heated to reflux (72.6° C.) before adding 50% NaOH solution (0.204 mL) dropwise. Stirring was continued for 30 minutes. The heating mantle was removed and the flask was cooled to room temperature over 2 hours. The reaction mixture was further cooled in an ice bath. The product was collected by filtration and dried. The product was obtained as a white crystalline solid (5.03 g). GC analysis showed the product to be mainly bis(hydroxyethyl) terephthalate (BHET).

[0073] Example 1B A three-necked, 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. TX1000 (70.10 g), NaOMe (25% in methanol, 2.80 g), Zn(OAc)2 (0.47 g), and ethylene glycol (139.33 g) were charged to the flask. The resulting mixture was heated to 195° C. under a nitrogen atmosphere. The reaction was held at 195° C. for 3 hours until no pellets remained. The resulting mixture was a hazy white solution. The heating mantle was removed and the solution was cooled to ambient temperature. Methanol (196.39 g) was charged to the mixture. The resulting mixture was heated to 50° C., after which 50% NaOH solution (0.306 g) was added dropwise. Stirring was continued for 30 minutes. The heating mantle was removed and the flask was cooled to room temperature over 2 hours. The reaction mixture was further cooled in an ice bath. The product was collected by filtration and dried. The DMT product was obtained as a white crystalline solid (43.61 g, 87% yield, GC purity 96%).

[0074] Example 1C A three-necked, 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. TX1000 (69.43 g), 25% NaOMe in methanol (2.69 g), and ethylene glycol (138.91 g) were charged to the flask. The resulting mixture was heated to 195° C. under nitrogen and held at 195° C. until no pellets remained. The resulting mixture was a hazy white mixture. The heating mantle was removed and the solution was cooled to ambient temperature. To this mixture was charged methanol (196.90 g). The resulting mixture was heated to 50° C., after which 50% NaOH solution (0.306 g) was added dropwise. Stirring was continued for 30 minutes. The heating mantle was removed and the flask was cooled to room temperature for 2 hours. The reaction mixture was further cooled in an ice bath. The product was collected by filtration and dried. The DMT product was obtained as a white crystalline solid (40.35 g, 83% yield, GC purity 97%).

[0075] Example 1D A three-necked, 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. TX1000 (37.49 g), FDST-5 (37.5 g), K2CO3 (0.75 g), and ethylene glycol (152.16 g) were charged to the flask. The resulting mixture was heated to 195°C under a nitrogen atmosphere. The reaction was held at 195°C for 3 hours. The resulting mixture was a hazy white solution with a few pellets remaining. The heating mantle was removed and the mixture was allowed to cool. The insoluble solids (22.82 g) were collected by filtration. Analysis showed that the insoluble solids contained 70.5% Tritan and 29.5% PET. The filtrate (183.65 g) was obtained, which contained 59.0% EG and 20.9% BHET.

[0076] Example 1E A 100 mL autoclave was equipped with a mechanical stirrer and thermocouple. Ground TX1000 (10.01 g), ethylene glycol (16.15 g), methanol (4.0 g), and potassium carbonate (0.07 g). The resulting mixture was heated to 195°C and held under 700 psig N2 pressure for 3 hours. The crude mixture was cooled to room temperature, after which methanol (36.3 g) and 50% aqueous sodium hydroxide (0.044 g) were added. The mixture was further heated to 50°C and held under 50 psig nitrogen pressure for 30 minutes. Heating was stopped and the mixture was allowed to cool slowly to room temperature over 2 hours. The product was isolated by filtration and dried. The DMT product was obtained as a white solid (6.51 g, 81% yield, 99% purity).

[0077] Example 1F A 100 mL autoclave was equipped with a mechanical stirrer and thermocouple. Ground TX1000 (10.01 g), ethylene glycol (4.03 g), methanol (16.0 g), and potassium carbonate (0.07 g). The resulting mixture was heated to 195°C and held under 700 psig N2 pressure for 3 hours. The crude mixture was cooled to room temperature, after which methanol (24.09 g) and 50% aqueous sodium hydroxide (0.044 g) were added. The mixture was further heated to 50°C and held under 50 psig nitrogen pressure for 30 minutes. Heating was stopped and the mixture was allowed to cool slowly to room temperature over 2 hours. The product was isolated by filtration and dried. The DMT product was obtained as a white solid (4.69 g, 66% yield, 99% purity).

[0078] Example 1G A 100 mL autoclave was equipped with a mechanical stirrer and thermocouple. Ground TX1000 (10.02 g), methanol (39.98 g), and potassium carbonate (0.07 g). The resulting mixture was heated to 195° C. and held under 700 psig N2 pressure for 3 hours. The crude mixture was cooled to room temperature, after which 50% aqueous sodium hydroxide (0.044 g) was added. The mixture was further heated to 50° C. and held under 50 psig nitrogen pressure for 30 minutes. Heating was stopped and the mixture was allowed to cool slowly to room temperature over 2 hours. The product was isolated by filtration and dried. The DMT product was obtained as a white solid (5.89 g, 83% yield, 99% purity).

[0079] [Table 1]

[0080] As can be seen in Table 1, in Example 1D, the K2CO3 catalyst was shown to be inefficient for depolymerizing the TMCD-containing polymer, with 30% solids recovered. Similarly, the FASCAT 4102 tin catalyst had low catalytic activity for the initial depolymerization of TX1000 (Example 1A). Changing to NaOMe or NaOMe / Zn(OAc)2 catalysts allowed the depolymerization of TX1000 in a two-step process to the DMT product in 82-87% yield (Examples 1B and 1C).

[0081] Example 1H: Two-step depolymerization and low-temperature methanolysis of GMX200 A three-necked, 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. GMX200 (75.11 g), K2CO3 (0.75 g), and ethylene glycol (150.29 g) were charged to the flask. The resulting mixture was heated to 195°C under a nitrogen atmosphere. The reaction was held at 195°C for 3 hours until no pellets remained. An aliquot was taken and tested. GC analysis showed that the glycolysis product contained 23.7% BHET and 9.6% unknowns.

[0082] The crude product was cooled to ambient temperature. To this mixture was charged methanol (299.93 g). The resulting mixture was heated to 50° C. and then 50% NaOH solution (0.468 g) was added dropwise. Stirring was continued for 30 minutes. The heating mantle was removed and the flask was allowed to cool to room temperature over 2 hours. The reaction mixture was further cooled in an ice bath. The product was collected by filtration and dried. The DMT product was obtained as a white crystalline solid (49.12 g, 74.4% yield, 96% GC purity).

[0083] The present disclosure may also be described according to the following numbered sections: Item 1. A method for recovering one or more dialkyl terephthalates from a feedstock, comprising exposing a feedstock composition comprising one or more tetramethylcyclobutanediol (TMCD)-containing polyesters to i) ethylene glycol (EG), methanol, or both; and ii) a depolymerization catalyst in a first reaction vessel under depolymerization conditions to provide a first mixture having a first solid component and a first liquid component, wherein the first liquid component comprises one or more depolymerization products, and the depolymerization conditions include a temperature of 150° C. to 260° C. and a pressure of 1 atm (14.7 psig) to 102 atm ( cooling at least a portion of the first mixture to a temperature below 150°C; exposing at least a portion of the first liquid component to an alcohol composition and an alcoholysis catalyst under conditions comprising a temperature of 23°C to 70°C and a pressure of 1 atm to 2 atm for a period of 0.5 hours to 5 hours to provide a second mixture, wherein the second mixture comprises one or more dialkyl terephthalates; and isolating at least a portion of the one or more dialkyl terephthalates by solid-liquid separation.

[0084] Item 2. The method according to item 1, wherein in the step of exposing a feedstock composition comprising one or more tetramethylcyclobutanediol (TMCD)-containing polyesters to i) ethylene glycol (EG), methanol, or both; and ii) a depolymerization catalyst, the weight ratio of EG, methanol, or both to the one or more tetramethylcyclobutanediol (TMCD)-containing polyesters is in the range of 4:1 to 2:1.

[0085] Item 3. The method according to items 1 to 2, wherein in the step of exposing a feedstock composition comprising one or more tetramethylcyclobutanediol (TMCD)-containing polyesters to i) ethylene glycol (EG), methanol, or both; and ii) a depolymerization catalyst, the weight ratio of EG to methanol is in the range of 10:0 to 0:10.

[0086] Item 4. The method according to any one of Items 1 to 3, wherein the weight ratio of the alcohol composition to the one or more tetramethylcyclobutanediol (TMCD)-containing polyesters is in the range of 2:1 to 10:1. Item 5. The method according to any one of Items 1 to 4, wherein the feedstock composition contains one or more foreign matter.

[0087] Item 6. The method of item 5, wherein the one or more foreign bodies include at least one member selected from the group consisting of polyesters other than TMCD-containing polyesters and polyethylene terephthalate (PET), polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates and polyamides, poly(lactic acid), polydimethylsiloxane, polysilane, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, plasticizers, adhesives, flame retardants, metals, aluminum, and iron.

[0088] Item 7. The method of items 5-6, wherein the one or more contaminants are present in an amount of 0.01 wt.% to 50 wt.%, based on the weight of the one or more TMCD-containing polyesters in the feedstock composition.

[0089] Item 8. The method of any one of items 1 to 7, wherein the depolymerization catalyst comprises a member selected from the group consisting of Li2CO3, CaCO3, Na2CO3, Cs2CO3, ZrCO3, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide (Mg(OMe)2, potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac)2), zinc acetate (Zn(OAc)2), manganese(II) acetate (Mn(OAc)2), hydrotalcite, zeolite, and lithium chloride.

[0090] Item 9. The method of item 8, wherein the depolymerization catalyst is NaOMe, Zn(OAc)2, or both. Item 10. The method according to any one of items 1 to 9, wherein the depolymerization catalyst is present in an amount of 0.1 wt.% to 10 wt.% based on the weight of the feedstock composition.

[0091] Item 11. The method according to any one of items 1 to 10, wherein the alcoholysis catalyst is present in an amount of 0.1 wt.% to 20 wt.% based on the weight of the feedstock composition. Item 12. The method of item 11, wherein the alcoholysis catalyst comprises K2CO3, Na2CO3, Li2CO3, Cs2CO3; KOH, LiOH, NaOH; NaOMe, Mg(OMe)2, KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or a combination thereof.

[0092] Item 13. The method of any one of items 1 to 12, wherein the one or more depolymerization products include monomers, oligomers, or combinations thereof. Item 14. The method according to item 13, wherein the oligomer has a degree of polymerization of 2 to 10.

[0093] Item 15. The method according to any one of items 1 to 14, further comprising a step of separating at least a portion of the first liquid component from the first solid component in the first mixture before exposing at least a portion of the first liquid component to the alcohol composition.

[0094] Item 16. The method according to Item 15, wherein the separation is carried out at a temperature of 50°C to 150°C. Item 17. The method according to any one of Items 5 to 7, wherein at least a portion of the foreign matter is present in the first solid component of the first mixture.

[0095] Item 18. The method according to any one of Items 1 to 17, wherein the second mixture comprises a second liquid component and a second solid component, and the one or more dialkyl terephthalates are present in the second solid component during separation of at least a portion of the one or more dialkyl terephthalates by solid-liquid separation.

[0096] Item 19. The method of item 18, wherein the second liquid component comprises methanol, EG, TMCD, or a combination thereof. Item 20. The method according to items 18 to 19, further comprising separating at least a portion of EG, methanol, TMCD, or a combination thereof from the second mixture.

[0097] Item 21. The method according to items 1 to 20, wherein the feedstock further comprises polyethylene terephthalate (PET). Item 22. The method according to item 21, wherein the weight ratio of PET to TMCD-containing polyester in the feedstock composition is 10:1 to 1:10.

[0098] Item 23. The method according to items 1 to 22, wherein the alcohol composition contains methanol. Item 24. The method according to any one of items 1 to 23, wherein the one or more dialkyl terephthalates include dimethyl terephthalate (DMT), and the step of separating at least a portion of the one or more dialkyl terephthalates by solid-liquid separation comprises separating at least a portion of DMT.

[0099] Item 25. The method according to item 24, wherein at least a portion of the DMT is at least 90% pure. Item 26. The method according to items 15 to 16, wherein the separation comprises filtration, centrifugation, sedimentation, sedimentation, or a combination thereof.

[0100] Item 27. The method of items 1 to 26, carried out as a batch process, a semi-continuous process, or a continuous process. The present disclosure has been described in detail with particular reference to certain embodiments thereof, but it will be understood that variations and modifications can be made within the spirit and scope of the disclosure.

Claims

1. 1. A method for recovering one or more dialkyl terephthalates from a feedstock, comprising exposing a feedstock composition comprising one or more tetramethylcyclobutanediol (TMCD)-containing polyesters to i) ethylene glycol (EG), methanol, or both; and ii) a depolymerization catalyst in a first reaction vessel under depolymerization conditions to provide a first mixture having a first solid component and a first liquid component, wherein the first liquid component comprises one or more depolymerization products, and the depolymerization conditions include a temperature of from 150° C. to 260° C. and a pressure of from 1 atm (14.7 psig) to 102 atm (1 cooling at least a portion of the first mixture to a temperature below 150° C.; exposing at least a portion of the first liquid component to an alcohol composition and an alcoholysis catalyst under conditions comprising a temperature of 23° C. to 70° C. and a pressure of 1 atm to 2 atm for a period of 0.5 to 5 hours to provide a second mixture, the second mixture comprising one or more dialkyl terephthalates; and isolating at least a portion of the one or more dialkyl terephthalates by solid-liquid separation.

2. 2. The method of claim 1, wherein in the step of exposing a feedstock composition comprising one or more tetramethylcyclobutanediol (TMCD)-containing polyesters to i) ethylene glycol (EG), methanol, or both; and ii) a depolymerization catalyst, the weight ratio of EG, methanol, or both to the one or more tetramethylcyclobutanediol (TMCD)-containing polyesters ranges from 4:1 to 2:

1.

3. 2. The method of claim 1, wherein in the step of exposing a feedstock composition comprising one or more tetramethylcyclobutanediol (TMCD)-containing polyesters to i) ethylene glycol (EG), methanol, or both; and ii) a depolymerization catalyst, the weight ratio of EG to methanol ranges from 10:0 to 0:

10.

4. 10. The method of claim 1, wherein the weight ratio of the alcohol composition to the one or more tetramethylcyclobutanediol (TMCD)-containing polyesters ranges from 2:1 to 10:

1.

5. 10. The method of claim 1, wherein the feedstock composition comprises one or more contaminants, the one or more contaminants comprising at least one member selected from the group consisting of polyesters other than TMCD-containing polyesters and polyethylene terephthalate (PET), polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates and polyamides, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, plasticizers, adhesives, flame retardants, metals, aluminum and iron.

6. 6. The method of claim 5, wherein the one or more contaminants are present in an amount of from 0.01 wt. % to 50 wt. %, based on the weight of the one or more TMCD-containing polyesters in the feedstock composition.

7. The depolymerization catalyst is Li 2 CO 3 , CaCO 3 , Na 2 CO 3 , Cs 2 CO 3 , ZrCO 3 , LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide (Mg(OMe) 2 , potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac) 2 ), zinc acetate (Zn(OAc) 2 ), Manganese(II) acetate (Mn(OAc) 2 ), a member selected from the group consisting of hydrotalcite, zeolite and lithium chloride.

8. 10. The method of claim 1, wherein the depolymerization catalyst is present in an amount of 0.1 wt. % to 10 wt. %, based on the weight of the feedstock composition.

9. The depolymerization catalyst is NaOMe, Zn(OAc) 2 or both.

10. The alcoholysis catalyst is present in an amount of 0.1 wt. % to 20 wt. % based on the weight of the feedstock composition, and the alcoholysis catalyst is 2 CO 3 , Na 2 CO 3 , Li 2 CO 3 , Cs 2 CO 3 ;KOH, LiOH, NaOH; NaOMe, Mg(OMe) 2 , KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof.

11. 2. The method of claim 1, wherein the one or more depolymerization products comprise monomers, oligomers, or combinations thereof, and the oligomers exhibit a degree of polymerization of 2 to 10.

12. 10. The method of claim 1, further comprising the step of separating at least a portion of the first liquid component from a first solid component in the first mixture prior to exposing the at least a portion of the first liquid component to the alcoholic composition, wherein the separation is performed at a temperature between 50°C and 150°C.

13. The method of claim 5 , wherein at least a portion of the foreign matter is present in the first solid component of the first mixture.

14. 2. The method of claim 1, wherein the second mixture comprises a second liquid component and a second solid component, and during separation of at least a portion of the one or more dialkyl terephthalates by solid-liquid separation, the one or more dialkyl terephthalates are present in the second solid component.

15. 15. The method of claim 14, wherein the second liquid component comprises methanol, EG, TMCD, or a combination thereof.

16. 16. The method of claim 15, further comprising separating at least a portion of the EG, methanol, TMCD, or combinations thereof from the second mixture.

17. The method of claim 1 , wherein the feedstock further comprises polyethylene terephthalate (PET).

18. The method of claim 17, wherein the weight ratio of PET to TMCD-containing polyester in the feedstock composition is from 10:1 to 1:

10.

19. The method of claim 1 , wherein the alcohol composition comprises methanol.

20. 2. The method of claim 1, wherein the one or more dialkyl terephthalates comprise dimethyl terephthalate (DMT), and the step of separating at least a portion of the one or more dialkyl terephthalates by solid-liquid separation comprises separating at least a portion of the DMT, wherein the at least a portion of the DMT is at least 90% pure.

Citation Information

Patent Citations

  • JP1975082028A

  • Obtaining method of dimethyl telephthalate

    JP1977077024A

  • Method for separating and recovering dimethyl terephthalate and ethylene glycol from polyester waste

    JP4067306B2

  • Chemical recycling of waste plastic materials with improved solvolysis catalyst

    WO2021211506A1