Aqueous polyvinylidene fluoride coating composition

Highly branched surfactants with a degree of 5 or more stabilize PVDF dispersions, addressing agglomeration issues and enabling redispersion, thus providing stable and environmentally friendly coating compositions.

JP2024538252AActive Publication Date: 2024-10-18DOW GLOBAL TECHNOLOGIES LLC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024525028
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-11-05
Publication Date
2024-10-18
Estimated Expiration
2041-11-05

AI Technical Summary

Technical Problem

Existing aqueous dispersions of polyvinylidene fluoride (PVDF) suffer from agglomeration and segregation, leading to uneven coatings and limited pot life due to the use of fluorinated surfactants, which also pose environmental concerns.

Method used

Aqueous dispersions of PVDF stabilized with highly branched surfactants having a degree of hydrophobe branching of 5 or more, along with a dispersant like a diisobutylene-maleic anhydride copolymer, to prevent tight agglomeration and maintain homogeneity for up to 7 days, allowing redispersion.

Benefits of technology

The solution results in stable, homogeneous PVDF dispersions that remain redispersible after 7 days, eliminating the need for fluorinated surfactants and reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538252000001
    Figure 2024538252000001
  • Figure 2024538252000002
    Figure 2024538252000002
  • Figure 2024538252000003
    Figure 2024538252000003
Patent Text Reader

Abstract

The coating composition includes water, a plurality of polyvinylidene fluoride particles, and a surfactant having a hydrophobe branching degree of 5 or greater, wherein the composition does not include a fluorinated surfactant.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to coating compositions, and more particularly to coating compositions comprising polyvinylidene fluoride. [Background technology]

[0002] Introduction Polyvinylidene fluoride ("PVDF") and other fluoropolymers such as polytetrafluoroethylene ("PTFE") are typically formed in a multi-step process. For example, U.S. Patent Application Publication No. 2021 / 0032381 describes that a method frequently used to produce PTFE involves aqueous emulsion polymerization of fluorinated monomers. The aqueous emulsion polymerization typically uses a fluorinated surfactant and may include a non-ionic surfactant such as a polyoxyethylene alkyl ether surfactant. The fluorinated surfactant is essential to maintain the emulsion. After the emulsion polymerization is completed, a step is performed to concentrate the solids to remove the fluorinated surfactant. The solid fluoropolymer can then be recovered and used.

[0003] PVDF is a fluoropolymer used to make high performance coatings that offer good resistance to solvents, chemicals, weather, and heat. Unlike PTFE and other fluoropolymers, PVDF is not a fully fluorinated polymer, but has a repeating chemical structure of CH2CF2. This unique chemical structure results in PVDF having a low surface energy and a relatively high density of 1.8 grams per cubic centimeter ("g / cc") to 1.9 g / cc. The low surface energy and high density of PVDF typically result in agglomeration and separation of PVDF particles when used in aqueous dispersions, and therefore fluorinated surfactants are typically used. The use of such aqueous dispersions in coating applications is difficult because the agglomeration and separation results in non-uniform coating of the particles on the substrate. In addition, the aggregates tend to become tightly packed within less than seven days of the formation of the aqueous dispersion. The tightly packed aggregates can no longer be redispersed, thereby limiting the pot life of the aqueous dispersion. It would therefore be advantageous to achieve a stable dispersion that can retain its uniformity or is at least redispersible after a seven-day period.

[0004] Fluorinated surfactants are typically required to make stable aqueous dispersions, but the inclusion of fluorinated surfactants presents environmental concerns regarding disposal.Various attempts to make stable PVDF aqueous dispersions without fluorinated surfactants have been tried.For example, US Patent Application Publication No. 2015 / 0030906 provides for the formation of an aqueous dispersion of PVDF using a non-fluorinated surfactant, but such dispersions are used immediately because PVDF tends to rapidly aggregate and separate.

[0005] In view of the above teachings, the discovery of an aqueous dispersion of PVDF that is initially homogeneous and redispersible after a seven day period would be surprising. Summary of the Invention

[0006] The present disclosure provides an aqueous dispersion of PVDF that is initially homogeneous and redispersible after a period of 7 days. The present invention is the result of discovering that not only can highly branched surfactants create initially homogeneous aqueous dispersions of PVDF, but also that highly branched surfactants can maintain the redispersibility of PVDF after extended storage times. Without being bound by theory, it is believed that surfactants with a hydrophobe branching degree of 5 or more can prevent the PVDF particles from agglomerating tightly, at least in part, by steric hindrance. By preventing the PVDF particles from agglomerating tightly, the aqueous dispersion can maintain a homogeneous dispersion over time or can be rapidly redispersible.

[0007] The present disclosure is particularly useful in forming coating compositions.

[0008] According to a first aspect of the present disclosure, a coating composition includes water, a plurality of polyvinylidene fluoride particles, and a surfactant having a hydrophobe branching degree of 5 or greater, wherein the composition does not include a fluorinated surfactant.

[0009] According to a second feature of the present disclosure, the surfactant is a non-ionic surfactant.

[0010] According to a third feature of the present disclosure, a weight ratio of the surfactant to the polyvinylidene fluoride particles is 2.0% to 15.0%.

[0011] According to a fourth aspect of the present disclosure, the coating composition comprises 20 wt % to 70 wt % of polyvinylidene fluoride particles, based on the total weight of the coating composition.

[0012] According to a fifth aspect of the present disclosure, the coating composition further comprises 0.1 wt % to 10.0 wt % of a dispersant, the dispersant being a random copolymer of diisobutylene and maleic anhydride.

[0013] According to a sixth feature of the present disclosure, the coating composition further comprises 0.1 wt.% to 10.0 wt.% of a dispersant, the dispersant having a structure (II), wherein each AO can independently be ethylene oxide, propylene oxide, butylene oxide, and combinations thereof in random or block order, and further wherein each n in structure (II) can independently be 5 to 40.

[0014] According to a seventh feature of the present disclosure, a surfactant has structure (I), wherein n in structure (I) is 3 to 11, and R1 for each n is independently selected from the group consisting of H, or alkyl having 1 or 2 carbons.

[0015] According to an eighth feature of the present disclosure, in structure (I), n is 8-11 and R1 is H.

[0016] According to a ninth feature of the present disclosure, a method includes dispersing a plurality of polyvinylidene fluoride particles in a mixture of water and a surfactant having a hydrophobe branching degree of 5 or greater, wherein the composition does not include a fluorinated surfactant.

[0017] According to a tenth aspect of the present disclosure, a method for coating a substrate comprises applying a coating composition according to claim 9 to the substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] As used herein, the term "and / or," when used with a list of two or more items, means that any one of the listed items can be used by itself, or any combination of two or more of the listed items can be used. For example, if a composition is described as containing components A, B, and / or C, the composition can contain A alone, B alone, C alone, A and B in combination, A and C in combination, B and C in combination, or A, B, and C in combination.

[0019] Unless otherwise stated, all ranges are inclusive of the endpoints.

[0020] As used herein, the term weight percent ("wt %"), unless otherwise specified, refers to the weight percentage that a component represents of the total weight of the coating composition.

[0021] As used herein, "CAS Number" is the Chemical Service Registry Number assigned by the Chemical Abstracts Service.

[0022] Coating Composition The present disclosure is directed to a coating composition. The coating composition includes water, a plurality of polyvinylidene fluoride particles, and a surfactant having a hydrophobe branching degree of 5 or more. The coating composition is free of fluorinated surfactants. As used herein, the term "free of" is defined to mean that the coating composition includes 0.001% by weight or less of the material that it is said to be free of. The coating composition may include a dispersant and / or other additives. For example, the coating composition may comprise 20% by weight or more, or 25% by weight or more, or 30% by weight or more, or 35% by weight or more, or 40% by weight or more, or 45% by weight or more, or 50% by weight or more, or 55% by weight or more, or 60% by weight or more, or 65% by weight or more, while at the same time comprising 70% by weight or less, or 65% by weight or less, or 60% by weight or less, or 55% by weight or less, or 50% by weight or less, or 45% by weight or less, or 40% by weight or less, or 35% by weight or less, or 30% by weight or less, or 25% by weight or less of water, based on the total weight of the coating composition. The coating composition may be useful in forming coatings on battery separators and other applications where uniform deposition of PVDF particles using an aqueous dispersion is advantageous. Furthermore, because the coating composition does not include a fluorinated surfactant, the coating composition has less associated environmental impact.

[0023] Polyvinylidene Fluoride The coating composition includes polyvinylidene fluoride. The PVDF is in the form of a plurality of particles. PVDF may include homopolymers, copolymers, and terpolymers within its meaning. The PVDF may be 50 mole percent ("mol %) or more, or 75 mole % or more, or 80 mole % or more, or 85 mole % or more polyvinylidene fluoride copolymerized with at least one comonomer selected from the group consisting of tetrafluoroethylene, trifluoroethylene, chlorotrifluoroethylene, hexafluoropropene, vinyl fluoride, pentafluoropropene, tetrafluoropropene, perfluoromethyl vinyl ether, perfluoropropyl vinyl ether, other monomers, and combinations thereof. The PVDF may be 100 mole % polyvinylidene fluoride and may not contain additional comonomers. PVDF particles may have a diameter or maximum linear dimension of 20 nm or more, or 50 nm or more, or 100 nm or more, or 200 nm or more, or 300 nm or more, or 400 nm or more, or 500 nm or less. PVDF can be formed by aqueous free radical emulsion polymerization, suspension polymerization, solution polymerization, and supercritical CO2 polymerization.

[0024] For example, the coating composition may comprise 20% by weight or more, or 25% by weight or more, or 30% by weight or more, or 35% by weight or more, or 40% by weight or more, or 45% by weight or more, or 50% by weight or more, or 55% by weight or more, or 60% by weight or more, or 65% by weight or more, while at the same time 70% by weight or less, or 65% by weight or less, or 60% by weight or less, or 55% by weight or less, or 50% by weight or less, or 45% by weight or less, or 40% by weight or less, or 35% by weight or less, or 30% by weight or less, or 25% by weight or less of PVDF particles, based on the total weight of the coating composition.

[0025] Surfactants The coating composition comprises a surfactant. The surfactant comprises both a hydrophobic portion ("hydrophobe") and a hydrophilic portion. The hydrophobe of the surfactant may be linear (i.e., straight chain) or branched (thus having a degree of branching of 2 or greater). The degree of branching is determined by counting the number of hydrophobes extending from the backbone of the hydrophobe. The surfactant has a degree of hydrophobe branching of 5 or greater, or 6 or greater, or 7 or greater, or 8 or greater, or 9 or greater. The surfactant may be a single surfactant or a mixture of surfactants. The surfactant may have the structure (I):

[0026] [ka] where n in structure (I) is 3 to 11 and R1 for each n is independently selected from the group consisting of H, or alkyl having 1 or 2 carbons. For example, n in structure (I) can be 3, or 4, or 5, or 6, or 7, or 8, or 9, or 10, or 11.

[0027] The coating composition comprises 0.1 wt% to 10.0 wt% of a surfactant based on the total weight of the coating composition. For example, the coating composition comprises 0.1 wt% or more, or 0.5 wt% or more, or 1.0 wt% or more, or 1.5 wt% or more, or 2.0 wt% or more, or 2.5 wt% or more, or 3.0 wt% or more, or 3.5 wt% or more, or 4.0 wt% or more, or 4.5 wt% or more, or 5.0 wt% or more, or 5.5 wt% or more, or 6.0 wt% or more, or 6.5 wt% or more, or 7.0 wt% or more, or 7.5 wt% or more, or 8.0 wt% or more, or 8.5 wt% or more, or 9.0 wt% or more, or 9.5 wt% or more based on the total weight of the coating composition. While simultaneously comprising 10.0% by weight or less, or 9.5% by weight or less, or 9.0% by weight or less, or 8.5% by weight or less, or 8.0% by weight or less, or 7.5% by weight or less, or 7.0% by weight or less, or 6.5% by weight or less, or 6.0% by weight or less, or 5.5% by weight or less, or 5.0% by weight or less, or 4.5% by weight or less, or 4.0% by weight or less, or 3.5% by weight or less, or 3.0% by weight or less, or 2.5% by weight or less, or 2.0% by weight or less, or 1.5% by weight or less, or 1.0% by weight or less, or 0.5% by weight or less, or 0.2% by weight or less of a surfactant.

[0028] The coating composition may have a weight ratio of surfactant to PVDF of 2% to 15%. For example, the weight ratio of surfactant to PVDF is 2.0% or more, or 2.5% or more, or 3.0% or more, or 3.5% or more, or 4.0% or more, or 4.5% or more, or 5.0% or more, or 5.5% or more, or 6.0% or more, or 6.5% or more, or 7.0% or more, or 7.5% or more, or 8.0% or more, or 8.5% or more, or 9.0% or more, or 9.5% or more, or 10.0% or more, or 10.5% or more, or 11.0% or more, or 11.5% or more, or 12.0% or more, or 12.5% ​​or more, or 13.0% or more, or 13.5% or more, or 14.0% or more, or 14.5% or more. % or more, while at the same time being 15.0% or less, or 14.5% or less, or 14.0% or less, or 13.5% or less, or 13.0% or less, or 12.5% ​​or less, or 12.0% or less, or 11.5% or more, or 11.0% or less, or 10.5% or less, or 10.0% or less, or 9.5% or less, or 9.0% or less, or 8.5% or less, or 8.0% or less, or 7.5% or less, or 7.0% or less, or 6.5% or less, or 6.0% or less, or 5.5% or less, or 5.0% or less, or 4.5% or less, or 4.0% or less, or 3.5% or less, or 3.0% or less, or 2.5% or less. The weight ratio of surfactant to PVDF is determined as described in detail below.

[0029] Dispersants The coating composition may include one or more dispersants. For purposes of this disclosure, a dispersant is a non-surfactant material that, when added to a suspension of solid particles in a liquid, promotes the dispersion of the particles or maintains the dispersed particles in suspension. Dispersants may include inorganic dispersants, polymeric dispersants, and small molecule dispersants. The dispersant may be a copolymer of diisobutylene (CAS number 25167-70-8) and maleic anhydride (CAS number 108-31-6). In one such example, the dispersant may comprise 30% by weight or more, or 35% by weight or more, or 40% by weight or more, or 45% by weight or more, or 50% by weight or more, or 55% by weight or more, or 60% by weight or more, or 65% by weight or more, while simultaneously 70% by weight or less, or 65% by weight or less, or 60% by weight or less, or 55% by weight or less, or 50% by weight or less, or 45% by weight or less, or 40% by weight or less, or 35% by weight or less diisobutylene, based on the total weight of the dispersant. The dispersant may comprise 30% by weight or more, or 35% by weight or more, or 40% by weight or more, or 45% by weight or more, or 50% by weight or more, or 55% by weight or more, or 60% by weight or more, or 65% by weight or more, while at the same time 70% by weight or less, or 65% by weight or less, or 60% by weight or less, or 55% by weight or less, or 50% by weight or less, or 45% by weight or less, or 40% by weight or less, or 35% by weight or less, of maleic anhydride, based on the total weight of the dispersant.

[0030] In the example of a diisobutylene and maleic anhydride copolymer of the dispersant, the dispersant may have a weight average molecular weight of from 10,000 Daltons to 30,000 Daltons. For example, the dispersing agent may have a molecular weight of 10,000 daltons or more, or 11,000 daltons or more, or 12,000 daltons or more, or 13,000 daltons or more, or 14,000 daltons or more, or 15,000 daltons or more, or 16,000 daltons or more, or 17,000 daltons or more, or 18,000 daltons or more, or 19,000 daltons or more, or 20,000 daltons or more, or 21,000 daltons or more, or 22,000 daltons or more, or 23,000 daltons or more, or 24,000 daltons or more, or 25,000 daltons or more, or 26,000 daltons or more, or 27,000 daltons or more, or 28,000 daltons or more, while simultaneously or less than 30,000 daltons, or less than 29,000 daltons, or less than 28,000 daltons, or less than 27,000 daltons, or less than 26,000 daltons, or less than 25,000 daltons, or less than 24,000 daltons, or less than 23,000 daltons, or less than 22,000 daltons, or less than 21,000 daltons, or less than 20,000 daltons, or less than 19,000 daltons, or less than 18,000 daltons, or less than 17,000 daltons, or less than 16,000 daltons, or less than 15,000 daltons, or less than 14,000 daltons, or less than 13,000 daltons, or less than 12,000 daltons, or less than 11,000 daltons. The weight average molecular weight of the dispersant is determined using gel permeation chromatography.

[0031] Another example of a suitable dispersant has the structure (II):

[0032] [ka] wherein each alkylene oxide ("AO") can independently be ethylene oxide, propylene oxide, butylene oxide, and / or combinations thereof in random or block order. Each n in structure (II) can independently be 5 to 40. For example, n can be 5 or more, or 10 or more, or 15 or more, or 20 or more, or 25 or more, or 30 or more, or 35 or more, while simultaneously being 40 or less, or 35 or less, or 30 or less, or 25 or less, or 20 or less, or 15 or less, or 10 or less, or 9 or less, or 8 or less, or 7 or less, or 6 or less. Ethylene oxide may comprise 25% or more by weight of the total weight of structure (II). For example, ethylene oxide may account for 25% by weight or more, or 30% by weight or more, or 40% by weight or more, or 50% by weight or more, or 60% by weight or more, or 70% by weight or more, or 80% by weight or more, while at the same time 90% by weight or less, or 80% by weight or less, or 70% by weight or less, or 60% by weight or less, or 50% by weight or less, or 40% by weight or less, or 30% by weight or less.

[0033] The coating composition may contain 0 wt% dispersant, or 0.1 wt% to 10.0 wt% dispersant, based on the total weight of the coating composition. For example, the coating composition may contain 0.1 wt% or more, or 0.5 wt% or more, or 1.0 wt% or more, or 1.5 wt% or more, or 2.0 wt% or more, or 2.5 wt% or more, or 3.0 wt% or more, or 3.5 wt% or more, or 4.0 wt% or more, or 4.5 wt% or more, or 5.0 wt% or more, or 5.5 wt% or more, or 6.0 wt% or more, or 6.5 wt% or more, or 7.0 wt% or more, or 7.5 wt% or more, or 8.0 wt% or more, or 8.5 wt% or more, or 9.0 wt% or more, or 9.5 wt% or more, based on the total weight of the coating composition. or less, while at the same time comprising 10.0% by weight or less, or 9.5% by weight or less, or 9.0% by weight or less, or 8.5% by weight or less, or 8.0% by weight or less, or 7.5% by weight or less, or 7.0% by weight or less, or 6.5% by weight or less, or 6.0% by weight or less, or 5.5% by weight or less, or 5.0% by weight or less, or 4.5% by weight or less, or 4.0% by weight or less, or 3.5% by weight or less, or 3.0% by weight or less, or 2.5% by weight or less, or 2.0% by weight or less, or 1.5% by weight or less, or 1.0% by weight or less, or 0.5% by weight or less, or 0.2% by weight or less of dispersant.

[0034] Method of making a coating composition and method of coating a substrate The coating composition is formed by a method including dispersing a plurality of polyvinylidene fluoride particles in a mixture of water and a surfactant having a hydrophobe branching degree of 5 or more, the composition being free of fluorinated surfactant. The act of dispersing the polyvinylidene fluoride particles in the mixture of water and surfactant can be accomplished in a variety of ways. For example, the coating composition can be placed in a grinding jar with beads (e.g., glass, ZrO, Al2O3, etc.) and ground for a predetermined period of time. Such grinding methods are advantageously used when the PVDF particles are added to the coating composition at a size larger than desired in the dispersion. Additionally or alternatively, the PVDF particles may be mixed or stirred directly in the combined water and surfactant. It will be understood that the PVDF particles, surfactant, water, dispersant, and any other additives may be added together in any order.

[0035] The coating composition is useful for forming a coated substrate. The method of coating a substrate can be performed using a step of applying the coating composition to the substrate. The coating composition can be applied to the substrate in various ways. For example, the substrate can be immersed in the composition, the composition can be sprayed onto the substrate, the substrate can be a continuous sheet passing through a bath away from the coating composition, and / or other methods of applying the coating composition to the substrate. The substrate can include polymeric materials, metals, ceramics, amorphous materials (e.g., glass), and / or other types of materials. Examples of polymeric material substrates can include low density polyethylene, medium density polyethylene, high density polyethylene, polyolefin elastomers, copolymers of one or more alpha olefins with another monomer, and other types of polymeric materials. In an exemplary use, the coating composition can be applied to a polymeric substrate to form a separator layer for a battery. EXAMPLES

[0036] material The following materials were used in forming the inventive examples ("IE") and comparative examples ("CE").

[0037] Surfactant 1 is a surfactant having a 90% by weight actives solution in water and structure (I) where n is 8 and R1 is H. Surfactant 1 has a hydrophobe branching level of 5. Surfactant 1 is available from The Dow Chemical Company, Midland Michigan.

[0038] Surfactant 2 is a surfactant having a 90% by weight actives solution in water and structure (I) where n is 11 and R1 is H. Surfactant 2 has a hydrophobe branching level of 5. Surfactant 2 is available from The Dow Chemical Company, Midland Michigan.

[0039] Dispersant 1 is formed from 45% to 55% by weight monomeric structural units of diisobutylene, the remainder being maleic anhydride. The dispersant has a weight average molecular weight of about 16,500 Daltons and is available from The Dow Chemical Company, Midland Michigan.

[0040] Dispersant 2 is a dispersant having structure (II) where each AO chain is composed of ethylene oxide and propylene oxide units in block sequence, and the average repeat unit n in each branch is about 37. Dispersant 2 is available from The Dow Chemical Company, Midland Michigan.

[0041] Surfactant 3 is 3,5,5-trimethylhexyl ethoxylate having a hydrophobe branching level of 4 and is available from Sigma Aldrich, St. Louis Missouri.

[0042] Surfactant 4 is a 2-ethylhexanol EO-PO nonionic surfactant having a CAS number of 64366-70-7 and a hydrophobe branching level of 2. Surfactant 4 is available from The Dow Chemical Company, Midland Michigan.

[0043] Surfactant 5 is a C12-14-secondary alcohol ethoxolates having a CAS number of 84133-50-6 and a hydrophobe branch of 2. Surfactant 5 is available from The Dow Chemical Company, Midland Michigan.

[0044] Surfactant 6 is an isotridecyl alcohol ethoxylate having an average hydrophobe branching of 4 and is commercially available as LUTENSOL™ TO from BASF corporation, Ludwigshafen, Germany.

[0045] PVDF is polyvinylidene fluoride homopolymer particles commercially available as KYNAR™ HSV900 from Arkema, Colombes, France.

[0046] The ZrO beads were 0.8–1.2 mm diameter ZrO beads from Sinopharm Chem.Reagent Co.Ltd., China.

[0047] Sample preparation Comparative examples and inventive examples were prepared by filling a grinding jar with a premixed mixture of surfactant, PVDF powder, dispersant (IE1), and water. ZrO beads were weighed and added. The jar was placed in a sand mill machine from Shanghai Dedong, and water cooling to the grinding jar was started before the grinding process began. The grinding process was carried out for 4 hours at 1400 revolutions per minute. After the allotted time, the ZrO beads were filtered out by passing the ground mixture through a 500 mesh nylon sieve. The ground PVDF dispersion samples were applied to conductive tape for characterization with a NOVA™ Nanosem 630 scanning electron microscope from FEI Company. All examples were stored at about 23° C. for 7 days without stirring to observe aggregation and settling. The weight ratio of surfactant to PVDF is calculated by dividing the weight in grams of surfactant present (taking into account any diluent in the surfactant) by the weight in grams of PVDF particles and multiplying by 100. The examples were evaluated both visually and with the use of a scanning electron microscope. Examples that could not be redispersed after storage were termed agglomerated or tightly agglomerated, the difference being the amount of material that could be liberated from the bottom of the jar by agitation. Examples where the PVDF could be agitated to resume a uniform dispersion were classified as redispersible.

[0048] result Table 1 provides the compositions of IE1-IE5 and CE1-CE4. The compositions of the examples are provided in grams.

[0049] [Table 1]

[0050] Table 2 provides the results for the different surfactants used in terms of the initial dispersion appearance, the morphology after 7 days of storage, and the average particle size peak present.

[0051] [Table 2]

[0052] Now, referring to Tables 1 and 2, all the inventive examples as well as Comparative Examples 1 and 4 showed uniform milky dispersions after the milling process. However, after 7 days of storage at 23°C, CE1-CE4 showed phase separation, which resulted in the formation of strong sediments at the bottom of the sample container. The sediments of CE1-CE4 could not be redispersed by manual shaking. IE1 remained uniform after 7 days of storage. IE2-IE5 showed phase separation, but the sediments could be redispersed by manual shaking. CE1-CE4 demonstrate that the selection of surfactants with hydrophobe branching of 4 or less cannot prevent aggregation, even though different surfactants are used. However, IE1-IE5 utilizing surfactants with hydrophobe branching of 5 are all able to achieve aqueous dispersions of PVDF that are initially uniform and redispersible after a period of 7 days. Surfactants with a hydrophobe branching degree of 6 or more show the same resistance to aggregation and are believed to be redispersible due to even greater steric hindrance effects.

Claims

1. 1. A coating composition comprising: Water, a plurality of polyvinylidene fluoride particles; a surfactant having a hydrophobe branching degree of 5 or more; A coating composition, wherein the composition does not comprise a fluorinated surfactant.

2. The coating composition of claim 1 , wherein the surfactant is a non-ionic surfactant.

3. 2. The coating composition of claim 1, wherein the weight ratio of the surfactant to the polyvinylidene fluoride particles is from 2.0% to 15.0%.

4. The coating composition of claim 1, wherein the coating composition comprises 20% to 70% by weight of the polyvinylidene fluoride particles, based on the total weight of the coating composition.

5. 10. The coating composition of claim 1, further comprising 0.1 wt. % to 10.0 wt. % of a dispersant, said dispersant being a random copolymer of diisobutylene and maleic anhydride.

6. Further comprising 0.1 wt. % to 10.0 wt. % of a dispersant, the dispersant having Structure (II): 【Chemistry 1】 wherein each AO can independently be ethylene oxide, propylene oxide, butylene oxide, and combinations thereof in random or block order, and further wherein each n in structure (II) can independently be 5 to 40.

7. 13. The surfactant of claim 12, wherein the surfactant has the structure (I): 【Chemistry 2】 wherein n in structure (I) is 3 to 11, and each n of R 1 The coating composition of any one of claims 1 to 6, wherein is independently selected from the group consisting of H, or alkyl having 1 or 2 carbons.

8. In structure (I), n is 8 to 11, and R 1 The coating composition of claim 7 , wherein:

9. 1. A method of forming a coating composition comprising:

1. A method comprising dispersing a plurality of polyvinylidene fluoride particles in a mixture of water and a surfactant having a hydrophobe branching degree of 5 or greater, wherein the composition does not include a fluorinated surfactant.

10. 1. A method of coating a substrate, comprising the steps of: A method comprising applying the coating composition of claim 9 to a substrate.

Citation Information

Patent Citations

  • Tetrafluoroethylene (TFE) copolymer

    JP2005171250A

  • Stable water-based fluoropolymer coating composition

    JP2017525835A

  • Ink set, image formation method, and image formation device

    JP2022143871A