Preparation method of high-strength titanium alloy capable of inhibiting cracks and high-strength titanium alloy
By using low-energy ball milling and SLM printing of graphene-Y2O3 composite powder and high-strength titanium alloy powder, combined with heat treatment, the problem of cracking in high-strength titanium alloy during SLM forming was solved, and a high-strength crack-free titanium alloy was prepared, achieving high mechanical properties and low-cost manufacturing.
Patent Information
- Application Number
- CN202411055434.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-02
AI Technical Summary
High-strength titanium alloys are prone to cracking during the existing SLM forming process, and traditional titanium alloy grades are limited, making it difficult to manufacture them using SLM.
A graphene-Y2O3-high-strength titanium alloy was prepared by low-energy ball milling of graphene and Y2O3 composite powder and high-strength titanium alloy powder, followed by SLM printing and heat treatment. This process refined the grains and suppressed crack formation.
The prepared high-strength titanium alloy has no internal cracks, fine grains, high room temperature tensile strength, yield strength and elongation, excellent high temperature tensile properties, and low cost.
Smart Images

Figure CN118957337A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a method for preparing a high-strength titanium alloy capable of suppressing cracks and the high-strength titanium alloy. Background Art
[0002] Titanium and titanium alloys have good comprehensive properties such as low density, high strength, good toughness, and good biocompatibility. They are widely used in the automotive, defense, biomedical, aerospace and other industries. However, the processing of traditional parts is complicated and often requires many processes such as casting, machining, and welding, which is economically inefficient. When a component with a complex geometry is required, part processing is even more difficult to achieve. With the development of metal additive technology, both traditional parts and complex design parts can be manufactured in an integrated manner, eliminating the need for post-processing, thereby reducing manufacturing time. In addition, additive technology can reduce material waste, reduce energy consumption, and provide the best design for lean production.
[0003] Graphene is a sp 2 The new material with hybrid connected carbon atoms tightly stacked into a single-layer two-dimensional honeycomb lattice structure has excellent properties such as low density, high specific strength, high thermal conductivity and self-lubrication. Taking advantage of the high chemical activity of titanium, it is easy to react chemically with graphene to obtain an in-situ reaction interface with strong bonding, and then combine the excellent properties of graphene such as light weight, high strength and toughness and large specific surface area with the high temperature resistance and fatigue resistance of titanium alloy, which is expected to prepare higher performance graphene-enhanced titanium-based composite materials.
[0004] As a new manufacturing concept, SLM technology has been widely used in various industries, such as medical, aerospace, and automotive prototypes. However, the corresponding grades of titanium alloys that can be printed using SLM (selective laser melting) technology on the market are relatively limited. Commonly used grades include pure titanium, TC4, TA15, etc. There are still many traditional grades of titanium alloys that have not been applied to the SLM manufacturing industry. During the SLM molding process, as the laser energy is input, the original powder particles absorb the energy of the image and melt. When the energy is insufficient, the powder does not absorb enough energy to melt the metal powder, resulting in too little liquid metal in the weld path, resulting in discontinuity of the weld path. The huge capillary force and strong convection of the liquid metal cause a large amount of spheroidization in the weld path. When the energy input of the energy laser is too high, the liquid metal in the molten pool will splash, causing spheroidization or overmelting of the metal powder, increasing the possibility of residual stress and cracks. At the same time, more liquid metal enters the molten pool, causing the instability of the molten pool to increase. As a result, the high temperature of the molten pool causes the melt to vaporize and the gas-liquid interface to form a reaction force and the splash of the high-temperature melt, which affects the stability of the molten pool and causes the molten pool to break. At the same time, the unmelted powder particles and pores in the SLM molding process become crack sources under the maximum residual stress, causing cracks; especially for high-strength titanium alloys, the fracture phenomenon is particularly serious.
[0005] In summary, there is an urgent need to develop a method for preparing high-strength titanium alloys that can suppress cracks. The high-strength titanium alloy formed by SLM not only has high mechanical strength but also does not produce cracks. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing a high-strength titanium alloy capable of suppressing cracks, which has the characteristics of simple method and low cost, and the prepared high-strength titanium alloy has not only high mechanical strength but also no cracks.
[0007] The present invention solves the technical problem by adopting the following technical solutions.
[0008] In one aspect, the present invention provides a method for preparing a high-strength titanium alloy capable of suppressing cracks, comprising the following steps:
[0009] Step S1: dispersing Y2O3 powder in an aqueous solution having a cationic surfactant to obtain a Y2O3 suspension coated with the cationic surfactant; dispersing graphene oxide in an alkaline solution to obtain a graphene oxide suspension;
[0010] Step S2: adding the graphene oxide suspension dropwise to the Y2O3 suspension coated with the cationic surfactant, mixing evenly by mechanical stirring, filtering and drying to obtain the graphene oxide-Y2O3 composite powder;
[0011] The dried graphene oxide-Y2O3 composite powder is placed in an atmosphere of a mixture of an inert gas and H2 for heat treatment to obtain a reduced graphene-Y2O3 composite powder;
[0012] Step S3: low-energy ball milling the high-strength titanium alloy powder and the reduced graphene-Y2O3 composite powder to obtain reduced graphene-Y2O3-high-strength titanium alloy composite powder;
[0013] Step S4: The reduced graphene-Y2O3-high-strength titanium alloy composite powder obtained in step S3 is subjected to SLM printing to obtain a high-strength titanium alloy that can suppress cracks.
[0014] Furthermore, in step S1, the mass ratio of graphene oxide to Y2O3 is 1:(1-3), the molar ratio of the cationic surfactant to Y2O3 is (1.25-1.3):1, and the concentration of the graphene oxide suspension is 0.01-0.02 g / mL.
[0015] Furthermore, in step S1, the particle size of Y2O3 is 40-60nm.
[0016] Furthermore, in step S1, the alkaline solution is a mixed alkaline solution of NaOH and Na2CO3, and the molar ratio of NaOH to Na2CO3 is 1:(2-3), and the concentration of NaOH is 0.04-0.05 g / mL.
[0017] Furthermore, in step S2, the volume ratio of the graphene oxide suspension to the Y2O3 suspension coated with the surfactant is (18-20):1.
[0018] Furthermore, in step S3, the mass proportion of the reduced graphene-Y2O3 composite powder is 0.1-0.5%.
[0019] Furthermore, in step S2, the specific process for obtaining the reduced graphene-Y2O3 composite powder is as follows: at a temperature of 850-920°C and a pressure of 0.1-0.6Mpa, the dried graphene oxide-Y2O3 composite powder is placed in an atmosphere of a mixture of inert gas and H2 for heat treatment for 3-6 hours to obtain the reduced graphene-Y2O3 composite powder, wherein the volume ratio of the inert gas to H2 is 100:(1-5).
[0020] Furthermore, in step S4, the laser energy density is 45-120 J / mm 3 ; The 3D printing parameters used are: laser power of 180-260W; laser scanning speed of 700-1300mm / s; scanning spacing of 0.08-0.12mm; interlayer thickness of 0.03-0.06mm.
[0021] Furthermore, it is characterized in that it also includes: step S5: heat treating the high-strength titanium alloy obtained in step S4, first heating it to 500-600°C in a vacuum atmosphere and keeping it warm for 0.5-1h, then continuing to heat it to 800°C-850°C and keeping it warm for 2-4h, introducing argon gas to 2-4bar and quickly cooling it to room temperature before taking it out, and the cooling zone rate is 45-80°C / min.
[0022] Another aspect of the present invention provides a high-strength titanium alloy, which is prepared by the above-mentioned preparation method.
[0023] The beneficial effects of the method for preparing a high-strength titanium alloy capable of suppressing cracks according to an embodiment of the present invention include:
[0024] (1) The titanium alloy prepared by the preparation method of the present invention has no cracks inside and fine grains. By adding a certain mass of graphene and Y2O3 for compounding, the heat conduction speed is accelerated during the selective laser melting forming process due to the excellent thermal conductivity of graphene, which provides a greater driving force for the process of decomposition of the α phase to transform into the β phase, and at the same time, the upper forming layer undergoes secondary forming, resulting in an increase in the number of transformations from the β phase to the α phase, which significantly increases the secondary α′ phase, and the α and α′ phases are finer. At the same time, the addition of Y2O3 refines the structure of the high-strength titanium alloy, and after annealing treatment, obvious recrystallization occurs, which refines the grains and improves the forming performance.
[0025] (2) The two-dimensional lattice mismatch between the (111) crystal plane of Y2O3 and the (110) crystal plane of TiC is δ=6.54%. Y2O3 can serve as an effective heterogeneous nucleation core of TiC to refine the grains. After adding graphene at the same time, under the action of high-energy laser beam, graphene and titanium alloy react in situ: Ti+C→TiC, producing a large number of TiC nanoparticles and undecomposed graphene. During the forming process, Y2O3 is encouraged to better form a composite phase structure with TiC, and the increase in nucleation cores makes the grains finer. The appearance of nano-TiC particles is also conducive to the formation of deformation twins, which promotes the atoms of the nano-composite materials in the alloy to maintain orderly arrangement during the deformation process, so that the severe lattice distortion and deformation twins at the interface formed by different orientations inhibit the movement of dislocations, thereby reducing the generation of cracks.
[0026] (3) Through the composite addition of graphene and Y2O3 of the present invention, finer α, α′, and β phases are generated during the printing and solidification process. At the same time, the in-situ generated TiC nanoparticles and the graphene that has not reacted and agglomerated will inhibit the growth of the titanium-based composite material grains, so that the grains can be refined; the addition of an appropriate amount of Y2O3 can increase the supercooling of the molten pool and increase the system nucleation rate, thereby refining the grains; the unmelted Y2O3 can serve as a heterogeneous nucleation core, increase the nucleation rate, and refine the grains. The TiC nanoparticles are dispersed and evenly distributed, which has the effect of dispersion strengthening. According to the Hall-Patch mechanism, the smaller the grain size, the higher its yield strength.
[0027] (4) By observing the organization of the printed melt with different process parameters, adding a certain amount of graphene and Y2O3 can reduce the crack and porosity problems of high-strength titanium alloys and refine the grains. When the mass fraction of the graphene and Y2O3 composite powder accounts for 0.3% of the total printed powder, the effect is optimal; the density of the melt is 99.3%, the room temperature tensile strength is as high as 1630MPa, the yield strength is as high as 1504MPa, the elongation can reach 9.6%, and its hardness value is as high as 348HV. In addition, the titanium alloy composite material prepared by the present invention has excellent high-temperature tensile properties, the elongation can reach 17% at a high temperature of 500℃, and the tensile strength can reach 1156MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 This is a metallographic diagram of the high-strength titanium alloy prepared in Example 1 of the present invention;
[0030] Figure 2 This is a metallographic diagram of a high-strength titanium alloy prepared in Example 2 of the present invention;
[0031] Figure 3 This is a metallographic diagram of a high-strength titanium alloy obtained in Example 3 of the present invention;
[0032] Figure 4 This is a metallographic diagram of the high-strength titanium alloy prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0033] The technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, rather than all the embodiments. Based on the embodiment in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiment, it is carried out according to the conditions recommended by the normal conditions or the manufacturers. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0034] In one aspect, the present invention provides a method for preparing a high-strength titanium alloy capable of suppressing cracks, comprising the following steps:
[0035] Step S1: dispersing Y2O3 powder in an aqueous solution having a cationic surfactant to obtain a Y2O3 suspension coated with the cationic surfactant; dispersing graphene oxide in an alkaline solution to obtain a graphene oxide suspension;
[0036] Step S2: adding the graphene oxide suspension dropwise to the Y2O3 suspension coated with the cationic surfactant, mixing evenly by mechanical stirring, filtering and drying to obtain the graphene oxide-Y2O3 composite powder;
[0037] The dried graphene oxide-Y2O3 composite powder is placed in an atmosphere of a mixture of an inert gas and H2 for heat treatment to obtain a reduced graphene-Y2O3 composite powder;
[0038] Step S3: low-energy ball milling the high-strength titanium alloy powder and the reduced graphene-Y2O3 composite powder to obtain reduced graphene-Y2O3-high-strength titanium alloy composite powder;
[0039] Step S4: The reduced graphene-Y2O3-high-strength titanium alloy composite powder obtained in step S3 is subjected to SLM printing to obtain a high-strength titanium alloy that can suppress cracks.
[0040] It should be noted that the high-strength titanium alloy described in the present invention refers to a titanium alloy having a tensile strength of 1100 to 1400 MPa at room temperature, which is composed of a near-β titanium alloy and a metastable β titanium alloy.
[0041] It should be noted that Y2O3 powder is dispersed in an aqueous solution containing a cationic surfactant to obtain a Y2O3 suspension coated with a cationic surfactant; graphene oxide is dispersed in an alkaline solution to obtain a graphene oxide suspension; both can be dispersed by ultrasound or other dispersion methods, and the embodiments of the present invention are described in terms of ultrasonic dispersion.
[0042] The cationic surfactants described herein include nitrogen-containing organic amine derivatives. Since the nitrogen atom in the molecule contains a lone pair of electrons, it can be combined with the hydrogen in the acid molecule by hydrogen bonding, so that the amino group carries a positive charge. The cationic surfactants are preferably hexadecyltrimethylammonium bromide, octadecyldimethylbenzylammonium chloride, and hexadecylpyridinium chloride.
[0043] The titanium alloy prepared by the preparation method of the present invention has no cracks inside and fine grains. By adding a certain mass of graphene and Y2O3 for compounding, the heat conduction speed is accelerated during the selective laser melting forming process due to the excellent thermal conductivity of graphene, which provides a greater driving force for the process of decomposition of the α phase to transform into the β phase, and at the same time causes the upper forming layer to undergo secondary forming, resulting in an increase in the number of transformations from the β phase to the α phase, which significantly increases the secondary α′ phase, and the α and α′ phases are finer. At the same time, the addition of Y2O3 refines the structure of the high-strength titanium alloy, and after annealing treatment, obvious recrystallization occurs, which refines the grains and improves the forming performance.
[0044] The two-dimensional lattice mismatch between the (111) crystal plane of Y2O3 and the (110) crystal plane of TiC is δ=6.54%. Y2O3 can be used as an effective heterogeneous nucleation core of TiC to refine the grains. After adding graphene at the same time, under the action of high-energy laser beam, graphene and titanium alloy react in situ: Ti+C→TiC, producing a large number of TiC nanoparticles and undecomposed graphene. During the molding process, Y2O3 is promoted to better form a composite phase structure with TiC, and the increase in nucleation cores makes the grains finer. The appearance of nano-TiC particles is also conducive to the formation of deformation twins, which promotes the atoms of the nano-composite materials in the alloy to maintain orderly arrangement during the deformation process, so that the severe lattice distortion and deformation twins at the interface formed by different orientations inhibit the movement of dislocations, thereby reducing the generation of cracks.
[0045] Through the composite addition of graphene and Y2O3 of the present invention, finer α, α′, and β phases are generated during the printing solidification process. At the same time, the in-situ generated TiC nanoparticles and the graphene that has not reacted and agglomerated will inhibit the growth of the titanium-based composite material grains, so that the grains can be refined; the addition of an appropriate amount of Y2O3 can increase the supercooling of the molten pool and increase the system nucleation rate, thereby refining the grains; the unmelted Y2O3 can serve as a heterogeneous nucleation core, increase the nucleation rate, and refine the grains. The TiC nanoparticles are dispersed and evenly distributed, which has the effect of dispersion strengthening. According to the Hall-Patch mechanism, the smaller the grain size, the higher its yield strength.
[0046] By observing the organization of the printed melt with different process parameters, adding a certain amount of graphene and Y2O3 can reduce the crack and porosity problems of high-strength titanium alloys and refine the grains. When the mass fraction of the graphene and Y2O3 composite powder is 0.3%, the effect is the best; the density of the melt is 99.3%, the room temperature tensile strength is as high as 1630MPa, the yield strength is as high as 1501MPa, the elongation can reach 9.6%, and its hardness value is as high as 342HV. In addition, the titanium alloy composite material prepared by the present invention has excellent high-temperature tensile properties, the elongation can reach 17% at a high temperature of 500℃, and the tensile strength can reach 1156MPa.
[0047] Specifically, in step S1, the mass ratio of graphene oxide to Y2O3 is 1:(1-3), the molar ratio of the cationic surfactant to Y2O3 is (1.25-1.3):1, and the concentration of the graphene suspension is 0.01-0.02 g / mL.
[0048] By limiting the ratio of graphene oxide and Y2O3, on the one hand, it is beneficial to fully mix the cation-coated Y2O3 and the negatively charged graphene suspension; on the other hand, it can avoid the agglomeration of the two.
[0049] Specifically, in step S1, the particle size of Y2O3 is 40-60nm.
[0050] If the Y2O3 particles are too large, they will not be able to play a refining role during the printing process due to their large particles, and may also become a source of cracks, resulting in printing failure or material failure.
[0051] Specifically, in step S1, the alkaline solution is a mixed alkaline solution of NaOH and Na2CO3, and the molar ratio of NaOH to Na2CO3 is 1:(2-3), and the concentration of NaOH is 0.04-0.05 g / mL.
[0052] Specifically, in step S2, the volume ratio of the graphene oxide suspension to the Y2O3 powder suspension coated with the surfactant is (18-20):1.
[0053] Specifically, in step S3, the mass proportion of the reduced graphene-Y2O3 composite powder is 0.1-0.5%.
[0054] Specifically, in step S2, the specific process of obtaining the reduced graphene-Y2O3 composite powder is: at a temperature of 850-920°C and a pressure of 0.1-0.6Mpa, the dried graphene oxide-Y2O3 composite powder is placed in an atmosphere mixed with inert gas and H2 for heat treatment for 3-6 hours to obtain the reduced graphene-Y2O3 composite powder, wherein the volume ratio of the inert gas to H2 is 100:(1-5).
[0055] Preferably, the particle size of the high-strength titanium alloy powder is 15-53 μm.
[0056] Specifically, in step S3, the spheroidal graphite speed of the low-energy spheroidal graphite is 60-300 r / min, the ratio of the spheroidal graphite to the material is 5:1, and the ball milling time is 3-24 h.
[0057] Specifically, in step S4, the laser energy density is 45-120 J / mm 3 ; The 3D printing parameters used are: laser power of 180-260W; laser scanning speed of 700-1300mm / s; scanning spacing of 0.08-0.12mm; interlayer thickness of 0.03-0.06mm.
[0058] Specifically, it also includes: Step S5: heat treating the high-strength titanium alloy obtained in Step S4, first heating the temperature to 500-600°C in a vacuum atmosphere and keeping it warm for 0.5-1h, then continuing to heat the temperature to 800°C-850°C and keeping it warm for 2-4h, introducing argon gas to 2-4bar and quickly cooling it to room temperature before taking it out, and the cooling zone rate is 45-80°C / min.
[0059] When the cooling rate is lower than 45°C / min, some of the corresponding specimens may break abnormally or the elongation may be as low as 2-4% during the tensile test.
[0060] Another aspect of the present invention provides a high-strength titanium alloy capable of suppressing cracks, wherein the high-strength titanium alloy is prepared by the above preparation method.
[0061] In order to further illustrate the present invention, a method for recycling unfinished aluminum alloy powder provided by the present invention is described in detail below in combination with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0062] The high-strength titanium alloy used in the following embodiments is represented by Ti-55531 titanium alloy, but it should not be understood as limiting the protection scope of the present invention.
[0063] Example 1
[0064] The present embodiment provides a method for preparing a high-strength titanium alloy capable of suppressing cracks, which comprises the following steps:
[0065] Step S1: weigh 36.4 g of hexadecyltrimethylammonium bromide and dissolve it in 50 ml of an aqueous solution to obtain an aqueous solution of hexadecyltrimethylammonium bromide, and use an ultrasonic dispersion method to disperse 18 g of Y2O3 powder with a particle size of 40-60 nm in 50 ml of the aqueous solution of hexadecyltrimethylammonium bromide to obtain a Y2O3 powder suspension coated with a cationic surfactant;
[0066] Weigh 40 g of NaOH and 212 g of Na2CO3 and dissolve them in 1000 ml of water to obtain a mixed alkaline solution, and use an ultrasonic dispersion method to disperse 6 g of graphene oxide in 1000 ml of the mixed alkaline solution at room temperature to obtain a graphene oxide suspension;
[0067] Step S2: adding 1000 ml of graphene oxide suspension to 50 ml of Y2O3 suspension coated with a cationic surfactant, mixing evenly by mechanical stirring, filtering and drying to obtain graphene oxide-Y2O3 composite powder;
[0068] The dried graphene oxide-Y2O3 composite powder was placed in an atmosphere of a mixture of inert gas and H2 for heat treatment at a temperature of 850°C and a pressure of 0.1 MPa for 3 h to obtain a reduced graphene-Y2O3 composite powder;
[0069] Step S3: weighing 1990 g of Ti-55531 titanium alloy powder with a particle size of 15-53 μm and 10 g of the reduced graphene-Y2O3 composite powder obtained in step S2, subjecting the weighed Ti-55531 titanium alloy powder and the reduced graphene-Y2O3 composite powder to low-energy spheroidal graphite, with a spheroidal graphite speed of 60 r / min, a ball-to-material ratio of 5:1, and a ball milling time of 3 h; obtaining a reduced graphene-Y2O3-high-strength titanium alloy composite powder;
[0070] Step S4: SLM printing is performed on the reduced graphene-Y2O3-high-strength titanium alloy composite powder obtained in step S3 to obtain a high-strength titanium alloy that can suppress cracks; the laser body energy density is 45J / mm3; the 3D printing parameters used are: laser power is 180W; laser scanning speed is 700mm / s; scanning spacing is 0.08mm; interlayer thickness is 0.03mm;
[0071] The high-strength titanium alloy obtained in step S4 is heat-treated in a vacuum environment, first heated to 500°C and kept warm for 0.5h, then continued to heat to 800°C and kept warm for 2h, argon gas is introduced to 2bar, and then quickly cooled to room temperature and taken out, with a cooling zone rate of 45°C / min.
[0072] The performance indicators of the high-strength titanium alloy finally obtained are shown in Table 1. The metallographic structure of the high-strength titanium alloy obtained is as follows: Figure 1 shown.
[0073] Example 2
[0074] The present embodiment provides a method for preparing a high-strength titanium alloy capable of suppressing cracks, which comprises the following steps:
[0075] Step S1: Weigh 42.5 g of octadecyl dimethyl benzyl ammonium chloride and dissolve it in 50 ml of an aqueous solution to obtain an octadecyl dimethyl benzyl ammonium chloride aqueous solution, and use an ultrasonic dispersion method to disperse 18 g of Y2O3 powder with a particle size of 40-60 nm in 50 ml of the octadecyl dimethyl benzyl ammonium chloride aqueous solution to obtain a Y2O3 powder suspension coated with a cationic surfactant;
[0076] Weigh 40 g of NaOH and 318 g of Na2CO3 and dissolve them in 800 ml of water to obtain a mixed alkaline solution, and use an ultrasonic dispersion method to disperse 9 g of graphene oxide in 800 ml of the mixed alkaline solution at room temperature to obtain a graphene oxide suspension;
[0077] Step S2: adding 800 ml of graphene oxide suspension to 50 ml of Y2O3 suspension coated with a cationic surfactant, mixing evenly by mechanical stirring, filtering and drying to obtain graphene oxide-Y2O3 composite powder;
[0078] The dried graphene oxide-Y2O3 composite powder was placed in an atmosphere of a mixture of inert gas and H2 for heat treatment at a temperature of 920°C and a pressure of 0.6 MPa for 6 hours to obtain a reduced graphene-Y2O3 composite powder;
[0079] Step S3: weighing 1994 g of Ti-55531 titanium alloy powder with a particle size of 15-53 μm and 6 g of the reduced graphene-Y2O3 composite powder obtained in step S2, and subjecting the weighed Ti-55531 titanium alloy powder and the reduced graphene-Y2O3 composite powder to low-energy spheroidal graphite, with a spheroidal graphite speed of 300 r / min, a ball-to-material ratio of 5:1, and a ball milling time of 24 h; obtaining a reduced graphene-Y2O3-high-strength titanium alloy composite powder;
[0080] Step S4: SLM printing is performed on the reduced graphene-Y2O3-high-strength titanium alloy composite powder obtained in step S3 to obtain a high-strength titanium alloy that can suppress cracks; the laser body energy density is 120J / mm3; the 3D printing parameters used are: laser power is 260W; laser scanning speed is 1300mm / s; scanning spacing is 0.12mm; interlayer thickness is 0.06mm;
[0081] The high-strength titanium alloy obtained in step S4 is heat-treated by first heating to 600°C and keeping it for 1 hour in a vacuum environment, then continuing to heat to 850°C and keeping it for 4 hours. Argon gas is introduced to 4 bar and then quickly cooled to room temperature and taken out. The cooling zone rate is 80°C / min.
[0082] The performance indicators of the high-strength titanium alloy finally obtained are shown in Table 1. The metallographic structure of the high-strength titanium alloy obtained is as follows: Figure 2 shown.
[0083] Example 3
[0084] The present embodiment provides a method for preparing a high-strength titanium alloy capable of suppressing cracks, which comprises the following steps:
[0085] Step S1: Weigh 34 g of cetylpyridinium chloride and dissolve it in 50 ml of an aqueous solution to obtain an aqueous solution of cetylpyridinium chloride, and use an ultrasonic dispersion method to disperse 18 g of Y2O3 powder with a particle size of 40-60 nm in the 50 ml of the aqueous solution of cetylpyridinium chloride to obtain a Y2O3 powder suspension coated with a cationic surfactant;
[0086] Weigh 40 g of NaOH and 212 g of Na2CO3 and dissolve them in 900 ml of water to obtain a mixed alkaline solution, and use an ultrasonic dispersion method to disperse 18 g of graphene oxide in 900 ml of the mixed alkaline solution at room temperature to obtain a graphene oxide suspension;
[0087] Step S2: adding 900 ml of graphene oxide suspension to 50 ml of Y2O3 suspension coated with a cationic surfactant, mixing evenly by mechanical stirring, filtering and drying to obtain graphene oxide-Y2O3 composite powder;
[0088] The dried graphene oxide-Y2O3 composite powder was placed in an atmosphere of a mixture of inert gas and H2 for heat treatment at a temperature of 885°C and a pressure of 0.3 MPa for 4.5 h to obtain a reduced graphene-Y2O3 composite powder;
[0089] Step S3: weighing 1992 g of Ti-55531 titanium alloy powder with a particle size of 15-53 μm and 8 g of the reduced graphene-Y2O3 composite powder obtained in step S2, subjecting the weighed Ti-55531 titanium alloy powder and the reduced graphene-Y2O3 composite powder to low-energy spheroidal graphite, with a spheroidal graphite speed of 180 r / min, a ball-to-material ratio of 5:1, and a ball milling time of 14 h; obtaining a reduced graphene-Y2O3-high-strength titanium alloy composite powder;
[0090] Step S4: SLM printing is performed on the reduced graphene-Y2O3-high-strength titanium alloy composite powder obtained in step S3 to obtain a high-strength titanium alloy that can suppress cracks; the laser body energy density is 80J / mm3; the 3D printing parameters used are: laser power is 220W; laser scanning speed is 1000mm / s; scanning spacing is 0.1mm; interlayer thickness is 0.45mm;
[0091] The high-strength titanium alloy obtained in step S4 is heat-treated by first heating to 550°C and keeping it for 0.8h in a vacuum environment, then continuing to heat to 825°C and keeping it for 3h. Argon gas is introduced to 3 bar and quickly cooled to room temperature before being taken out. The cooling zone rate is 60°C / min.
[0092] The performance indicators of the high-strength titanium alloy finally obtained are shown in Table 1. The metallographic structure of the high-strength titanium alloy obtained is as follows: Figure 3 shown.
[0093] Comparative Example 1 (Compared with Example 2, the mass proportion of reduced graphene-Y2O3 composite powder in step S3 is too high)
[0094] Compared with Example 2, the difference is that in step S3, 1980 g of Ti-55531 titanium alloy powder with a particle size of 15-53 μm and 20 g of reduced graphene-Y2O3 composite powder obtained in step S2 are weighed.
[0095] The performance indicators of the high-strength titanium alloy finally obtained are shown in Table 1. The metallographic structure of the high-strength titanium alloy obtained is as follows: Figure 4 shown.
[0096] Comparative Example 2 (Compared with Example 2, the mass ratio of reduced graphene-Y2O3 composite powder in step S3 is too low)
[0097] Compared with Example 2, the difference is that in step S3, 1998 g of Ti-55531 titanium alloy powder with a particle size of 15-53 μm and 2 g of reduced graphene-Y2O3 composite powder obtained in step S2 are weighed.
[0098] The performance indicators of the high-strength titanium alloy finally obtained are shown in Table 1.
[0099] Comparative Example 3 (different heat treatment system in step S4 compared to Example 2 - slow cooling rate)
[0100] Compared with Example 2, the difference is that in step S4, the obtained high-strength titanium alloy is heat treated by heating to 550°C in a vacuum atmosphere and then keeping it for 3 hours, cooling it to room temperature and then taking it out, with a cooling rate of 10°C / min.
[0101] Comparative Example 4 (different heat treatment system in step S4 compared to Example 2 - fast cooling rate)
[0102] Compared with Example 2, the difference is that in step S4, the cooling rate is 120°C / min.
[0103] Comparative Example 5 (Compared with Example 2, graphene was dispersed and added to water in step S1)
[0104] Compared with Example 2, the difference is that in step S1, 6 g of graphene oxide is dispersed in 1000 mL of aqueous solution at room temperature by ultrasonic dispersion method to obtain a graphene oxide suspension.
[0105] The performance indicators of the high-strength titanium alloy finally obtained are shown in Table 1.
[0106] The performance indicators of the titanium alloys obtained in Examples 1-3 and Comparative Examples 1-3 are compared in Table 1:
[0107] Table 1
[0108]
[0109]
[0110] The high strength titanium alloys prepared in Examples 1-3 are as follows Figure 1-3 As shown, the high-strength titanium alloy has no crack and void problems, and its mechanical properties are good; the density of the melt measured in the experiment can be as high as 99.3%, and as shown in Table 1, the obtained high-strength titanium alloy has no cracks, and the density, tensile strength, yield strength, elongation and hardness are all high.
[0111] By comparing comparative examples 1-2 with embodiments 1-3, it can be seen that as the content of graphene-Y2O3 gradually increases, no cracks are generated inside the melt, and the number of pores first decreases and then increases. When the content of graphene-Y2O3 is less, the ideal gain effect cannot be achieved, but the crack situation in the melt can also be effectively improved. As the content of graphene-Y2O3 increases to a certain proportion, the heat conduction speed can be accelerated well in the molding process, and the titanium alloy has an in-situ reaction, producing a large amount of TiC nanoparticles, while Y2O3 can also be combined with the generated TiC process composite structure, increase the nucleation core, refine the grains, and the increase in grain boundaries can suppress the movement of dislocations and reduce the generation of cracks. As its content continues to increase, graphene cannot be decomposed during the molding process, and agglomeration will inevitably occur, and coarsening of larger TiC particles will occur, resulting in the degradation of the pinning effect, while a large amount of graphene-Y2O3 composite powders are not melted during the printing process, and holes and cracks are easily formed around these unmelted particles during the printing process.
[0112] By comparing Comparative Examples 3-4 with Example 2, the heat treatment temperature is low, the corresponding phase transition temperatures are not reached, only the internal stress is eliminated, and the internal structure of the material does not change, which is equivalent to the printed state in additive manufacturing. After heat treatment, the β phase in the organization is precipitated, and different phases will affect the deformation mechanism of the material, thereby improving the plasticity of the alloy to a certain extent. After the cooling rate is less than the cooling rate of the present application, the corresponding tensile strength and yield strength will decrease slightly, but the elongation decreases significantly, and the elongation is only 2%. After the cooling rate is greater than the cooling rate of the present application, the corresponding tensile strength is reduced by nearly 100MPa, but the elongation is still low.
[0113] By comparing Example 5 with Example 2, graphene does not adsorb negative ions and cannot be evenly mixed with Y2O3 coated with the anode active agent, resulting in graphene agglomeration, resulting in more cracks in the printed high-strength titanium alloy and poor mechanical properties.
[0114] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
[0115] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-strength titanium alloy capable of suppressing cracks, It is characterized in that The following steps are involved: Step S1: Y 2 O 3 The powder is dispersed in an aqueous solution containing a cationic surfactant to obtain Y coated with the cationic surfactant. 2 O 3 suspension; dispersing graphene oxide in an alkaline solution to obtain a graphene oxide suspension; Step S2: Add the graphene oxide suspension dropwise to the Y coated with the cationic surfactant. 2 O 3 The suspension was mixed evenly by mechanical stirring, filtered and dried to obtain graphene oxide-Y 2 O 3 Composite powder; The dried graphene oxide-Y 2 O 3 The composite powder is placed in an inert gas and H 2 Heat treatment in a mixed atmosphere to obtain reduced graphene-Y 2 O 3 Composite powder; Step S3: High-strength titanium alloy powder and reduced graphene-Y 2 O 3 The composite powder was subjected to low energy ball milling to obtain reduced graphene-Y 2 O 3 -High-strength titanium alloy composite powder; Step S4: Reducing the graphene-Y obtained in step S3 2 O 3 -SLM printing of high-strength titanium alloy composite powder can obtain high-strength titanium alloy with suppressed cracks.
2. The preparation method according to claim 1, It is characterized in that In step S1, graphene oxide and Y 2 O 3 The mass ratio is 1:(1-3), the cationic surfactant and Y 2 O 3 The molar ratio is (1.25-1.3):1, and the concentration of the graphene oxide suspension is 0.01-0.02 g / mL.
3. The preparation method according to claim 1, It is characterized in that In step S1, Y 2 O 3 The particle size is 40-60nm.
4. The preparation method according to claim 3, It is characterized in that In step S1, the alkaline solution is NaOH and Na 2 CO 3 A mixed alkaline solution of NaOH and Na 2 CO 3 The molar ratio is 1:(2-3), and the concentration of NaOH is 0.04-0.05 g / mL.
5. The preparation method according to claim 1, It is characterized in that In step S2, the graphene oxide suspension is reacted with the Y 2 O 3 The volume ratio of the suspension is (18-20):
1.
6. The preparation method according to claim 1, It is characterized in that In step S3, graphene-Y is reduced 2 O 3 The mass proportion of composite powder is 0.1-0.5%.
7. The preparation method according to claim 1, It is characterized in that In step S2, reduced graphene-Y is obtained 2 O 3 The specific process of composite powder is: dry graphene oxide-Y is mixed at a temperature of 850-920℃ and a pressure of 0.1-0.6Mpa. 2 O 3 The composite powder is placed in an inert gas and H 2 Heat treatment in a mixed atmosphere for 3-6 hours to obtain reduced graphene-Y 2 O 3 Composite powder, in which the inert gas and H 2 The volume ratio is 100:(1-5).
8. The preparation method according to claim 1, It is characterized in that In step S4, the laser energy density is 45-120 J / mm 3 ; The 3D printing parameters used are: laser power of 180-260W; laser scanning speed of 700-1300mm / s; scanning spacing of 0.08-0.12mm; interlayer thickness of 0.03-0.06mm.
9. The preparation method according to claim 9, It is characterized in that Also includes: Step S5: heat-treat the high-strength titanium alloy obtained in step S4 by first heating it to 500-600°C in a vacuum environment and keeping it for 0.5-1h, then continuing to heat it to 800°C-850°C and keeping it for 2-4h. Then, introduce argon gas to 2-4 bar and quickly cool it to room temperature before taking it out. The cooling zone rate is 45-80°C / min.
10. A high-strength titanium alloy that can suppress cracks. It is characterized in that Prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Titanium alloy surface multi-element laser alloyed layer and preparation method thereof
CN103966598A
Preparation method for titanium-based composite material with graphene-rare earth mixed micro-structure
CN110434347A
High-performance titanium alloy added with rare earth oxide and preparation method of high-performance titanium alloy
CN113430417A
High-performance (TiB + TiC) / Ti composite material and preparation method thereof
CN117926079A
High strength titanium alloy and its production method
JP2004107691A
Cited By
Titanium alloy plate surface microcrack inhibition method based on thickness difference
CN120330639A
Sn / Y synergistic microalloyed graphene / TC4 composite material and preparation method thereof
CN122256742A
A Sn / Y synergistic microalloyed graphene / TC4 composite material and its preparation method
CN122256742B
Graphene / TA1 composite material and preparation method thereof
CN122256743A
Y2O3 reinforced graphene / TC4 composite material as well as preparation method and application thereof