Thin film thermocouple with high temperature measurement upper limit and preparation method thereof
By depositing indium tin oxide sensitive layer and alumina zirconium oxide protective layer on ceramic plates using inkjet printing technology, the problem of ablation and volatility of thin film thermocouples at high temperatures is solved, the upper temperature measurement limit is improved to 1300°C and simplified The preparation process is suitable for high temperature measurement of complex curved surfaces.
Patent Information
- Application Number
- CN202411012531.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing thin-film thermocouples are prone to ablation and volatility in high temperature environments, resulting in a low upper temperature limit and the inability to effectively measure the temperature of high-temperature components such as aircraft engines.
Indium tin oxide and indium oxide are deposited on ceramic plates using inkjet printing technology, combined with alumina and yttrium oxide stable zirconia as protective layer, and a stable film thermocouple is formed through high-temperature sintering to improve its durability at high temperatures. sex.
It effectively improves the upper limit of the temperature measurement of film thermocouples to 1300℃, and simplifies the preparation process, achieving high-temperature temperature measurement of complex curved surfaces. It has a simple structure and good adhesion, which is suitable for multiple high-temperature cycles.
Smart Images

Figure CN118930327A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thin film thermocouples, and in particular relates to a thin film thermocouple with a high temperature measurement upper limit and a preparation method thereof. Background Art
[0002] Accurate and precise temperature measurement is the core data support for the design, life prediction, performance optimization and other aspects of advanced high-temperature mechanical components such as aircraft engines and rocket engines. However, for aircraft engines, which are high-temperature, high-pressure, and high-speed internal flow rotating machinery, the various existing temperature measurement methods such as armored thermocouple temperature measurement, temperature indicating paint temperature measurement, and radiation temperature measurement all have disadvantages to varying degrees, such as high testing costs, few experimental measurement points, high measurement difficulty, and a large impact of the temperature measurement method on the physical field. Thin-film thermocouple temperature measurement stands out with its advantages of miniaturization, non-invasiveness, high precision, and low interference. At present, most of the traditional thin-film thermocouple preparation methods at home and abroad are based on physical vapor deposition (PVD) technology, which requires high-purity target material preparation, masking, etching, and high-energy particle bombardment. The target material is evaporated and deposited on the temperature measurement target. The entire process has high process requirements, low flexibility, long time consumption, and no digital features. It is also not competent for the preparation of thin-film thermocouples on the surface of complex high-temperature components such as aircraft engine turbine blades. Ink-jet printing can make nano-particles of functional materials into nano-inks, and deposit them on the surface of the target substrate through an inkjet printing device to prepare thin-film thermocouples. The process is simple, flexible, and highly digitalized. However, when the thin-film thermocouples prepared by inkjet printing work for a long time in a high-temperature environment, the sensitive layer of the thin film will be ablated and volatilized, causing the thin-film thermocouple to fail, so that the upper limit of temperature measurement is generally around 1000°C, the upper limit of temperature measurement is low, and the high-temperature service life is short, making it difficult to achieve effective temperature measurement of high-temperature components such as aircraft engine turbine blades. Therefore, designing and inventing a thin-film thermocouple that is easy to prepare and has a high upper limit of temperature measurement is of great significance for advanced high-temperature mechanical temperature measurement. Summary of the invention
[0003] The purpose of the present invention is to provide a thin film thermocouple with a high temperature measurement upper limit and a preparation method thereof, so as to solve the problem that the sensitive layer of the thin film of the existing thin film thermocouple prepared by inkjet printing will undergo ablation and volatilization when working in a high temperature environment for a long time, resulting in failure of the thin film thermocouple, so that the temperature measurement upper limit is generally around 1000°C, the temperature measurement upper limit is low, the high temperature service life is short, and it is difficult to achieve effective temperature measurement of high temperature components such as aircraft engine turbine blades.
[0004] The technical solution adopted by the present invention to solve the technical problem is as follows:
[0005] A method for preparing a thin film thermocouple with a high temperature measuring upper limit of the present invention specifically comprises the following steps:
[0006] (1) Indium tin oxide particles and indium oxide particles with diameters of 30-50 nm are dispersed in an ink solvent to prepare a 10% sensitive layer ink by mass, and aluminum oxide and yttria-stabilized zirconium oxide with diameters of 30-50 nm are mixed and dispersed in an ink solvent at a mass ratio of 1:1 to prepare a 10% protective layer ink by mass; the sensitive layer ink and the protective layer ink are ultrasonically dispersed at a power of 180-220 W for more than 2 hours; after the ultrasonic dispersion is completed, the ink is filtered to remove impurities;
[0007] (2) Selecting an alumina ceramic flat plate as a printing substrate and pre-treating it, placing the treated printing substrate on a heating platform, raising the surface temperature of the printing substrate to 140-150°C and maintaining it constant; using an inkjet printer to deposit the sensitive layer ink on the surface of the printing substrate, with a horizontal dot spacing of 0.04-0.05 mm, a vertical dot spacing of 0.04-0.05 mm, and a printing speed of 13-17 mm / s; placing the inkjet-printed sensitive layer film in a sintering furnace, heating it from room temperature to 900°C at a heating rate of 10°C / min, and keeping it at 900°C for 30-60 minutes, and then naturally cooling it to room temperature;
[0008] (3) placing the sintered printed substrate with the sensitive layer film on a heating platform and heating it to 140-150° C. and maintaining a constant temperature; using the XYZ displacement system of the inkjet printer to locate the initial printing position of the protective layer, so that the protective layer can completely cover the initially sintered sensitive layer film, and reserve the sensitive layer wiring position; using the inkjet printer to inkjet the protective layer ink on the surface of the sensitive layer film, during the inkjet printing process, the horizontal dot spacing is set to 0.035-0.045 mm, the vertical dot spacing is set to 0.025-0.035 mm, and the printing speed is set to 13-17 mm / s;
[0009] (4) Sintering of the thin film thermocouple as a whole: The printed thin film thermocouple with protective layer is placed in a sintering furnace and heated from room temperature to 1200°C at a heating rate of 10°C / min, and kept at 1200°C for 30-60 minutes to allow the sensitive layer and protective layer to be finally sintered and stabilized. The thin film thermocouple is then naturally cooled to room temperature to obtain a thin film thermocouple.
[0010] Furthermore, the ink solvent is preferably prepared by mixing pure ethylene glycol and isopropanol in a mass ratio of 1:1.
[0011] Furthermore, the protection layer is 0.5-1.0 mm wider than the sensitive layer.
[0012] Furthermore, when pre-treating the printed substrate, the surface of the printed substrate is repeatedly rinsed with anhydrous ethanol and wiped in one direction with dust-free paper until the surface of the printed substrate is clean and free of impurities.
[0013] Furthermore, in step (1), after the ultrasonic dispersion is completed, the ink is filtered through a 0.45 μm PTFE filter membrane to further remove impurities.
[0014] The present invention also provides a high temperature measuring upper limit thin film thermocouple prepared by the above preparation method, wherein the high temperature measuring upper limit thin film thermocouple is composed of YSZ / Al arranged in sequence. 2 O 3 Protective layer, ITO / In 2 O 3 Sensitive layer and Al 2 O 3 Ceramic base composition.
[0015] The beneficial effects of the present invention are:
[0016] The present invention uses semiconductor metal oxide materials indium tin oxide (ITO) and indium oxide (In 2 O 3 ) as the sensitive material of the thin film thermocouple, the nano-scale particles of the two materials are made into ink and deposited on the surface of the ceramic plate by inkjet printing, and then initially sintered in a sintering furnace to form a relatively stable conductive circuit. 2 O 3 ) and yttria-stabilized zirconia (YSZ) particles are mixed in a mass ratio of 1:1 to prepare a protective layer ink, which is then deposited on the surface of the sintered thin film thermocouple by inkjet printing to form a protective layer, and then sintered again at a high temperature in a sintering furnace to form a stable thin film thermocouple with a protective layer.
[0017] Compared with the prior art, the present invention has the following technical effects:
[0018] 1. The present invention effectively improves the upper limit of thin film thermocouple temperature measurement. Generally, when thin film thermocouples are used in high temperature environments, phenomena such as material aggregation, ablation, and sublimation will occur, resulting in failure, making it impossible to achieve high temperature measurement. However, the present invention deposits a dense and uniform protective layer on the sensitive layer of the metal oxide semiconductor material, thereby effectively preventing the high temperature failure of the sensitive layer material, thereby raising the upper limit of thin film thermocouple temperature measurement to 1300°C, and has the potential for further improvement.
[0019] 2. The thin film thermocouple prepared by the present invention has a simple structure, is easy to prepare, has good adhesion, and can be recycled for many times. Generally, the preparation and protection of thin film thermocouples in high temperature environments require the addition of a multi-layer structure to protect the sensitive layer or to match the thermal stress between different layers in the thermal cycle to prevent the film from cracking. The present invention optimizes the inkjet printing parameters to prepare a uniform and dense sensitive layer and protective layer. Only two layers of structure are deposited on the ceramic substrate to achieve 1300°C temperature measurement, which greatly simplifies the preparation process and improves the preparation efficiency. The film has good adhesion and will not crack or fall off after multiple high-temperature thermal cycles.
[0020] 3. The thin film thermocouple prepared by the present invention can be used for temperature measurement on complex curved surfaces. Traditional thin film thermocouple preparation technologies such as magnetron sputtering cannot achieve the preparation of thin film thermocouples on complex curved surfaces due to the limitations of mask requirements and low degree of digitization. The thin film thermocouple with a high upper temperature measurement limit and its preparation method of the present invention can be adapted to inkjet printers and multi-axis displacement mechanisms, thereby achieving the preparation and temperature measurement of thin film thermocouples on complex curved surfaces such as turbine blades. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic diagram of the structure of a thin film thermocouple with a high temperature measurement upper limit prepared by the present invention.
[0022] Figure 2 This is a schematic diagram of the structure of a thin film thermocouple with a high temperature measurement upper limit prepared by the present invention.
[0023] Figure 3 The present invention provides a calibration curve for a thin-film thermocouple with a high temperature measurement upper limit. DETAILED DESCRIPTION
[0024] The invention provides a method for preparing a thin film thermocouple with a high upper temperature measuring limit, comprising the following steps: ink preparation, inkjet printing of a sensitive layer, inkjet printing of a protective layer and overall sintering of the thin film thermocouple.
[0025] The present invention provides a method for preparing a thin film thermocouple with a high temperature measuring upper limit, which specifically comprises the following steps:
[0026] (1) Ink preparation;
[0027] (1.1) Prepare ink solvent;
[0028] Pure ethylene glycol and isopropyl alcohol were selected and mixed in a mass ratio of 1:1 to prepare the ink solvent.
[0029] (1.2) Ink dispersion;
[0030] Indium tin oxide (ITO) particles and indium oxide (In 2 O 3 ) particles were dispersed in the ink solvent, and a 10% mass fraction of sensitive layer ink was initially prepared. Aluminum oxide (Al 2 O 3 ) and yttria-stabilized zirconia (YSZ) are mixed and dispersed in the ink solvent in a mass ratio of 1:1 to initially prepare a protective layer ink with a mass fraction of 10%; the sensitive layer ink and the protective layer ink are ultrasonically dispersed at a power of 180-220W for more than 2h.
[0031] (1.3) Ink filtration;
[0032] After ultrasonic dispersion is completed, the ink is filtered through a 0.45μm PTFE filter membrane to further remove impurities to prevent them from affecting the quality of inkjet printing.
[0033] (2) Inkjet printing of sensitive layer;
[0034] (2.1) Printing substrate processing;
[0035] An alumina ceramic flat plate was selected as the printing substrate. The surface of the printing substrate was repeatedly rinsed with anhydrous ethanol and wiped in one direction with dust-free paper until the surface of the printing substrate was clean and free of impurities.
[0036] (2.2) Inkjet printing;
[0037] Place the processed printing substrate on a heating platform to raise the surface temperature of the printing substrate to 140-150°C and maintain it constant; use an inkjet printer to deposit the sensitive layer ink on the surface of the printing substrate. During the inkjet printing process, set the horizontal dot spacing to 0.04-0.05mm, the vertical dot spacing to 0.04-0.05mm, and the printing speed to 13-17mm / s.
[0038] (2.3) Sintering treatment;
[0039] The inkjet printed sensitive layer film is placed in a sintering furnace and heated from room temperature to 900°C at a rate of 10°C / min, then kept at 900°C for 30-60 minutes, and then naturally cooled to room temperature. The initially sintered sensitive layer can effectively prevent the subsequent protective layer inkjet printing from wetting the deposited sensitive layer circuit and causing local mixing of particles, thereby effectively ensuring the excellent and stable thermoelectric characteristics of the sensitive layer circuit.
[0040] (3) Inkjet printing of protective layer;
[0041] (3.1) Substrate positioning;
[0042] Place the sintered printed substrate with the sensitive layer film on a heating platform and heat it to 140-150°C and maintain a constant temperature; use the inkjet printer's XYZ displacement system to locate the initial printing position of the protective layer so that the protective layer can completely cover the initially sintered sensitive layer film and reserve the sensitive layer wiring position.
[0043] (3.2) Inkjet printing;
[0044] The protective layer ink is printed on the surface of the sensitive layer film by an inkjet printer. To ensure that the sensitive layer circuit is completely covered, the protective layer can be 0.5-1mm wider than the sensitive layer. During the inkjet printing process, the horizontal dot spacing is set to 0.035-0.045mm, the vertical dot spacing is set to 0.025-0.035mm, and the printing speed is 13-17mm / s.
[0045] (4) Integral sintering of thin film thermocouple;
[0046] The printed thin-film thermocouple with protective layer is placed in a sintering furnace and heated from room temperature to 1200°C at a heating rate of 10°C / min, and kept at 1200°C for 30-60 minutes to allow the sensitive layer and protective layer films to be finally sintered and stabilized, and then naturally cooled to room temperature to obtain a thin-film thermocouple.
[0047] The present invention also provides a high temperature upper limit thin film thermocouple prepared by the above preparation method, wherein the high temperature upper limit thin film thermocouple is mainly composed of YSZ / Al 2 O 3 Protective layer, ITO / In 2 O 3 Sensitive layer, Al 2 O 3 Ceramic substrate composition, among which YSZ / Al 2 O 3 Protective layer, ITO / In 2 O 3 Sensitive layer and Al 2 O 3 The ceramic substrate is arranged from top to bottom, such as Figure 1 and Figure 2 shown.
[0048] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0049] Example 1
[0050] The preparation method of a thin film thermocouple with a high temperature measuring upper limit of this embodiment has the following specific preparation steps:
[0051] (1) Pure ethylene glycol and isopropanol are mixed in a mass ratio of 1:1 to prepare an ink solvent; indium tin oxide particles and indium oxide particles with a diameter of 40 nm are respectively dispersed in the ink solvent to preliminarily prepare a sensitive layer ink with a mass fraction of 10%, and aluminum oxide and yttria-stabilized zirconium oxide with a diameter of 40 nm are mixed and dispersed in the ink solvent in a mass ratio of 1:1 to preliminarily prepare a protective layer ink with a mass fraction of 10%; the sensitive layer ink and the protective layer ink are respectively ultrasonically dispersed at a power of 200 W for more than 2 hours; after the ultrasonic dispersion is completed, the ink is filtered through a 0.45 μm PTFE filter membrane to further filter out impurities to prevent the quality of inkjet printing from being affected;
[0052] (2) An alumina ceramic plate was selected as a printing substrate, and the surface of the printing substrate was repeatedly rinsed with anhydrous ethanol and wiped in a single direction with dust-free paper until the surface of the printing substrate was clean and free of impurities; the treated printing substrate was placed on a heating platform, and the surface temperature of the printing substrate was raised to 145°C and maintained constant; the sensitive layer ink was deposited on the surface of the printing substrate by inkjet printing with an inkjet printer, with a horizontal dot spacing of 0.045 mm, a vertical dot spacing of 0.045 mm, and a printing speed of 15 mm / s; the sensitive layer film after inkjet printing was placed in a sintering furnace and heated from room temperature to 900°C at a heating rate of 10°C / min, and kept at 900°C for 45 minutes, and then naturally cooled to room temperature;
[0053] (3) placing the sintered printed substrate with the sensitive layer film on a heating platform and heating it to 140-150° C. and maintaining a constant temperature; using the XYZ displacement system of the inkjet printer to locate the initial printing position of the protective layer, so that the protective layer can completely cover the initially sintered sensitive layer film, and reserve the sensitive layer wiring position; using the inkjet printer to inkjet the protective layer ink on the surface of the sensitive layer film, to ensure that the sensitive layer circuit is completely covered, the protective layer can be 0.75 mm wider than the sensitive layer; during the inkjet printing process, the horizontal dot spacing is set to 0.04 mm, the vertical dot spacing is set to 0.03 mm, and the printing speed is 15 mm / s;
[0054] (4) Overall sintering of thin film thermocouple: The printed thin film thermocouple with protective layer is placed in a sintering furnace and heated from room temperature to 1200°C at a heating rate of 10°C / min, and kept at 1200°C for 45 minutes to allow the sensitive layer and protective layer to be sintered and stabilized. The thin film thermocouple is then naturally cooled to room temperature to obtain a thin film thermocouple.
[0055] Example 2
[0056] The preparation method of a thin film thermocouple with a high temperature measuring upper limit of this embodiment has the following specific preparation steps:
[0057] (1) Pure ethylene glycol and isopropanol are mixed in a mass ratio of 1:1 to prepare an ink solvent; indium tin oxide particles and indium oxide particles with a diameter of 30 nm are respectively dispersed in the ink solvent to preliminarily prepare a sensitive layer ink with a mass fraction of 10%, and aluminum oxide and yttria-stabilized zirconium oxide with a diameter of 30 nm are mixed and dispersed in the ink solvent in a mass ratio of 1:1 to preliminarily prepare a protective layer ink with a mass fraction of 10%; the sensitive layer ink and the protective layer ink are respectively ultrasonically dispersed at a power of 180 W for more than 2 hours; after the ultrasonic dispersion is completed, the ink is filtered through a 0.45 μm PTFE filter membrane to further filter out impurities to prevent them from affecting the inkjet printing quality;
[0058] (2) An alumina ceramic flat plate was selected as the printing substrate. The surface of the printing substrate was repeatedly rinsed with anhydrous ethanol and wiped in one direction with dust-free paper until the surface of the printing substrate was clean and free of impurities. The treated printing substrate was placed on a heating platform, and the surface temperature of the printing substrate was raised to 140°C and maintained constant. The sensitive layer ink was deposited on the surface of the printing substrate by inkjet printing with an inkjet printer, with a horizontal dot spacing of 0.04 mm, a vertical dot spacing of 0.04 mm, and a printing speed of 13 mm / s. The sensitive layer film after inkjet printing was placed in a sintering furnace and heated from room temperature to 900°C at a heating rate of 10°C / min, and kept at 900°C for 30 minutes, and then naturally cooled to room temperature.
[0059] (3) placing the sintered printed substrate with the sensitive layer film on a heating platform and heating it to 140° C. and maintaining a constant temperature; using the XYZ displacement system of the inkjet printer to locate the initial printing position of the protective layer, so that the protective layer can completely cover the initially sintered sensitive layer film, and reserve the wiring position of the sensitive layer; using the inkjet printer to inkjet the protective layer ink on the surface of the sensitive layer film, to ensure that the sensitive layer circuit is completely covered, the protective layer can be 0.5 mm wider than the sensitive layer; during the inkjet printing process, the horizontal dot spacing is set to 0.035 mm, the vertical dot spacing is set to 0.025 mm, and the printing speed is 13 mm / s;
[0060] (4) Overall sintering of thin film thermocouple: The printed thin film thermocouple with protective layer is placed in a sintering furnace and heated from room temperature to 1200°C at a heating rate of 10°C / min, and kept at 1200°C for 30 minutes to allow the sensitive layer and protective layer to be sintered and stabilized. The thin film thermocouple is then naturally cooled to room temperature to obtain a thin film thermocouple.
[0061] Example 3
[0062] The preparation method of a thin film thermocouple with a high temperature measuring upper limit of this embodiment has the following specific preparation steps:
[0063] (1) Pure ethylene glycol and isopropanol are mixed in a mass ratio of 1:1 to prepare an ink solvent; indium tin oxide particles and indium oxide particles with a diameter of 50 nm are dispersed in the ink solvent to prepare a preliminary sensitive layer ink with a mass fraction of 10%, and aluminum oxide and yttria-stabilized zirconium oxide with a diameter of 50 nm are mixed and dispersed in the ink solvent in a mass ratio of 1:1 to prepare a preliminary protective layer ink with a mass fraction of 10%; the sensitive layer ink and the protective layer ink are ultrasonically dispersed at a power of 220 W for more than 2 hours; after the ultrasonic dispersion is completed, the ink is filtered through a 0.45 μm PTFE filter membrane to further filter out impurities to prevent them from affecting the inkjet printing quality;
[0064] (2) An alumina ceramic plate was selected as a printing substrate, and the surface of the printing substrate was repeatedly rinsed with anhydrous ethanol and wiped in a single direction with dust-free paper until the surface of the printing substrate was clean and free of impurities; the treated printing substrate was placed on a heating platform, and the surface temperature of the printing substrate was raised to 150°C and maintained constant; the sensitive layer ink was deposited on the surface of the printing substrate by inkjet printing with an inkjet printer, with a horizontal dot spacing of 0.05 mm, a vertical dot spacing of 0.05 mm, and a printing speed of 17 mm / s; the inkjet-printed sensitive layer film was placed in a sintering furnace and heated from room temperature to 900°C at a heating rate of 10°C / min, and kept at 900°C for 60 min, and then naturally cooled to room temperature;
[0065] (3) placing the sintered printed substrate with the sensitive layer film on a heating platform and heating it to 150° C. and maintaining a constant temperature; using the XYZ displacement system of the inkjet printer to locate the initial printing position of the protective layer, so that the protective layer can completely cover the initially sintered sensitive layer film, and reserve the sensitive layer wiring position; using the inkjet printer to inkjet the protective layer ink on the surface of the sensitive layer film. To ensure that the sensitive layer circuit is completely covered, the protective layer can be 1 mm wider than the sensitive layer; during the inkjet printing process, the horizontal dot spacing is set to 0.045 mm, the vertical dot spacing is set to 0.035 mm, and the printing speed is 17 mm / s;
[0066] (4) Overall sintering of thin film thermocouple: The printed thin film thermocouple with protective layer is placed in a sintering furnace and heated from room temperature to 1200°C at a heating rate of 10°C / min, and kept at 1200°C for 60 min to allow the sensitive layer and protective layer to be sintered and stabilized. The thin film thermocouple is then naturally cooled to room temperature to obtain a thin film thermocouple.
[0067] The present invention compares the output thermoelectric potential of a thermocouple with a protective layer and a thermocouple without a protective layer as the temperature changes. Figure 3As shown, when the temperature is 100℃-1000℃, as the temperature gradually increases, the output thermoelectric potential also gradually increases. When the temperature is 1013℃, the thermocouple without a protective layer fails, while the thermocouple with a protective layer does not fail and continues to work. The present invention deposits a dense and uniform protective layer on the sensitive layer of the metal oxide semiconductor material, thereby effectively preventing the high-temperature failure of the sensitive layer material, and raising the upper limit of the temperature measurement of the thin film thermocouple to 1300℃, and has the potential for further improvement.
[0068] The core idea of the present invention is to prepare a thin film thermocouple with a protective layer on a ceramic plate by inkjet printing. Semiconductor metal oxides as electrode materials of the sensitive layer of thin film thermocouples are relatively stable and have good high temperature resistance under high temperature environments. At the same time, inkjet printing on the surface of the sensitive layer of the thin film thermocouple to prepare a dense protective layer can effectively prevent high temperature ablation and volatilization of the sensitive layer material, thereby effectively improving the upper limit of the temperature measurement of the thin film thermocouple.
[0069] The present invention discloses a thin film thermocouple with a high upper temperature limit and a method for preparing the same. Those skilled in the art can refer to the contents of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in the present invention. The products of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the products described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
Claims
1. A method for preparing a thin film thermocouple with a high upper temperature limit, characterized in that: The following steps are involved: (1) Indium tin oxide particles and indium oxide particles with diameters of 30-50 nm are dispersed in an ink solvent to prepare a 10% sensitive layer ink by mass, and aluminum oxide and yttria-stabilized zirconium oxide with diameters of 30-50 nm are mixed and dispersed in an ink solvent at a mass ratio of 1:1 to prepare a 10% protective layer ink by mass; the sensitive layer ink and the protective layer ink are ultrasonically dispersed at a power of 180-220 W for more than 2 hours; after the ultrasonic dispersion is completed, the ink is filtered to remove impurities; (2) Selecting an alumina ceramic flat plate as a printing substrate and pre-treating it, placing the treated printing substrate on a heating platform, raising the surface temperature of the printing substrate to 140-150°C and maintaining it constant; using an inkjet printer to deposit the sensitive layer ink on the surface of the printing substrate, with a horizontal dot spacing of 0.04-0.05 mm, a vertical dot spacing of 0.04-0.05 mm, and a printing speed of 13-17 mm / s; placing the inkjet-printed sensitive layer film in a sintering furnace, heating it from room temperature to 900°C at a heating rate of 10°C / min, and keeping it at 900°C for 30-60 minutes, and then naturally cooling it to room temperature; (3) placing the sintered printed substrate with the sensitive layer film on a heating platform and heating it to 140-150° C. and maintaining a constant temperature; using the XYZ displacement system of the inkjet printer to locate the initial printing position of the protective layer, so that the protective layer can completely cover the initially sintered sensitive layer film, and reserve the sensitive layer wiring position; using the inkjet printer to inkjet the protective layer ink on the surface of the sensitive layer film, during the inkjet printing process, the horizontal dot spacing is set to 0.035-0.045 mm, the vertical dot spacing is set to 0.025-0.035 mm, and the printing speed is set to 13-17 mm / s; (4) Sintering of the thin film thermocouple as a whole: The printed thin film thermocouple with protective layer is placed in a sintering furnace and heated from room temperature to 1200°C at a heating rate of 10°C / min, and kept at 1200°C for 30-60 minutes to allow the sensitive layer and protective layer to be finally sintered and stabilized. The thin film thermocouple is then naturally cooled to room temperature to obtain a thin film thermocouple.
2. The method for preparing a thin film thermocouple with a high upper temperature limit according to claim 1, characterized in that: The ink solvent is prepared by mixing pure ethylene glycol and isopropyl alcohol in a mass ratio of 1:
1.
3. The method for preparing a thin film thermocouple with a high upper temperature limit according to claim 1, characterized in that: The protection layer is 0.5-1.0 mm wider than the sensitive layer.
4. The method for preparing a thin film thermocouple with a high upper temperature limit according to claim 1, characterized in that: When pre-treating the printed substrate, the printed substrate surface is repeatedly rinsed with anhydrous ethanol and wiped in one direction with dust-free paper until the printed substrate surface is clean and free of impurities.
5. The method for preparing a thin film thermocouple with a high upper temperature limit according to claim 1, characterized in that: In step (1), after the ultrasonic dispersion is completed, the ink is filtered through a 0.45 μm PTFE filter membrane to further remove impurities.
6. A thin film thermocouple with a high upper temperature limit prepared by the preparation method according to any one of claims 1 to 5, characterized in that: The high temperature measuring upper limit thin film thermocouple is composed of a YSZ / Al2O3 protective layer, an ITO / In2O3 sensitive layer and an Al2O3 ceramic substrate which are arranged in sequence.
Citation Information
Cited By
High-temperature co-sintered multilayer special-shaped ceramic high-temperature sensor and preparation method thereof
CN120213091A