Low-cost high-toughness super-thick acid-resistant pipeline hot-rolled coil plate and production method thereof

Through low C, low Mn, low Nb composite microalloyation and low pressure ultrafast cooling + laminar flow cooling processes, X42MS hot rolled coils with a thickness of 20mm to 25mm were prepared, solving the problems of high cost and insufficient acid resistance in the prior art. , achieves ultra-thick acid-resistant pipeline steel with low cost, high strength and excellent acid-resistant corrosion resistance, meeting the needs of long-distance oil and gas pipelines.

CN119040747APending Publication Date: 2024-11-29HBIS LAOTING STEEL CO LTD +2

Patent Information

Application Number
CN202411240700.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-26
Filing Date
2024-09-05
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, low-cost, high-strength and toughness, ultra-thick acid-resistant pipeline steel has a high production cost, and its anti-HIC and SSC performance is insufficient in acidic environments, making it difficult to meet the needs of long-distance and high-pressure oil and gas pipelines.

Method used

Using low C, low Mn and low Nb composite microalloy design, combined with low pressure ultra-fast cooling + laminar flow cooling technology, X42MS hot rolled coil with a thickness of 20mm to 25mm is prepared, with chemical compositions of C: 0.030 to 0.060%, Mn: 0.80~1.10%, Si: 0.07~0.25%, S≤0.0015%, P≤0.0012%, Ti: 0.015~0.030%, Cr, Cu, Ni, Mo and other precious alloy elements are not added, and smelted through decarbonization converter, LF +RH refining, continuous casting, casting billet heating and controlled rolling processes to achieve ultrafast cooling and laminar flow cooling.

Benefits of technology

Ultra-thick acid-resistant pipeline steel with low cost, high strength, high toughness and excellent acid-resistant corrosion resistance are achieved, meeting the use requirements in high strength, low temperature and acid environments, and has significant economic and social benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a low-cost high-toughness super-thick acid-resistant pipeline hot-rolled coil plate and a production method thereof. The hot-rolled coil plate comprises the following chemical components in percentage by mass: 0.030-0.060% of C, 0.80-1.10% of Mn, 0.07-0.25% of Si, less than or equal to 0.0015% of S, less than or equal to 0.0012% of P, 0.015-0.030% of Ti, 0.020-0.030% of Nb, less than or equal to 0.0001% of H and the balance of Fe and inevitable impurities. The production method comprises the working procedures of converter treatment, LF refining, RH refining, slab continuous casting, hot continuous rolling, controlled cooling and controlled coiling. The low-C, low-Mn and low-Nb composite microalloying component design is utilized, the low heating temperature is adopted, and the reasonable low-pressure ultra-fast cooling and layer cooling process is matched, so that the material performance and the HIC and SSCC resistance of the ultra-thick hot-rolled coil plate are guaranteed, and the material cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of vanadium chemical metallurgy, and specifically relates to a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil and a production method thereof. Background Art

[0002] With the rapid growth of energy demand, the scope of oil and gas resource exploitation is constantly expanding. More and more oil and gas wells are distributed in harsh environments such as frozen soil, seismic zones, deserts and deep seas, which puts forward higher requirements on the comprehensive mechanical properties of pipeline steel. Long-distance, high-pressure oil and gas pipelines require pipeline steel to have high strength, excellent welding performance and corrosion resistance under service conditions. With the advancement of technology, although oil and natural gas must be processed before pipeline transportation, acidic substances such as H2S and CO2 are still inevitable. Corrosion damage caused by H2S is one of the main forms of pipeline corrosion damage. For the transportation of oil and natural gas media containing H2S, pipeline steel is required to have resistance to HIC (hydrogen-induced cracking) and SSC (sulfide stress cracking) to ensure the safety of pipeline steel products serving in acidic environments.

[0003] The acid-resistant pipelines in Southeast Asia and the Middle East are generally X42MS to X65MS grades, and the hot-rolled steel strip X42MS with ultra-thick specifications of 20 to 25 mm for small diameter pipes is currently the most widely used. In the existing technology, the high toughness requirements of pipeline steel are mainly met by adopting low C, low S and P, using Nb, V, Ti micro-alloying, and adding Cr, Cu, Ni, Mo and other alloying elements to make it have excellent acid corrosion resistance. Ni, Cu, Mo and other precious alloying elements are expensive; generally, metal manganese is used to ensure low carbon content alloying; in order to fully refine the grains, a high Nb content is added.

[0004] The patent application with publication number CN102021476A discloses "A low-cost acid-resistant pipeline steel hot-rolled coil and its manufacturing method", whose chemical composition and main process are: C: 0.04-0.10%, Si: 0.05-0.50%, Mn: 1.00-1.70%, P≤0.015%, S≤0.002%, Nb≤0.08%, Ti: 0.005-0.030%, Als: 0.010-0.050%, Ca: 0.0010-0.0040%, N≤0.0060%, H≤0.0002%, O≤0.0010%, no precious alloy elements such as Cu, Ni, Mo are added, the final cooling temperature is 550-700℃, but the final specification of the finished steel coil is 12.5mm, and the 7.0mm specification Rt0.5≤302MPa, Rm:415MPa, which is as low as the lower limit of X42MS. Considering the Bauschinger effect, there is a risk of unqualified performance after pipe making.

[0005] The patent with the publication number CN104099522B discloses a method for manufacturing copper-nickel-free acid-resistant pipeline steel X52MS and its hot-rolled coil, the chemical composition of which is mainly C: 0.02-0.06%, Si: 0.05-0.35%, Mn: 1.0-1.4%, P≤0.018%, S≤0.003%, Cr: 0.10-0.50%, Ti: 0.005-0.10%, Nb: 0.005-0.10%, V: 0-0.05%. The controlled cooling step adopts slow cooling measures such as sparse cooling or air cooling. The lowest coiling temperature of the finished steel coil in the embodiment is 577°C, and the final microstructure is polygonal ferrite and pearlite, while the brittle pearlite is easy to induce HIC cracking resistance, which has a potential adverse effect on acid resistance, and the addition of Cr element also increases part of the cost.

[0006] The invention patent with publication number CN108893678A discloses "An Acid-Resistant Pipeline Steel and Rolling Method", whose chemical composition is C: 0.014-0.024%, Si: 0.10-0.35%, Mn: 0.60-0.80%, Nb: 0.030-0.070%, Ti: 0.006-0.020%, Cr: 1.00-1.10%, Ni: 0.10-0.30%, Mo: 0.15-0.20%, Cu: 0.10-0.30%, V: 0.010%, Al: 0.015-0.050%, and the balance is Fe and impurities. The C content of this patent is too low, and the smelting production is extremely difficult. Cr, Cu, Ni, Mo, etc. are precious alloys and the addition amount is large, the alloy cost is too high, and the low-temperature (350-400℃) coiling process is adopted, which makes production control difficult.

[0007] The invention patent application with publication number CN111607739A discloses "A low-cost HIC-resistant and SSC-resistant excellent performance pipeline steel and its manufacturing method", whose chemical composition and mass percentage are C: 0.03-0.06%, Si: 0.10-0.35%, Mn: 0.60-0.95%, Nb: 0.025-0.060%, Ti: 0.006-0.030%, Cr: 0.15-0.45%, Al: 0.020-0.060%, P≤0.015%, S≤0.0020%, O≤0.0030%, H≤0.0002%, and the remainder is Fe and impurities. The final cooling temperature is controlled at 450℃~500℃, which meets the performance requirements of 5.0-16mm, -20℃ low-temperature acidic working conditions pipeline steel. The thickness is thin, and the Cr element is added, so the cost is relatively high.

[0008] The invention patent application with publication number CN110846565A discloses "Low-cost, large-wall, acid-resistant pipeline steel with stable structure and performance and production method thereof", C: 0.03%~0.08%, Si: 0.15%~0.20%, Mn: 1.05%~1.15%, P≤0.01%, S≤0.002%, Nb: 0.025%~0.035%, Ti: 0.015%~0.025%, Al≤0.05%, Ca≤0.006%, and the rest are Fe and inevitable trace impurities. The Nb content is relatively high, and the cost is relatively high. Ordinary layer cooling is adopted to meet the requirements of acid-resistant pipelines below 19mm. Summary of the invention

[0009] In view of the deficiencies in the prior art, the present invention provides a low-cost, high-strength and toughness, ultra-thick acid-resistant pipeline X42MS hot-rolled coil and a preparation method, which ensures the performance requirements of 20mm to 25mm thick specification X42MS on the basis of significantly reducing production costs.

[0010] To solve the above technical problems, the technical solution adopted by the present invention is: a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil, the chemical composition of the hot-rolled coil and its mass percentage are: C: 0.030-0.060%, Mn: 0.80-1.10%, Si: 0.07-0.25%, S≤0.0015%, P≤0.0012%, Ti: 0.015-0.030%, Nb: 0.020-0.030%, H≤0.0001%, and the rest are Fe and unavoidable impurities.

[0011] The hot-rolled coil of the present invention has a yield strength of 382-432 MPa, a tensile strength of 481-526 MPa, a yield strength ratio of ≤0.90, a low-temperature Charpy impact energy of -60°C ≥300 J, a drop hammer shear area of ​​-40°C ≥85%, a thickness of 20-25 mm, ABCD four types of non-metallic inclusions ≤1.0, HIC performance: CLR≤0.5%, CTR≤0.5%, CSR≤1%, SSC performance: no cracks.

[0012] Another object of the present invention is to provide a production method for the above-mentioned low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil, the production method comprising smelting the raw materials through a decarburization converter, LF+RH refining, continuous casting, heating of the ingot, controlled rolling, ultra-fast cooling + laminar cooling, and coiling to finally produce the hot-rolled coil; the low-pressure ultra-fast cooling + laminar cooling process has a cooling rate of 15 to 26°C / s, and the coiling is performed after cooling to 460 to 520°C.

[0013] The raw materials of the present invention are treated by KR desulfurization to ensure that the S content of molten iron is ≤0.0050%.

[0014] The converter smelting process of the present invention adopts bottom blowing of argon throughout the whole process, and the final C content is ≤0.030%. The converter alloying sequence is aluminum block, metallic manganese, ferrosilicon, and ferroniobium.

[0015] In the LF+RH refining process of the present invention, high carbon ferromanganese and medium carbon ferromanganese are used to supplement manganese in LF refining, and carbon powder is used to supplement carbon when the carbon content of the converter is insufficient.

[0016] In the LF+RH refining process of the present invention, the RH refining vacuum degree is required to be ≤200Pa for ≥20 minutes, and the vacuum degree is required to be ≤100Pa for ≥15 minutes.

[0017] The continuous casting process of the present invention comprises full protection casting, a casting speed of 0.9-1.5 m / min, and a superheat of 15-30°C.

[0018] In the casting billet heating process of the present invention, the casting billet heating temperature is 1160-1200° C., the furnace discharge temperature is 1130-1170° C., and the furnace residence time is controlled to be 180-300 minutes.

[0019] The controlled rolling process of the present invention adopts fixed width, rough rolling and finishing rolling, the fixed width of the fixed width press is 50-150mm, the rough rolling adopts the 1+5 mode, the intermediate billet is 50-60mm, the steel is swung before finishing rolling, the finishing rolling inlet temperature is controlled at 940-990°C, the final rolling temperature is 850-890°C, the rolling speed is 2.8-3.2m / s, and the final reduction rate is ≥12%.

[0020] The beneficial effects of the above technical solution are as follows: 1. The present invention adopts a low-cost component design of low C, low Mn, low Nb composite microalloying and no increase in Cr, Cu, Ni, and Mo. Under the premise of ensuring sufficient solid solution of the alloy elements, a low heating temperature is adopted and a reasonable low-pressure ultra-fast cooling + layer cooling process is combined to obtain a uniform and fine grain structure. The hot-rolled coil produced achieves excellent acid and corrosion resistance on the basis of meeting the requirements of high strength, high toughness, and ultra-thickness, has broad prospects for promotion and application, and can produce significant economic and social benefits. 2. The present invention realizes the production of high-strength and ultra-thick acid-resistant pipeline steel X42MS hot-rolled coil under a low-cost component system, with no banded structure, four types of non-metallic inclusions ≤1.0, yield strength 382-432MPa, tensile strength 481-526MPa, yield strength ratio ≤0.90, -60℃ low-temperature Charpy impact energy ≥300J, -40℃ drop hammer shear area ≥85%, and HIC performance: CLR ≤0.5%, CTR ≤0.5%, CSR ≤1%, SSC performance: no cracks. It meets the use requirements under harsh service conditions such as low temperature and acidity. DETAILED DESCRIPTION

[0021] The present invention will be further described in detail below in conjunction with specific embodiments.

[0022] A low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil, the chemical composition and mass percentage of the hot-rolled coil are: C: 0.030-0.060%, Mn: 0.80-1.10%, Si: 0.07-0.25%, S≤0.0015%, P≤0.0012%, Ti: 0.015-0.030%, Nb: 0.020-0.030%, H≤0.0001%, and the rest are Fe and unavoidable impurities.

[0023] The yield strength of hot-rolled coil is 382~432MPa, the tensile strength is 481~526MPa, the yield strength ratio is ≤0.90, the low-temperature Charpy impact energy at -60℃ is ≥300J, the drop hammer shear area at -40℃ is ≥85%, and the thickness is 20~25mm.

[0024] A method for producing low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coils, the production method comprising: smelting the raw materials through a decarburization converter, LF+RH refining, continuous casting, heating the ingot, controlled rolling, ultra-fast cooling+laminar cooling, and coiling to finally produce the hot-rolled coils. The specific control process is as follows: Example 1

[0025] A production method for a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil, the production method comprising: smelting raw materials through a decarburization converter, LF+RH refining, continuous casting, heating of ingots, controlled rolling, ultra-fast cooling+laminar cooling, and coiling to finally obtain a hot-rolled coil X42MS, the thickness of the hot-rolled coil is 25.0 mm, the chemical composition and mass percentage thereof are shown in Table 1, the properties of the hot-rolled coil are shown in Table 2, the inclusion results are shown in Table 3, the HIC resistance properties are shown in Table 4, and the SSCC resistance properties are shown in Table 5.

[0026] The specific control process is as follows: 1) Converter smelting: KR desulfurization treatment is used to ensure that the sulfur content of molten iron is 0.0020%; The whole process adopts bottom blowing of argon, the final C content is 0.028%, the alloying sequence of converter is aluminum block → metallic manganese → ferrosilicon → ferroniobium, metallic manganese is matched with manganese, and the manganese content of the big bag is 0.88%.

[0027] 2) LF+RH refining: LF refining uses high carbon ferromanganese and medium carbon ferromanganese to supplement manganese. The amount of high carbon ferromanganese added is 300kg, and the amount of medium carbon ferromanganese is 180kg. The Mn content at the end of LF is 0.98%; the RH refining vacuum degree requirement is ≤200Pa for 22 minutes, and the vacuum degree requirement is ≤100Pa for 16 minutes.

[0028] 3) Continuous casting with full protection, casting speed 1.2m / min, superheat 19~22℃, and billet thickness 230mm.

[0029] 4) Ingot heating: temperature is 1165-1182℃, furnace outlet temperature is 1161℃, and furnace residence time is controlled at 193min.

[0030] 5) Controlled rolling: fixed width, rough rolling and finishing rolling are adopted. The fixed width of the fixed width press is 100mm. The rough rolling adopts the 1+5 mode, the intermediate billet is 60mm, the steel is swung before finishing rolling, the finishing rolling inlet temperature is controlled at 960℃, the final rolling temperature is 850℃, the rolling speed is 2.9m / s, and the final reduction rate is 13%.

[0031] 6) Low-pressure ultra-fast cooling + laminar cooling: The total valve opening ratio of the low-pressure ultra-fast cooling mode is 66.7%, the cooling rate is 19°C / s, and it is cooled to 460°C for coiling. Example 2

[0032] A production method for a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil, the production method comprising: smelting raw materials through a decarburization converter, LF+RH refining, continuous casting, heating of ingots, controlled rolling, ultra-fast cooling+laminar cooling, and coiling to finally obtain a hot-rolled coil X42MS, the thickness of the hot-rolled coil is 20.0 mm, the chemical composition and mass percentage thereof are shown in Table 1, the properties of the hot-rolled coil are shown in Table 2, the inclusion results are shown in Table 3, the HIC resistance properties are shown in Table 4, and the SSCC resistance properties are shown in Table 5.

[0033] The specific control process is as follows: 1) Converter smelting: KR desulfurization treatment is used to ensure that the sulfur content of molten iron is 0.0030%; The process uses bottom blowing of argon throughout, the final C content is 0.021%, and the order of converter alloying is aluminum block → metallic manganese → ferrosilicon → ferroniobium.

[0034] 2) LF+RH refining: LF refining uses high carbon ferromanganese and medium carbon ferromanganese to supplement manganese, and carbon powder to supplement carbon. The amount of high carbon ferromanganese added is 306kg, medium carbon ferromanganese is 185kg, and carbon powder is 50kg. The Mn content at the end of LF is 0.97%; the RH refining vacuum degree requirement is ≤200Pa for 21 minutes, and the vacuum degree requirement is ≤100Pa for 16 minutes.

[0035] 3) Continuous casting with full protection, casting speed 1.4m / min, superheat 18~20℃, and billet thickness 230mm.

[0036] 4) Ingot heating: temperature is 1170~1192℃, furnace outlet temperature is 1165℃, and furnace dwelling time is controlled at 191min.

[0037] 5) Controlled rolling: fixed width, rough rolling and finishing rolling are adopted. The fixed width of the fixed width press is 100mm. The rough rolling adopts the 1+5 mode, the intermediate billet is 58mm, the steel is swung before finishing rolling, the finishing rolling inlet temperature is controlled at 980℃, the final rolling temperature is 870℃, the rolling speed is 3.2m / s, and the final reduction rate is 13%.

[0038] 6) Low-pressure ultra-fast cooling + laminar cooling: The total valve opening ratio of the low-pressure ultra-fast cooling mode is 66.7%, the cooling rate is 23℃ / s, and it is cooled to 500℃ for coiling. Example 3

[0039] A production method for a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil, the production method comprising: smelting raw materials through a decarburization converter, LF+RH refining, continuous casting, heating of ingots, controlled rolling, ultra-fast cooling+laminar cooling, and coiling to finally obtain a hot-rolled coil X42MS, the thickness of the hot-rolled coil is 22.0 mm, the chemical composition and mass percentage thereof are shown in Table 1, the properties of the hot-rolled coil are shown in Table 2, the inclusion results are shown in Table 3, the HIC resistance properties are shown in Table 4, and the SSCC resistance properties are shown in Table 5.

[0040] The specific control process is as follows: 1) Converter smelting: KR desulfurization treatment is used to ensure that the sulfur content of molten iron is 0.0050%; The whole process adopts bottom blowing of argon, the final C content is 0.019%, the alloying sequence of converter is aluminum block → metallic manganese → ferrosilicon → ferroniobium, metallic manganese is matched with manganese, and the manganese content of the big bag is 0.80%.

[0041] 2) LF+RH refining: LF refining uses high carbon ferromanganese and medium carbon ferromanganese to supplement manganese, and carbon powder to supplement carbon. The amount of high carbon ferromanganese added is 312kg, medium carbon ferromanganese is 190kg, and carbon powder is 70kg. The Mn content at the end of LF is 0.90%; the RH refining vacuum degree requires ≤200Pa for 20 minutes, and the vacuum degree requires ≤100Pa for 15 minutes.

[0042] 3) Continuous casting with full protection, casting speed 1.0m / min, superheat 20-23℃, and billet thickness 230mm.

[0043] 4) Ingot heating: temperature is 1171~1200℃, furnace discharge temperature is 1170℃, and furnace residence time is controlled at 202min.

[0044] 5) Controlled rolling: fixed width, rough rolling and finishing rolling are adopted, the fixed width of the fixed width press is 50mm, the rough rolling adopts the 1+5 mode, the intermediate billet is 58mm, the steel is swung before finishing rolling, the finishing rolling inlet temperature is controlled at 985℃, the final rolling temperature is 860℃, the rolling speed is 3.0m / s, and the final reduction rate is 13%.

[0045] 6) Low-pressure ultra-fast cooling + laminar cooling: The total valve opening ratio of the low-pressure ultra-fast cooling mode is 66.7%, the cooling rate is 21°C / s, and it is cooled to 480°C for coiling. Example 4

[0046] A production method for a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil, the production method comprising: smelting raw materials through a decarburization converter, LF+RH refining, continuous casting, heating of ingots, controlled rolling, ultra-fast cooling+laminar cooling, and coiling to finally obtain a hot-rolled coil X42MS, the thickness of the hot-rolled coil is 23.5 mm, the chemical composition and mass percentage thereof are shown in Table 1, the hot-rolled coil properties are shown in Table 2, the inclusion results are shown in Table 3, the HIC resistance properties are shown in Table 4, and the SSCC resistance properties are shown in Table 5.

[0047] The specific control process is as follows: 1) Converter smelting: KR desulfurization treatment is used to ensure that the sulfur content of molten iron is 0.0022%; The whole process adopts bottom blowing of argon, the final C content is 0.028%, the alloying sequence of converter is aluminum block → metallic manganese → ferrosilicon → ferroniobium, metallic manganese is matched with manganese, and the manganese content of the big bag is 0.85%.

[0048] 2) LF+RH refining: LF refining uses high carbon ferromanganese and medium carbon ferromanganese to supplement manganese, and carbon powder to supplement carbon. The amount of high carbon ferromanganese added is 336kg, and the amount of medium carbon ferromanganese is 194kg. The Mn content at the end of LF is 0.99%; the RH refining vacuum degree requirement is ≤200Pa for 23 minutes, and the vacuum degree requirement is ≤100Pa for 16 minutes.

[0049] 3) Continuous casting with full protection, casting speed 0.9m / min, superheat 25-30℃, and billet thickness 230mm.

[0050] 4) Ingot heating: temperature is 1160~1186℃, furnace outlet temperature is 1166℃, and furnace residence time is controlled at 185min.

[0051] 5) Controlled rolling: fixed width, rough rolling and finishing rolling are adopted, the fixed width of the fixed width press is 150mm, the rough rolling adopts 1+5 mode, the intermediate billet is 54mm, the steel is swung before finishing rolling, the finishing rolling inlet temperature is controlled at 990℃, the final rolling temperature is 875℃, the rolling speed is 3.0m / s, and the final reduction rate is 13%.

[0052] 6) Low-pressure ultra-fast cooling + laminar cooling: The total valve opening ratio of the low-pressure ultra-fast cooling mode is 66.7%, the cooling rate is 26℃ / s, and it is cooled to 490℃ for coiling. Example 5

[0053] A production method for a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil, the production method comprising: smelting raw materials through a decarburization converter, LF+RH refining, continuous casting, heating of ingots, controlled rolling, ultra-fast cooling+laminar cooling, and coiling to finally obtain a hot-rolled coil X42MS, the thickness of the hot-rolled coil is 24.2 mm, the chemical composition and mass percentage thereof are shown in Table 1, the hot-rolled coil properties are shown in Table 2, the inclusion results are shown in Table 3, the HIC resistance properties are shown in Table 4, and the SSCC resistance properties are shown in Table 5.

[0054] The specific control process is as follows: 1) Converter smelting: KR desulfurization treatment is used to ensure that the sulfur content of molten iron is 0.0045%; The process uses bottom blowing of argon throughout, the final C content is 0.025%, the alloying sequence of the converter is aluminum block → metallic manganese → ferrosilicon → ferroniobium, metallic manganese is matched with manganese, and the manganese content of the bulk package is 0.93%.

[0055] 2) LF+RH refining: LF refining uses high carbon ferromanganese and medium carbon ferromanganese to supplement manganese, and carbon powder to supplement carbon. The amount of high carbon ferromanganese added is 240kg, and the amount of medium carbon ferromanganese is 165kg. The Mn content at the end of LF is 1.03%; the RH refining vacuum degree requirement is ≤200Pa for 21 minutes, and the vacuum degree requirement is ≤100Pa for 17 minutes.

[0056] 3) Continuous casting with full protection, casting speed 1.5m / min, superheat 15~19℃, and billet thickness 230mm.

[0057] 4) Ingot heating: temperature is 1180~1195℃, furnace outlet temperature is 1130℃, and furnace residence time is controlled at 180min.

[0058] 5) Controlled rolling: fixed width, rough rolling and finishing rolling are adopted. The fixed width of the fixed width press is 100mm. The rough rolling adopts the 1+5 mode, the intermediate billet is 50mm, the steel is swung before finishing rolling, the finishing rolling inlet temperature is controlled at 940℃, the final rolling temperature is 850℃, the rolling speed is 2.8m / s, and the final reduction rate is 12%.

[0059] 6) Low-pressure ultra-fast cooling + laminar cooling: The total valve opening ratio of the low-pressure ultra-fast cooling mode is 66.7%, the cooling rate is 15℃ / s, and it is cooled to 520℃ for coiling.

[0060] Table 1 Chemical composition and composition of hot-rolled coils of Examples 1-5 (%)

[0061] Table 2 Performance of hot rolled coils of Examples 1-5

[0062] Table 3 Inclusions in hot rolled coils of Examples 1-5

[0063] Table 4 Test data of HIC resistance of hot rolled coils in Examples 1-5

[0064] Table 5 Test data of hot rolled coil anti-SSC performance of Example 1-5

[0065] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil, characterized in that: The chemical composition and mass percentage of the hot-rolled coil are: C: 0.030-0.060%, Mn: 0.80-1.10%, Si: 0.07-0.25%, S≤0.0015%, P≤0.0012%, Ti: 0.015-0.030%, Nb: 0.020-0.030%, H≤0.0001%, and the rest are Fe and unavoidable impurities.

2. The low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil according to claim 1, characterized in that: The hot-rolled coil has a yield strength of 382-432 MPa, a tensile strength of 481-526 MPa, a yield strength ratio ≤0.90, a -60°C low-temperature Charpy impact energy ≥300 J, a -40°C drop hammer shear area ≥85%, a thickness of 20-25 mm, ABCD four types of non-metallic inclusions ≤1.0, HIC performance: CLR≤0.5%, CTR≤0.5%, CSR≤1%, SSC performance: no cracks.

3. A method for producing a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil according to claim 1 or 2, characterized in that: The production method comprises the following steps: smelting the raw materials through a decarbonization converter, LF+RH refining, continuous casting, heating the ingot, controlled rolling, ultrafast cooling+laminar cooling, and coiling to finally obtain a hot-rolled coil; in the low-pressure ultrafast cooling+laminar cooling process, the cooling rate is 15-26°C / s, and the coiling is performed after cooling to 460-520°C.

4. The method for producing a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil according to claim 3, characterized in that: The raw materials are treated with KR desulfurization to ensure that the S content of the molten iron is ≤0.0050%.

5. The method for producing a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil according to claim 3, characterized in that: The converter smelting process adopts bottom blowing of argon throughout the process, and the final C content is ≤0.030%. The converter alloying sequence is aluminum block, metallic manganese, ferrosilicon, and ferroniobium.

6. The method for producing a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil according to any one of claims 3 to 5, characterized in that: In the LF+RH refining process, high carbon ferromanganese and medium carbon ferromanganese are used to supplement manganese in LF refining, and carbon powder is used to supplement carbon when the carbon content in the converter is insufficient.

7. A method for producing low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil according to any one of claims 3 to 5, characterized in that: In the LF+RH refining process, the RH refining vacuum degree is required to be ≤200Pa for ≥20 minutes, and the vacuum degree is required to be ≤100Pa for ≥15 minutes.

8. The method for producing a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil according to any one of claims 3 to 5, characterized in that: The continuous casting process includes full protection casting, a casting speed of 0.9-1.5 m / min, and a superheat of 15-30°C.

9. The method for producing a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil according to any one of claims 3 to 5, characterized in that: In the casting billet heating process, the casting billet heating temperature is 1160-1200°C, the furnace discharge temperature is 1130-1170°C, and the furnace residence time is controlled to be 180-300 minutes.

10. The method for producing a low-cost, high-toughness, ultra-thick, acid-resistant pipeline hot-rolled coil according to any one of claims 3 to 5, characterized in that: The controlled rolling process adopts fixed width, rough rolling and finishing rolling. The fixed width of the fixed width press is 50-150mm, the rough rolling adopts the 1+5 mode, the intermediate billet is 50-60mm, the steel is swung before finishing rolling, the finishing rolling inlet temperature is controlled at 940-990°C, the final rolling temperature is 850-890°C, the rolling speed is 2.8-3.2m / s, and the final reduction rate is ≥12%.

Citation Information

Patent Citations

  • Low-cost acid resistant pipeline steel hot-rolled plate and manufacturing method thereof

    CN102021476A

  • Copper-nickel-free acid-resistant pipeline steel x52ms and its hot-rolled coil manufacturing method

    CN104099522B

  • Acid-resistant pipeline steel and production method thereof

    CN108893678A

  • Low-cost large-wall-thickness acid-resistant pipeline steel with stable structure and performance and production method thereof

    CN110846565A

  • Pipeline steel with excellent performance of low cost and HIC and SSC resistance and manufacturing method of pipeline steel

    CN111607739A

Cited By

  • Limit specification X100 pipeline steel and production method thereof

    CN120738562A