Preparation method of ultra-thin S460M / ML medium-thickness steel plate
Through low-content chemical composition and specific blank stacking and rolling production mode, the problems of extreme thin S460M/ML steel plates in high strength and low cost are solved, efficient production and good plate shape control are achieved, and low-temperature toughness and production are improved. efficiency.
Patent Information
- Application Number
- CN202411379230.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-26
AI Technical Summary
When the prior art produces 5-9mm ultra-thin S460M/ML medium-thick steel plates, it is difficult to ensure high strength and toughness, low alloy cost and high production efficiency at the same time, and the thin specification steel plate has a low rolling yield and poor plate straightness. Inadequate low temperature toughness.
Using a simple and low-content chemical composition design, the thickness of the slab is controlled through specific blank smelting methods and stacking production modes, including converter smelting, LF refining, continuous casting, blank slab assembly, heating, rough rolling, finishing rolling and cooling processes, and Width design, using low-pressure vacuum evacuation and nitrogen blown argon to ensure that the steel plate undergoes dynamic recrystallization and static recrystallization at high temperatures to form a fine crystal structure.
It significantly improves the high strength, high toughness and high production efficiency of the 5-9mm ultimate thin specification S460M/ML steel plate, reduces alloy cost, expands production regulation space, and ensures plate straightness and welding performance.
Smart Images

Figure CN119020670A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of medium and thick steel plates, and specifically relates to a method for preparing an extremely thin S460M / ML medium and thick steel plate. The thickness of the steel plate is 5-9 mm, which is an extremely thin specification among medium and thick steel plates. Background Art
[0002] In steel enterprises, the conventional definition of medium and thick plates is that steel plates with a thickness of 4-20mm are called medium plates; steel plates with a thickness of 20-60mm are called thick plates; and steel plates with a thickness of more than 60mm are called extra thick plates; and for S460M / ML, the industry usually calls the thickness of 8-100mm as medium and thick plates. The thickness of 5-9mm prepared by the present invention can be called an ultra-thin plate within the range of medium and thick plates. The implementation standard of S460M and S460ML products is EN 10025-4:2019. They are thermomechanically rolled weldable fine-grained structural steels with an applicable thickness range of ≤150mm. The specified minimum impact energy value at a temperature not lower than -20℃ / -50℃ is represented as "M / ML" and is widely used in large ships, bridges, high-pressure boilers, high-pressure vessels, lifting machinery, mining machinery and other large welded structures.
[0003] This type of steel needs to meet the performance requirements through thermomechanical rolling, and the production is difficult, especially for thin specifications below 10mm. If the conventional TMCP controlled rolling and controlled cooling process is used for production, during low-temperature rolling, due to the high strength of the steel plate itself and the increased deformation resistance, it is very easy to have quality defects such as upwarping, buckling, sickle bending, and longitudinal cracking, and the rolling rate is low. At the same time, during subsequent water-cooling strengthening, due to the strong sensitivity of thin specifications, it is difficult to control the plate shape, and it is very easy to have serious middle waves, side waves, and horizontal scoops. On the one hand, hot-rolled coils can be used as a substitute, but it is limited to the type of demand with smaller width requirements; on the other hand, in order to reduce the difficulty of controlled rolling and controlled cooling of thin specifications, it is mainly through increasing the content of alloy elements and increasing the phase transformation temperature, so as to achieve 460MPa grade high-strength steel through higher rolling temperature and water cooling temperature, but this will bring about a significant increase in alloy input costs, and insufficient performance of low-temperature or ultra-low-temperature toughness margin. Therefore, it is urgent to research and develop methods to add low levels of alloy elements and match them with conventional controlled rolling and controlled cooling processes, so as to obtain excellent strength and toughness indicators while significantly improving the production efficiency and first-time pass rate of 5-9mm ultra-thin S460M / ML medium and thick plates.
[0004] Comparative Document 1: In the prior art, there are many 460MPa grade high-strength steels with a thickness of 16 to 120mm, and the production methods are becoming more mature, such as application number: CN 107326279, which is suitable for S460M with a thickness of 70 to 110mm; application number: CN108998738, which produces S460M with a thickness of 100mm; application number: CN110951955, which produces Q460MD with a steel plate of 16 to 30mm; application number: CN111850414, which produces S460ML with a steel plate thickness of 120mm; application number: CN114395730, which produces S460ML with a thickness range of 60 to 100mm. For medium and thick specifications above 10mm, the steel plate has good rolling formability, high flatness, and excellent one-time pass rate, but its guiding significance for production control of extremely thin specifications <10mm is not very significant.
[0005] Comparative Document 2: Patent "A high-toughness Q460 grade high-strength steel plate and its manufacturing method" (application number: CN110846570), adopts "C: 0.07-0.11%, Si: 0.10-0.40%, Mn: 1.20-1.50%, P≤0.015%, S≤0.003%, Alt: 0.010-0.050%, Mo: 0.08-0.14%, Ni: 0.10-0.30%, V: 0.03-0.06%, Ti: 0.006-0.030%, Nb≤0.03%, Cr≤0.20%, Cu≤0.30%, B≤0.0008%" composition design. The final rolling temperature of 6mm steel plate is 800-850℃, and air cooling is performed after rolling. Offline heat treatment is also carried out, with quenching temperature of 900-920℃, quenching holding time of 10-30min, tempering temperature of 650-665℃, and tempering holding time of 20-40min. The yield strength of the steel plate is 605MPa, the tensile strength is 665MPa, the elongation is 19.5%, and the impact energy at -60℃ is 97J. The patented composition adopts a low-carbon design system. In order to ensure performance requirements, high content of Mo and Ni noble elements are added, which is bound to significantly increase the cost of the alloy. In addition, in order to ensure strength and toughness, tempering heat treatment is also carried out, which increases the production process and reduces efficiency. In addition, the steel plate is reheated, resulting in great energy consumption, which increases the manufacturing cost and is not conducive to the needs of green development.
[0006] Comparative Document 3: Patent "Q460E high-strength steel plate with a thickness of less than 12mm and its production method" (application number: CN107974615), adopts the composition design of "C: 0.12-0.15%, Si: 0.30-0.45%, Mn: 1.50-1.65%, P≤0.015%, S≤0.010%, Nb: 0.04-0.05%, V: 0.01-0.02%, Ti≤0.05%", and adopts two-stage controlled rolling, with the rough rolling start temperature ≥1080℃, the rolling passes ≤7 passes, the pass reduction ≥23mm, the finishing rolling temperature 850~950℃, the rolling passes ≤9 passes, the pass reduction rate ≥10%, and the final cooling temperature 550~580℃. In the embodiment, the yield strength is 470-480MPa, the difference between the same plate is 0.20-0.23mm, and the unevenness is 3-4mm / m. Although the patent adopts the design of medium carbon 0.12-0.15% and Nb, V, and Ti micro-alloying, in order to ensure the rolling rate and plate shape of the thin plate, the finishing rolling control temperature is set high, which leads to the yield strength close to the lower limit of the standard, the margin is small, and the low-temperature toughness index is not reflected. At the same time, due to the mismatch of the thin rolling method, the precision control of the same plate difference is low, and there is a risk of thickness exceeding the tolerance. Summary of the invention
[0007] The present invention provides a preparation method of an ultra-thin S460M / ML medium-thick steel plate, which utilizes a simple low-content component design and realizes roll-to-roll production through a specific billet assembly method, thereby increasing the thickness of the rolling process, thereby significantly reducing the difficulty of TMCP process control of thin-gauge steel plates, and ultimately obtaining 5-9 mm ultra-thin S460M / ML steel plates with high strength and toughness, high production efficiency, and high first-time qualified rate.
[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is: A method for preparing an ultra-thin S460M / ML medium-thick steel plate, characterized in that the steel plate comprises the following components in percentage by mass: C: 0.13-0.16%, Si: 0.20-0.40%, Mn: 1.40-1.60%, P≤0.015%, S≤0.005%, Alt: 0.020-0.050%, Ti: 0.010-0.020%, Nb: 0.020-0.050%, V: 0.015-0.040%, N: 40-80ppm, the remainder is Fe and unavoidable impurities, and the carbon equivalent CEV: 0.36-0.43%.
[0009] Among them: the thickness of the steel plate is 5 to 9 mm.
[0010] The method for preparing an ultra-thin S460M / ML medium-thick steel plate comprises the following steps: Step A, slab design, target steel plate thickness, width, length, trimming amount, head and tail amount, length multiples are expressed as h (mm), b (mm), l (mm), Δb (mm), Δl (mm), n, slab thickness, width, length are H (mm), B (mm), L (mm), where H ≥ 15 × h, B ≥ 0.6 × b, then according to the formula H × B × L = h × (b + Δb) × (l + Δl) × n, the required length L of the slab is calculated; for several target steel plates with specifications of different thickness (or same thickness) × same width × same length, the corresponding slabs need to be designed with the same width and length; Step B, converter smelting, the low-phosphorus molten iron that has been pre-treated, desulfurized and slag-stripped is smelted by the converter double slag method, and the slag thickness is ≤40mm; the blowing process adopts the bottom blowing argon mode, the blowing end point C is ≥0.07%, and the tapping temperature is 1640-1660℃; Step C, refining, make white slag in LF refining process, make FeO+MnO≤1.0%, keep white slag operation ≥10min, and control the end slag sample CaO / Al2O3=1.7~2.0; RH high vacuum treatment time ≥10min, and use nitrogen as lifting gas, flow rate ≥55m 3 / h, ensuring that the nitrogen content in the slab is in the range of 40-80ppm; the soft argon blowing time after vacuum is released is ≥10min, and the net blowing end temperature is 1560-1575℃; Step D, continuous casting, full protection casting, control superheat at 10-20°C, put into secondary cooling electromagnetic stirring and light pressure at the end of solidification to ensure that the center segregation of the slab is ≤C class 1.0; Step E, assembling, firstly, the rough slab smelted in steps B to D is preliminarily rolled into shape according to the design size in step A; then, the surface to be composited of the formed slab is polished, cleaned, and coated with a release agent; finally, the assembling is completed by stacking, pressing, welding, and vacuuming; the maximum assembling thickness depends on the maximum rolling thickness and the maximum rolling unit weight of the rolling mill; Step F, heating, heating and keeping the assembled slabs warm, the temperature of the heating section is 1220° C., the temperature of the keeping section is 1200° C., and the heating rate is 1.0 min / mm; Step G, rough rolling, the starting temperature of rough rolling is ≥1050℃, firstly one pass of down rolling is performed to make the reduction rate ≥8%, and the reduction rate of the last three passes is ≥15%, the finishing temperature of rough rolling is ≥980℃; the thickness of the intermediate billet is ≥70mm; Step H, finishing rolling, the starting temperature of finishing rolling is ≤900℃, the reduction rate of each pass is ≥12%, the finishing temperature of finishing rolling is 820~850℃, and the final rolling thickness is (h1+h2+…h n ) mm; Step I, cooling: the steel plate is pre-straightened once after rolling to make it flat, and then enters the ACC laminar cooling device for cooling, with the water inlet temperature ≥ 740°C, the cooling rate 5-8°C / s, and the red-return temperature 600-640°C; Step J, cutting, the laminated rolled steel plates are subjected to warm trimming, the cutting temperature is ≥100°C, and the cutting sequence is cutting cleanly the head and tail double-sided welds, dividing into sections according to length multiples, and cutting cleanly the width double-sided welds.
[0011] Further: in step A, the target steel plate width b≤3500mm, and the required slab length L cannot be less than the minimum length of the heating furnace.
[0012] Furthermore, when the nitrogen content in the steel is less than 40-80 ppm after the RH vacuum is released in step C, an appropriate amount of vanadium-nitrogen alloy is added to supplement the nitrogen content.
[0013] Further: in step E, the blank is vacuumed to a pressure of 0.01-0.05 Pa and sealed and welded on all sides to prevent the blank gap from having a "blow-up" phenomenon and cracking of the edge weld during the rolling process due to a large amount of residual air.
[0014] Among them, the isolation agent is a prior art, which can be magnesium oxide powder or the like.
[0015] Furthermore: the cutting temperature range in step J is 100-200°C to avoid phase change after cutting in the high temperature zone. In addition, there is no end constraint at this time, which leads to the plate curvature.
[0016] The advantages of the present invention are: The present invention rationally designs the chemical composition of the S460M / ML steel plate, and sets the carbon and manganese contents. While ensuring that the steel plate obtains high strength, it also reduces the amount of microalloys such as Nb and Ti, and replaces the addition of precious elements such as Ni, Cu, and Mo, which is conducive to the needs of green development. Silicon is an effective deoxidizing element in steel and can also improve the strength of the steel plate, so Si is set to 0.20-0.40. Nb and Ti elements can give full play to the fine grain and precipitation composite strengthening effects, so that the steel plate still maintains high plastic toughness at an ultra-low temperature of -50°C. In addition, by adding an appropriate amount of V element and coupling with nitrogen blowing in the RH process, VN particles are introduced. On the one hand, the grain boundaries are pinned during the heating process to prevent the growth of austenite grains, and on the other hand, the occurrence of austenite recrystallization is hindered during the rolling process, so as to achieve precipitation strengthening and grain refinement, greatly improve the performance of the steel plate, and effectively reduce the cost of manufacturing alloys. Through a reasonable chemical composition ratio, the carbon equivalent is stably controlled at 0.36-0.43%, ensuring the welding performance of the steel plate.
[0017] The present invention rationally designs the slabs used in the production of 5-9mm ultra-thin specifications S460M / ML by rolling, fully considering factors such as the amount of steel plate trimming, head and tail, multiple lengths, and the maximum furnace weight and minimum furnace length that affect the design size of the slab, which is very close to the actual production conditions and fully possesses the operability and reproducibility of industrial mass production. Through a specific billet assembly and rolling production mode, ≥2 sheets of steel plates with different thicknesses (same thickness) can be produced at a time, and the production efficiency is greatly improved. It also focuses on solving the difficult problems of low rolling rate, poor plate flatness, high alloy cost, and insufficient toughness of single ultra-thin specifications high-strength steel TMCP controlled rolling and controlled cooling, while expanding the TMCP process window, and the production control space becomes larger.
[0018] The reasonably matched heating process of the present invention allows the alloy elements to be fully dissolved, and at the same time, with a stable heating rate, it ensures that the temperature difference between the surface and the core of the slab is ≤30°C, so that the deformation can fully penetrate the interior. The reason why the first rough rolling pass is rolled ≥8% is to ensure the elimination of the assembly gap, ensure the accurate slab thickness, and then obtain the target thickness accuracy of the same plate. The two-stage controlled rolling strategy and the large reduction pass distribution accurately locate the timing of the occurrence of coupled dynamic recrystallization and static recrystallization, accumulate a large amount of dislocation density, significantly improve the dislocation strengthening effect, and fully refine the original austenite grains. The target red return temperature is set at 600-640°C, avoiding the medium and low temperature transformation phase zone and avoiding the formation of supercooled structure. At the same time, the low cooling rate of 5-8°C / s makes the steel plate cool more evenly and ensures the flatness of the plate shape. Reasonable cutting method and cutting temperature effectively control the dimensional accuracy and plate appearance of the finished product of the extremely thin gauge laminated steel plate, and ensure the closure of the systematic production route of the whole process. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a metallographic microstructure diagram of a 5 mm thin S460ML steel plate rolled in Example 1; Figure 2 This is a metallographic microstructure diagram of a 7 mm thin gauge S460ML steel plate rolled in Example 1; Figure 3 This is the actual appearance of the steel plate after the 5mm and 7mm steel plates were cut and separated in Example 1. DETAILED DESCRIPTION
[0020] The present invention is further described in detail below in conjunction with specific examples. It should be clear that these examples are only used to describe the specific implementation methods of the present invention and are not intended to constitute any limitation on the protection scope of the present invention.
[0021] Taking a domestic five-meter wide and thick plate plant as an example, the maximum rolling thickness of the roughing mill is 1200mm, the maximum rolling thickness of the finishing mill is 550mm, the maximum rolling unit weight is 30 tons, and the minimum loading length of the slab of the regenerative walking beam heating furnace is 2400mm, as follows.
[0022] Example 1: The target thicknesses of the S460ML steel plates rolled on a roll-formed basis are 5 mm and 7 mm respectively; The mass percentage of each component of 5mm and 7mm steel plates are: C: 0.14%, Si: 0.30%, Mn: 1.55%, P: 0.012%, S: 0.003%, Alt: 0.034%, Ti: 0.016%, Nb: 0.036%, V: 0.023%, N: 67ppm, the balance is Fe and unavoidable impurities, carbon equivalent CEV: 0.40%.
[0023] The target steel plate thickness, width, length, trimming amount, head and tail amount, and length multiple in step A are 5mm / 7mm, 2200mm, 8000mm, 200mm, 1400mm, and 4, respectively. The designed slab thickness, width, and length of the 5mm steel plate are 90.96mm, 1550mm, and 3200mm, respectively; the designed slab thickness, width, and length of the 7mm steel plate are 127.35mm, 1550mm, and 3200mm, respectively.
[0024] In step B, the slag thickness is 35 mm; blowing end point C: 0.083%, tapping temperature 1652°C; In step C, FeO+MnO=0.85%, white slag operation 15min, end slag sample CaO / Al2O3=1.8; RH high vacuum treatment time 15min, nitrogen flow 70m 3 / h; soft blowing time 12min, net blowing end temperature 1568℃; In step D, the superheat is 15°C and the center segregation of the slab is Class C 0.5; The thickness, width and length of the slab after assembly in step E are 218.31 mm (90.96 mm + 127.35 mm), 1550 mm and 3200 mm respectively, and the vacuum degree is 0.02 Pa.
[0025] In step F, the temperature of the slab heating section is 1220°C, the temperature of the insulation section is 1200°C, and the heating rate is 1.0 min / mm; In step G, the starting temperature of rough rolling is 1083°C, the first rolling pass has a reduction rate of 8.6%, the last three passes have reduction rates of 17.2%, 20.4%, and 16.8%, the ending temperature of rough rolling is 994°C, and the thickness of the intermediate billet is 75mm; In step H, the finishing rolling start temperature is 891° C., the finishing rolling is performed for 8 passes, the reduction rates of each pass are 23.3%, 20.2%, 20.0%, 22.4%, 21.3%, 20.4%, 17.7%, and 16.2%, the finishing rolling end temperature is 836° C., and the final rolling thickness is 12 mm (5 mm + 7 mm); In step I, the water inlet temperature is 763°C, the cooling rate is 6°C / s, and the red-return temperature is 623°C; In step J, the cutting temperature is 157° C. After cutting, 4 S460ML steel plates with specifications of 5 mm×2200 mm×8000 mm and 4 S460ML steel plates with specifications of 7 mm×2200 mm×8000 mm are produced.
[0026] Example 2: The target thicknesses of the S460M steel plates rolled on a roll-formed basis are 6 mm and 8 mm respectively; The mass percentage of each component of 6mm and 8mm steel plates are: C: 0.15%, Si: 0.33%, Mn: 1.52%, P: 0.010%, S: 0.001%, Alt: 0.038%, Ti: 0.015%, Nb: 0.033%, V: 0.029%, N: 74ppm, the balance is Fe and unavoidable impurities, carbon equivalent CEV: 0.41%.
[0027] The target steel plate thickness, width, length, trimming amount, head and tail amount, and length multiple in step A are 6mm / 8mm, 2000mm, 6000mm, 200mm, 800mm, and 5. The designed slab thickness, width, and length of the 6mm steel plate are 104.45mm, 1540mm, and 2790mm, respectively; the designed slab thickness, width, and length of the 8mm steel plate are 139.27mm, 1540mm, and 2790mm, respectively.
[0028] The slag thickness in step B is 33 mm; blowing end point C: 0.088%, tapping temperature 1648°C; In step C, FeO+MnO=0.83%, white slag operation 14min, end slag sample CaO / Al2O3=1.9; RH high vacuum treatment time 16min, nitrogen flow 62m 3 / h; soft blowing time 13min, net blowing end temperature 1571℃; In step D, the superheat degree is 17°C and the center segregation of the slab is Class C 0.5; The thickness, width and length of the slab after assembly in step E are 243.72 mm (104.45 mm + 139.27 mm), 1540 mm and 2790 mm respectively, and the vacuum degree is 0.01 Pa.
[0029] In step F, the temperature of the slab heating section is 1220°C, the temperature of the insulation section is 1200°C, and the heating rate is 1.0 min / mm; In step G, the starting temperature of rough rolling is 1077°C, the first rolling pass has a reduction rate of 8.1%, the last three passes have reduction rates of 16.1%, 15.7%, and 19.0%, the ending temperature of rough rolling is 1013°C, and the thickness of the intermediate billet is 76mm; In step H, the finishing rolling start temperature is 885° C., the finishing rolling is performed for 7 passes, the reduction rate of each pass is 21.4%, 21.4%, 22.1%, 21.6%, 20.4%, 21.7%, 22.2%, the finishing rolling end temperature is 841° C., and the final rolling thickness is 14 mm (6 mm + 8 mm); In step I, the water inlet temperature is 751°C, the cooling rate is 8°C / s, and the red-return temperature is 617°C; In step J, the cutting temperature is 142° C. After cutting, 5 S460M steel plates with specifications of 6 mm×2000 mm×6000 mm and 5 S460M steel plates with specifications of 8 mm×2000 mm×6000 mm are produced.
[0030] Example 3: The target thicknesses of the S460M steel plates rolled on a roll-formed basis are 7 mm and 9 mm respectively; The mass percentage of each component of 7mm and 9mm steel plates are: C: 0.14%, Si: 0.25%, Mn: 1.47%, P: 0.011%, S: 0.001%, Alt: 0.042%, Ti: 0.017%, Nb: 0.045%, V: 0.036%, N: 72ppm, the balance is Fe and unavoidable impurities, carbon equivalent CEV: 0.39%.
[0031] The target steel plate thickness, width, length, trimming amount, head and tail amount, and length multiple in step A are 7mm / 9mm, 3000mm, 8000mm, 300mm, 1000mm, and 3. The designed slab thickness, width, and length of the 7mm steel plate are 106.17mm, 2005mm, and 2930mm, respectively; the designed slab thickness, width, and length of the 9mm steel plate are 136.50mm, 2005mm, and 2930mm, respectively.
[0032] The slag thickness in step B is 35 mm; blowing end point C: 0.076%, tapping temperature 1654°C; In step C, FeO+MnO=0.74%, white slag operation 13min, end slag sample CaO / Al2O3=1.8; RH high vacuum treatment time 15min, nitrogen flow 60m 3 / h; soft blowing time 12min, net blowing end temperature 1566℃; In step D, the superheat is 14°C and the center segregation of the slab is Class C 0.5; The thickness, width and length of the slab after assembly in step E are 242.67 mm (106.17 mm + 136.50 mm), 2005 mm and 2930 mm respectively, and the vacuum degree is 0.01 Pa.
[0033] In step F, the temperature of the slab heating section is 1220°C, the temperature of the insulation section is 1200°C, and the heating rate is 1.0 min / mm; In step G, the starting temperature of rough rolling is 1069°C, the first rolling pass has a reduction rate of 10.2%, the last three passes have reduction rates of 19.9%, 17.2%, and 21.7%, the ending temperature of rough rolling is 984°C, and the thickness of the intermediate billet is 77mm; In step H, the finishing rolling start temperature is 877° C., the finishing rolling is performed for 8 passes, the reduction rates of each pass are 19.6%, 18.1%, 19.0%, 18.9%, 15.2%, 17.9%, 17.4%, and 15.8%, the finishing rolling end temperature is 828° C., and the final rolling thickness is 16 mm (7 mm + 9 mm); In step I, the water inlet temperature is 753°C, the cooling rate is 7°C / s, and the red-return temperature is 624°C; In step J, the cutting temperature is 169° C. After cutting, 3 S460M steel plates with specifications of 7 mm×3000 mm×8000 mm and 3 S460M steel plates with specifications of 9 mm×3000 mm×8000 mm are produced.
[0034] The mechanical properties and physical weight of the steel plates of each embodiment are shown in the table below. In the table, the standard is EN 10025-4:2019, and the thickness of the same plate is measured at 2 points at the head, 2 points in the middle, and 2 points at the tail.
[0035] As can be seen from the table, the 5-9 mm ultra-thin S460M / ML medium and thick plates manufactured by the present invention have high strength, plasticity and toughness, with a yield strength margin of 26-38 MPa, a tensile strength margin of 55-78 MPa, an elongation margin of 5.5-7.0%, a -20°C impact energy margin of 67-89 J, and a -50°C impact energy margin of 41-54 J, which has sufficient margin. It can be seen from the impact toughness test that the toughness transition temperature of the steel is below -50°C, thereby showing good low-temperature toughness. Through the specific assembly rolling method of the present invention, the difference between the same plates of the ultra-thin specifications can still be controlled within the range of 0.01-0.03 mm, with good thickness accuracy; the unevenness of the steel plate is 1.0-2.5 mm / m, and the plate shape is highly straight, which improves the user experience and lays the foundation for high-precision processing of downstream processes.
[0036] Mechanical properties table Example Steel plate thickness, mm Yield strength, MPa Tensile strength, MPa Elongation after break,% -20℃ longitudinal impact energy, J Measure thickness of the same plate, mm Roughness, mm / m 1 5 498 618 23.5 68 4.99 / 4.99、5.01 / 4.99、4.98 / 4.97 2.5 1 7 494 605 24.0 81 7.01 / 7.01、6.99 / 7.01、7.02 / 7.03 2.0 2 6 491 611 22.5 127 5.99 / 5.98、5.99 / 6.01、6.02 / 6.01 2.0 2 8 487 599 23.0 114 8.01 / 8.02、8.01 / 7.99、7.98 / 7.99 1.5 3 7 495 603 23.0 136 6.99 / 6.99、7.01 / 7.01、7.01 / 6.99 1.5 3 9 486 595 23.5 121 9.01 / 9.01、8.99 / 8.99、8.99 / 9.01 1.0 standard ≥460 540-720 ≥17.0 ≥47 / /
[0037] By the attached Figures 1-2It can be seen that the metallographic structure of the steel plate is typical pearlite + ferrite, the ferrite grain size reaches above level 9, the structure is uniform and fine, and there is no bainite or martensite undercooled structure, which is attributed to the reasonable composition, controlled rolling and cooling matching of the present invention. Figure 3 It can be seen that after cutting and separation, the plate shape is straight and the ends are flush. In summary, the present invention effectively solves the problem of coordinated regulation of high strength, high toughness and high flatness plate shape of 460MPa grade ultra-thin specifications, and has high application value.
Claims
1. A method for preparing an ultra-thin S460M / ML medium-thick steel plate, characterized in that: The steel plate comprises the following components in percentage by mass: C: 0.13-0.16%, Si: 0.20-0.40%, Mn: 1.40-1.60%, P≤0.015%, S≤0.005%, Alt: 0.020-0.050%, Ti: 0.010-0.020%, Nb: 0.020-0.050%, V: 0.015-0.040%, N: 40-80ppm, the balance is Fe and unavoidable impurities, carbon equivalent CEV: 0.36-0.43%; the thickness of the steel plate is 5-9mm; The preparation method comprises the following steps: Step A, slab design, for several target steel plates with the same width × length, select the corresponding number of slabs with the same width × length, and calculate the required length L of the slab according to the formula H×B×L=h×(b+Δb)×(l+Δl)×n, and H≥15×h, B≥0.6×b; where: H, B, L are the millimeters of the thickness, width and length of the slab respectively, h, b, l, Δb, Δl are the millimeters of the thickness, width, length, trimming amount and head and tail trimming amount of the target steel plate respectively, and n is the length multiple; Step B, converter smelting, the low-phosphorus molten iron that has been pre-treated, desulfurized and slag-stripped is smelted by the converter double slag method, and the slag thickness is ≤40mm; the blowing process adopts the bottom blowing argon mode, the blowing end point C is ≥0.07%, and the tapping temperature is 1640-1660℃; Step C, refining, make white slag in LF refining process, make FeO+MnO≤1.0%, keep white slag operation ≥10min, and control the end slag sample CaO / Al2O3=1.7~2.0; RH high vacuum treatment time ≥10min, and use nitrogen as lifting gas, flow rate ≥55m 3 / h, ensuring that the nitrogen content in the slab is in the range of 40-80ppm; the soft argon blowing time after vacuum is released is ≥10min, and the net blowing end temperature is 1560-1575℃; Step D, continuous casting, full protection casting, control superheat at 10-20°C, put into secondary cooling electromagnetic stirring and light pressure at the end of solidification to ensure that the center segregation of the slab is ≤C class 1.0; Step E, assembling, firstly, the rough slab smelted in steps B to D is preliminarily rolled into shape according to the design size in step A; then, the surface to be composited of the formed slab is polished, cleaned, and coated with a release agent; finally, the assembling is completed by stacking, pressing, welding, and vacuuming; Step F, heating, heating and keeping the assembled slabs warm, the temperature of the heating section is 1220° C., the temperature of the keeping section is 1200° C., and the heating rate is 1.0 min / mm; Step G, rough rolling, the starting temperature of rough rolling is ≥1050℃, firstly one pass of forward rolling is performed to make the reduction ratio ≥8%, and the reduction ratio of the last three passes is ≥15%, the finishing temperature of rough rolling is ≥980℃; the thickness of the intermediate billet is ≥70mm; Step H, finishing rolling, the starting temperature of finishing rolling is ≤900℃, the reduction rate of each pass is ≥12%, the finishing temperature of finishing rolling is 820~850℃, and the final rolling thickness is (h1+h2+…h n ) mm; Step I, cooling: the steel plate is pre-straightened once after rolling to make it flat, and then enters the ACC laminar cooling device for cooling, with the water inlet temperature ≥ 740°C, the cooling rate 5-8°C / s, and the red-return temperature 600-640°C; Step J, cutting, the laminated rolled steel plates are subjected to warm trimming, the cutting temperature is ≥100°C, and the cutting sequence is cutting cleanly the head and tail double-sided welds, dividing into sections according to length multiples, and cutting cleanly the width double-sided welds.
2. The method for preparing an ultra-thin S460M / ML medium-thick steel plate according to claim 1, characterized in that: The yield strength of the steel plate is ≥480MPa, the tensile strength is ≥590MPa, the elongation after fracture is ≥22%, the longitudinal impact energy at -20℃ is ≥100J, and the longitudinal impact energy at -50℃ is ≥60J; the thickness difference of the same plate is ≤0.05mm, the unevenness is ≤3mm / m, and one rolling can produce ≥2 steel plates of different or same thickness.
Citation Information
Patent Citations
Hot mechanical rolled type super-thick easily-welded S460M structural steel plate and producing method
CN107326279A
Q460E high strength steel plate with thickness less than 12mm and manufacturing method thereof
CN107974615A
High toughness Q460 grade high strength steel plate and manufacturing method thereof
CN110846570A
Low-cost high-strength engineering machinery steel Q460MD and production method thereof
CN110951955A
S460ML extra-thick steel plate and production method thereof
CN111850414A