A method for controlling the shape of NiCrMo thin-gauge quenched and tempered plate

The method for controlling the shape of thin-gauge NiCrMo steel plates through shot blasting, reversible heating, and controlled quenching with adjusted water ratios and flow parameters addresses shape quality and energy efficiency issues, achieving high yield and reduced energy consumption.

CN117512279BActive Publication Date: 2024-12-03CHAOHU UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311601823.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-28
Publication Date
2024-12-03
Estimated Expiration
2043-11-28

AI Technical Summary

Technical Problem

Existing methods for producing thin-gauge NiCrMo marine engineering steel plates face challenges in controlling shape quality due to high alloy content, residual iron oxide scale, and rapid cooling, leading to deformation and high energy consumption, which affects yield and profitability.

Method used

A method involving shot blasting to remove iron oxide scale, reversible heating to ensure full alloy dissolution, controlled quenching with adjusted water ratios and flow parameters, and a quenching support mechanism to enhance cooling uniformity, resulting in improved shape quality and reduced energy consumption.

Benefits of technology

The method achieves a first-time qualified rate of steel plates with ≤5/1000mm unevenness and saves over 15% energy per ton compared to traditional processes, enhancing yield and reducing thermal stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117512279B_ABST
    Figure CN117512279B_ABST
Patent Text Reader

Abstract

The invention discloses a method for controlling the shape of a NiCrMo thin-gauge quenched and tempered plate, comprising the following steps: S100, steel plate quality preparation before quenching: the surface of the steel plate needs to be shot blasted before quenching to ensure that the surface roughness of the steel plate is less than 2.5sa, and no obvious iron oxide scale remains; S200, steel plate heating: the steel plate is heated in a reversible manner in a furnace, and the temperature is quickly raised to a quenching target temperature of 880-920°C after entering the furnace, and then the temperature is lowered to a furnace exit temperature of 450-500°C, and the temperature is kept; S300, steel plate quenching: the steel plate start quenching temperature is ≥Bs+50°C, and the quenching temperature is ≥Bs+50°C. During the process, the water ratio, water convexity and flow parameters of different positions of the high-pressure section and the low-pressure section steel plates are controlled; the upper and lower water ratios of different positions of the high-pressure section steel plates are all between 0.75-0.85, the water flow rate at the middle position of the upper part of the steel plate is 120-180m3 / h, the edge is 30-60m3 / h, and the flow ratio between the middle and the edge is 3-4; the upper and lower water ratios of the middle part of the low-pressure section steel plate are 0.8-0.90, the upper and lower water ratios of the edge are 0.95-1.05, the water convexity ratio is 2.0-3.0, and the water flow rate at the middle position of the upper part of the steel plate is 50-120m3 / h. The present invention improves the machining accuracy of the 3-8mm NiCrMo series quenched plate shape.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for controlling the shape of a NiCrMo thin quenched and tempered steel plate, in particular to a method for controlling the shape of a 3-8mm thick steel plate by quenching and tempering process with high efficiency and low energy consumption. Background Art

[0002] In recent years, with the increasing tension in global energy supply, countries around the world are actively exploiting oil resources in the ocean. Therefore, a large amount of NiCrMo steel for marine structural engineering with good strength and toughness matching, corrosion resistance, and excellent welding performance is needed. Due to the harsh service environment of marine engineering steel, in order to meet the above performance requirements, the content of alloy elements in NiCrMo marine engineering steel is generally higher (NiCrMo>5%), and the alloy cost is therefore relatively high. For thin-gauge NiCrMo marine engineering steel with a thickness of 3-8mm, the current main process is hot rolling + quenching + tempering process, that is, hot rolling + quenching and tempering process. NiCrMo marine engineering steel has a high alloying element content, and the iron oxide scale on the surface of the steel plate has a large viscosity and is difficult to remove. The residual iron oxide scale generates a large internal stress during the cooling process due to the different cooling rate from the matrix, and the plate quality is therefore poor. In addition, due to the thin thickness of the steel plate and the fast cooling rate during quenching, the steel plate is easily deformed by the interaction of phase change stress and thermal stress, resulting in a low yield rate and affecting its profitability. Therefore, optimizing the quenching process of NiCrMo thin-gauge marine steel and improving its plate quality have been hot topics and focuses of research at home and abroad in recent years.

[0003] At present, there are many studies on the shape quality of thin-gauge quenched and tempered plates at home and abroad, especially the quenched shape. Since it is the key to the shape quality control of quenched and tempered plates, there are many related reports and literature. For example, the patent "A production method for high-quality thin-gauge high-strength hot-rolled wear-resistant steel plates (CN202210322850.8)" discloses a shape control method for the entire process of thin-gauge wear-resistant steel. The key technology of quenching shape is constant-speed aerosol cooling, but for steel plates with a thickness of more than 3mm, aerosol cooling has a low cooling rate and it is difficult to quench the steel plate. The patent "A quenching method for ultra-thin wear-resistant steel plates (CN201810147766.0)" discloses a quenching method for ultra-thin wear-resistant steel plates. Its core technology is segmented heating (heat inlet section temperature 860℃-920℃, outlet section temperature 600℃-750℃, high-speed quenching (quenching roller speed ≥50m / min), but for different series of wear-resistant steels, when the outlet temperature is in the range of 600℃-750℃, it is lower than the Ar3 temperature (the temperature at which austenite begins to undergo a ferrite phase transformation during cooling), and austenite will undergo a partial ferrite phase transformation. Although the plate shape quality is improved during quenching, the final structure is ferrite + martensite, which reduces the wear resistance of the steel plate. In addition, the roller speed during quenching is ≥50m / min, which is difficult to control in actual production on the one hand, and on the other hand It is also difficult to fully quench the steel plate if the quenching rate is too high. Therefore, this invention is difficult to promote and apply in actual production. The patent "A segmented quenching control process for ultra-thin high-hardness steel plates (CN202210603316.4)" discloses a segmented control cooling process for the quenching process of steel plates, that is, the steel plate is divided into a high-temperature section and a low-temperature section, and quenched by different cooling methods, but in the actual industrial production process, the steel plate is continuously produced after it comes out of the furnace, and the high-pressure section and the low-pressure section of the quenching machine are adjacent, so it is difficult to separate and accurately control them. The patent "A method for controlling the shape of steel plate quenching (CN201210558638.8)" discloses a method for controlling the shape of quenched plates with a Ni content of 8-10% and a specification of 5-7mm, but its process parameters have little reference significance for other production lines and other types of steel.

[0004] The present invention provides a method for controlling the shape of a thin NiCrMo quenched and tempered steel plate, in particular, a method for controlling the shape of a 3-8 mm thick steel plate during quenching by using a quenching + tempering process. Compared with the existing production process, the invented process has low production energy consumption, high surface quality, and good plate shape quality, which can greatly improve the yield rate of steel plates and has a good prospect for promotion and application. Summary of the invention

[0005] To this end, the present invention provides a control method for the shape of NiCrMo quenched plate with a thickness specification of 3-8mm. By combining reasonable shot blasting process, heating process, quenching process, etc., the unevenness value of the steel plate can be ≤5 / 1000mm, the first pass rate of the plate shape can be ≥95%, and the energy consumption per ton of steel can be saved by more than 15% compared with the traditional process, so as to solve the above-mentioned defects in the prior art.

[0006] A method for controlling the shape of a NiCrMo thin-gauge quenched and tempered plate comprises the following steps:

[0007] S100, steel plate quality preparation before quenching: the steel plate surface needs to be shot blasted before quenching to ensure that the surface roughness of the steel plate is less than 2.5sa, and there is no obvious iron oxide scale residue;

[0008] S200, steel plate heating: the steel plate is heated in a reversible manner in the furnace. After entering the furnace, the temperature is quickly raised to the quenching target temperature of 880-920℃, and then cooled to the furnace exit temperature of 450-500℃, that is, Bs+ (50-80℃) and kept warm;

[0009] S300, steel plate quenching: the steel plate quenching temperature is ≥ Bs + 50 ° C, and the water ratio, water convexity and flow parameters at different positions of the high-pressure section and low-pressure section of the steel plate are controlled during the quenching process;

[0010] In the high-pressure section, the water ratio between the upper and lower parts of the steel plate is between 0.75-0.85, the water flow rate in the middle of the upper part of the steel plate is 120-180m3 / h, and the water flow rate at the edge is 30-60m3 / h, and the flow rate ratio between the middle and the edge is 3-4;

[0011] In the low-pressure section, the upper and lower water ratio in the middle of the steel plate is 0.8-0.90, the upper and lower water ratio in the edge is 0.95-1.05, the water convexity ratio is 2.0-3.0, and the water flow rate in the middle position of the steel plate is 50-120m3 / h.

[0012] Preferably, in S100, the steel plates with unevenness ≥ 30 mm / m are subjected to single straightening repair or directly scrapped to ensure that the unevenness is less than 30 mm / m before entering the furnace.

[0013] Preferably, in S200, the heating time is 4-8 min / mm, and the cooling time and the heat preservation time are 2-3 min / mm and 1-2 min / mm respectively.

[0014] Preferably, in S300, for 3-6 mm steel plates, the quenching rate is 20-35 m / min, and for steel plates > 6-8 mm, the quenching rate is 12-20 m / min.

[0015] Preferably, the adjustment and control of the parameters in the auxiliary step S300 can be achieved through the quenching support mechanism, the quenching support mechanism includes a quenching water tank, a swinging mechanism arranged at the bottom of the quenching water tank, and a support frame installed above the swinging mechanism for placing the steel plate, overflow troughs are arranged on both sides of the quenching water tank, guide wheels are arranged on the other two opposite supporting walls of the quenching water tank, the four guide wheels correspond to the positions of the four corners of the support frame one by one, the pull rope connected to the corner of the support frame passes through the corresponding guide wheel and is connected to the winch outside the quenching water tank, and a drainage pipe and a water inlet pipe group are arranged in the quenching water tank.

[0016] Preferably, the swing mechanism includes a fixed shaft seat arranged at the bottom of the swing mechanism, a first rotating shaft is arranged between the fixed shaft seats parallel to the X-axis, a swing shaft seat is rotatably arranged in the middle of the first rotating shaft, a second rotating shaft parallel to the Y-axis is mounted on the swing shaft seat, and the support frame is arranged on the second rotating shaft.

[0017] The present invention has the following advantages:

[0018] (1) The present invention limits the surface quality and plate shape of the quenched incoming steel plate, which can increase the cooling rate of the steel plate in the subsequent processing process and improve the processing quality of the steel plate;

[0019] (2) Different from the prior art in which the steel plate is rapidly heated to the quenching temperature for a period of time and then kept warm for a period of time before being taken out of the furnace for quenching, the steel plate heating of the present invention adopts reversible heating. After entering the furnace, the steel plate is directly heated to the quenching temperature and kept warm for a period of time to ensure that the alloy elements in the steel are fully dissolved. Then, the steel plate is cooled to Bs+ (50-80°C) in the furnace and kept warm for a period of time before quenching. The alloy elements in NiCrMo series steel are relatively high, and no ferrite phase transformation occurs when the steel plate is cooled, that is, there is no Ar3 temperature point. In this way, it can be ensured that the austenite of the steel plate is still in a solid solution state at a temperature above Bs+50°C. In the subsequent quenching process, all martensite or bainite can be obtained. When the steel plate is quenched, due to the low quenching temperature, the thermal stress generated when the steel plate is cooled is small. Only under the action of phase transformation stress, the internal stress of the steel plate is also small, so the quality of the quenched plate shape is greatly improved;

[0020] (3) The present invention adopts segmented reversible heating, and the heating temperature of the rear stage is lower, and the required energy consumption is correspondingly reduced, thereby improving the utilization rate of energy;

[0021] (4) The present invention controls the water ratio, water convexity and flow parameters at different positions of the high-pressure section and the low-pressure section of the steel plate during the quenching process, and cooperates with the quenching support mechanism of the steel plate with multi-angle swing to improve the uniformity of cooling of various parts of the steel plate;

[0022] (5) The thin-gauge NiCrMo steel produced by the technology of the present invention can achieve a first-time qualified rate of steel plates with an unevenness value of ≤5 / 1000mm of ≥95%. Compared with the traditional process adjustment process, the energy consumption per ton of steel can be saved by more than 15% compared with the traditional process. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic flow chart of the control method of the present invention;

[0024] Figure 2 is the CCT curve of typical NiCrMo steel;

[0025] Figure 3 This is a schematic diagram of a steel plate in Example 1 of the present invention;

[0026] Figure 4 This is a schematic diagram of a steel plate in Example 2 of the present invention;

[0027] Figure 5 This is a schematic diagram of a steel plate in Example 3 of the present invention;

[0028] Figure 6 It is a structural schematic diagram of the quenching support mechanism of the present invention;

[0029] Figure 7 It is a schematic diagram of the local structure of the quenching support mechanism of the present invention.

[0030] In the figure:

[0031] 100-quenching support mechanism; 1-quenching water tank; 101-support wall; 2-support frame; 201-support roller; 4-swing mechanism; 401-fixed shaft seat; 402-first rotating shaft; 403-swinging shaft seat; 404-second rotating shaft; 5-overflow trough; 6-pull rope; 7-guide wheel; 8-winch; 9-drain pipe; 10-overflow trough. DETAILED DESCRIPTION

[0032] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0033] like Figure 1 As shown, the present invention provides a method for controlling the shape of a thin NiCrMo quenched and tempered plate, which belongs to the thin ultra-high strength steel plate shape control technology, including key processes such as heating and quenching. Its basic control principle is to reduce the thermal stress during quenching and improve the cooling uniformity to improve the quenched plate shape quality. The specific production process includes the following steps:

[0034] S100, Steel plate quality preparation before quenching: Before quenching, the steel plate surface needs to be shot blasted to ensure that the surface roughness of the steel plate is less than 2.5sa and there is no obvious iron oxide scale residue.

[0035] When there is a certain amount of residual iron oxide on the surface of the steel plate, it will further expand during the subsequent high-temperature heating. When the steel plate is quenched, these iron oxide scales hinder the direct contact between the cooling water and the steel plate, resulting in uneven cooling and deformation of the steel plate surface. When there is iron oxide scale on the surface of the steel plate, its surface cooling rate will be reduced by more than 20%. Therefore, by treating the iron oxide scale on the surface of the steel plate before quenching, it will be beneficial to increase the cooling rate of the steel plate and improve the processing quality of the steel plate.

[0036] In addition, in S100, the steel plates with unevenness ≥ 30 mm / m are repaired or directly scrapped to ensure that the unevenness is less than 30 mm / m before entering the furnace. When the unevenness of the incoming steel plate exceeds 30 mm / m, it is difficult to improve it through heating and quenching processes, and it is easy for production accidents such as steel jamming to occur when the steel plate is passed through the furnace.

[0037] S200, steel plate heating: the steel plate is heated in a reversible manner in the furnace. After entering the furnace, the temperature is quickly raised to the quenching target temperature of 880-920℃, the heating time is 4-8min / mm, and then cooled to the furnace outlet temperature of 450-500℃, that is, Bs+ (50-80℃) and kept warm. The cooling time and the holding time are 2-3min / mm and 1-2min / mm respectively.

[0038] In the present invention, the steel plate is heated by reversible heating, which is completely different from the existing heating process of quenched and tempered plates. The existing heating process of quenched and tempered plates generally involves rapid heating to the quenching temperature for a period of time, and then keeping the temperature for a period of time before quenching.

[0039] In the present invention, the steel plate is directly heated to the quenching temperature after entering the furnace and kept warm for a period of time to ensure that the alloy elements in the steel are fully dissolved, and then cooled to Bs+ (50-80°C) in the furnace and kept warm for a period of time before quenching. This is mainly because the alloy elements in NiCrMo steel are relatively high, and no ferrite phase transformation occurs when the steel plate is cooled (such as Figure 2 The CCT curve shown in the figure) does not have an Ar3 temperature point, which ensures that the austenite of the steel plate is still in a solid solution state when the temperature is above Bs+50°C, and all martensite or bainite can be obtained in the subsequent quenching process.

[0040] When the steel plate is quenched, the thermal stress generated when the steel plate is cooled is small due to the low quenching temperature. Only under the action of phase change stress, the internal stress of the steel plate is also small, and the quality of the quenched plate shape is greatly improved.

[0041] In addition, the heating temperature in the rear section of the segmented reversible heating is lower, and the energy consumption required is also reduced accordingly.

[0042] S300, steel plate quenching: steel plate quenching temperature ≥ Bs + 50 ℃, for 3-6mm steel plate, the quenching rate is 20-35m / min, for > 6-8mm steel plate, the quenching rate is 12-20m / min.

[0043] To control the quality of the quenched plate shape, in addition to reducing the internal stress of the steel plate, it is also necessary to ensure that the steel plate is cooled evenly and symmetrically during quenching. To improve the uniformity of cooling of each part of the steel plate, the present invention controls the water ratio, water convexity, and flow parameters at different positions of the high-pressure section and the low-pressure section of the steel plate during the quenching process. Specifically:

[0044] In the high-pressure section, the water ratio at different positions of the steel plate is between 0.75-0.85, the water flow rate at the middle position of the upper part of the steel plate is 120-180m3 / h, and the water flow rate at the edge is 30-60m3 / h. The flow rate ratio between the middle and the edge (i.e., the water convexity ratio) is 3-4;

[0045] In the low-pressure section, the upper and lower water ratio in the middle of the steel plate is 0.8-0.90, the upper and lower water ratio in the edge is 0.95-1.05, the water convexity ratio is 2.0-3.0, and the water flow rate in the middle position of the steel plate is 50-120m3 / h.

[0046] This is mainly because during quenching, the cooling water on the lower surface of the steel plate falls immediately due to gravity after contacting the steel plate, while the cooling water on the upper surface needs to roll a certain distance before falling after contacting the steel plate. Therefore, the amount of cooling water on the lower surface is higher than that on the upper surface.

[0047] The water volume in the middle of the steel plate is higher than that on both sides because the cooling water in the middle of the steel plate needs to flow out from both sides of the steel plate to take away some heat. Therefore, the cooling water volume in the middle is high and that on both sides is low.

[0048] As for the quenching rate, in the present invention, the quenching rate is still relatively high. This is because the NiCrMo series steel has high alloying elements and good hardenability of the steel plate. At a higher rate, sufficient hardening of the steel plate and production line production efficiency can be ensured.

[0049] The steel plates in existing quenching equipment are mostly supported horizontally. Although some of them have a tilting function, they are mostly tilted on one side, resulting in uneven cooling of the steel plates. Figure 6 and Figure 7As shown, in the embodiment of the present invention, the adjustment and control of the parameters in step S300 can be assisted by a quenching support mechanism 100, wherein the quenching support mechanism 100 comprises a quenching water tank 1, a swing mechanism 4 arranged at the bottom of the quenching water tank 1, and a support frame 2 installed above the swing mechanism 4 for placing a steel plate 10, overflow troughs 5 are arranged on both sides of the quenching water tank 1, and guide wheels 7 are arranged on the other two opposite support walls 101 of the quenching water tank 1, and the four guide wheels 7 correspond to the positions of the four corners of the support frame 2 one by one, and the pull rope 6 connected to the corner of the support frame 2 bypasses the corresponding guide wheel 7 and is connected to the winch 8 outside the quenching water tank 1, and a drainage pipe 9 and a water inlet pipe group (not shown in the figure) are arranged in the quenching water tank 1.

[0050] Among them, the swing mechanism 4 includes a fixed shaft seat 401 arranged at the bottom of the swing mechanism 4, a first rotating shaft 402 is arranged between the fixed shaft seats 401 parallel to the X-axis, a swing shaft seat 403 is rotatably arranged in the middle of the first rotating shaft 402, a second rotating shaft 404 parallel to the Y-axis is mounted on the swing shaft seat 403, and the support frame 2 is arranged on the second rotating shaft 404.

[0051] By adjusting the height of the corners of the support frame 2 connected to each pull rope 6 by the winch 8, the steel plate has more adjustment directions and angles during the quenching process.

[0052] Embodiment 1:

[0053] The steel type selected is 10CrNi5MoV steel, and its chemical composition is: 0.08%C, 0.62%Mn, 0.31%Si, P≤0.010%, S<0.005%, 4.95% Ni, 0.62% Cr, 0.502% Mo, 0.07%V, and the remainder is Fe. Its Bs temperature is 480℃. The steel plate specification is 3×1600mm. Before quenching, the surface roughness of the steel plate is 2.0 and the unevenness is 30mm / m. After the steel plate enters the furnace, it starts to heat and keep warm, and then quench. The specific process is shown in Table 1 and Table 2. After the steel plate is quenched, its unevenness is 5 / 1000mm. The specific object is as follows Figure 3 shown.

[0054] Embodiment 2:

[0055] The steel type selected is 9NiCrMo steel, and its chemical composition is: 0.07%C, 0.60%Mn, 0.15%Si, P≤0.010%, S<0.005%, 9.15% Ni, 0.50% Cr, 0.45% Mo, and the balance is Fe. The steel plate specification is 5×1800mm. Before quenching, the surface roughness of the steel plate is 1.8 and the unevenness is 20mm / m. After the steel plate enters the furnace, it starts to heat and keep warm, and then quench. The specific process is shown in Table 1 and Table 2. After the steel plate is quenched, its unevenness is 4 / 1000mm. The specific object is as follows Figure 4 shown.

[0056] Embodiment 3:

[0057] The steel type selected is 10CrNi7Mo steel, and its chemical composition is: 0.07%C, 0.50%Mn, 0.20%Si, P≤0.010%, S<0.005%, 6.90% Ni, 0.50% Cr, 0.48% Mo, and the balance is Fe. The steel plate specification is 8×2000mm. Before quenching, the surface roughness of the steel plate is 1.5 and the unevenness is 10mm / m. After the steel plate enters the furnace, it starts to heat and keep warm, and then quench. The specific process is shown in Table 1 and Table 2. After the steel plate is quenched, its unevenness is 2 / 1000mm. The specific object is as follows Figure 5 shown.

[0058] Embodiment 4:

[0059] The chemical composition of the steel selected is the same as that of Example 1. The steel plate specification is 6×1800 mm. Before quenching, the surface roughness of the steel plate is 1.8 and the unevenness is 12 mm / m. After the steel plate is put into the furnace, it is heated and kept warm, and then quenched. The specific process is shown in Table 1 and Table 2. After quenching, the unevenness of the steel plate is 3 / 1000 mm.

[0060] Embodiment 5:

[0061] The chemical composition of the steel selected is the same as that of Example 2. The steel plate specification is 4×1700mm. Before quenching, the surface roughness of the steel plate is 1.5 and the unevenness is 18mm / m. After the steel plate is put into the furnace, it starts to be heated and kept warm, and then quenched. The specific process is shown in Table 1 and Table 2. After quenching, the unevenness of the steel plate is 3 / 1000mm.

[0062] Table 1 Example steel plate heating process

[0063]

[0064] Table 2 Example steel plate quenching process

[0065]

[0066] The thin-gauge NiCrMo series steel produced by the technology of the present invention can make the first-time qualified rate of steel plates with unevenness values ​​≤5 / 1000mm ≥95%. Compared with the traditional process adjustment process, the energy consumption per ton of steel can be saved by more than 15% compared with the traditional process.

[0067] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.

Claims

1. A method for controlling the shape of a thin NiCrMo quenched and tempered plate, characterized in that: The following steps are included S100, steel plate quality preparation before quenching: the steel plate surface needs to be shot blasted before quenching to ensure that the surface roughness of the steel plate is less than 2.5Sa and there is no obvious iron oxide scale residue. The thickness of the steel plate is 3-8mm; S200, steel plate heating: The steel plate is heated in a reversible manner in the furnace. After entering the furnace, the temperature is quickly raised to the quenching target temperature of 880-920℃, and then the temperature is lowered to Bs+ (50-80℃) and kept warm; S300, steel plate quenching: the steel plate quenching temperature is ≥ Bs + 50 ° C, and the water ratio, water convexity and flow parameters at different positions of the high-pressure section and low-pressure section of the steel plate are controlled during the quenching process; In the high-pressure section, the water ratio at different positions of the steel plate is between 0.75-0.85, and the water flow rate at the middle position of the upper part of the steel plate is 120-180m 3 / h, edge 30-60m 3 / h, the flow ratio between the middle and the edge is 3-4; In the low-pressure section, the upper and lower water ratios in the middle of the steel plate are 0.8-0.90, the upper and lower water ratios in the edge are 0.95-1.05, the flow ratio between the middle and edge is 2.0-3.0, and the water flow in the middle of the steel plate is 50-120m 3 / h; in S100, the steel plates with unevenness ≥30mm / m are subjected to single correction or direct scrapping to ensure that the unevenness is less than 30mm / m before entering the furnace; in S200, the heating time is 4-8min / mm, the cooling time and the holding time are 2-3min / mm and 1-2min / mm respectively; in S300, for 3-6mm steel plates, the quenching rate is 20-35m / min, and for 6-8mm steel plates excluding 6mm, the quenching rate is 12-20m / min; The NiCrMo is a thin quenched and tempered steel, which is 10CrNi5MoV steel, 9NiCrMo steel or 10CrNi7Mo steel; The adjustment and control of the parameters in step S300 can be assisted by a quenching support mechanism (100), wherein the quenching support mechanism (100) comprises a quenching water tank (1), a swing mechanism (4) arranged at the bottom of the quenching water tank (1), and a support frame (2) installed above the swing mechanism (4) for placing a steel plate (10), overflow grooves (5) are arranged on both sides of the quenching water tank (1), and guide wheels (7) are arranged on the other two opposite support walls (101) of the quenching water tank (1), and the four guide wheels (7) correspond to the positions of the four corners of the support frame (2) one by one, and the pull rope (6) connected to the corner of the support frame (2) bypasses the corresponding guide wheel (7) and is connected to the winch (8) outside the quenching water tank (1), and a drainage pipe (9) and a water inlet pipe group are arranged in the quenching water tank (1); The swing mechanism (4) comprises a fixed shaft seat (401) arranged at the bottom of the swing mechanism (4); a first rotating shaft (402) is arranged between the fixed shaft seats (401) and parallel to the X-axis; a swing shaft seat (403) is rotatably arranged in the middle of the first rotating shaft (402); a second rotating shaft (404) parallel to the Y-axis is sleeved on the swing shaft seat (403); and the support frame (2) is arranged on the second rotating shaft (404).

Citation Information

Patent Citations

  • Plate shape control method for steel plate quenching

    CN103014304B

  • Quenching method of ultra-thin abrasion-resistant steel plate

    CN108441605A

  • A method for producing high-strength, thin-gauge, hot-rolled wear-resistant steel plates with high profile and thin dimensions.

    CN114682642B

  • A segmented quenching control process for ultra-thin high-hardness steel plates

    CN115011764B

  • Method for controlling plate shape of thin quenched steel plate

    CN110983027A