Curing of intumescent coating compositions by pulsed infrared radiation

Pulsed infrared radiation efficiently cures intumescent coatings, reducing time and energy while maintaining fire resistance, addressing the inefficiencies of traditional curing methods.

JP2024538523AActive Publication Date: 2024-10-23PPG COATINGS EURO BV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024516973
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-16
Filing Date
2022-09-16
Publication Date
2024-10-23
Estimated Expiration
2042-09-16

AI Technical Summary

Technical Problem

Existing methods for curing intumescent coatings are time-consuming and energy-intensive, which affects their efficiency in imparting fire resistance to substrates.

Method used

Applying pulsed infrared radiation to intumescent coating compositions to accelerate curing while maintaining fire performance.

Benefits of technology

Significantly reduces curing time and energy consumption while preserving the fire-resistant properties of intumescent coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538523000006
    Figure 2024538523000006
  • Figure 2024538523000007
    Figure 2024538523000007
  • Figure 2024538523000001
    Figure 2024538523000001
Patent Text Reader

Abstract

The present disclosure relates to a method of imparting fire resistance to a substrate by applying an intumescent coating composition onto a surface of the substrate or forming the intumescent coating composition into a self-supporting film or sheet, irradiating with pulsed infrared radiation to form a cured intumescent coating or a cured self-supporting film or sheet, and applying the self-supporting film or sheet to a portion of a surface of the substrate. The present disclosure further relates to the use of the intumescent coating composition and the use of pulsed infrared radiation.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method of imparting fire resistance to a substrate by applying an intumescent coating composition onto a surface of the substrate or forming the intumescent coating composition into a self-supporting film or sheet and irradiating with pulsed infrared radiation to form a cured intumescent coating or a cured self-supporting film or sheet. The present disclosure further relates to the use of the intumescent coating composition and the use of pulsed infrared radiation. [Background technology]

[0002] Intumescent coatings are widely used in various aspects of daily life and industry. Intumescent coatings are generally applied to the surface of a substrate to change the burning properties of the substrate surface so as to retard the rapid spread of fire. Such coatings protect by forming a carbonaceous char when exposed to intense heat. Numerous substrates may benefit from being coated with intumescent coatings, including batteries, e.g., lithium-ion batteries, or structural building components used in commercial facilities and transportation infrastructure, e.g., hotels, airports, concert halls, or offshore sites, chemical plants, oil rigs, etc., that are exposed to extreme heat during fires. However, the method of curing the intumescent coating composition requires a significant amount of time and energy.

[0003] It is therefore an object of the present disclosure to provide a more efficient process for curing intumescent coatings that impart fire resistance to substrates, with the objective of reducing energy consumption and processing time while maintaining the fire performance of the cured intumescent coating.

[0004] This object is solved by the subject matter defined in the appended claims. By irradiating the intumescent coating composition with pulsed infrared radiation, the cure time can be significantly reduced and the fire performance of such intumescent coatings is maintained. Summary of the Invention

[0005] The present disclosure relates to a method of imparting fire resistance to a substrate, the method comprising: (I) applying (i) an intumescent coating composition to a portion of a surface of a substrate, or (ii) forming the intumescent coating composition into a self-supporting film or sheet; (II) irradiating the (i) applied intumescent coating composition or (ii) the self-supporting film or sheet with pulsed infrared light to form a cured intumescent coating or a cured self-supporting film or sheet; and applying the self-supporting film or sheet to a portion of a surface of the substrate.

[0006] The present disclosure also relates to substrates coated according to the methods of the present disclosure. Additionally, the present disclosure is directed to articles comprising substrates according to the present disclosure.

[0007] The present disclosure further relates to the use of the intumescent coating composition in a method of curing the intumescent coating composition by irradiating it with pulsed infrared radiation.

[0008] The present disclosure also relates to the use of pulsed infrared radiation in a method for curing an intumescent coating composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] For the purposes of the following detailed description, it is to be understood that the present disclosure may assume various alternative variations and step sequences, unless expressly specified to the contrary. Moreover, other than in any example or unless otherwise indicated, all numbers expressing the amount of ingredients used in the specification and claims, for example, should be understood as being modified in any case by the term "about". Thus, unless indicated to the contrary, the numerical parameters set forth in the following specification and the appended claims are approximations that may vary depending on the desired properties obtained by the present disclosure. At the very least, and without intending to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should be construed at least in light of the number of reported significant digits and by applying ordinary rounding techniques.

[0010] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the disclosure are approximations, the numerical values ​​set forth in the specific examples are reported as precisely as possible, however, any numerical values ​​inherently contain certain errors necessarily resulting from the standard deviation found in their respective testing measurements.

[0011] It is also to be understood that any numerical range recited herein is intended to include all subranges subsumed therein. For example, a range "1 to 10" is intended to have all subranges between (and including) the recited minimum value of 1 and the recited maximum value of 10, i.e., minimum values ​​equal to or greater than 1 and maximum values ​​equal to or less than 10.

[0012] In this application, the use of the singular includes the plural and the plural encompasses the singular unless otherwise specified. In addition, in this application, although "and / or" may be explicitly used in certain instances, the use of "or" means "and / or" unless otherwise specified. Furthermore, in this application, the use of "a" or "an" means "at least one" unless otherwise specified. For example, "a" polymer, "a" film-forming resin, etc. refer to one or more than one of any of these items.

[0013] The present disclosure relates to a method of imparting fire resistance to a substrate, the method comprising: (I) applying (i) an intumescent coating composition to a portion of a surface of a substrate, or (ii) forming the intumescent coating composition into a self-supporting film or sheet; (II) irradiating the (i) applied intumescent coating composition or (ii) the self-supporting film or sheet with pulsed infrared radiation to form a cured intumescent coating or a cured self-supporting film or sheet; and applying the self-supporting film or sheet to a portion of a surface of the substrate.

[0014] As used herein, the term "intumescent coating" refers to a coating that undergoes expansion, thus increasing in volume and decreasing in density, as well as charring when exposed to heat, e.g., the high temperatures experienced during a fire. As used herein, the term "self-supporting film or sheet" refers to a film or sheet that is capable of supporting itself and holding firm without the support of a substrate.

[0015] According to the present disclosure, a method of imparting fire resistance to a substrate includes the steps of: (I) applying an intumescent coating composition to a portion of a surface of the substrate; and (II) irradiating the applied intumescent coating composition with pulsed infrared radiation to form a cured intumescent coating.

[0016] According to the present disclosure, the expandable coating composition may include a film-forming resin (a). As used herein, the term "film-forming resin" refers to a resin that is capable of forming a self-supporting continuous film on a horizontal surface of a substrate upon removal of any diluent or carrier present in the composition or upon curing at ambient conditions, e.g., at a temperature in the range of 20-25°C, or at elevated temperatures, e.g., at a temperature in the range of 40-200°C. Terms such as "resin" and "resinous" are used interchangeably with terms such as "polymer" and "polymeric". Furthermore, the term "polymer" is used herein in its general sense in the art to refer to a macromolecular compound, i.e., a compound having a relatively high molecular weight (e.g., 500 Da or greater), the structure of which actually or conceptually includes multiple repeating units (also referred to as "mers") derived from a relatively low molecular weight species. Unless otherwise indicated, molecular weights are given on a weight average basis ("M w "), as determined by gel permeation chromatography using polystyrene standards.

[0017] By ambient conditions it is meant that the composition cures without the assistance of heat, such as baking in an oven, the use of forced air, and the like.

[0018] Any film-forming composition can be used according to the present invention. The film-forming resin can react with itself, i.e., undergo a self-crosslinking reaction, or can react with a crosslinking agent. Thus, the expandable coating composition can further comprise a crosslinking agent (b) suitable for crosslinking the film-forming resin (a). The crosslinking agent comprises a functional group capable of reacting with the film-forming resin.

[0019] As used herein, the term "crosslinking" refers to the formation of covalent bonds between polymer chains of constituent polymer molecules. The terms "crosslinking agent", "curing agent", and "crosslinker" are used interchangeably herein. The curing or crosslinking reaction can be induced, for example, by exposing the coating composition to heat or radiation, but can also be carried out at ambient conditions to form a cured coating.

[0020] The type of film-forming resin (a) used in the expandable coating composition is not particularly limited, as any known type of resin can be used in principle. For example, the film-forming resin (a) can include epoxy resin, acrylic resin, polyurethane resin, polyvinyl resin, urea-formaldehyde resin, polyimide resin, melamine resin, polyester resin, cyanate resin, copolymers thereof, or mixtures thereof. According to the present disclosure, the film-forming resin can include epoxy resin, acrylic resin, polyurethane resin, copolymers thereof, or mixtures thereof. In particular, the film-forming resin can include epoxy resin.

[0021] The film-forming resins used in accordance with the present disclosure may contain one or more functional groups that react with each other and / or with the functional groups of the crosslinker. Examples of suitable functional groups include, but are not limited to, ketone, hydrazide, carbodiimide, oxazoline, epoxy, amine, vinyl, amide, carbamate, urea, mercaptan, carboxylic acid, (meth)acryloyl, isocyanate, alkoxysilyl, anhydride, hydroxyl, alkoxy, and combinations thereof.

[0022] Suitable functional groups capable of reacting with each other include, for example, n-methylol amide groups; silane groups with silicone-bonded hydrolyzable or condensable groups, such as chloro, hydroxy, alkoxy, acetoxy, and / or ketoximo groups; azomethine groups; azetidine groups; and groups capable of thermally reversible Diels-Alder reactions, such as furan / maleimide. If the film-forming resin contains functional groups capable of reacting with each other, it is considered to be self-crosslinking, and the presence of a crosslinking agent is not required in the expandable coating composition.

[0023] The film-forming resin may also contain a combination of functional groups capable of self-crosslinking and functional groups that are reactive with the functional groups of the crosslinking agent. In such cases, a crosslinking agent may be present, and upon curing, two crosslinking mechanisms occur: a self-crosslinking reaction of the functional groups of the film-forming resin and a reaction between the functional groups of the crosslinking agent and the functional groups of the film-forming resin.

[0024] According to the present disclosure, the film-forming resin may include an epoxy resin. Suitable epoxy resins may be prepared in a known manner, for example, by reacting a compound containing an epoxide functional group with a cyclic co-reactant containing at least two hydroxyl groups. Examples of suitable compounds containing one epoxide functional group include, but are not limited to, glycidol, epichlorohydrin, glycidolamine, and mixtures thereof. As used herein, the terms "epoxy" and "epoxide" are used interchangeably. Examples of suitable cyclic co-reactants containing at least two hydroxyl groups include, but are not limited to, bisphenol A, hydrated bisphenol A, bisphenol F, hydrated bisphenol F, novolac resins (e.g., phenol novolac, cresol novolac), and mixtures thereof.

[0025] Epoxy resins suitable for use in the present disclosure may include polyepoxides. Polyepoxides typically have at least two 1,2-epoxy groups. The epoxy equivalent weight of the polyepoxides may range from 80 to 600, e.g., 100 to 700. The epoxy equivalent weight may be determined by potentiometric titration according to ASTM D1652. The epoxy compounds may be saturated or unsaturated, cyclic, aliphatic, cycloaliphatic, aromatic, or heterocyclic. The epoxy compounds may include a substituent(s), e.g., halogen, hydroxy, and ether groups.

[0026] Suitable polyepoxides may include, but are not limited to, polyglycidyl ethers of polyphenols, such as 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), resorcinol, hydroquinone, benzenedimethanol, phloroglucinol, bisphenol F, and catechol, or polyols. As used herein, the term "polyol" refers to a compound having more than one hydroxyl group per molecule, such as 2, 3, 4, 5, 6, or more than 6 hydroxyl groups per molecule. Suitable polyols include cycloaliphatic polyols such as 1,2-cyclohexanediol, 1,4-cyclohexanediol, 2,2-bis(4-hydroxycyclohexyl)propane, 1,1-bis(4-hydroxycyclohexyl)ethane, 2-methyl-1,1-bis(4-hydroxycyclohexyl)propane, 2,2-bis(4-hydroxy-3-tert-butylcyclohexyl)propane, 1,3-bis(hydroxymethyl)cyclohexane, and 1,2-bis(hydroxymethyl)cyclohexane, or aliphatic polyols such as trihydroxymethylpentane, ... Examples of suitable polyether glycols include, but are not limited to, ethanediol, ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,2,6-hexanetriol, cyclohexanedimethanol, glycerol, trimethylolpropane, hydrogenated bisphenol A, hydrogenated bisphenol F, or polyether glycols such as poly(oxatetramethylene) glycol, poly(oxyethylene) glycol, poly(oxypropylene) glycol, and neopentanediol.

[0027] Further suitable epoxy resins may include, but are not limited to, polyglycidyl ethers of polycarboxylic acids. As used herein, the term "polycarboxylic acid" refers to a compound having more than one carboxylic acid group per molecule, for example, two, three, four, five, six or more than six carboxylic acid groups per molecule, including the anhydrides of the corresponding acids. Suitable polycarboxylic acids may be formed by the reaction of an epoxy compound, for example, epichlorohydrin, with an aliphatic or aromatic polycarboxylic acid, for example, oxalic acid, succinic acid, glutaric acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, or dimerized linoleic acid. Such resins are commercially available, for example, from Hexion Inc. (USA) under the EPIKOTE and EPON lines.

[0028] Other suitable epoxy resins that may be used in accordance with the present disclosure may include epoxidized olefinically unsaturated alicyclic materials such as epoxy alicyclic ethers and esters, epoxy resins containing oxyalkylene groups, epoxy novolac resins, which are prepared by reacting an epihalohydrin with the condensation product of an aldehyde and a mono- or polyhydric phenol, such as epoxy phenol novolac resins, or epoxy cresol novolac resins.

[0029] It may be advantageous to use flexible polyepoxide resins as the film-forming resins of the expanding coating composition. Flexible polyepoxide resins are generally essentially linear resins, although a small amount of branching is tolerated. Suitable examples of flexible polyepoxides include, but are not limited to, epoxidized soybean oil, dimer acid-based materials, such as EPOL 1010 resin available from BASF (Germany), and rubber-modified polyepoxide resins, such as the product of polyglycidyl ether of bisphenol A and acid-functional polybutadiene. Other suitable examples of flexible polyepoxides may include epoxy-functional adducts prepared from flexible acid-functional polyesters and polyepoxides.

[0030] The acid functional polyester may have an acid number of at least 10 mg KOH / g, e.g., 140-350 mg KOH / g, or 180-260 mg KOH / g. The acid number may be determined according to ASTM D974. The acid functional polyester may be prepared by polyesterification of an organic polycarboxylic acid or anhydride with an organic polyol. The polycarboxylic acid and polyol may be aliphatic or aromatic dibasic acids and diols. Linear polyesters may be preferred over branched polyesters.

[0031] Suitable polyols that can be used to make the polyesters include, but are not limited to, alkylene glycols such as ethylene glycol, diethylene glycol, neopentyl glycol, hydrogenated bisphenol A, cyclohexanediol, cyclohexanedimethanol, carpolactone diol, hydroxyalkylated bisphenols; polyether glycols such as poly(oxytetramethylene) glycol, poly(oxyethylene) glycol, poly(oxypropylene) glycol, and the like; trimethylolpropane; trimethylolethane; pentaerythritol; glycerol; isosorbide; and tetramethylcyclobutenediol. Suitable polycarboxylic acids that can be used to make the polyesters include dicarboxylic acids or anhydrides having 2 to 36 carbon atoms per molecule, such as phthalic acid, isophthalic acid, terephthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, adipic acid, azelaic acid, sebacic acid, maleic acid, glutaric acid, chlorendic acid, tetrachlorophthalic acid, tetrabromophthalic acid, decanedioic acid, dodecanedioic acid, rosin acid, diphenolic acid, gallic acid, and various types of other dicarboxylic acids (e.g., unsaturated C 18 Examples of suitable epoxy functional adducts include, but are not limited to, Diels-Alder adducts of fatty acids. In particular, polyesters used to make the epoxy functional adducts can be prepared from a polycarboxylic acid component comprising a polycarboxylic acid having 7 to 16 carbon atoms, and a polyol comprising diethylene glycol.

[0032] Alternatively or additionally, the film-forming resin may include an acrylic resin. Suitable acrylic resins may be homopolymers or copolymers, which may be obtained by polymerizing one or more monomers, including substituted or unsubstituted (meth)acrylic acids and (meth)acrylates. As used herein, the terms "(meth)acrylic acid" and "(meth)acrylate" and similar terms refer to both the acrylic acid or acrylate and the corresponding methacrylic acid or methacrylate, respectively. Suitable (meth)acrylates may include, but are not limited to, alkyl (meth)acrylates, cycloalkyl (meth)acrylates, alkylcycloalkyl (meth)acrylates, aralkyl (meth)acrylates, alkylaryl (meth)acrylates, aryl (meth)acrylates, and functional group-containing (meth)acrylates. As used herein, the term "functional group" refers to a group that is selected from the group consisting of hydrogen and sp 3It refers to a group that contains one or more atoms other than carbon atoms. Examples of functional groups include, but are not limited to, hydroxyl, carboxylic acid, amide, isocyanate, urethane, thiol, amino, sulfone, sulfoxide, phosphine, phosphite, phosphate, halide, and the like. Non-limiting examples of acrylic resins include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, 4-methyl-2-pentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isobornyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, octadecyl (meth)acrylate, stearyl ...ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth)acrylate, ethyl (meth and acrylic resins derived from butyl (meth)acrylate, benzyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, 3,3,5-trimethyl-cyclohexyl (meth)acrylate, 3-methylphenyl (meth)acrylate, 1-naphthyl (meth)acrylate, 3-phenyl-n-propyl (meth)acrylate, 2-phenyl-aminoethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycidyl (meth)acrylate, or combinations thereof.

[0033] Suitable acrylic resins may include epoxy-functional acrylic resins, which may be prepared by free radical addition polymerization of (meth)acrylate monomers, optionally in combination with vinyl monomers or other monomers containing carbon-carbon double bonds, where the monomer composition includes an epoxy-functional compound having a carbon-carbon double bond.

[0034] Suitable epoxy-functional ethylenically unsaturated monomers include, for example, glycidyl (meth)acrylate, allyl glycidyl ether, vinyl glycidyl ether, vinylcyclohexene oxide, limonene oxide, 2-ethyl glycidyl acrylate, 2-ethyl glycidyl methacrylate, 2-(n-propyl)glycidyl (meth)acrylate, 2-(n-butyl)glycidyl (meth)acrylate, glycidyl methyl (meth)acrylate, (3',4'-epoxyheptyl)-ethyl (meth)acrylate, 6',7'-epoxyheptyl)(meth)acrylate, 7',8'-epoxyheptyl)(meth)acrylate, 8',9'-epoxyheptyl)(meth)acrylate, 9',10'-epoxyheptyl)(meth)acrylate, 10',11'-epoxyheptyl)(meth)acrylate, 10',12'-epoxyheptyl)(meth)acrylate, 10',13'-epoxyheptyl)(meth)acrylate, 10',14'-epoxyheptyl)(meth)acrylate, 10',15'-epoxyheptyl)(meth)acrylate, 10',16'-epoxyheptyl)(meth)acrylate, 10',17'-epoxyheptyl)(meth)acrylate, 10',18'-epoxyheptyl)(meth)acrylate, 10',19'-epoxyheptyl)(meth)acrylate, 10',11'-epoxyheptyl)(meth)acrylate, 10',12'-epoxyheptyl)(meth)acrylate, 10',13'-epoxyheptyl)(meth)acrylate, 10',14'-epoxyheptyl)(meth)acrylate, 10',15'-epoxyheptyl)(meth)acrylate, 10',16'-epoxyheptyl) p-vinylbenzyl glycidyl ether, 3-vinylcyclohexene oxide, α-methylglycidyl methacrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, allyl-3,4-epoxyheptyl ether, 6,7-epoxyheptyl allyl ether, vinyl-3,4-epoxyheptyl ether, 3,4-epoxyheptyl vinyl ether, 6,7-epoxyheptyl vinyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, 3-vinylcyclohexene oxide, α-methylglycidyl methacrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and combinations thereof.

[0035] In preparing the epoxy-functional acrylic resins, additional monomers may be used, such as ethylenically unsaturated nitrile compounds; vinyl aromatic monomers; amides of ethylenically unsaturated acids; ethylenically unsaturated sulfonic acids; ethylenically unsaturated phosphorus-containing acids; vinyl carboxylates; conjugated dienes; monomers having at least two ethylenically unsaturated groups; and combinations thereof.

[0036] Suitable examples of ethylenically unsaturated nitrile monomers include, but are not limited to, aliphatic nitrile monomers containing 2-4 carbon atoms in a linear or branched arrangement and which may be substituted with an acetyl group. Such nitrile monomers include acrylonitrile, methacrylonitrile, α-cyanoethyl acrylonitrile, fumaronitrile, and combinations thereof, with acrylonitrile being particularly suitable.

[0037] Suitable vinyl aromatic monomers can include, but are not limited to, styrene, alpha-methylstyrene, p-methylstyrene, t-butylstyrene, and vinyltoluene.

[0038] Suitable amides of ethylenically unsaturated acids can include, but are not limited to, (meth)acrylamide, and diacetone acrylamide.

[0039] Suitable vinyl ester monomers can include, but are not limited to, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl benzoate, vinyl-2-ethylhexanoate, vinyl stearate, and vinyl esters of versatic acid.

[0040] Suitable ethylenically unsaturated carboxylic acid monomers include, but are not limited to, mono- and dicarboxylic acid monomers, and monoesters of dicarboxylic acids. Ethylenically unsaturated aliphatic mono- or dicarboxylic acids or anhydrides containing 3 to 5 carbon atoms are particularly suitable. Examples of monocarboxylic acid monomers include, but are not limited to, (meth)acrylic acid, crotonic acid, and examples of dicarboxylic acid monomers include, but are not limited to, fumaric acid, itaconic acid, maleic acid, and maleic anhydride. Examples of other suitable ethylenically unsaturated acids include vinyl acetic acid, vinyl lactic acid, vinyl sulfonic acid, 2-methyl-2-propene-1-sulfonic acid, styrene sulfonic acid, acrylamidomethylpropane sulfonic acid, and salts thereof.

[0041] Suitable conjugated diene monomers include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 1,3-octadiene, 2-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-hexadiene, 2,3-diethyl-1,3-butadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, 3,7-dimethyl-1,3,6-octatriene, 2-methyl-6-methylene-1,7-octadiene, 7-methyl-3-methylene-1,7-octadiene, 8-methyl-1,3-hexadiene, 9-methyl-1,3-hexadiene, 10-methyl-1,3-hexadiene, 11-methyl-1,3-hexadiene, 12-methyl-1,3-hexadiene, 13-methyl-1,3-hexadiene, 14-methyl-1,3-hexadiene, 15-methyl-1,3-hexadiene, 16-methyl-1,3-hexadiene, 17-methyl-1,3-hexadiene, 18-methyl-1,3-hexadiene, 19-methyl-1,3-hexadiene, 20-methyl-1,3-hexadiene, 21-methyl-1,3-hexadiene, 22-methyl-1,3-hexadiene, 23-methyl-1,3-hexadiene, 24-methyl-1,3-hexadiene, 25-methyl-1,3-hexadi ,6-octadiene, 1,3,7-octatriene, 2-ethyl-1,3-butadiene, 2-amyl-1,3-butadiene, 3,7-dimethyl-1,3,7-octatriene, 3,7-dimethyl-dimethyl-1,3,6-octariene, 3,7,11-trimethyl-1,3,6,10-dodecatetraene, 7,11-dimethyl-3-methylene-1,6,10-dodecatriene, 2,6-dimethyl-2,4,6-octatriene, 2-phenyl-1,3-butadiene, and 2-methyl-3-isopropyl-1,3-butadiene, 1,3-cyclohexadiene, and combinations thereof.

[0042] Alternatively or additionally, the film-forming resin may comprise a polyurethane resin.Suitable polyurethane resins may be prepared in a known manner, for example by reacting a polyisocyanate with a polyol.As used herein, the term "polyisocyanate" refers to a compound having more than one isocyanate group per molecule, for example, two, three, four, five, six or more than six isocyanate groups per molecule. Suitable polyisocyanates include aliphatic polyisocyanates such as 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, 1,6-hexamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and 4,4'-methylene-bis(cyclohexylisocyanate); aromatic polyisocyanates such as 4,4'-diphenylmethane diisocyanate, toluene diisocyanate, 1,2,4-benzene triisocyanate, tetramethylxylylene diisocyanate, and polymethylene polyphenylisocyanate; and combinations thereof. Non-limiting examples of suitable polyols are the polyols described above. In particular, polyurethanes prepared by reacting polyester polyols or acrylic polyols with polyisocyanates at OH / NCO equivalent ratios greater than 1:1, such that free hydroxyl groups are present in the product, are suitable. A suitable polyurethane resin that may be used according to the present disclosure may be exemplified by the reaction product of Desmodur N 3300, available from Covestro (Germany), with an alkylene glycol, such as ethylene glycol or propylene glycol.

[0043] Alternatively or additionally, the film-forming resin can comprise polyvinyl resin.Suitable polyvinyl resin can be homopolymer or copolymer, which can be obtained by polymerizing one or more monomers, including vinyl aromatic compounds, such as styrene and vinyltoluene; nitriles, such as (meth)acrylonitrile; vinyl and vinylidene halides, such as vinyl chloride and vinylidene fluoride; and vinyl esters, such as vinyl acetate.Suitable polyvinyl resins that can be used according to the present disclosure can be exemplified by the vinyl resins under the trademark LUMIFLON™, available from AGC Chemicals Europe, Ltd. (Netherlands).

[0044] Alternatively or additionally, the film-forming resin can comprise urea-formaldehyde resin.Suitable urea-formaldehyde resin can be prepared in a known manner, for example by condensation of formaldehyde with urea.Suitable examples of urea-formaldehyde resin can include, but are not limited to, urea-formaldehyde resin with the trademark Kaurit (registered trademark) available from BASF (Germany) and urea-formaldehyde resin with the trademark Casco (registered trademark) Resin available from Hexion Inc. (USA), for example Casco (registered trademark) Resin CR-5H.

[0045] Alternatively or additionally, the film-forming resin may comprise a polyimide resin. Suitable polyimide resins may be prepared in a known manner, for example by reacting a polyanhydride with a polyamine or by reacting a polyanhydride with a polyisocyanate. Suitable polyanhydrides and polyisocyanates are those described above. As used herein, the term "polyamine" refers to a compound having more than one amine group per molecule, for example, two, three, four, five, six or more amine groups per molecule.Suitable polyamines include aliphatic diamines, such as 1,2-ethanediamine, 1,2-propanediamine, 1,3-propanediamine, 1,2-butanediamine, 1,3-butanediamine, 1,4-butanediamine, 1,3-pentanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 2-methyl-1,5-pentanediamine, 2,5-dimethylhexane-2,5-diamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 3,3-amino-bis-propylamine, triethylenetetramine, and tetraethylenepentamine; alicyclic diamines, such as 2,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, silmethane, isophoronediamine, 1,3-bis(aminoethyl)cyclohexane, bis(4-aminocyclohexyl)methane-aminoethylpiperazine, and 3,3'-diethyl-4,4'-diaminodicyclohexylmethane; and aromatic diamines such as 1,2-benzenediamine, 1,3-benzenediamine, 1,4-benzenediamine, 1,5-naphthalenediamine, 1,8-naphthalenediamine, 2,4-toluenediamine, 2,5-toluenediamine, 2,6-toluenediamine, xylylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-diethyldiphenylmethane, diaminodiphenylsulfone, and 3,3'-dimethyl-4,4'-biphenyldiamine, and reaction products of polyamines with aliphatic fatty acids, such as, but not limited to, the VERSAMID series of materials available from BASF (Germany). Suitable examples of polyimide resins include, but are not limited to, polyimide resins sold under the trademark Kerimid® by Huntsman Corp. (USA), such as 701 A N-70, Kerimid 8292 N-75, and Kerimid 8292 NPM 60.

[0046] Alternatively or additionally, the film-forming resin may comprise a melamine resin.Suitable melamine resins may be prepared in a known manner, for example by reacting melamine with formaldehyde.Suitable examples of melamine resins may include, but are not limited to, CYMEL 1156, available from Allnex (Germany).

[0047] Alternatively or additionally, the film-forming resin may comprise a polyester resin. Suitable polyester resins may be prepared in a known manner, for example, by condensation of a polyol with a polycarboxylic acid or by ring-opening polymerization of a lactone. Non-limiting examples of suitable polyols are the polyols described above, and non-limiting examples of polycarboxylic acids are the polycarboxylic acids described above. Suitable lactones may include, but are not limited to, β-propiolactone, γ-butyrolactone, δ-valerolactone, ε-caprolactone, α-angelica lactone, and mixtures thereof. Suitable polyester resins that may be used according to the present disclosure may be exemplified by polyester resins under the trademark SETAL®, such as SETAL® 1715 VX-74, SETAL® 91703 SS-53, and SETAL® 91715 SS-55, available commercially from Allnex Germany GmbH (Germany).

[0048] Alternatively or additionally, the film-forming resin may comprise a cyanate resin. Suitable cyanate resins may be exemplified by those cyanate resins under the trademark AroCy® available from Huntsman Corp. (USA), such as AroCy L-10, AroCy XU 366, AroCy 371, or Arocy XU 378.

[0049] According to the present disclosure, the film-forming resin may include, for example, a combination of an epoxy resin and an acrylic resin, or an epoxy resin and a polyurethane resin, as disclosed in US Pat. No. 5,108,832, or US Pat. No. 5,070,119.

[0050] The expandable coating composition may comprise any suitable amount of film-forming resin (a). For example, the expandable coating composition may comprise 5% or more by weight, for example 8% or more by weight, or 10% or more by weight, or 12% or more by weight, or 15% or more by weight of film-forming resin (a). The expandable coating composition may comprise, for example, less than 40% or less by weight, for example less than 35% or less by weight, or 32% or less by weight, or 30% or less by weight, or 28% or less by weight, or 25% or less by weight of film-forming resin. The expandable coating composition may, for example, comprise the film-forming resin (a) in an amount ranging between any of the values ​​mentioned above, such as, for example, 5-40% by weight, or 8-35% by weight, or 10-35% by weight, or 10-30% by weight, or 10-28% by weight, or 12-25% by weight, the weight percentages being based on the total solids weight of the expandable coating composition.

[0051] As mentioned above, the expandable coating composition may also include a crosslinking agent (b). Any suitable crosslinking agent (b) may be used according to the present disclosure, which is selected by those skilled in the art to react with the functional groups of the film-forming resin. According to the present disclosure, the crosslinking agent (b) may include a polyamine, such as a polyetheramine, a polyamide, a polyepoxide, an aminoplast resin, a phenolic resin, a polyisocyanate, a polythiol, a polyol, a copolymer thereof, or a mixture thereof. The crosslinking agent (b) may specifically include a polyamine.

[0052] The crosslinking agent may be a latent or blocked crosslinking agent, where the functional groups of the crosslinking agent that react with the functional groups of the film-forming resin are generated or restored in a reaction that unblocks at curing conditions, e.g., at elevated temperatures, e.g., above 120°C. Suitable crosslinking agents of this type are, for example, blocked polyisocyanates. As used herein, the term "polyisocyanate" is intended to include blocked polyisocyanates, as well as free polyisocyanates. Latent or blocked crosslinking agents are particularly suitable for providing single-component compositions to ensure sufficient storage stability and pot life prior to application and curing. Examples of suitable blocking agents include materials that unblock at elevated temperatures, e.g., above 120°C, such as lower aliphatic alcohols having 1 to 6 carbon atoms, e.g., methanol, ethanol, and n-butanol; alicyclic alcohols, e.g., cyclohexanol; aromatic alkyl alcohols, e.g., phenylcarbinol and methylphenylcarbinol; and phenolic compounds, e.g., phenol itself, as well as substituted phenols, e.g., cresol and nitrophenol, where the substituents do not affect the coating operation. Glycol ethers can also be used as blocking agents.Suitable glycol ethers include ethylene glycol butyl ether, diethylene glycol butyl ether, ethylene glycol methyl ether, and propylene glycol methyl ether.Other suitable blocking agents include oximes such as methyl ethyl ketoxime, acetone oxime, and cyclohexanone oxime;lactams such as epsilon-caprolactam;pyrazoles such as dimethylpyrazole;and amines such as dibutylamine.

[0053] Crosslinker (b) can include polyamine. As used herein, the term "polyamine" refers to a compound having more than one amine group per molecule, for example, two, three, four, five, six or more amine groups per molecule. Suitable crosslinkers can include, for example, aliphatic polyamines, aromatic polyamines, polyamine amides, polyether amines, polysiloxane amines, polysulfide amines, or combinations thereof.

[0054] Suitable polyamines include aliphatic diamines, such as 1,2-ethanediamine, 1,2-propanediamine, 1,3-propanediamine, 1,2-butanediamine, 1,3-butanediamine, 1,4-butanediamine, 1,3-pentanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 2-methyl-1,5-pentanediamine, 2,5-dimethylhexane-2,5-diamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 3,3-amino-bis-propylamine, triethylenetetramine, and tetraethylenepentamine; alicyclic diamines, such as 2,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, silmethane, isophoronediamine, 1,3-bis(aminoethyl)cyclohexane, bis(4-aminocyclohexyl)methane-aminoethylpiperazine, and 3,3'-diethyl-4,4'-diaminodicyclohexylmethane; and aromatic diamines such as 1,2-benzenediamine, 1,3-benzenediamine, 1,4-benzenediamine, 1,5-naphthalenediamine, 1,8-naphthalenediamine, 2,4-toluenediamine, 2,5-toluenediamine, 2,6-toluenediamine, xylylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-diethyldiphenylmethane, diaminodiphenylsulfone, and 3,3'-dimethyl-4,4'-biphenyldiamine, and reaction products of polyamines with aliphatic fatty acids, such as, but not limited to, the VERSAMID series of materials available from BASF (Germany).

[0055] In addition, any of the above polyamine adducts may be used. The polyamine adducts may be formed by reacting a polyamine with a suitable reactive compound, such as an epoxy resin. This reaction reduces the free amine content in the curing agent, making it more useful in low temperature and / or high humidity environments.

[0056] According to the present disclosure, polyamines can include polyetheramines, such as Jeffamines commercially available from Huntsman Corp. (USA), including, but not limited to, Jeffamine D-230, Jeffamine D-400, Jeffamine 600, Jeffamine 1000, Jeffamine 2005, and Jeffamine 2070.

[0057] Alternatively or additionally, the crosslinker (b) may comprise a polyamide. Suitable polyamides may be prepared by reacting a polyamine with a polycarboxylic acid or by ring-opening polymerization of a lactam. Non-limiting examples of suitable polyols are the polyols described above, and non-limiting examples of suitable polyamines are the polyamines described above. Suitable lactams may include, but are not limited to, β-propiolactam, γ-butyrolactam, δ-valerolactam, ε-caprolactam, and mixtures thereof. Specifically, the polyamide may contain the reaction product of a dimer fatty acid with a polyethyleneamine, and a small amount of a monomeric fatty acid. The dimer fatty acid is prepared by oligomerization of a monomeric fatty acid. The polyethyleneamine may be any higher polyethyleneamine, such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, with diethylenetriamine being the most commonly used. When a polyamide is used as a crosslinker, it may impart one or more desirable properties to the intumescent coating, such as corrosion resistance, water resistance, and / or good flexibility.

[0058] Alternatively or additionally, the crosslinker (b) may comprise a polyepoxide. Non-limiting examples of suitable polyepoxides are those described above.

[0059] Alternatively or additionally, the crosslinker (b) may comprise an aminoplast resin. Suitable aminoplast resins may be obtained from the condensation reaction of an aldehyde, such as formaldehyde, with a compound containing at least two amine or amide groups per molecule. Suitable examples of aldehydes include, but are not limited to, formaldehyde, acetaldehyde, crotonaldehyde, and benzaldehyde. Suitable examples of compounds containing at least two amine or amide groups include, but are not limited to, melamine, urea, and benzoguanamine. Suitably, the aminoplast resin may be etherified, typically with an alcohol, such as methanol, ethanol, butanol, or mixtures thereof. Suitable aminoplast resins that may be used in accordance with the present disclosure may be exemplified by Maprenal® Amino Resins, such as Maprenal MF 612 / 70B, Maprenal MF 613 / 71B, and Maprenal MF 650 / 55IB, available from Prefere Resin Holding GmbH (Germany); Cymel® Amino Crosslinkers, such as Cymel 303, Cymel 202, Cymel 1161, Cymel 325, and Cymel 1133, available from Allnex Industries (Germany); Setamine® amino resins, such as Setamine US-138 BB-70, and Setamine US-146 BB-72, available from Allnex (Germany).

[0060] Alternatively or additionally, the crosslinker (b) may comprise a phenoplast resin. Suitable phenoplast resins may be obtained by either acid-catalyzed (novolac) or base-catalyzed (resol) addition polymerization of phenol and formaldehyde. Suitable phenoplast resins that may be used according to the present disclosure may be exemplified by EPON™ Epoxy Novolac resins, such as EPON™ Resin SU-8, available from Hexion Inc. (USA).

[0061] Alternatively or additionally, the crosslinking agent (b) may comprise a polyisocyanate. Non-limiting examples of suitable polyisocyanates are those described above.

[0062] Alternatively or additionally, crosslinker (b) can comprise polythiol.Suitable polythiol can include, but is not limited to, polysulfide thiol, polyether thiol, polyester thiol, pentaerythritol-based thiol, or combinations thereof.A particularly suitable polythiol is Thioplast G4, available from Akzo Nobel Functional Chemicals GmbH&Co.KG (Germany).

[0063] Alternatively or additionally, the cross-linking agent (b) may comprise a polyol. Non-limiting examples of suitable polyols are those described above.

[0064] As mentioned above, when the film-forming resin (a) comprises an epoxy resin, the crosslinker (b) comprises a polyamine, a polythiol, or a combination thereof, specifically, when the film-forming resin (a) comprises an epoxy resin, the crosslinker (b) comprises a polyamine.

[0065] The intumescent coating composition may include the crosslinker (b) in any suitable amount. For example, the intumescent coating composition may include 5% or more by weight, e.g., 8% or more by weight, or 10% or more by weight, or 12% or more by weight, or 15% or more by weight of the crosslinker (b). The intumescent coating composition may include, for example, 40% or less by weight, e.g., 35% or less by weight, or 32% or less by weight, or 30% or less by weight, or 28% or less by weight, or 25% or less by weight of the film-forming resin. The expandable coating composition may, for example, comprise the crosslinker (b) in an amount ranging between any of the values ​​mentioned above, such as, for example, 5-40% by weight, or 8-35% by weight, or 10-35% by weight, or 10-30% by weight, or 10-28% by weight, or 12-25% by weight. The weight percentages are based on the total solids weight of the expandable coating composition.

[0066] The intumescent coating composition may further comprise a compound (c) that provides an expansion gas upon pyrolysis. The expansion gas serves to foam and expand the intumescent composition when exposed to high temperatures, e.g., above 150°C, or flame. As a result of this expansion, the char formed is a thick, multi-cell material that serves to insulate and protect the underlying substrate. Any suitable source of expansion gas that may be used in the intumescent composition of the present disclosure is a nitrogen-containing material. Suitable nitrogen-containing materials include, but are not limited to, melamine, phosphates, guanidine, methylolated melamine, hexamethoxymethylmelamine, urea, dimethylurea, melamine pyrophosphate, dicyandiamide, guanylurea phosphate, and glycine. Other conventional sources of expansion gas, such as materials that liberate carbon dioxide, may also be used. Suitable examples of materials that liberate carbon dioxide are alkaline earth metals, e.g., calcium carbonate or magnesium carbonate. Compounds that release water vapor upon decomposition upon heating, such as calcium hydroxide, magnesium dihydroxide, or aluminum trihydroxide, may also be used, as may expandable graphite. Other examples of such compounds are also borate sources, such as boric acid, and boric acid derivatives, such as boric acid esters and metal borates. Specifically, the compound (c) that provides expansion gas upon pyrolysis may include melamine, melamine derivatives, guanidine, methylol melamine, hexamethoxymethyl melamine, urea, dimethyl urea, melamine pyrophosphate, dicyandiamide, guanylurea phosphate, glycine, alkaline earth metal carbonates, calcium hydroxide, magnesium dihydroxide, aluminum trihydroxide, expandable graphite, or mixtures thereof.

[0067] For example, a compound (c) that provides an expansion gas upon thermal decomposition, such as melamine, may be used in the intumescent coating composition of the present disclosure in an amount of 1% or more by weight, such as 2% or more by weight, or 3% or more by weight. The composition according to the present disclosure may contain the compound (c) that provides an expansion gas upon thermal decomposition in an amount of, for example, less than 10% or less by weight, or less than 8% or less by weight, or less than 7% or less by weight, or less than 5% or less by weight. The composition may contain the compound (c) that provides an expansion gas upon thermal decomposition in an amount ranging between any of the values ​​mentioned above, such as 1-10% by weight, or 2-7% by weight. The weight percentage is based on the total solids weight of the intumescent coating composition.

[0068] The expandable coating composition of the present disclosure includes, inter alia, (a) a film-forming resin, (b) a crosslinker, and (c) a compound that provides an expanding gas upon thermal decomposition. According to the present disclosure, compounds (a)-(c) are different from each other.

[0069] The expandable coating composition of the present disclosure may further comprise an epoxy-reactive diluent. Suitably, the epoxy-reactive diluent is operable to reduce the viscosity of the composition.

[0070] Suitable epoxy reactive diluents may be produced by any suitable method. Such epoxy reactive diluents may be formed from the reaction of a compound containing an aliphatic epoxide functional group, such as a diglycidyl ether, with an aliphatic alcohol or polyol. Examples of suitable compounds containing an epoxide functional group may include, but are not limited to, monoglycidyl ethers, diglycidyl ethers, triglycidyl ethers, and mixtures thereof. Examples of suitable alcohols and polyols may include, but are not limited to, hexanediol, butanediol, glycerol, trimethylolpropane, trimethylolethane, pentaerythritol, neopentyl glycol, and mixtures thereof. Specifically, the epoxy reactive diluent may include a diglycidyl ether of an aliphatic alcohol. Suitably, the epoxy reactive diluent may include a diglycidyl ether of hexanediol and / or a diglycidyl ether of neopentyl glycol.

[0071] The intumescent coating composition of the present disclosure, when present, may comprise reactive epoxy diluents in an amount of at or above 1 wt%, e.g., at or above 2 wt%, or at or above 3 wt%, or at or above 4 wt%, or at or above 5 wt%, or at or above 6 wt%. The intumescent coating composition, when present, may comprise reactive epoxy diluents in an amount of less than at or below 30 wt%, e.g., less than at or below 20 wt%, or less than at or below 15 wt%, or less than at or below 10 wt%. The intumescent coating composition, when present, may comprise reactive epoxy diluents in an amount ranging between any of the values ​​mentioned above, e.g., 1-30 wt%, e.g., 2-20 wt%, or 3-15 wt%, or 5-10 wt%. The weight percentages are based on the total solids weight of the intumescent coating composition.

[0072] The intumescent coating composition of the present disclosure may further comprise a phosphate compound. As used herein, the term "phosphate compound" refers to any phosphorus-containing material, including phosphoric acid or its condensation or dehydration products (including oxides), or salts, esters, amides, or other derivatives of any of the foregoing. The phosphate compound may include a variety of materials, such as phosphoric acid, mono- and diammonium phosphates, triphenyl phosphate, tris-(2-chloroethyl) phosphate, tris-(2-chloroisopropyl) phosphate, ammonium polyphosphate, melamine pyrophosphate, and combinations thereof. Ammonium polyphosphate has the formula (NH 4 ) n+2 P n O 3n+1 where n is an integer of at least 2, and preferably n is an integer of at least 50.

[0073] The intumescent coating composition of the present disclosure, when present, may comprise a phosphate compound in an amount of 15% or more by weight, e.g., 20% or more by weight, or 25% or more by weight, or 30% or more by weight, or 35% or more by weight, or 40% or more by weight. The intumescent coating composition, when present, may comprise a phosphate compound in an amount of less than 55% or less by weight, e.g., 50% or less by weight, or 45% or less by weight, or 40% or less by weight, or 35% or less by weight. The intumescent coating composition, when present, may comprise a phosphate compound in an amount ranging between any of the above mentioned values, e.g., 15-55% by weight, e.g., 20-50% by weight, or 25-40% by weight, or 40-55% by weight. The weight percentages are based on the total solids weight of the intumescent coating composition.Phosphorus is believed to function as a char promoter in the intumescent composition.

[0074] The expandable coating composition of the present disclosure may further comprise a borate compound. As used herein, the term "borate compound" refers to any boron-containing material, which contains boric acid or its condensation or dehydration products (including oxides), or any of the salts or esters of the foregoing. According to the present disclosure, the borate compound may include ammonium pentaborate, boric acid, metal borates such as zinc borate, boron oxide, sodium borate, potassium borate, ammonium borate, borate esters such as butyl borate and phenyl borate, or mixtures thereof.

[0075] The intumescent coating composition of the present disclosure, when present, may comprise borate compounds in an amount of 5% or more by weight, e.g., 6% or more by weight, or 7% or more by weight, or 8% or more by weight, or 9% or more by weight, or 10% or more by weight. The intumescent coating composition, when present, may comprise borate compounds in an amount of less than 35% or less by weight, e.g., 30% or less by weight, or 25% or less by weight, or 20% or less by weight. The intumescent coating composition, when present, may comprise borate compounds in an amount ranging between any of the values ​​mentioned above, e.g., 5-35% by weight, or 5-30% by weight, or 9-15% by weight. The weight percentage is based on the total solids weight of the intumescent coating composition.

[0076] The expandable coating composition of the present disclosure may further include an aluminum compound. As used herein, the term "aluminum compound" refers to any aluminum-containing material. Typically, the aluminum compound may include inorganic aluminum compounds. Suitable aluminum compounds may include aluminum hydroxide, aluminum oxide (alumina), aluminum salts such as aluminum chloride, and combinations thereof. For example, the aluminum compound may include aluminum hydroxide and / or aluminum oxide.

[0077] The intumescent coating composition of the present disclosure, when present, may comprise aluminum compounds in an amount of greater than or equal to 0.1% by weight, such as greater than or equal to 0.2% by weight, or greater than or equal to 0.3% by weight, or greater than or equal to 0.5% by weight, or greater than or equal to 1% by weight, greater than or equal to 3% by weight, or greater than or equal to 5% by weight. The intumescent coating composition, when present, may comprise aluminum compounds in an amount of less than or equal to 10% by weight, such as less than or equal to 9% by weight, or less than or equal to 8% by weight, or less than or equal to 5% by weight, or less than or equal to 3% by weight, or less than or equal to 1% by weight, or less than or equal to 0.7% by weight. The intumescent coating composition, when present, may include the aluminum compound in an amount ranging between any of the values ​​mentioned above, such as, for example, 0.1 to 10 weight percent, or 0.2 to 8 weight percent, or 0.3 to 1 weight percent, the weight percentages being based on the total solids weight of the intumescent coating composition.

[0078] The expandable coating composition of the present disclosure may further comprise a silica compound.As used herein, the term "silica compound" refers to any silicon-containing material, which contains silicic acid, its condensation products or dehydration products (including oxides), or any of the salts or esters of the foregoing.Suitable silica compounds may include fumed silica, or quartz, or materials containing silica, such as bentonite or kaolin, or mixtures thereof.

[0079] The intumescent coating composition of the present disclosure, when present, may contain silica compounds in an amount of more than 0.1% by weight, e.g., more than 0.2% by weight, or more than 0.3% by weight, more than 0.4% by weight, or more than 0.5% by weight. The intumescent coating composition, when present, may contain silica compounds in an amount of less than 5% by weight, e.g., less than 3% by weight, or less than 2% by weight, or less than 1% by weight, or less than 0.8% by weight. The intumescent coating composition, when present, may contain silica compounds in an amount ranging between any of the values ​​mentioned above, e.g., 0.1-5% by weight, or 0.4-1% by weight. The weight percentage is based on the total solids weight of the intumescent coating composition.

[0080] The expandable coating composition of the present disclosure may include a borate compound, an aluminum compound, or a silica compound. Thus, the expandable coating composition of the present disclosure may contain, for example, one of a borate compound, an aluminum compound, or a silica compound. For example, the expandable coating composition may include a borate compound. Alternatively, the expandable coating composition may include an aluminum compound or a silica compound. On the other hand, the expandable coating composition may also include a combination of two or more than two of a borate compound, an aluminum compound, and / or a silica compound. For example, the expandable coating composition according to the present disclosure may include an aluminum compound and a silica compound, or a borate compound and an aluminum compound, or a borate compound and a silica compound. The expandable coating composition may include a borate compound, an aluminum compound, and a silica compound.

[0081] The intumescent coating composition of the present disclosure is comprised of titanium dioxide (TiO 2 The expandable coating composition according to the present disclosure, when present, may further comprise TiO 2The intumescent coating composition, when present, may comprise at or above 5 wt.%, for example at or above 6 wt.%, or at or above 7 wt.%, or at or above 8 wt.%, or at or above 9 wt.%, or at or above 10 wt.%. 2 In some embodiments, the intumescent coating composition may comprise at or below 20% by weight, e.g., at or below 19% by weight, or at or below 18% by weight, or at or below 17% by weight, or at or below 15% by weight, or at or below 13% by weight, or at or below 10% by weight. 2 in an amount ranging between any of the above-mentioned values, such as 5-20 wt.%, or 5-10 wt.%, or 10-18 wt.%, the weight percentages being based on the total solids weight of the expandable coating composition.

[0082] Specifically, the intumescent coating composition comprises TiO 2 and a phosphate source may include a borate compound, an aluminum compound, or a silica compound in the ranges described above. Such intumescent coating compositions provide intumescent coatings with desirable char formation, in particular in combination with desirable adhesion to the substrate. "Desired char formation" means that the char is not easily cracked or removed by direct flame blasting, and the expansion coefficient, which is the ratio between the thickness of the char and the thickness of the coating film, may be 5 to 25, for example 7 to 20. "Desired adhesion" means that the char remains substantially intact during direct flame blasting, and no appreciable detachment of the char from the substrate occurs during or after the fire test.

[0083] According to the present disclosure, the intumescent coating composition may be applied to a portion of a surface of a substrate by any means standard in the art, such as electrocoating, spray application, electrostatic spray application, dipping, rolling, brushing, and the like. The intumescent coating composition of the present invention may be applied to provide various dry film thicknesses ("DFT") as needed. The intumescent coating composition may be applied to a portion of a surface of a substrate to obtain a dry coating thickness ranging from 0.1 to 15 mm, e.g., 0.2 to 14 mm, or 0.5 to 13 mm, or 0.5 to 12 mm, or 0.7 to 10 mm. The thickness may be determined according to DIN EN ISO 2178:2016. As used herein, "dry coating thickness" is the thickness of a coating applied to a portion of a surface of a substrate and measured on the substrate after the coating has cured. The desired dry film thickness ("DFT") may vary depending on the application. For use on architectural structural components, a DFT ranging from 0.1 to 15 mm, e.g., 0.3 to 1 mm, or 3 to 15 mm may be suitable. For use in lithium batteries, a DFT in the range of 0.2 to 5 mm, for example 0.2 to 1 mm, or 1 to 5 mm, may be suitable.

[0084] Alternatively, the intumescent coating composition of the present disclosure is formed into a self-supporting film or sheet. In general, the intumescent coating composition of the present disclosure may be formed into a film or sheet by any technique known to those skilled in the art, such as by impregnating a mesh with the coating, by a casting molding process, or the like. The film or sheet may be cured to form a cured intumescent self-supporting film or sheet prior to application of the cured intumescent self-supporting film or sheet to a substrate. It is also within the scope of the present disclosure for an uncured film or sheet to be applied to a substrate after the forming step and then subsequently cured to obtain a cured intumescent layer according to the present disclosure. The film or sheet may be applied to a substrate through an adhesive. The intumescent coating composition may be formed into a self-supporting film or sheet having a dry film thickness ranging from 0.1 to 15 mm, for example, from 0.2 to 14 mm, or from 0.5 to 13 mm, or from 0.5 to 12 mm, or from 0.7 to 10 mm.

[0085] The intumescent coating composition of the present disclosure may further comprise one or more additional additives suitable for use in intumescent coatings. Examples of such additives include zinc sources, acid sources, reinforcing fillers, carbon sources, inorganic fillers, rheological additives, organic solvents, pigments, foam stabilizers, and combinations thereof.

[0086] The zinc source may contribute to the formation of small cell structures in the char. Small cells in the char may provide better insulation of the substrate and better preserve the integrity of the char and adhere to the substrate. Thus, cracking and breaking of the char from the substrate is minimized, providing a stronger measure of protection to the underlying substrate. Suitable examples of zinc sources may include, but are not limited to, zinc oxide, zinc salts such as zinc borate and zinc phosphate, zinc carbonate, and zinc metal.

[0087] Suitable examples of acid sources can include, but are not limited to, ammonium phosphate, ammonium polyphosphate, diammonium diphosphate, diammonium pentaborate, phosphoric acid generating materials, boric acid, metal or organic borates, and combinations thereof.

[0088] It should be understood that many of the components of the intumescent coating composition can serve more than one function in the composition. For example, the phosphorus compound, zinc source, borate compound, and compound that provides an expanding gas upon pyrolysis can each be provided by separate feedstocks, or alternatively, a single material can be the source of more than one of these components. For example, melamine pyrophosphate can provide both a source of phosphorus and an expanding gas, zinc borate can provide a zinc source and a borate source, and zinc phosphate can provide a zinc source and a phosphate source.

[0089] The reinforcing filler may be selected from a number of conventionally used materials, including fibrous and platelet reinforcements, which may be more suitable than other fillers. Examples of fibrous reinforcements include glass fiber, ceramic fibers, such as aluminum oxide / silicon oxide, graphite fiber, mineral fiber, and basalt fiber. Platelet reinforcements include hammer mill glass flake, mica, and wollastonite. Other suitable fillers include metal oxides, clay, talc, silica, diatomaceous earth, LAPINUS fiber, and various pigments. It is believed that the reinforcing filler helps to control the expansion of the fire-resistant composition before and during char formation so that the resulting char is hard and uniform. When present, reinforcing fillers, such as glass fiber and / or mineral fiber, are usually present in the intumescent coating composition in an amount of 5.0% or less by weight, such as 4% or less by weight, such as 3% or less by weight. The intumescent coating composition according to the present disclosure may include reinforcing fillers in an amount of, for example, 0.1% or more by weight, for example, 0.2% or more by weight, 0.5% or more by weight, or 1% or more by weight. The intumescent coating composition may include reinforcing fillers in an amount ranging between any of the values ​​mentioned above, for example, 0.1-5.0% by weight, or 1-4% by weight. The weight percentages are based on the total solids weight of the intumescent coating composition.

[0090] The intumescent coating composition of the present disclosure may further comprise a fibrous reinforcement. According to the present disclosure, the fibrous reinforcement may comprise mineral fibers, ceramic fibers, glass fibers, carbon fibers, basalt fibers, or mixtures thereof. The intumescent coating composition of the present disclosure may comprise, when present, fibrous reinforcement in an amount of 0.1% or more by weight, for example, 0.2% or more by weight, or 0.5% or more by weight, or 0.7% or more by weight, 1% or more by weight, or 1.5% or more by weight. The intumescent coating composition, if present, may comprise fibrous reinforcement in an amount of less than 5.0% or 5.0% by weight, such as less than 4.5% or 4.0% or 4.0% by weight, or less than 3.5% or 3.0% by weight, or less than 2.5% or 2.5% by weight. The intumescent coating composition, if present, may comprise fibrous reinforcement in an amount ranging between any of the values ​​mentioned above, such as 0.5-5.0% by weight, or 0.7-4.0% by weight, or 1.0-3.0% by weight. The weight percentages are based on the total solids weight of the intumescent coating composition.

[0091] The intumescent coating composition of the present disclosure may also contain various conventional additives, such as rheological additives, organic solvents, foam stabilizers, pigments, flame spread control agents, and the like. These components may be added in various amounts, as needed. Typically, when additional additives are used, they are present in a total amount of 1% or more by weight, such as 2% or more by weight, or 5% or more by weight, or 10% or more by weight. Additional additives, when present, may be present, for example, in an intumescent coating composition according to the present disclosure, in an amount of less than 20% or less by weight, such as 15% or less by weight, or 12% or less by weight. The intumescent coating composition may contain the optional additional additives in an amount ranging between any of the values ​​mentioned above, such as 1-20% by weight, such as 2-20% by weight, or 5-15% by weight. The weight percentages are based on the total solids weight of the intumescent coating composition.

[0092] The intumescent coating composition can be either a one component ("1K"), or a multi-component composition, e.g., two components ("2K") or more than two components. As used herein, a "1K composition" refers to a composition in which all coating components are maintained in the same container after manufacture, during storage, etc. A 1K composition can be applied to a substrate and cured by any conventional means, e.g., heating, forced air, etc. An intumescent coating composition can also be multi-component, which will be understood as a composition in which the various components are kept separate until just prior to application. For example, the composition can be packaged as a 2K system, with the film-forming resin in a first package (A) and the crosslinker in a second package (B), whereby all other components used in the coating composition can be used in any combination in either package (A) or package (B), or both, or some or all can be in one or more additional packages (C). The individual packages are mixed before using the intumescent composition. In particular, the intumescent coating composition can be a two-component ("2K") coating composition.

[0093] The expandable coating composition may be in the form of a thick material, such as a mastic. The composition is solvent-free and is particularly suitable for spray application. If desired, dilution may be accomplished with a variety of conventional solvents, such as xylene, methylene chloride, or 1,1,1-trichloroethane.

[0094] The intumescent coating composition may be applied by any means standard in the art, such as electrocoating, spray application, electrostatic spray application, including robotic application, dipping, rolling, brushing, and the like.

[0095] As mentioned above, in the method of the present disclosure, the expandable coating composition is cured by irradiating with pulsed infrared radiation. As used herein, the term "pulse" refers to radiation emitted in time-limited portions (pulses). The term "infrared radiation" refers to electromagnetic radiation having a wavelength in the range of 780 nm to 1 mm. Thus, the term "pulsed infrared radiation" refers to electromagnetic radiation having a wavelength in the infrared spectrum range that is irradiated in pulses. The pulses have a pulse duration at a pulse frequency.

[0096] The terms "cure", "cured", or similar terms, when used in connection with the intumescent coating compositions described herein, mean that at least a portion of the components forming the coating composition are cured to form a coating. Pulsed infrared radiation may be irradiated to the intumescent coating composition to form an at least partially cured intumescent coating or an at least partially cured intumescent film or sheet. As used herein, the term "at least partially cured" means that reaction of at least a portion of the reactive groups of the components of the intumescent coating composition occurs. In accordance with the present disclosure, pulsed infrared radiation may be irradiated to the intumescent coating composition to form a fully cured intumescent coating or a fully cured intumescent film or sheet. Full cure is achieved when further curing does not result in significant further improvement in the coating properties, for example, the hardness of the cured coating or cured self-supporting film or sheet. The hardness of the cured coating or cured self-supporting film or sheet may be determined by Shore hardness, such as by determining the Shore D hardness at room temperature using a Shore D durometer in the range of 40 to 90, or by determining the Shore A hardness at room temperature using a Shore A durometer of at least 50.

[0097] According to the present disclosure, the pulsed infrared radiation may be applied for a time period of less than 50 minutes, or less than 40 minutes, or less than 35 minutes, or less than 30 minutes, or less than 25 minutes, or less than 20 minutes, or less than 15 minutes, or less than 10 minutes to form a cured coating or a cured self-supporting film or sheet. According to the present disclosure, the pulsed infrared radiation may be applied for a time period of at least 2 minutes, or at least 4 minutes, or at least 5 minutes, or at least 6 minutes, or at least 8 ..., in a range between any of the values ​​mentioned above, for example, 2 minutes to 50 minutes, or 2 minutes to 35 minutes, or 2 minutes to 30 minutes, or 4 minutes to 25 minutes, or 5 minutes to 20 minutes, or 6 minutes to 15 minutes, or 8 minutes to 10 minutes to form a cured coating or a cured self-supporting film or sheet. Compared to curing the expanding coating composition in an oven, shorter curing times may be achieved, resulting in energy savings. The method further offers high efficiency since the infrared emitter is activated immediately after switching on without a long pre-heating period and only the desired partial area (e.g. the substrate on which the swellable coating composition is applied) is heated.

[0098] When using pulsed infrared radiation, the transfer of energy to the coating composition is not achieved primarily by thermal convection or conduction, but by non-visible electromagnetic waves in the infrared spectrum range at the speed of light, since electromagnetic waves propagate in the same manner and at the same speed as light waves. Infrared radiation penetrates the surface of the substrate quickly and effectively, ensuring rapid curing of the applied expandable coating composition or the formed self-supporting film or sheet. This allows the transfer of radiation with high energy density, thus allowing for energetically very efficient curing of the coating composition according to the present disclosure. Faster and more energy-efficient curing at low temperatures can be achieved.

[0099] According to the present disclosure, the surface temperature of the substrate during the application of the intumescent coating composition to form a cured intumescent coating can be less than 100°C, or less than 90°C. According to the present disclosure, the surface temperature of the substrate during the application of the intumescent coating composition to form a cured intumescent coating can be at least 60°C, for example at least 70°C. The surface temperature of the substrate during the application of the intumescent coating composition to form a cured intumescent coating can range from 60°C to 100°C, for example from 70°C to 90°C. The surface temperature of the substrate can be determined according to DIN EN 60584-1:2014.

[0100] The pulsed infrared radiation according to the present disclosure may have a peak wavelength of at least 3 μm. As used herein, the term "peak wavelength" refers to the maximum emission wavelength of the pulsed infrared radiation. The pulsed infrared radiation used in the method of the present disclosure may have a peak wavelength of 10 μm or less, for example, 6 μm or less, or 4 μm or less. The pulsed infrared radiation used in the method of the present application may range between any of the values ​​mentioned above, for example, 3 μm to 10 μm, or 3 μm to 6 μm, or 3 μm to 4 μm.

[0101] According to the present disclosure, pulse infrared radiation can be emitted with a pulse duration of at least 5 μs, for example, at least 8 μs, or at least 10 μs. As used herein, the term "pulse duration", also referred to as "pulse width", refers to the full width at half maximum (FWHM) amplitude of the pulse of pulse infrared radiation. Pulse infrared radiation can be emitted with a pulse duration of 100 μs or less, for example, 75 μs or less, or 50 μs or less, or 25 μs or less, or 15 μs or less, or 14 μs or less, or 12 μs or less. Pulsed infrared radiation according to the present disclosure may be irradiated with a pulse duration ranging between any of the values ​​mentioned above, for example, from 5 μs to 12 μs, or from 8 μs to 12 μs, or from 10 μs to 12 μs, or from 5 μs to 14 μs, or from 8 μs to 14 μs, or from 10 μs to 14 μs, or from 5 μs to 15 μs, or from 8 μs to 15 μs, or from 10 μs to 15 μs, or from 5 μs to 25 μs, or from 8 μs to 25 μs, or from 10 μs to 25 μs, or from 5 μs to 50 μs, or from 8 μs to 50 μs, or from 10 μs to 50 μs, or from 5 μs to 75 μs, or from 8 μs to 75 μs, or from 10 μs to 75 μs, or from 5 μs to 100 μs, or from 8 μs to 100 μs, or from 10 μs to 100 μs.

[0102] In particular, pulsed infrared radiation according to the present disclosure that is applied to form a cured coating or a cured self-supporting film or sheet can have a peak wavelength in the range of 3 μm to 10 μm, e.g., 3 μm to 6 μm, with a pulse duration of less than 100 μs, e.g., less than 25 μs, or less than 14 μs.

[0103] Pulsed infrared radiation according to the present disclosure may be irradiated at a pulse frequency of at least 350 Hz, for example, at least 370 Hz, or at least 390 Hz, or at least 400 Hz. As used herein, the term "pulse frequency" refers to the number of pulses per second of pulsed infrared radiation. Pulsed radiation according to the present disclosure may be irradiated at a pulse frequency of 450 Hz or less than 450 Hz, for example, 430 Hz. Pulsed infrared radiation may be irradiated at a pulse frequency in the range of 350 Hz to 450 Hz, for example, 350 Hz to 430 Hz, or 370 Hz to 450 Hz, or 370 Hz to 430 Hz, or 390 Hz to 450 Hz, or 390 Hz to 430 Hz, or 400 Hz to 450 Hz, or 400 Hz to 430 Hz. According to the present disclosure, pulsed infrared light may be irradiated at a pulse frequency ranging between any of the values ​​mentioned above, for example, from 350 Hz to 450 Hz, or from 370 Hz to 450 Hz, or from 390 Hz to 450 Hz, or from 400 Hz to 450 Hz.

[0104] Pulsed infrared radiation according to the present disclosure has a power of at least 250 W / cm 2 , e.g., at least 270 W / cm 2 , or at least 290 W / cm 2 As used herein, the term "impact energy" refers to the total radiant power of electromagnetic radiation received by a surface per unit area. Pulsed radiation according to the present disclosure can be irradiated with an impingement energy of 350 W / cm. 2 Or 350W / cm 2 Less than, for example, 330W / cm 2 Or 330W / cm 2 Less than or equal to 320W / cm 2 Or 320W / cm 2 Pulsed infrared radiation may be irradiated with impulse energies of less than 100 W / cm. Pulsed infrared radiation may range between any of the values ​​mentioned above, for example, 250 W / cm. 2 ~350W / cm 2 , or 250 W / cm 2 ~330W / cm 2 , or 250 W / cm 2 ~320W / cm 2, or 270 W / cm 2 ~350W / cm 2 , or 270 W / cm 2 ~330W / cm 2 , or 270 W / cm 2 ~320W / cm 2 , or 290 W / cm 2 ~350W / cm 2 , or 290 W / cm 2 ~330W / cm 2 , or 290 W / cm 2 ~320W / cm 2 The impact energy can be as high as 100 .mu.m.

[0105] According to the present disclosure, the pulsed infrared radiation can be provided by an infrared light source comprising a surface comprising a ceramic composition. The ceramic composition can be capable of absorbing heat and emitting pulsed infrared radiation, specifically having a peak wavelength in the range mentioned above. According to the present disclosure, the infrared light source can comprise a surface comprising a ceramic composition capable of absorbing heat and emitting pulsed infrared radiation. Preferably, the infrared light source can comprise a surface comprising a ceramic composition capable of absorbing heat and emitting pulsed infrared radiation in the range of 3 μm to 10 μm. The use of pulsed infrared radiation generated by the ceramic composition can provide a favorable effect on the curing of the intumescent coating composition according to the present disclosure.

[0106] For curing, the infrared radiation surface of the infrared light source may face the surface of the substrate on which the intumescent coating composition is applied or the surface of the self-supporting film or sheet on which the curing is performed. Herein, the distance between the infrared radiation surface of the infrared light source and the surface of the substrate on which the intumescent coating composition is applied or the surface of the self-supporting film or sheet on which the curing is performed may be at least 5 cm, for example, at least 10 cm, or at least 15 cm. Herein, the distance between the infrared radiation surface of the infrared light source and the surface of the substrate on which the intumescent coating composition is applied or the surface of the self-supporting film or sheet on which the curing is performed may be at or less than 50 cm, for example, at or less than 45 cm, or at or less than 40 cm, or at or less than 35 cm, or at or less than 30 cm, or at or less than 25 cm, or at or less than 20 cm, or at or less than 15 cm. The infrared emitting surface of the infrared light source may face the surface of the substrate onto which the curing expandable coating composition has been applied, or the surface of the self-supporting film or sheet, at a distance ranging between any of the values ​​mentioned above, for example, from 5 cm to 50 cm, or from 5 cm to 30 cm, or from 5 cm to 15 cm, or from 10 cm to 20 cm, or from 15 cm to 25 cm.

[0107] According to the present disclosure, the infrared light source may face the surface of the substrate on which the curing intumescent coating composition is applied, or the surface of the self-supporting film or sheet from at least one side. At least one or more infrared light sources of the present disclosure may surround the surface of the substrate on which the curing intumescent coating composition is applied, or the surface of the self-supporting film or sheet from at least one side. Suitable arrangements of infrared light sources are described, for example, in EP 1 690 842 A1 (particularly in paragraphs

[0044] to

[0049] ) and WO 2011 / 015164 (particularly in pages 12-13). The infrared light source according to the present disclosure may have any desired shape, for example, the shape of a rod, a tube, a flat plate or a curved plate.

[0108] The infrared light source may further include a heat source for directly or indirectly heating the ceramic composition. Heat transfer from the heat source may include various heat transfer methods, including radiation transfer, convection, contact transfer, or transfer via a thermally conductive material between the heat source and the ceramic composition. The infrared light source may further include a carrier material for heat absorption and / or transfer from the heat source to the ceramic composition. The carrier material may be one of the following materials: Fe, SiO 2 , 3Al 2 O 3 2SiO 2 , and / or 2Al 2 O 3 1SiO 2 (mullite), Al, or Cu. In addition, the infrared light source may include a reflector device. The ceramic composition may generate infrared light, and may radiate infrared light in undesired directions, among other things. The reflector device, which may include one or more reflectors, may be applied to reflect the infrared light radiated in undesired directions and redirect it to a specific area, for example, the surface of a substrate on which the coating composition to be cured is applied, or the surface of a self-supporting film or sheet to be cured.

[0109] The ceramic composition according to the present disclosure comprises: (a) (ai) a metal element selected from the group consisting of an alkaline earth element, a transition metal element, a lanthanide, and an actinide, and (a-ii) a metal oxide component containing oxygen; and (b) 3Al 2 O 3 2SiO 2 and / or 2Al 2 O 3 SiO 2 A preferable example of the metal oxide component (a) is Cr. 2 O 3 , ZrO 2 , Ho 2 O 3 , Fe 2 O 3 , LaCrO 3 , CEO 2 , Y 2 O 3, YCrO 3 , Gd 2 O 3 , MgAl 2 O 4 , MgCrO 4 , CaCrO 4 , YCrO 3 , CuO, La 2 O 3 , CuCrO 4 , and FeCrO 3 The ceramic composition may comprise a metal oxide component (a) and a remaining mullite component (b).

[0110] The ceramic composition may comprise at least 0.1 wt.%, such as at least 0.5 wt.%, such as at least 1.0 wt.%, such as at least 5.0 wt.%, of the metal oxide component (a) based on the total weight of the ceramic composition. The ceramic composition may comprise less than 70.0 wt.%, such as less than 60.0 wt.%, such as less than 50.0 wt.%, such as less than 40.0 wt.%, such as less than 30.0 wt.%, such as less than 20.0 wt.%, of the metal oxide component (a) based on the total weight of the ceramic composition. The ceramic composition may comprise 0.1 to 70.0 wt.%, or 0.5 to 70.0 wt.%, or 1.0 to 70.0 wt.%, or 5.0 to 70.0 wt.%, or 0.1 to 60.0 wt.%, or 0.5 to 60.0 wt.%, or 1.0 to 60.0 wt.%, or 5.0 to 60.0 wt.%, or 0.1 to 50.0 wt.%, or 0.5 to 50.0 wt.%, or 1.0 to 50.0 wt.%, or 5.0 to 50.0 wt.%, based on the total weight of the ceramic composition. %, or 0.1 to 40.0% by weight, or 0.5 to 40.0% by weight, or 1.0 to 40.0% by weight, or 5.0 to 40.0% by weight, or 0.1 to 30.0% by weight, or 0.5 to 30.0% by weight, or 1.0 to 30.0% by weight, or 5.0 to 30.0% by weight, or 0.1 to 20.0% by weight, or 0.5 to 20.0% by weight, or 1.0 to 20.0% by weight, or 5.0 to 20.0% by weight of the metal oxide component (a). According to the present disclosure, the ceramic composition may contain the metal oxide component (a) in the range of 0.1 to 70.0 wt %, for example, 0.5 to 60.0 wt %, for example, 0.5 to 50.0 wt %, for example, 1.0 to 40.0 wt %, for example, 1.0 to 30.0 wt %, for example, 5.0 to 20.0 wt %, based on the total weight of the ceramic composition.

[0111] The ceramic composition may comprise at least 30.0 wt.%, such as at least 40.0 wt.%, such as at least 50.0 wt.%, such as at least 60.0 wt.%, such as at least 70.0 wt.%, such as at least 80.0 wt.% of a mullite remainder component (b) based on the total weight of the ceramic composition. The ceramic composition may comprise at or less than 99.9 wt.%, at or less than 99.5 wt.%, such as at or less than 99.0 wt.%, such as at or less than 95.0 wt.% of a mullite remainder component (b) based on the total weight of the ceramic composition. The ceramic composition may comprise 30.0 to 99.9 wt.%, or 30.0 to 99.5 wt.%, or 30.0 to 99.0 wt.%, or 30.0 to 95.0 wt.%, or 40.0 to 99.9 wt.%, or 40.0 to 99.5 wt.%, or 40.0 to 99.0 wt.%, or 40.0 to 95.0 wt.%, or 50.0 to 99.9 wt.%, or 50.0 to 99.5 wt.%, or 50.0 to 99.0 wt.%, or 50.0 to 95.0 wt.%, based on the total weight of the ceramic composition. %, or 60.0 to 99.9 wt%, or 60.0 to 99.5 wt%, or 60.0 to 99.0 wt%, or 60.0 to 95.0 wt%, or 70.0 to 99.9 wt%, or 70.0 to 99.5 wt%, or 70.0 to 99.0 wt%, or 70.0 to 95.0 wt%, or 80.0 to 99.9 wt%, or 80.0 to 99.5 wt%, or 80.0 to 99.0 wt%, or 80.0 to 95.0 wt%. According to the present disclosure, the ceramic composition may comprise a mullite remainder component (b) in the range of 30.0 to 99.9 wt%, or 40.0 to 99.9 wt%, or 50.0 to 99.5 wt%, or 60.0 to 99.0 wt%, or 70.0 to 95.0 wt%, or 80.0 to 95.0 wt%, based on the total weight of the ceramic composition.

[0112] The ceramic composition may be processed by standard ceramic processing procedures known to those skilled in the art. The ceramic composition according to the present disclosure may be ground to a fine powder by conventional grinding procedures, e.g., arc grinding, mixed until homogeneity is achieved, and melted, typically at a temperature of 2.600°C. Melting may be carried out in an oxidizing atmosphere, e.g., air. The resulting molten material may be ground to a particle size, e.g., in the range of 100-250 μm, and the powder may then be formed into a desired shape. Suitable procedures for processing the ceramic composition are disclosed, for example, in WO 99 / 01401 A1. The process of forming the ceramic composition may include high pressure processing of the ceramic composition using a press and shaping the formed body of the object produced from the ceramic composition. The process of forming the ceramic composition into an object may further include further temperature treatments, e.g., sintering processes, and further pressure processes as required. Shaping the ceramic composition to form any object may include standard forming procedures, e.g., mechanical processing, powder processing, or ceramic injection molding. Thus, the ceramic composition may be formed into almost any shape by standard ceramic forming procedures.

[0113] According to the present disclosure, the intumescent coating composition or the cured self-supporting film or sheet may be applied to any substrate known in the art, such as automotive substrates, marine substrates, industrial substrates, heavy equipment, packaging substrates, lumber, wood flooring and furniture, apparel, electronics including housings and circuit boards, including consumer electronics such as housings for computers, notebooks, smartphones, tablets, televisions, gaming devices, computer equipment, computer accessories, MP3 players, etc., glass and transparencies, sporting goods such as golf balls, etc. The substrate to which the intumescent coating composition is applied may comprise a material selected from metal, plastic, ceramic, glass, wood, paper, paperboard, rubber, leather, textiles, existing coatings, or mixtures thereof.

[0114] The substrate may be part of a structure or part of a vehicle. As used herein, "structure" refers to buildings, bridges, transportation infrastructure, oil rigs, oil platforms, water towers, power transmission towers, support structures, wind turbines, walls, piers, docks, dikes, dams, shipping containers, trailers, battery components, batteries, and any part of any metal structure exposed to a corrosive environment. As used herein, "vehicle" refers in its broadest sense to all types of vehicles, including, but not limited to, cars, trucks, buses, tractors, harvesters, heavy equipment, vans, golf carts, motorcycles, bicycles, rail cars, subway cars, airplanes, helicopters, boats of all sizes, and the like. The substrate may be part of a battery or part of a battery component.

[0115] The present disclosure further relates to substrates coated according to the methods of the present disclosure.

[0116] Additionally, the present disclosure is directed to articles comprising a substrate coated according to the methods of the present disclosure.

[0117] The article according to the present disclosure may include a battery or a battery component. The battery may be, for example, an electric vehicle battery. According to the present invention, the battery may be a lithium ion battery. As used herein, the term "battery component" refers to any component found in a battery, for example, a lithium ion battery. According to the present disclosure, the battery component may be an electric vehicle battery component. The battery component may include an electrode, a battery cell, a battery shell, a battery module, a battery pack, a battery box, a battery cell casing, a pack shell, a battery lid, a battery tray, a thermal management system, a battery housing, a module housing, a module track, a battery side plate, a battery cell enclosure, a cooling module, a cooling tube, a cooling fin, a cooling plate, a bus bar, a battery frame, an electrical connection, a metal wire, a copper or aluminum conductor or cable, or any combination thereof.

[0118] The battery may include an exterior wall element defining a housing, and optionally an interior wall element, and the expandable coating composition or self-supporting film or sheet is applied at least partially to the exterior and / or interior of any of the exterior wall elements, and / or to any side of any of the interior wall elements, if present. The exterior and / or interior wall elements may include composites, steel, aluminum, polycarbonate, or combinations thereof.

[0119] The battery, particularly the lithium ion battery, may be a battery pack including a plurality of individual battery cells, and the intumescent coating composition or the self-supporting film or sheet is positioned to insulate at least two of the individual battery cells from each other in an inflated state, and optionally in a charred state, such as between two battery cells. The battery may further include one or more additional flame retardant materials and / or fire mitigation means, such as within and / or around the battery. For example, one or more additional flame retardant materials and / or fire mitigation means may be wrapped or otherwise positioned between the battery cells, or around or inside the battery housing. Suitable examples of flame retardant materials and / or fire mitigation means include glass fiber, mineral wool, silica, silica fiber, alumina, Kevlar, Nomex, calcium silicate, calcium silicate fiber, or combinations thereof, examples of which may be, for example, a sheet or other self-supporting form. Foams, such as polyurethane / polyurea foams with flame retardants, may also be used. Physical barriers, such as cooling fins between the battery cells, mica boards, aerogel blankets, mineral / glass / carbon fiber-containing blankets, or combinations thereof, may also be used.

[0120] The article according to the present disclosure can be a battery or a battery component.

[0121] It is also within the scope of the present invention to apply a coating composition or a self-supporting film or sheet to a portion of the article adjacent to the battery between the battery and the article to provide fire protection to the article and its user that includes the battery, thereby insulating the article from the battery. In such cases, a conventional battery or a battery according to the present disclosure may be used. The article may be, for example, a mobile phone, a tablet, or a laptop computer.

[0122] Alternatively, the article may include a vehicle, such as a hybrid or electric car, a bus, or a truck. In such vehicles, it is common to position the battery, particularly the lithium ion battery, as a flat battery pack under the vehicle body, such as the floor portion of the vehicle body, due to the weight of the battery. In such a case, the intumescent coating or the self-supporting film or sheet may be applied to the vehicle floor portion adjacent to the battery between the battery and the vehicle body. Thereby, in the event of a thermal runaway of the battery or a battery fire, the vehicle body, particularly the passenger cabin, is protected by the hardened intumescent coating or the self-supporting film or sheet so that the fire does not spread to the passenger cabin, and the temperature rise of the passenger cabin is limited for an extended period of time so that the passengers have enough time to safely escape the vehicle in the event of such an event. Alternatively, the article may include a structure.

[0123] Further, the present disclosure relates to the use of an intumescent coating composition according to the present disclosure in a method for curing an intumescent coating composition by irradiating the composition with pulsed infrared radiation. The present disclosure further relates to the use of pulsed infrared radiation in a method for curing an intumescent coating composition.

[0124] As used herein, unless expressly specified otherwise, all numbers, such as those expressing values, ranges, amounts, or percentages, can be read as if preceded by the word "about" even if the term does not expressly appear.

[0125] The following examples are intended to illustrate the present disclosure and should not be construed as limiting the disclosure in any way. [Brief description of the drawings]

[0126] [Figure 1] 1 shows an intumescent coating cured using pulsed infrared radiation at 50% power from 20 cm for 14 minutes (a), 100% power from 30 cm for 7 minutes (b), and oven heating at 90° C. for 25 minutes (c). [Diagram 2] Figure 1 shows char formation after 5 minutes at 1200°C for intumescent coatings cured for 10 days (a) using oven heating at 90°C for 120 minutes, (b) using pulsed infrared at 50% power for 30 minutes from 20 cm distance, (c) using pulsed infrared at 100% power for 20 minutes from 30 cm distance, and (d) at room temperature. EXAMPLES

[0127] Preparation of Expandable Coating Composition Coating formulations were prepared using the components shown in Table 1 (base formulation) and Table 2 (hardener formulation). [Table 1] [Table 2]

[0128] The base for the formulation was prepared by dispersing all the components in a disperser equipped with a Brook Crompton motor of 0.75-1 kW, at a rotation speed of 2000-3000 rpm, and a dispersion plate diameter of 80-90 mm, until the size of the particles in the formulation was less than 100 microns. The hardener for the coating formulation was prepared by dispersing all the components in a disperser equipped with a Brook Crompton motor of 0.75-1 kW, at a rotation speed of 2000-3000 rpm, and a dispersion plate diameter of 80-90 mm, until the size of the particles in the formulation was less than 100 microns. Just before application, the base and hardener were mixed in the relative amounts shown in Tables 1 and 2. The base and hardener were mixed by mixer or spatula until the mixture was homogenous in color and free of lumps. The coating formulation was applied onto 150x75x1.2 mm aluminum panels using airless spray application.

[0129] Curing coated substrates using pulsed infrared and conventional curing The substrates coated with the intumescent coating compositions shown above were cured using a pulsed infrared light source IR.X Infrarot Modul D2 available from SPS Group GmbH (Germany). The following settings of the pulsed infrared light source were applied, as shown in Table 3: [Table 3]

[0130] The pulsed infrared light source faced the substrate on which the coating composition was applied to be cured at various distances, as shown in Table 4. The light source IR.X Infrarot Modul D2 has a power of 2000 W when 100% power is applied. Therefore, 50% power represents a power of 1000 W. [Table 4]

[0131] Cure time refers to the time to achieve a cured coating that is dry enough to handle. Dry enough to handle means that the coated surface or film, when subjected to typical handling pressures, does not show undesirable marks, peeling, loosening, wrinkling, or other forms of distortion and can be determined by a Shore A hardness tester, whose value must be greater than 55. Thickness was determined according to DIN EN ISO 2178:2016.

[0132] Conventional curing is accomplished using heated air in an oven at 90°C for 30 minutes, after which the coating is dry enough to handle. Cure times were significantly longer to achieve a cured coating.

[0133] Fire testing of cured intumescent coatings Coatings applied on 150x75x1.2mm aluminum panels and cured by pulsed infrared radiation as well as oven cured and cured at room temperature (approximately 25°C) were subjected to a 10 minute test against a torch power of 1200±50°C. The temperature of the backside of the aluminum panel was monitored. Additionally, the coefficient of expansion was determined, which indicates the ratio between the char thickness before the fire test and the cured coating. The results are summarized in Table 5 below. [Table 5]

[0134] As can be seen from the results above, curing using pulsed infrared radiation results in similar fire performance of the intumescent coating compared to conventionally cured intumescent coatings. Cure times can be significantly reduced while maintaining the fire performance of the cured coating.

Claims

1. 1. A method for imparting fire resistance to a substrate, comprising the steps of: (I) (i) applying an expandable coating composition to a portion of a surface of the substrate, or (ii) forming the expandable coating composition into a self-supporting film or sheet; (II) irradiating (i) the applied intumescent coating composition or (ii) the self-supporting film or sheet with pulsed infrared light to form a cured intumescent coating or a cured self-supporting film or sheet, and applying the self-supporting film or sheet to a portion of a surface of the substrate.

2. The expandable coating composition comprises: (a) a film-forming resin; (b) a crosslinking agent; and (c) a compound that provides an expansion gas upon pyrolysis.

3. 3. The method of claim 2, wherein the film-forming resin (a) comprises an epoxy resin, an acrylic resin, a polyurethane resin, a polyvinyl resin, a urea-formaldehyde resin, a polyimide resin, a melamine resin, a polyester resin, a cyanate resin, copolymers thereof, or mixtures thereof.

4. The method of claim 2 or 3, wherein the film-forming resin (a) comprises an epoxy resin.

5. The method of any one of claims 2 to 4, wherein the crosslinking agent (b) comprises a polyamine, such as a polyetheramine, a polyamide, a polyepoxide, an aminoplast resin, a phenolic resin, a polyisocyanate, a polythiol, a polyol, a copolymer thereof, or a mixture thereof.

6. The method of any one of claims 2 to 5, wherein the cross-linking agent (b) comprises a polyamine.

7. 7. The method of any one of claims 2 to 6, wherein the compound (c) which provides an expanding gas upon pyrolysis comprises melamine, a melamine derivative, guanidine, methylol melamine, hexamethoxymethyl melamine, urea, dimethyl urea, melamine pyrophosphate, dicyandiamide, guanylurea phosphate, glycine, an alkaline earth metal carbonate, calcium hydroxide, magnesium dihydroxide, aluminum trihydroxide, expandable graphite, or a mixture thereof.

8. 8. The method of claim 2, wherein the compound (c) that provides an expanding gas upon pyrolysis comprises melamine, a melamine derivative, a methylol melamine, a hexamethoxymethyl melamine, a melamine pyrophosphate, or a mixture thereof.

9. 10. The method of any one of the preceding claims, wherein the expandable coating composition comprises an epoxy reactive diluent.

10. 10. The method of claim 9, wherein the epoxy reactive diluent comprises a diglycidyl ether of an aliphatic alcohol.

11. 10. The method of any one of the preceding claims, wherein the expandable coating composition comprises a phosphate compound.

12. 12. The method of claim 11, wherein the phosphate compounds include phosphoric acid, mono- and di-ammonium phosphate, triphenyl phosphate, tris-(2-chloroethyl) phosphate, tris-(2-chloroisopropyl) phosphate, ammonium polyphosphate, melamine pyrophosphate.

13. 13. The method of any one of the preceding claims, wherein the expandable coating composition comprises a borate compound.

14. 14. The method of claim 13, wherein the borate compound comprises ammonium pentaborate, boric acid, metal borates, boron oxide, sodium borate, potassium borate, ammonium borate, butyl borate, phenyl borate, or mixtures thereof.

15. 10. The method of any one of the preceding claims, wherein the expandable coating composition comprises an aluminum compound.

16. 16. The method of claim 15, wherein the aluminum compound comprises aluminum hydroxide, aluminum oxide, aluminum chloride, or a mixture thereof.

17. 10. The method of any one of the preceding claims, wherein the expandable coating composition comprises a silica compound.

18. 18. The method of claim 17, wherein the silica compound comprises fumed silica, quartz, or a mixture thereof.

19. The expandable coating composition comprises TiO 2 13. A method according to any one of the preceding claims, comprising:

20. 10. The method of any one of the preceding claims, wherein the intumescent coating composition comprises a fibrous reinforcement.

21. 21. The method of claim 20, wherein the fibrous reinforcement comprises mineral fibers, ceramic fibers, glass fibers, carbon fibers, basalt fibers, or mixtures thereof.

22. 13. The method of any one of the preceding claims, wherein the intumescent coating composition is applied to the substrate at a dry film thickness in the range of 0.1 mm to 15 mm, or the intumescent coating composition is formed into a self-supporting film or sheet having a dry film thickness in the range of 0.1 mm to 15 mm.

23. 10. A method according to any one of the preceding claims, wherein the pulsed infrared radiation has a peak wavelength in the range of 3 μm to 10 μm, for example 3 μm to 6 μm.

24. 10. The method of any one of the preceding claims, wherein the pulsed infrared radiation is applied with a pulse duration of less than 100 μs.

25. 10. A method according to any one of the preceding claims, wherein the pulsed infrared radiation is applied with a pulse duration in the range of 5 μs to 15 μs, such as 8 μs to 12 μs, or 10 μs to 14 μs.

26. 10. The method according to any one of the preceding claims, wherein the pulsed infrared radiation is applied at a pulse frequency of 350Hz to 450Hz, or 400Hz to 450Hz.

27. The pulsed infrared ray is 250 W / cm 2 ~350 W / cm 2 4. The method according to any one of the preceding claims, wherein the target is irradiated with an impact energy of

28. 10. The method of any one of the preceding claims, wherein the pulsed infrared radiation is applied for a period of less than 25 minutes, or less than 20 minutes, or less than 15 minutes, or less than 10 minutes to form a cured coating or a cured self-supporting film or sheet.

29. 2. The method of any one of the preceding claims, wherein the surface temperature of the substrate in (II) is less than 100°C, or less than 90°C.

30. 13. The method according to any one of the preceding claims, wherein the pulsed infrared emitting surface of the infrared light source in (II) faces the surface of the substrate onto which the coating composition to be cured has been applied, or the surface of the self-supporting film or sheet to be cured, at a distance of from 5 cm to 50 cm, such as from 5 cm to 30 cm, or from 5 cm to 15 cm, or from 10 cm to 20 cm, or from 15 cm to 25 cm.

31. 10. The method of any one of the preceding claims, wherein the pulsed infrared radiation is provided by an infrared light source comprising a surface comprising a ceramic composition capable of absorbing heat and emitting infrared radiation having a peak wavelength in the range of 3 μm to 10 μm.

32. 10. The method of any one of the preceding claims, wherein the portion of the surface of the substrate to which the coating composition or the self-supporting film or sheet is applied comprises a material selected from metal, plastic, ceramic, glass, wood, paper, paperboard, rubber, leather, textiles, existing coatings, or mixtures thereof.

33. Use of an intumescent coating composition in a method for curing the intumescent coating composition by irradiating it with pulsed infrared radiation.

34. Use of pulsed infrared radiation in a method for curing an intumescent coating composition.

35. A substrate coated according to the method of any one of claims 1 to 32.

36. 36. An article comprising the substrate of claim 35.

37. 37. The article of claim 36, wherein the article comprises a battery or a battery component.

38. 38. The article of claim 37, wherein the battery is a lithium ion battery.

39. 40. The article of claim 37 or 38, wherein the battery comprises an electric vehicle battery or an electric vehicle battery component.

40. 40. The article of any one of claims 37 to 39, wherein the battery comprises an outer wall element defining a housing and, optionally, an inner wall element, and wherein the expandable coating composition or self-supporting film or sheet is applied at least partially to the outside and / or the inside of any of the outer wall elements and / or to any side of any of the inner wall elements, if present.

41. 41. The article of claim 40, wherein any of the exterior and / or interior wall elements comprise composite, steel, aluminum, polycarbonate, or combinations thereof.

42. 42. The article of any one of claims 37-41, wherein the battery is a battery pack including a plurality of individual battery cells, and the coating composition or self-supporting film or sheet is positioned to insulate at least two of the individual battery cells from each other in an expanded and optionally charred state, and the battery optionally includes one or more additional flame retardant materials and / or fire mitigation means.

43. 40. The article of any one of claims 37-39, wherein the battery component comprises an electrode, a battery cell, a battery shell, a battery module, a battery pack, a battery box, a battery cell casing, a pack shell, a battery lid, a battery tray, a thermal management system, a battery housing, a module housing, a module track, a battery side plate, a battery cell enclosure, a cooling module, a cooling tube, a cooling fin, a cooling plate, a bus bar, a battery frame, an electrical connection, a metal wire, a copper or aluminum conductor or cable, or any combination thereof.

44. 37. The method of claim 36, wherein the article comprises a vehicle.

45. The method of claim 36 , wherein the article comprises a structure.

Citation Information

Patent Citations

  • Flame retardant powder coating for MDF (medium density fireboard) as well as preparation method and application of flame retardant powder coating

    CN104893501A

  • Intumescent coating composition

    JP2018515645A

  • Curable film-forming compositions containing photothermally active materials, coated metal substrates and methods of coating substrates

    JP2018520223A

  • Pulsed heating process for curing substrates with near infrared radiation

    US20050255238A1

  • Battery comprising an intumescent layer

    WO2020047059A1